WO2020085310A1 - 液晶化合物配向層転写用フィルム - Google Patents
液晶化合物配向層転写用フィルム Download PDFInfo
- Publication number
- WO2020085310A1 WO2020085310A1 PCT/JP2019/041326 JP2019041326W WO2020085310A1 WO 2020085310 A1 WO2020085310 A1 WO 2020085310A1 JP 2019041326 W JP2019041326 W JP 2019041326W WO 2020085310 A1 WO2020085310 A1 WO 2020085310A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- layer
- film
- liquid crystal
- crystal compound
- transfer film
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- G—PHYSICS
- G02—OPTICS
- G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
- G02B5/00—Optical elements other than lenses
- G02B5/30—Polarising elements
- G02B5/3016—Polarising elements involving passive liquid crystal elements
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B29—WORKING OF PLASTICS; WORKING OF SUBSTANCES IN A PLASTIC STATE IN GENERAL
- B29C—SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING
- B29C55/00—Shaping by stretching, e.g. drawing through a die; Apparatus therefor
- B29C55/02—Shaping by stretching, e.g. drawing through a die; Apparatus therefor of plates or sheets
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B23/00—Layered products comprising a layer of cellulosic plastic substances, i.e. substances obtained by chemical modification of cellulose, e.g. cellulose ethers, cellulose esters, viscose
- B32B23/04—Layered products comprising a layer of cellulosic plastic substances, i.e. substances obtained by chemical modification of cellulose, e.g. cellulose ethers, cellulose esters, viscose comprising such cellulosic plastic substance as the main or only constituent of a layer, which is next to another layer of the same or of a different material
- B32B23/08—Layered products comprising a layer of cellulosic plastic substances, i.e. substances obtained by chemical modification of cellulose, e.g. cellulose ethers, cellulose esters, viscose comprising such cellulosic plastic substance as the main or only constituent of a layer, which is next to another layer of the same or of a different material of synthetic resin
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B27/00—Layered products comprising a layer of synthetic resin
- B32B27/28—Layered products comprising a layer of synthetic resin comprising synthetic resins not wholly covered by any one of the sub-groups B32B27/30 - B32B27/42
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B27/00—Layered products comprising a layer of synthetic resin
- B32B27/32—Layered products comprising a layer of synthetic resin comprising polyolefins
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B27/00—Layered products comprising a layer of synthetic resin
- B32B27/36—Layered products comprising a layer of synthetic resin comprising polyesters
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B7/00—Layered products characterised by the relation between layers; Layered products characterised by the relative orientation of features between layers, or by the relative values of a measurable parameter between layers, i.e. products comprising layers having different physical, chemical or physicochemical properties; Layered products characterised by the interconnection of layers
- B32B7/02—Physical, chemical or physicochemical properties
- B32B7/023—Optical properties
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B7/00—Layered products characterised by the relation between layers; Layered products characterised by the relative orientation of features between layers, or by the relative values of a measurable parameter between layers, i.e. products comprising layers having different physical, chemical or physicochemical properties; Layered products characterised by the interconnection of layers
- B32B7/04—Interconnection of layers
- B32B7/12—Interconnection of layers using interposed adhesives or interposed materials with bonding properties
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J5/00—Manufacture of articles or shaped materials containing macromolecular substances
- C08J5/18—Manufacture of films or sheets
-
- G—PHYSICS
- G01—MEASURING; TESTING
- G01M—TESTING STATIC OR DYNAMIC BALANCE OF MACHINES OR STRUCTURES; TESTING OF STRUCTURES OR APPARATUS, NOT OTHERWISE PROVIDED FOR
- G01M11/00—Testing of optical apparatus; Testing structures by optical methods not otherwise provided for
-
- G—PHYSICS
- G01—MEASURING; TESTING
- G01N—INVESTIGATING OR ANALYSING MATERIALS BY DETERMINING THEIR CHEMICAL OR PHYSICAL PROPERTIES
- G01N21/00—Investigating or analysing materials by the use of optical means, i.e. using sub-millimetre waves, infrared, visible or ultraviolet light
- G01N21/84—Systems specially adapted for particular applications
- G01N21/88—Investigating the presence of flaws or contamination
-
- G—PHYSICS
- G02—OPTICS
- G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
- G02B1/00—Optical elements characterised by the material of which they are made; Optical coatings for optical elements
- G02B1/08—Optical elements characterised by the material of which they are made; Optical coatings for optical elements made of polarising materials
-
- G—PHYSICS
- G02—OPTICS
- G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
- G02B5/00—Optical elements other than lenses
- G02B5/30—Polarising elements
-
- G—PHYSICS
- G02—OPTICS
- G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
- G02B5/00—Optical elements other than lenses
- G02B5/30—Polarising elements
- G02B5/3083—Birefringent or phase retarding elements
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B29—WORKING OF PLASTICS; WORKING OF SUBSTANCES IN A PLASTIC STATE IN GENERAL
- B29C—SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING
- B29C48/00—Extrusion moulding, i.e. expressing the moulding material through a die or nozzle which imparts the desired form; Apparatus therefor
- B29C48/03—Extrusion moulding, i.e. expressing the moulding material through a die or nozzle which imparts the desired form; Apparatus therefor characterised by the shape of the extruded material at extrusion
- B29C48/07—Flat, e.g. panels
- B29C48/08—Flat, e.g. panels flexible, e.g. films
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B32—LAYERED PRODUCTS
- B32B—LAYERED PRODUCTS, i.e. PRODUCTS BUILT-UP OF STRATA OF FLAT OR NON-FLAT, e.g. CELLULAR OR HONEYCOMB, FORM
- B32B2307/00—Properties of the layers or laminate
- B32B2307/40—Properties of the layers or laminate having particular optical properties
- B32B2307/42—Polarizing, birefringent, filtering
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J2301/00—Characterised by the use of cellulose, modified cellulose or cellulose derivatives
- C08J2301/02—Cellulose; Modified cellulose
Definitions
- the present invention relates to a transfer film for transferring a liquid crystal compound alignment layer. More specifically, when manufacturing a polarizing plate or a retardation plate such as a circularly polarizing plate in which a retardation layer composed of a liquid crystal compound alignment layer is laminated, or when manufacturing a polarizing plate having a polarizing layer composed of a liquid crystal compound alignment layer.
- the present invention relates to a transfer film for transferring a liquid crystal compound alignment layer.
- a circularly polarizing plate is arranged on the viewer-side panel surface of the image display panel in order to reduce reflection of extraneous light.
- This circularly polarizing plate is composed of a laminated body of a linearly polarizing plate and a retardation film such as ⁇ / 4, and converts external light traveling toward the panel surface of the image display panel into linearly polarized light by the linearly polarizing plate, and then ⁇ / It is converted into circularly polarized light by a retardation film such as 4.
- Circularly polarized extraneous light reverses the direction of rotation of the polarization plane when reflected on the surface of the image display panel, and this reflected light is conversely shielded by a linear polarizing plate by a retardation film such as ⁇ / 4. Since the light is converted into linearly polarized light in the direction indicated by the arrow and is then shielded by the linearly polarizing plate, it is possible to suppress the emission to the outside.
- the circularly polarizing plate is formed by laminating a retardation film such as ⁇ / 4 on the polarizing plate.
- a single retardation film such as a cyclic olefin (see Patent Document 1), polycarbonate (see Patent Document 2), or a stretched film of triacetyl cellulose (see Patent Document 3) is used.
- a retardation film of a laminate having a retardation layer made of a liquid crystal compound on a transparent film see Patent Documents 4 and 5) is used. It is described above that the liquid crystal compound may be transferred when the retardation layer (liquid crystal compound alignment layer) made of the liquid crystal compound is provided.
- Patent Document 6 a method for producing a retardation film by transferring a retardation layer made of a liquid crystal compound to a transparent film is known from Patent Document 6 and the like.
- Patent Documents 7 and 8 a method of forming a ⁇ / 4 film by providing a retardation layer made of a liquid crystal compound such as ⁇ / 4 on a transparent film by such a transfer method.
- the cyclic polyolefin film is preferable because it has no refractive index anisotropy, and thus the state of the retardation layer can be inspected (evaluated) in the state where the retardation layer is provided on the film substrate.
- a method for producing a polarizing plate by transferring a polarizing layer (liquid crystal compound alignment layer) containing a liquid crystal compound and a dichroic dye laminated on a transfer film to a protective film is also known.
- a polarizing layer liquid crystal compound alignment layer
- a dichroic dye laminated on a transfer film to a protective film.
- the present invention has been made against the background of such problems of the conventional technology. That is, the object of the present invention is a cyclic polyolefin-based transfer film for transferring a liquid crystal compound alignment layer, in which the occurrence of defects such as pinholes is reduced and a retardation layer or a polarizing layer (liquid crystal compound alignment layer). It is intended to provide a transfer film capable of forming a film.
- the present inventor has a drawback such as a pinhole in a retardation layer laminated polarizing plate (circular polarizing plate) manufactured by using a cyclic polyolefin film as a film substrate for transfer.
- a drawback such as a pinhole in a retardation layer laminated polarizing plate (circular polarizing plate) manufactured by using a cyclic polyolefin film as a film substrate for transfer.
- the microstructure on the surface of the film substrate greatly affects the alignment state and the retardation of the liquid crystal compound in the retardation layer made of the liquid crystal compound formed on the film substrate, and the alignment state as designed. It has been found that, in some cases, a phase difference cannot be obtained, which causes defects such as pinholes.
- the present inventor pays attention to the surface roughness of the film base material represented by specific parameters among these microstructures, and uses the film base material whose surface roughness is controlled within a specific range.
- a retardation layer or a polarizing layer liquid crystal compound alignment layer
- the present invention has the following configurations (1) to (4).
- a film for transferring a liquid crystal compound alignment layer. (2) The film for transferring a liquid crystal compound alignment layer according to (1), wherein the release surface of the transfer film has a 10-point surface roughness (SRz) of 5 nm or more and 200 nm or less.
- a liquid crystal compound alignment layer comprising a laminate of a liquid crystal compound alignment layer and a transfer film, wherein the transfer film is the transfer film according to (1) or (2). Transfer laminate.
- the liquid crystal compound in the retardation layer or the polarizing layer is It is possible to form the retardation layer and the polarizing layer (liquid crystal compound orientation layer) in which the orientation state and the retardation can be made as designed and the occurrence of defects such as pinholes is reduced.
- the transfer film of the present invention is for transferring the liquid crystal compound alignment layer to an object (other transparent resin film, polarizing plate, etc.), and has a surface roughness (SRa) of the release surface of the transfer film. It is characterized by being 1 nm or more and 30 nm or less.
- the transfer film may be a single film, or a release film may be provided on the film serving as a base material by coating or the like. Further, an antistatic layer, a slipping layer or the like may be provided on the back surface.
- a transfer film those used as a transfer film alone without using a layer such as a release coat, and those used as a transfer film by providing a release coat or a back coat are collectively referred to as a transfer film.
- the film in the state before the coating is provided is called the base film.
- the resin constituting the film substrate used in the transfer film of the present invention is a cyclic polyolefin type resin.
- the cyclic polyolefin is a compound containing an alicyclic structure in the repeating unit of the polymer. Examples of the alicyclic structure include a cycloalkane structure and a cycloalkene structure, and the cycloalkane structure is preferable from the viewpoint of transparency.
- the proportion of repeating units having an alicyclic structure in the cyclic polyolefin may be appropriately selected according to the purpose of use, but is usually 50% by weight or more, preferably 70% by weight or more, more preferably 90% by weight or more. .
- Preferred cyclic polyolefins include norbornene-based polymers, and hydrogenated norbornene-based polymers are particularly preferred. As these, those used as an optical film can be used as a suitable example.
- the transfer film of the present invention may have a single-layer structure or a multi-layer structure by co-extrusion.
- it may have a multilayer structure of four or more layers.
- Transfer film is industrially supplied by a roll that winds the film.
- the lower limit of the roll width is preferably 30 cm, more preferably 50 cm, further preferably 70 cm, particularly preferably 90 cm, and most preferably 100 cm.
- the upper limit of the roll width is preferably 5000 cm, more preferably 4000 cm, and further preferably 3000 cm.
- the lower limit of the roll length is preferably 100 m, more preferably 500 m, even more preferably 1000 m.
- the upper limit of the roll length is preferably 100,000 m, more preferably 50,000 m, and further preferably 30,000 m.
- the release surface (A layer surface) of the transfer film of the present invention is preferably smooth.
- the “release surface” of the transfer film means the surface of the transfer film intended to be provided with the liquid crystal compound alignment layer to be transferred by the transfer film.
- the surface of these flattening layer or release layer (contact with the liquid crystal compound alignment layer) Surface) is the "release surface" of the transfer film.
- the lower limit of the three-dimensional arithmetic mean roughness (SRa) of the release surface of the transfer film of the present invention is preferably 1 nm, more preferably 2 nm. If it is less than the above, it may be difficult to achieve the numerical value.
- the upper limit of SRa of the release surface of the transfer film of the present invention is preferably 30 nm, more preferably 25 nm, further preferably 20 nm, particularly preferably 15 nm, most preferably 10 nm. . If it exceeds the above range, the alignment of the liquid crystal compound may be disturbed.
- the lower limit of the three-dimensional ten-point average roughness (SRz) of the release surface of the transfer film of the present invention is preferably 5 nm, more preferably 10 nm, and further preferably 13 nm. If it is less than the above, it may be difficult to achieve the numerical value.
- the upper limit of SRz of the release surface of the transfer film of the present invention is preferably 200 nm, more preferably 150 nm, further preferably 120 nm, particularly preferably 100 nm, and most preferably 80 nm. . If it exceeds the above range, the alignment of the liquid crystal compound may be disturbed.
- the lower limit of the maximum height of the release surface (SRy: maximum release surface peak height SRp + release surface maximum valley depth SRv) of the transfer film of the present invention is preferably 10 nm, more preferably 15 nm, and It is preferably 20 nm. If it is less than the above, it may be difficult to achieve the numerical value.
- the upper limit of SRy of the release surface of the transfer film of the present invention is preferably 300 nm, more preferably 250 nm, further preferably 150 nm, particularly preferably 120 nm, most preferably 100 nm. . If it exceeds the above range, the alignment of the liquid crystal compound may be disturbed.
- the upper limit of the number of projections having a height difference of 0.5 ⁇ m or more on the release surface of the transfer film of the present invention is preferably 5 / m 2 , more preferably 4 / m 2 , and further preferably 3 / M 2 , particularly preferably 2 / m 2 , and most preferably 1 / m 2 . If it exceeds the above range, the alignment of the liquid crystal compound may be disturbed.
- an alignment control layer such as a rubbing alignment control layer or a photo alignment control layer can be provided between the transfer film and the liquid crystal compound alignment layer.
- the control layer it is considered that the orientation control layer of the convex portion is peeled off during rubbing, and the rubbing of the foot portion and the concave portion of the convex portion is insufficient, which causes the defects.
- the thickness of the liquid crystal compound alignment layer may be formed at the convex portion of the release surface of the transfer film when the liquid crystal compound is applied. It is also a cause of the defect that the retardation as designed cannot be obtained because the thickness of the liquid crystal compound alignment layer becomes thicker in the concave portion of the release surface of the transfer film. Conceivable.
- the release surface side layer (surface layer) of the base film does not contain particles. -If the release surface side layer (surface layer) of the base film contains particles, the particles have a small particle size. ⁇ Smooth the surface of the roll (casting roll or touch roll) on the side that becomes the release surface. -Provide a flattening coat on the release surface side of the base film.
- the “release surface side layer” of the base film means a layer having a release surface among the layers of the resin constituting the base film.
- the substrate film is a single layer, it may be referred to as a release surface side layer.
- the back surface side layer and the release surface side layer described later are the same layer.
- the surface layer preferably contains substantially no particles for smoothing.
- substantially free of particles is meant that the particle content is less than 50 ppm, preferably less than 30 ppm.
- the surface layer may contain particles to improve the slipperiness of the surface.
- the lower limit of the surface layer particle content is preferably 30 ppm, more preferably 50 ppm, and further preferably 100 ppm.
- the upper limit of the surface layer particle content is preferably 20000 ppm, more preferably 10000 ppm, further preferably 8000 ppm, and particularly preferably 6000 ppm. If it exceeds the above range, the roughness of the surface layer may not be within the preferred range.
- the lower limit of the surface layer particle size is preferably 0.005 ⁇ m, more preferably 0.01 ⁇ m, and further preferably 0.02 ⁇ m.
- the upper limit of the surface layer particle size is preferably 3 ⁇ m, more preferably 1 ⁇ m, further preferably 0.5 ⁇ m, and particularly preferably 0.3 ⁇ m. If it exceeds the above range, the roughness of the surface layer may not be within the preferred range.
- the release surface layer may have a higher roughness due to the effect of the particles in the lower layer. In such a case, it is preferable to increase the thickness of the release surface layer or to provide a lower layer (intermediate layer) containing no particles.
- the lower limit of the surface layer thickness is preferably 0.1 ⁇ m, more preferably 0.5 ⁇ m, further preferably 1 ⁇ m, particularly preferably 3 ⁇ m, and most preferably 5 ⁇ m.
- the upper limit of the surface layer thickness is preferably 97%, more preferably 95%, and further preferably 90% based on the total thickness of the transfer film.
- the content of particles is less than 50 ppm, preferably less than 30 ppm, in the sense that the intermediate layer containing no particles contains substantially no particles.
- the lower limit of the thickness of the intermediate layer with respect to the total thickness of the transfer film is preferably 10%, more preferably 20%, and further preferably 30% with respect to the total thickness of the transfer film.
- the upper limit is preferably 95%, more preferably 90%.
- a flattening coat may be provided.
- the resin used for the flattening coat include those generally used as the resin for the coating agent such as polyester, acryl, polyurethane, polystyrene and polyamide. It is also preferable to use a crosslinking agent such as melamine, isocyanate, epoxy resin, or oxazoline compound. These are applied as a coating agent dissolved or dispersed in an organic solvent or water and dried. Alternatively, in the case of acrylic, it may be coated without a solvent and cured by radiation.
- the planarization coat may be an oligomer block coat. When the release layer is provided as a coat, the release layer itself may be thickened.
- the lower limit of the thickness of the surface flattening coat layer is preferably 0.01 ⁇ m, more preferably 0.1 ⁇ m, further preferably 0.2 ⁇ m, and particularly preferably 0.3 ⁇ m. If it is less than the above, the flattening effect may be insufficient.
- the upper limit of the thickness of the surface flattening coat layer is preferably 10 ⁇ m, more preferably 7 ⁇ m, further preferably 5 ⁇ m, and particularly preferably 3 ⁇ m. Even if it exceeds the above range, no further flattening effect may be obtained.
- the flattening coat may be provided as an in-line coat during the film formation process, or may be provided as a separate offline coat.
- the obtained substrate film can be used as it is as a transfer film as long as it has a releasability from the transferred product (liquid crystal compound alignment layer).
- the film may be surface-treated in order to adjust the releasability. Examples of the surface treatment include corona treatment and plasma treatment.
- a release layer may be provided.
- a known release agent can be used, and alkyd resins, amino resins, long-chain acrylic acrylates, silicone resins, and fluororesins are preferred examples. These can be appropriately selected according to the adhesion to the transfer material.
- the base film may be surface-treated. Examples of the surface treatment include the above treatments. Further, an easy adhesion coat may be applied.
- a transfer film provided with a liquid crystal compound alignment layer may be wound with a masking film attached to protect the liquid crystal compound alignment layer, but it is often wound as it is for cost reduction.
- the liquid crystal compound alignment layer When the liquid crystal compound alignment layer is wound in this manner, it is considered that the liquid crystal compound alignment layer has a phenomenon in which the projections on the back surface cause depressions, holes, or disordered alignment. Even when the liquid crystal compound alignment layer is not wound in the state of being provided, but the liquid crystal compound alignment layer is provided later, a phenomenon such that holes are formed in the liquid crystal compound alignment layer due to the convex portion on the back surface and the alignment is disturbed occurs. It is thought that In particular, the pressure is high at the core portion, and these phenomena are likely to occur. From the above findings, it was found that the above-mentioned defects can be prevented by setting the roughness of the surface (back surface) opposite to the release surface within a specific range.
- the lower limit of the three-dimensional arithmetic mean roughness (SRa) of the back surface of the transfer film of the present invention is preferably 3 nm, more preferably 4 nm, and further preferably 5 nm. If it is less than the above range, the slipperiness may be deteriorated, and the roll may not be slipped smoothly during roll conveyance or winding, and may be easily scratched.
- the upper limit of SRa on the back surface of the transfer film of the present invention is preferably 50 nm, more preferably 45 nm, and further preferably 40 nm. If it exceeds the above, there may be many defects.
- the lower limit of the three-dimensional ten-point average roughness (SRz) of the back surface of the transfer film of the present invention is preferably 15 nm, more preferably 20 nm, further preferably 25 nm.
- the upper limit of SRz on the back surface of the transfer film of the present invention is preferably 1500 nm, more preferably 1200 nm, further preferably 1000 nm, particularly preferably 700 nm, and most preferably 500 nm. If it exceeds the above, there may be many defects.
- the lower limit of the maximum height of the back surface of the transfer film of the present invention (SRy: maximum back surface peak height SRp + back surface maximum valley depth SRv) is preferably 20 nm, more preferably 30 nm, further preferably 40 nm, Particularly preferably, it is 50 nm.
- the upper limit of the maximum height SRy of the back surface of the transfer film of the present invention is preferably 2000 nm, more preferably 1500 nm, further preferably 1200 nm, particularly preferably 1000 nm, most preferably 700 nm. is there. If it exceeds the above, there may be many defects.
- the upper limit of the number of protrusions having a height difference of 2 ⁇ m or more on the back surface of the transfer film of the present invention is preferably 5 / m 2 , more preferably 4 / m 2 , and further preferably 3 / m 2 . Yes, particularly preferably 2 / m 2 , and most preferably 1 / m 2 . If it exceeds the above, there may be many defects.
- the roughness of the back surface of the transfer film of the present invention represented by the above parameters is less than the above range, the slipperiness of the film is deteriorated, and when the film is conveyed by a roll, it is less likely to slip during winding, etc., It may be easily scratched. Further, during winding during film production, the winding is not stable and wrinkles occur, resulting in defective products, and the irregularities at the ends of the wound roll become large, and the film tends to meander in the next step. Or it is easy to break. If the roughness of the back surface of the transfer film of the present invention exceeds the above, the above-mentioned defects are likely to occur.
- the following method can be used to set the roughness of the back surface within the above range.
- -The surface roughness of the roll (casting roll or touch roll) on the back side is set within a specific range.
- the backside layer (backside layer) of the base film contains specific particles.
- -Use a substrate film containing particles as the intermediate layer, and reduce the thickness by making the back surface layer side (back surface layer) free of particles.
- a flattening coat is provided.
- a slippery coat particle-containing coat
- the lower limit of the particle diameter of the back surface layer is preferably 0.005 ⁇ m, more preferably 0.01 ⁇ m, further preferably 0.05 ⁇ m, and particularly preferably 0.1 ⁇ m. If it is less than the above range, slipperiness may be deteriorated and winding failure may occur.
- the upper limit of the particle diameter of the back surface layer is preferably 5 ⁇ m, more preferably 3 ⁇ m, and further preferably 2 ⁇ m. If it exceeds the above range, the back surface may be too rough.
- the lower limit of the back surface layer particle content is preferably 50 ppm, more preferably 100 ppm. If it is less than the above range, the effect of slipperiness due to addition of particles may not be obtained.
- the upper limit of the content of the back surface layer particles is preferably 10,000 ppm, more preferably 7,000 ppm, and further preferably 5000 ppm. If it exceeds the above range, the back surface may be too rough.
- the lower limit of the thickness of the back surface layer is preferably 0.1 ⁇ m, more preferably 0.5 ⁇ m, further preferably 1 ⁇ m, particularly preferably 3 ⁇ m, and most preferably 5 ⁇ m.
- the upper limit of the thickness of the back surface layer is preferably 95%, more preferably 90%, and further preferably 85% based on the total thickness of the transfer film.
- the particle size and amount of particles in the middle layer are the same as those in the back layer.
- the lower limit of the thickness of the back surface layer is preferably 0.5 ⁇ m, more preferably 1 ⁇ m, and further preferably 2 ⁇ m.
- the upper limit of the thickness is preferably 30 ⁇ m, more preferably 25 ⁇ m, further preferably 20 ⁇ m.
- the back surface of the base film is rough, it is also preferable to provide a flattening coat.
- a flattening coat those mentioned for the surface flattening coat can be similarly used.
- the lower limit of the thickness of the back surface flattening coat layer is preferably 0.01 ⁇ m, more preferably 0.03 ⁇ m, and further preferably 0.05 ⁇ m. If it is less than the above, the flattening effect may be reduced.
- the upper limit of the thickness of the back surface flattening coat layer is preferably 10 ⁇ m, more preferably 5 ⁇ m, and further preferably 3 ⁇ m. Even if it exceeds the above, the flattening effect will be saturated.
- a slippery coat containing particles may be provided on the back surface.
- the easy-sliding coat is effective when the back surface side of the base film does not contain particles or when the roughness is insufficient.
- the lower limit of the particle size of the back surface easy-sliding coat layer is preferably 0.01 ⁇ m, more preferably 0.05 ⁇ m. If it is less than the above range, slipperiness may not be obtained.
- the upper limit of the particle size of the back surface easy-sliding coat layer is preferably 5 ⁇ m, more preferably 3 ⁇ m, further preferably 2 ⁇ m, and particularly preferably 1 ⁇ m. If it exceeds the above range, the back surface roughness may be too high.
- the lower limit of the particle content of the back surface easy-sliding coat layer is preferably 0.1% by mass, more preferably 0.5% by mass, further preferably 1% by mass, particularly preferably 1.5% by mass. And most preferably 2% by mass. If it is less than the above range, slipperiness may not be obtained.
- the upper limit of the particle content of the back surface easy-sliding coat layer is preferably 20% by mass, more preferably 15% by mass, and further preferably 10% by mass. If it exceeds the above range, the back surface roughness may be too high.
- the lower limit of the thickness of the back surface easy-sliding coat layer is preferably 0.01 ⁇ m, more preferably 0.03 ⁇ m, and further preferably 0.05 ⁇ m.
- the upper limit of the thickness of the back surface easy-sliding coat layer is preferably 10 ⁇ m, more preferably 5 ⁇ m, further preferably 3 ⁇ m, particularly preferably 2 ⁇ m, and most preferably 1 ⁇ m.
- the base film When providing these coats, it is preferable to subject the base film to the above-mentioned surface treatment or easy-adhesion coat.
- the cyclic polyolefin film can be generally manufactured by a melt extrusion method. Hereinafter, this method will be briefly described.
- the cyclic polyolefin resin is a single-screw or twin-screw extruder and is usually (Tg + 30) to (Tg + 180) ° C., preferably (Tg + 50) to (Tg + 150) ° C., particularly preferably (Tg + 60) to (Tg + 140). It is heated and melted at °C and extruded from a die onto a cast roll.
- Tg is the glass transition temperature of the cyclic polyolefin resin.
- the molten resin In order to achieve proper surface roughness, it is preferable to filter the molten resin with a filter between the extruder and the die to remove coarse particles.
- the lower limit of the filtration accuracy of the filter used is preferably 0.5 ⁇ m, more preferably 1 ⁇ m.
- the upper limit of the filtration accuracy of the filter is preferably 100 ⁇ m, more preferably 50 ⁇ m, further preferably 25 ⁇ m, particularly preferably 20 ⁇ m, and most preferably 10 ⁇ m. This value is appropriately determined depending on the particle size of the particles to be added.
- Roll roughness By adjusting the roughness of the roll, the roughness of the surface of the formed film can be adjusted. For example, in the case where the casting roll is the release surface and the touch roll is the back surface, preferable roughness of the roll will be described below.
- the lower limit of the three-dimensional arithmetic mean surface roughness (SRa) of the casting roll when the casting roll is used as the release surface is preferably 1 nm, more preferably 1.3 nm, and further preferably 1.5 nm.
- the upper limit of the three-dimensional arithmetic mean surface roughness (SRa) of the casting roll when the casting roll is used as the release surface is preferably 250 nm, more preferably 200 nm, further preferably 150 nm, and particularly preferably 100 nm. And most preferably 50 nm.
- the lower limit of the three-dimensional 10-point average roughness (SRz) of the casting roll when the casting roll is used as the release surface is preferably 3 nm, more preferably 5 nm, and further preferably 7 nm.
- the upper limit of the three-dimensional ten-point average roughness (SRz) of the casting roll when the casting roll is used as the release surface is preferably 1000 nm, more preferably 700 nm, further preferably 500 nm, and particularly preferably 300 nm. And most preferably 250 nm.
- the lower limit of the maximum height (SRy) of the casting roll when the casting roll is used as the release surface is preferably 5 nm, more preferably 8 nm, further preferably 10 nm.
- the upper limit of the maximum height (SRy) of the casting roll when the casting roll is used as the release surface is preferably 1500 nm, more preferably 1000 nm, further preferably 800 nm, and particularly preferably 600 nm.
- the lower limit of the three-dimensional arithmetic average surface roughness (SRa) of the touch roll when the touch roll is used as the back surface is preferably 5 nm, more preferably 10 nm, and further preferably 15 nm.
- the upper limit of the three-dimensional arithmetic mean surface roughness (SRa) of the touch roll when the touch roll is used as the back surface is preferably 500 nm, more preferably 400 nm, further preferably 300 nm, particularly preferably 250 nm. , And most preferably 200 nm.
- the lower limit of the three-dimensional 10-point average roughness (SRz) of the touch roll when the touch roll is used as the back surface is preferably 20 nm, more preferably 30 nm, and further preferably 40 nm.
- the upper limit of the three-dimensional ten-point average roughness (SRz) of the touch roll when the touch roll is used as the back surface is preferably 2000 nm, more preferably 1500 nm, further preferably 1200 nm, and particularly preferably 1000 nm. , And most preferably 800 nm.
- the lower limit of the maximum height (SRy) of the touch roll when the touch roll is used as the back surface is preferably 30 nm, more preferably 40 nm, and further preferably 50 nm.
- the upper limit of the maximum height (SRy) of the touch roll when the touch roll is used as the back surface is preferably 3000 nm, more preferably 2500 nm, further preferably 2000 nm, particularly preferably 1500 nm, and most preferably It is 1000 nm.
- the film forming conditions and the roughness of the film surface have the following relationship, and the roughness of the roll is determined in consideration of these. -If the casting roll and the touch roll have the same roughness, the casting roll surface of the film becomes rougher. -The smaller the distance between the die and the casting roll, the greater the roughness of the casting roll surface of the film. -The closer the position where the molten resin contacts the casting roll and the position where the touch roll presses, the greater the roughness of each surface. -The lower the melt viscosity of the resin, the greater the roughness of each surface. -The higher the temperature of the casting roll and the touch roll, the greater the roughness of each surface. -The higher the pressing force of the touch roll, the greater the roughness of each surface.
- the temperature of the casting roll is preferably (Tg-30) to (Tg + 30) ° C, more preferably (Tg-20) to (Tg + 20) ° C.
- the temperature of the touch roll is preferably (Tg-100) to (Tg + 30) ° C, more preferably (Tg-90) to (Tg + 20) ° C. Further, it is preferable that the temperature is set to be 0 to 50 ° C., further 5 to 40 ° C. lower than the temperature of the casting roll.
- the pressing pressure (line pressure) of the touch roll is preferably 10 to 250 kgf / cm, more preferably 20 to 200 kgf / cm.
- the film is peeled from the casting roll, cooled while passing through the roll, and wound on the core. At the time of winding, both ends may be thickened (knurled).
- the wound film When performing coating, the wound film may be set in a coating device, unwound and coating dried. In the above film-forming step, the film may be coated and dried after being peeled off from the casting roll and wound up, and then wound up.
- the air in these processes is passed through a HEPA filter or the like to be air of class 10000 or less, further class 1000 or less.
- the transfer film of the present invention preferably has a low in-plane retardation.
- the in-plane retardation of the transfer film of the present invention is preferably 50 nm or less, more preferably 30 nm or less, further preferably 20 nm or less, and particularly preferably 10 nm or less.
- the sample is irradiated with linearly polarized light in an oblique direction (for example, 45 degrees) with respect to the slow axis of the retardation layer to be inspected, so that the retardation layer converts the light into elliptical polarization.
- the polarized light is returned to the linearly polarized light by passing through another retardation layer, and the linearly polarized light is received through the polarizing plate in the extinction state. Accordingly, when the retardation layer has a pinhole-like defect, the defect can be detected as a bright spot.
- the retardation of the transfer film can be obtained by measuring the refractive index and the thickness in the biaxial direction, and can also be obtained using a commercially available automatic birefringence measuring device such as KOBRA-21ADH (Oji Scientific Instruments). .
- the lower limit of haze of the transfer film of the present invention is preferably 0.01%, more preferably 0.1%. If it is less than the above, it may be difficult to achieve the numerical value.
- the upper limit of haze of the transfer film of the present invention is preferably 3%, more preferably 2.5%, further preferably 2%, and particularly preferably 1.7%. If it exceeds the above range, polarized light may be disturbed during irradiation of polarized UV, and a retardation layer as designed may not be obtained. In addition, light leakage may occur due to irregular reflection during the inspection of the retardation layer, which makes it difficult to perform the inspection.
- the lower limit of the antistatic property (surface resistance) of the transfer film of the present invention is preferably 1 ⁇ 10 5 ⁇ / ⁇ , more preferably 1 ⁇ 10 6 ⁇ / ⁇ . Even if it is less than the above, the effect may be saturated, and further effect may not be obtained.
- the upper limit of the antistatic property (surface resistance) of the transfer film of the present invention is preferably 1 ⁇ 10 13 ⁇ / ⁇ , more preferably 1 ⁇ 10 12 ⁇ / ⁇ , and further preferably 1 ⁇ 10. It is 11 ⁇ / ⁇ . If it exceeds the above range, cissing due to static electricity may occur or the alignment direction of the liquid crystal compound may be disturbed.
- antistatic property surface resistance
- kneading an antistatic agent into a transfer film providing an antistatic coating layer on the lower layer or the opposite surface of the release layer, or adding an antistatic agent to the release layer. It can be set within the above range by the above.
- Antistatic agents added to antistatic coating layers, release layers, and transfer films include conductive polymers such as polyaniline and polythiophene, ionic polymers such as polystyrene sulfonate, tin-doped indium oxide, antimony-doped tin oxide. Conductive fine particles such as
- a release layer may be provided on the transfer film.
- the release layer may not be provided. If the adhesion is too low, the surface may be corona treated to adjust the adhesion.
- the release layer can be formed using a known release agent, and alkyd resins, amino resins, long-chain acrylic acrylates, silicone resins, and fluororesins are preferred examples. These can be appropriately selected according to the adhesion to the transfer material.
- the liquid crystal compound alignment layer transfer laminate of the present invention has a structure in which the liquid crystal compound alignment layer and the transfer film of the present invention are laminated.
- the liquid crystal compound alignment layer must be coated on the transfer film for alignment.
- a method for orienting a method for giving an orientation control function by rubbing a lower layer (release surface) of the liquid crystal compound orientation layer, or irradiating polarized ultraviolet rays after coating the liquid crystal compound to orient the liquid crystal compound directly There is a way.
- the alignment layer and the liquid crystal compound alignment layer may be collectively referred to as a liquid crystal compound alignment layer, instead of the liquid crystal compound alignment layer alone.
- the orientation control layer any orientation control layer may be used as long as it can bring the liquid crystal compound orientation layer into a desired orientation state, but a rubbing treatment orientation control layer obtained by rubbing a resin coating film or A preferable example is a photo-alignment control layer that orients molecules by polarized light irradiation to produce an alignment function.
- a rubbing treatment orientation control layer coating liquid containing the above-mentioned polymer material is applied onto the release surface of the film, and then dried by heating to obtain an orientation control layer before the rubbing treatment.
- the orientation control layer coating liquid may contain a crosslinking agent.
- any solvent that dissolves the polymer material can be used without limitation.
- Specific examples thereof include alcohols such as water, methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol and cellosolve; ester solvents such as ethyl acetate, butyl acetate and gamma-butyrolactone; acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone. , And the like; ketone-based solvents such as; and aromatic hydrocarbon solvents such as toluene and xylene; and ether-based solvents such as tetrahydrofuran and dimethoxyethane. These solvents may be used alone or in combination.
- the concentration of the coating solution for rubbing alignment control layer can be appropriately adjusted depending on the type of polymer and the thickness of the alignment control layer to be produced, but it is preferably 0.2 to 20% by mass in terms of solid content concentration. The range of 0.3 to 10% by mass is particularly preferable.
- a coating method known methods such as a gravure coating method, a die coating method, a bar coating method and an applicator method, and a printing method such as a flexo method are used.
- the heating and drying temperature is preferably in the range of 30 ° C to 170 ° C, more preferably 50 to 150 ° C, and further preferably 70 to 130 ° C.
- the heating and drying time may be, for example, 0.5 to 30 minutes, more preferably 1 to 20 minutes, and further preferably 2 to 10 minutes.
- the thickness of the rubbing orientation control layer is preferably 0.01 to 10 ⁇ m, more preferably 0.05 to 5 ⁇ m, and particularly preferably 0.1 ⁇ m to 1 ⁇ m.
- the rubbing treatment can be generally performed by rubbing the surface of the polymer layer with paper or cloth in a certain direction.
- the surface of the orientation control layer is rubbed by using a rubbing roller made of a raised cloth of fibers such as nylon, polyester, and acrylic.
- the rubbing direction of the alignment control layer also needs to be at an angle suitable for it. The angle can be adjusted by adjusting the angle between the rubbing roller and the film, and adjusting the transport speed of the film and the rotation speed of the roller.
- the photo-alignment control layer a coating solution containing a polymer or monomer having a photoreactive group and a solvent is applied to the film, polarized, preferably of an alignment film that imparts an alignment regulating force by irradiating polarized ultraviolet light.
- the photoreactive group refers to a group that produces a liquid crystal aligning ability when irradiated with light. Specifically, it is one that causes a photoreaction that is the origin of the liquid crystal alignment ability, such as an orientation induction or isomerization reaction, a dimerization reaction, a photocrosslinking reaction, or a photodecomposition reaction of a molecule generated by irradiation with light. is there.
- the photoreactive groups those that cause a dimerization reaction or a photocrosslinking reaction are preferable because they have excellent alignment properties and maintain the smectic liquid crystal state of the liquid crystal compound alignment layer.
- a group having at least one selected from the above is particularly preferable.
- a photoreactive group capable of causing a photodimerization reaction is preferable
- a cinnamoyl group and a chalcone group have a relatively small amount of polarized light irradiation necessary for photoalignment, and a photoalignment layer having excellent thermal stability and stability over time. It is preferable because it is easily obtained.
- a polymer having a photoreactive group a polymer having a cinnamoyl group such that the end portion of the polymer side chain has a cinnamic acid structure is particularly preferable.
- the main chain structure include polyimide, polyamide, (meth) acrylic, polyester, and the like.
- Specific alignment control layers include, for example, JP-A 2006-285197, JP-A 2007-76839, JP-A 2007-138138, JP-A 2007-94071, and JP-A 2007-121721. , JP-A-2007-140465, JP-A-2007-156439, JP-A-2007-133184, JP-A-2009-109831, JP-A-2002-229039, JP-A-2002-265541, and Alignment described in Japanese Unexamined Patent Publication No. 2002-317013, Special Table 2003-520878, Special Table 2004-529220, JP2013-33248, JP2015-7702, and JP2015-129210. A control layer is included.
- the solvent for the photo-alignment control layer forming coating liquid can be used without limitation as long as it dissolves the polymer and monomer having a photoreactive group. Specific examples include those mentioned in the method of forming the rubbing orientation control layer. It is also preferable to add a photopolymerization initiator, a polymerization inhibitor, and various stabilizers to the coating liquid for forming the photo-alignment control layer. Further, a polymer other than the polymer having the photoreactive group and the monomer, or a monomer having no photoreactive group which is copolymerizable with the monomer having the photoreactive group may be added.
- the concentration, coating method, and drying conditions of the coating liquid for forming the photo-alignment control layer can be the same as those mentioned in the method for forming the rubbing-alignment control layer.
- the thickness is the same as the preferable thickness of the rubbing treatment orientation control layer.
- the polarized light may be irradiated either from the direction of the photo-alignment control layer surface before alignment or from the direction of the transfer film surface through the transfer film.
- the wavelength of polarized light is preferably in the wavelength range where the photoreactive group of the polymer or monomer having a photoreactive group can absorb light energy.
- ultraviolet rays having a wavelength of 250 to 400 nm are preferable.
- Examples of polarized light sources include xenon lamps, high-pressure mercury lamps, ultra-high pressure mercury lamps, metal halide lamps, and ultraviolet light lasers such as KrF and ArF. High-pressure mercury lamps, ultra-high-pressure mercury lamps and metal halide lamps are preferable. .
- Polarized light is obtained, for example, by passing light from the light source through a polarizer.
- the polarization direction can be adjusted by adjusting the polarization angle of the polarizer.
- the polarizer include a polarizing filter, a polarizing prism such as Glan-Thompson and Glan-Teller, and a wire grid type polarizer.
- the polarized light is preferably substantially collimated light.
- the direction of the alignment control force of the photo-alignment control layer can be adjusted arbitrarily.
- the irradiation intensity is different in kind and amount of a polymerization initiator or a resin (monomer), for example, preferably 10 ⁇ 10000mJ / cm 2 at 365nm reference, and more preferably 20 ⁇ 5000mJ / cm 2.
- the liquid crystal compound alignment layer is not particularly limited as long as the liquid crystal compound is aligned. Specific examples include a polarizing film (polarizer) containing a liquid crystal compound and a dichroic dye, and a retardation layer containing a rod-shaped or discotic liquid crystal compound.
- polarizer polarizing film
- retardation layer containing a rod-shaped or discotic liquid crystal compound.
- the polarizing film has a function of passing polarized light in only one direction and contains a dichroic dye.
- the dichroic dye is a dye having a property that the absorbance in the long axis direction of the molecule and the absorbance in the short axis direction of the molecule are different.
- the dichroic dye preferably has an absorption maximum wavelength ( ⁇ MAX) in the range of 300 to 700 nm.
- a dichroic dye examples include an acridine dye, an oxazine dye, a cyanine dye, a naphthalene dye, an azo dye and an anthraquinone dye, and among them, an azo dye is preferable.
- the azo dye examples include a monoazo dye, a bisazo dye, a trisazo dye, a tetrakisazo dye and a stilbeneazo dye, and a bisazo dye and a trisazo dye are preferable.
- the dichroic dyes may be used alone or in combination, but it is preferable to combine two or more kinds in order to adjust the color tone (achromatic color). Particularly, it is preferable to combine three or more kinds. In particular, it is preferable to combine three or more kinds of azo compounds.
- Preferred azo compounds include dyes described in JP-A 2007-126628, 2010-168570, 2013-101328, and 2013-210624.
- the dichroic dye is a dichroic dye polymer introduced into the side chain of a polymer such as acrylic.
- dichroic dye polymers include polymers described in JP-A-2016-4055 and polymers obtained by polymerizing the compounds of [Chemical formula 6] to [Chemical formula 12] in JP-A-2014-206682.
- the content of the dichroic dye in the polarizing film is preferably 0.1 to 30% by mass, more preferably 0.5 to 20% by mass, from the viewpoint of improving the orientation of the dichroic dye. , 1.0 to 15 mass% is more preferable, and 2.0 to 10 mass% is particularly preferable.
- the polarizing film preferably further contains a polymerizable liquid crystal compound in order to improve film strength, polarization degree and film homogeneity.
- the polymerizable liquid crystal compound also includes a substance after polymerization as a film.
- the polymerizable liquid crystal compound is a compound having a polymerizable group and exhibiting liquid crystallinity.
- the polymerizable group means a group that participates in the polymerization reaction, and is preferably a photopolymerizable group.
- the photopolymerizable group refers to a group capable of undergoing a polymerization reaction with an active radical or an acid generated from a photopolymerization initiator described later.
- Examples of the polymerizable group include vinyl group, vinyloxy group, 1-chlorovinyl group, isopropenyl group, 4-vinylphenyl group, acryloyloxy group, methacryloyloxy group, oxiranyl group and oxetanyl group. Among them, an acryloyloxy group, a methacryloyloxy group, a vinyloxy group, an oxiranyl group and an oxetanyl group are preferable, and an acryloyloxy group is more preferable.
- the compound exhibiting liquid crystallinity may be a thermotropic liquid crystal or a lyotropic liquid crystal, and may be a nematic liquid crystal or a smectic liquid crystal in the thermotropic liquid crystal.
- the polymerizable liquid crystal compound is preferably a smectic liquid crystal compound, and more preferably a high-order smectic liquid crystal compound, in that higher polarization characteristics can be obtained.
- the liquid crystal phase formed by the polymerizable liquid crystal compound is a higher order smectic phase, a polarizing film having a higher degree of orientational order can be manufactured.
- Specific preferred polymerizable liquid crystal compounds include, for example, JP-A-2002-308832, JP-A-2007-16207, JP-A-2015-163596, JP-A-2007-510946, and JP-A-2013-114131.
- Publication, WO 2005/045485, Lub et al. Recl. Trav. Chim. Examples include those described in Pays-Bas, 115, 321-328 (1996) and the like.
- the content ratio of the polymerizable liquid crystal compound in the polarizing film is preferably 70 to 99.5% by mass, more preferably 75 to 99% by mass, further from the viewpoint of increasing the orientation of the polymerizable liquid crystal compound. It is preferably 80 to 97% by mass, and particularly preferably 83 to 95% by mass.
- the polarizing film can be provided by applying a coating composition for the polarizing film.
- the polarizing film composition coating material may contain a solvent, a polymerization initiator, a sensitizer, a polymerization inhibitor, a leveling agent, a polymerizable non-liquid crystal compound, a crosslinking agent and the like.
- solvent those mentioned as the solvent for the alignment layer coating solution are preferably used.
- the polymerization initiator is not limited as long as it polymerizes the polymerizable liquid crystal compound, but a photopolymerization initiator that generates an active radical by light is preferable.
- the polymerization initiator include benzoin compounds, benzophenone compounds, alkylphenone compounds, acylphosphine oxide compounds, triazine compounds, iodonium salts and sulfonium salts.
- the photosensitizer is preferable as the sensitizer.
- a xanthone compound, an anthracene compound, phenothiazine, rubrene, etc. are mentioned.
- polymerization inhibitors examples include hydroquinones, catechols, and thiophenols.
- the polymerizable non-liquid crystal compound those which are copolymerizable with the polymerizable liquid crystal compound are preferable, and for example, when the polymerizable liquid crystal compound has a (meth) acryloyloxy group, (meth) crates can be mentioned.
- the (meth) acrylates may be monofunctional or polyfunctional. By using polyfunctional (meth) acrylates, the strength of the polarizing film can be improved.
- a polymerizable non-liquid crystal compound it is preferably contained in the polarizing film in an amount of 1 to 15% by mass, more preferably 2 to 10% by mass, and particularly preferably 3 to 7% by mass. If it exceeds 15% by mass, the degree of polarization may decrease.
- cross-linking agent examples include compounds capable of reacting with a functional group of a polymerizable liquid crystal compound and a polymerizable non-liquid crystal compound, such as an isocyanate compound, melamine, an epoxy resin and an oxazoline compound.
- a polarizing film is provided by directly applying a coating composition for a polarizing film on a transfer film or an orientation control layer, and then drying, heating, and curing if necessary.
- the coating method known methods such as a gravure coating method, a die coating method, a bar coating method and an applicator method, and a printing method such as a flexo method are used as the coating method.
- the transfer film after coating is introduced into a warm air dryer, an infrared dryer or the like, and dried at 30 to 170 ° C, more preferably 50 to 150 ° C, further preferably 70 to 130 ° C.
- the drying time is preferably 0.5 to 30 minutes, more preferably 1 to 20 minutes, and even more preferably 2 to 10 minutes.
- Heating can be performed to more strongly align the dichroic dye and the polymerizable liquid crystal compound in the polarizing film.
- the heating temperature is preferably in the temperature range in which the polymerizable liquid crystal compound forms a liquid crystal phase.
- the coating composition for the polarizing film contains a polymerizable liquid crystal compound
- it is preferably cured.
- the curing method include heating and light irradiation, and light irradiation is preferable.
- the dichroic dye can be fixed in the oriented state.
- the curing is preferably performed in a state where a liquid crystal phase is formed in the polymerizable liquid crystal compound, and may be cured by irradiation with light at a temperature showing the liquid crystal phase.
- the light in the light irradiation include visible light, ultraviolet light and laser light. From the viewpoint of easy handling, ultraviolet light is preferable.
- the irradiation intensity is different in kind and amount of a polymerization initiator or a resin (monomer), for example, preferably 100 ⁇ 10000mJ / cm 2 at 365nm reference, more preferably 200 ⁇ 5000mJ / cm 2.
- Polarizing film by coating a polarizing film composition coating on the orientation control layer, the dye is oriented along the orientation direction of the orientation layer, as a result, it has a polarization transmission axis of a predetermined direction,
- the polarizing film can be oriented by irradiating polarized light to cure the polarizing film forming composition.
- polarized light in a desired direction for example, polarized light in an oblique direction
- the dichroic dye is strongly aligned along the alignment direction of the polymer liquid crystal by further heat treatment thereafter.
- the thickness of the polarizing film is 0.1 to 5 ⁇ m, preferably 0.3 to 3 ⁇ m, more preferably 0.5 to 2 ⁇ m.
- retardation layer Representative examples of the retardation layer include a layer provided for optical compensation between a polarizer of a liquid crystal display device and a liquid crystal cell, and a ⁇ / 4 layer and a ⁇ / 2 layer of a circularly polarizing plate.
- a polarizer of a liquid crystal display device and a liquid crystal cell
- a ⁇ / 4 layer and a ⁇ / 2 layer of a circularly polarizing plate As the liquid crystal compound, a raw or negative A plate, a positive or negative C plate, an O plate, or the like, and a rod-shaped liquid crystal compound, a discotic liquid crystal compound, or the like can be used depending on the purpose.
- the degree of retardation is appropriately set depending on the type of liquid crystal cell and the properties of the liquid crystal compound used in the cell when used for optical compensation of a liquid crystal display device.
- an O plate using discotic liquid crystal is preferably used.
- a C plate or A plate using a rod-shaped liquid crystal compound or a discotic liquid crystal compound is preferably used.
- a rod-shaped compound it is preferable to use a rod-shaped compound to form an A plate.
- the liquid crystal compound used for these retardation layers is preferably a polymerizable liquid crystal compound having a polymerizable group such as a double bond from the viewpoint that the alignment state can be fixed.
- rod-shaped liquid crystal compounds examples include JP-A-2002-030042, JP-A-2004-204190, JP-A-2005-263789, JP-A-2007-119415, JP-A-2007-186430, and Examples thereof include rod-like liquid crystal compounds having a polymerizable group described in Kaihei 11-513360.
- rod-shaped liquid crystal compounds may be used in combination at an arbitrary ratio.
- discotic liquid crystal compound examples include benzene derivatives, truxene derivatives, cyclohexane derivatives, azacrown-based and phenylacetylene-based macrocycles, and various compounds are described in JP-A-2001-155866. Is preferably used. Among them, a compound having a triphenylene ring represented by the following general formula (1) is preferably used as the discotic compound.
- R 1 to R 6 are each independently hydrogen, halogen, an alkyl group, or a group represented by —O—X (where X is an alkyl group, an acyl group, an alkoxybenzyl group, an epoxy-modified group).
- R 1 to R 6 are preferably an acryloyloxy-modified alkoxybenzyl group represented by the following general formula (2) (where m is 4 to 10).
- the retardation layer can be provided by applying the composition coating for the retardation layer.
- the retardation layer composition coating material may contain a solvent, a polymerization initiator, a sensitizer, a polymerization inhibitor, a leveling agent, a polymerizable non-liquid crystal compound, a crosslinking agent and the like. As these, those described in the alignment control layer and the liquid crystal polarizer can be used.
- the retardation layer is provided by applying the composition coating for the retardation layer on the release surface of the transfer film or the orientation control layer, followed by drying, heating and curing.
- the conditions explained in the orientation control layer and the liquid crystal polarizer are used as preferable conditions.
- a plurality of retardation layers may be provided.
- a plurality of retardation layers may be provided on one transfer film and transferred onto an object, and a single retardation layer may be provided on one transfer film. It is also possible to prepare a plurality of types provided with the retardation layer and to transfer these in order to the object.
- the polarizing layer and the retardation layer may be provided on a single transfer film and transferred to an object.
- a protective layer may be provided between the polarizer and the retardation layer, or a protective layer may be provided on the retardation layer or between the retardation layers. These protective layers may also be provided on the transfer film together with the retardation layer or the polarizing layer and transferred to the object.
- a transparent resin coating layer may be used as the protective layer.
- the transparent resin is not particularly limited, such as polyvinyl alcohol, ethylene vinyl alcohol copolymer, polyester, polyurethane, polyamide, polystyrene, acrylic resin and epoxy resin.
- a cross-linking structure may be formed by adding a cross-linking agent to these resins. Further, it may be one obtained by curing a photocurable composition such as acrylic as a hard coat. Further, after the protective layer is provided on the transfer film, the protective layer may be rubbed, and the liquid crystal compound alignment layer may be provided thereon without providing the alignment layer.
- the method for producing a liquid crystal compound alignment layer laminated polarizing plate of the present invention includes a step of laminating a liquid crystal compound alignment layer surface of the liquid crystal compound alignment layer transfer laminate of the present invention to form an intermediate laminate, and an intermediate laminate. The step of peeling the transfer film from the body is included.
- the liquid crystal compound alignment layer is the liquid crystal compound alignment layer used for the circularly polarizing plate.
- a ⁇ / 4 layer is used as the retardation layer (referred to as a liquid crystal compound alignment layer in the transfer laminate).
- the front retardation of the ⁇ / 4 layer is preferably 100 to 180 nm. More preferably, it is 120 to 150 nm.
- the orientation axis (slow axis) of the ⁇ / 4 layer and the transmission axis of the polarizer are preferably 35 to 55 degrees, more preferably 40 degrees to 50 degrees, and further preferably Is 42 to 48 degrees.
- the absorption axis of the polarizer is generally in the length direction of the long polarizer film, ⁇ / When four layers are provided, it is preferable to orient the liquid crystal compound within the above range with respect to the length direction of the long transfer film.
- the liquid crystal compound is oriented so as to have the above relationship by taking the angle of the transmission axis of the polarizer into consideration.
- the polarizing plate may have a protective film provided on both sides of the polarizer, but preferably has a protective film provided on only one side. In the case of a polarizing plate in which a protective film is provided only on one surface, it is preferable to attach a retardation layer to the opposite surface (polarizer surface) of the protective film.
- the retardation layer is attached to the side that is supposed to be on the image cell side.
- the surface that is assumed to be on the image cell side is a surface that is not generally surface-treated such as a low reflection layer, an antireflection layer, and an antiglare layer, which is provided on the viewing side.
- the protective film on the side to which the retardation layer is attached is preferably a protective film such as TAC, acrylic, or COP having no retardation.
- polarizer a PVA-based film alone is stretched to form a polarizer, or an unstretched substrate such as polyester or polypropylene is coated with PVA, and the polarizer is stretched to protect the polarizer.
- examples thereof include those transferred to a film and those obtained by coating or transferring a polarizer comprising a liquid crystal compound and a dichroic dye on a polarizer protective film, and any of them is preferably used.
- a conventionally known one such as an adhesive or an adhesive can be used.
- an adhesive a polyvinyl alcohol adhesive, an ultraviolet curable adhesive such as acrylic or epoxy, or a thermosetting adhesive such as epoxy or isocyanate (urethane) is preferably used.
- the adhesive include acrylic, urethane-based and rubber-based adhesives. It is also preferable to use an acrylic baseless transparent optical pressure-sensitive adhesive sheet.
- the polarizer When a transfer type is used as the polarizer, the polarizer is transferred onto the retardation layer (liquid crystal compound alignment layer) of the transfer laminate, and then the polarizer and the retardation layer are targeted (polarizer protective film). It may be transferred to.
- the retardation layer liquid crystal compound alignment layer
- the polarizer protective film on the side opposite to the side where the retardation layer is provided commonly known ones such as TAC, acrylic, COP, polycarbonate, polyester can be used. Among them, TAC, acrylic, COP and polyester are preferable.
- the polyester is preferably polyethylene terephthalate. In the case of polyester, a zero retardation film having an in-plane retardation of 100 nm or less, particularly 50 nm or less, or a high retardation film of 3000 nm to 30,000 nm is preferable.
- the angle between the transmission axis of the polarizer and the slow axis of the polyester high retardation film is 30 to 30 mm in order to prevent blackout and coloring when viewing the image with polarized sunglasses.
- the range of 60 degrees is preferable, and the range of 35 to 55 degrees is more preferable.
- the angle between the transmission axis of the polarizer and the slow axis of the polyester high retardation film should be 10 degrees or less, and even 7 degrees or less, in order to reduce rainbow spots when observed from a shallow angle with the naked eye. Alternatively, it is preferably 80 to 100 degrees, more preferably 83 to 97 degrees.
- the polarizer protective film on the opposite side may be provided with an antiglare layer, an antireflection layer, a low reflection layer, a hard coat layer and the like.
- the ⁇ / 4 layer may be used in combination with the ⁇ / 2 layer.
- the front retardation of the ⁇ / 2 layer is preferably 200 to 360 nm. More preferably, it is 240 to 300 nm.
- the angle ( ⁇ ) between the orientation axis (slow axis) of the ⁇ / 2 layer and the transmission axis of the polarizer is preferably 5 to 20 degrees, more preferably 7 to 17 degrees.
- the angle between the orientation axis (slow axis) of the ⁇ / 2 layer and the orientation axis of ⁇ / 4 (slow axis) is preferably 2 ⁇ + 45 ° ⁇ 10 °, more preferably 2 ⁇ + 45 ° ⁇ 5 °. Yes, and more preferably within the range of 2 ⁇ + 45 ° ⁇ 3 °.
- the absorption axis of the polarizer is in the length direction of the long polarizer film, and therefore, for transfer of a long film.
- the film is provided with a ⁇ / 2 layer or a ⁇ / 4 layer, it is preferable to align the liquid crystal compound so as to be in the above range with respect to the lengthwise direction of the long transfer film or the direction perpendicular to the lengthwise direction.
- the liquid crystal compound is oriented so as to have the above relationship by taking the angle of the transmission axis of the polarizer into consideration.
- a C plate layer on the ⁇ / 4 layer in order to reduce the change in coloring when viewed from an angle.
- a positive or negative C plate layer is used according to the characteristics of the ⁇ / 4 layer and the ⁇ / 2 layer.
- a ⁇ / 2 layer is provided on the polarizer by transfer, and a ⁇ / 4 layer is further provided on it by transfer.
- a ⁇ / 4 layer and a ⁇ / 2 layer are provided in this order on the transfer film, and this is transferred onto the polarizer.
- a ⁇ / 4 layer, a ⁇ / 2 layer and a polarizing layer are provided in this order on the transfer film, and this is transferred to an object.
- a ⁇ / 2 layer and a polarizing layer are provided in this order on the transfer film, and this is transferred to an object, and further a ⁇ / 4 layer is transferred onto this.
- Various methods such as can be adopted.
- a method of transferring the C plate layer onto the ⁇ / 4 layer provided on the polarizer, or providing a C plate layer on the film, and further forming a ⁇ / 4 layer on the film Various methods such as a method of providing a ⁇ / 2 layer and a ⁇ / 4 layer and transferring the layer can be adopted.
- the thickness of the circularly polarizing plate thus obtained is preferably 120 ⁇ m or less. It is more preferably 100 ⁇ m or less, still more preferably 90 ⁇ m or less, particularly preferably 80 ⁇ m or less, and most preferably 70 ⁇ m or less.
- Three-dimensional surface roughness SRa, SRz, SRy Using a stylus type three-dimensional roughness meter (SE-3AK, manufactured by Kosaka Laboratory Ltd.), with a needle radius of 2 ⁇ m and a load of 30 mg, with a cutoff value of 0.25 mm in the longitudinal direction of the film, The measurement was performed at a needle feed speed of 0.1 mm / sec over a measurement length of 1 mm, divided into 500 points at a pitch of 2 ⁇ m, and the height of each point was incorporated into a three-dimensional roughness analyzer (SPA-11).
- SE-3AK stylus type three-dimensional roughness meter
- the same operation as above was continuously performed 150 times at intervals of 2 ⁇ m in the width direction of the film, that is, over 0.3 mm in the width direction of the film, and the data was captured by the analyzer.
- the center plane average roughness (SRa), the ten-point average roughness (SRz), and the maximum height (SRy) were obtained using an analyzer.
- the portion thus detected is cut into an appropriate size from the test piece, and a three-dimensional shape measuring device (Micromap TYPE550, manufactured by Ryoka Systems Inc .; measurement conditions: wavelength 550 nm, WAVE mode, objective lens 10 times) is used. It was used and observed from the direction perpendicular to the film surface and measured. At this time, the irregularities that are close to each other within 50 ⁇ m when observed from the direction perpendicular to the film surface are assumed to be the same scratch and a rectangle covering them as foreign matter, and the length and width of this rectangle are scratched, and the length of the foreign matter is long. And width.
- a three-dimensional shape measuring device Micromap TYPE550, manufactured by Ryoka Systems Inc .; measurement conditions: wavelength 550 nm, WAVE mode, objective lens 10 times
- the number of defects was quantified using a cross-sectional image (SURFACE PROFILE DISPLAY). The measurement was performed on 20 test pieces and converted into the number of defects per 1 m 2 . The number of defects having a height difference (difference between the highest point and the lowest point) of 0.5 ⁇ m or more on the release surface and the number of defects having a height difference of 2.0 ⁇ m or more on the back surface were counted.
- a rubbing-treated alignment control layer or a photo-alignment control layer as an alignment control layer disposed between the transfer film and the liquid crystal compound alignment layer was prepared as an inspection sample.
- the specific creation procedure is as follows.
- the transfer film was cut into a size A4, the coating for the rubbing orientation control layer having the following composition was applied to the release layer surface using a bar coater, and dried at 80 ° C. for 5 minutes to form a film having a thickness of 100 nm. . Subsequently, the surface of the obtained film was treated with a rubbing roll wound with a nylon raised cloth to obtain a transfer film having a rubbing-treated orientation control layer laminated thereon. The rubbing was performed at 45 degrees with respect to the lengthwise direction of the transfer film.
- a solution for forming a retardation layer having the following composition was applied to the surface subjected to the rubbing treatment by a bar coating method. It was dried at 110 ° C. for 3 minutes, irradiated with ultraviolet rays to be cured, and a 1 ⁇ 4 wavelength layer was provided to obtain an inspection sample.
- LC242 manufactured by BASF 95 parts by mass Trimethylolpropane triacrylate 5 parts by mass Irgacure 379 3 parts by mass Surfactant 0.1 parts by mass Methyl ethyl ketone 250 parts by mass
- the transfer film was cut into a size of A4, the photo-alignment control layer coating composition having the above composition was applied to the release layer surface using a bar coater, and dried at 80 ° C. for 1 minute to form a film having a thickness of 80 nm. Formed. Subsequently, polarized UV light was irradiated in a direction of 45 degrees with respect to the lengthwise direction of the film to obtain a transfer film in which a photo-alignment control layer was laminated. These paints were filtered with a membrane filter having a pore size of 0.2 ⁇ m, and coating and drying were performed in a clean room.
- the retardation layer forming solution was applied to the surface on which the optical alignment control layer was laminated by the bar coating method. It was dried at 110 ° C. for 3 minutes, irradiated with ultraviolet rays to be cured, and a 1 ⁇ 4 wavelength layer was provided to obtain an inspection sample.
- the defects of the retardation layer were inspected by the following procedure.
- a lower polarizing plate is placed on a surface emitting light source using a white LED using a yellow phosphor as a light source, and the inspection sample prepared as described above is placed on the lower polarizing plate. (Direction) was placed parallel to the long side direction of the test sample. Further, a ⁇ / 4 film made of a stretched film of a cyclic polyolefin is placed thereon so that the orientation main axis is in the direction of 45 degrees with the extinction axis of the lower polarizing plate, and the upper polarizing plate is placed on the upper polarizing plate.
- the extinction axis of was placed parallel to the extinction axis of the lower polarizing plate. In this state, the extinction state was observed with the naked eye (central part 15 cm ⁇ 20 cm) and a 20-fold magnifying glass (5 cm ⁇ 5 cm), and evaluated according to the following criteria. ⁇ : No bright spots were observed with the naked eye, and almost no bright spots were observed by loupe observation (2 or less at 5 cm ⁇ 5 cm). ⁇ : No bright spots were observed with the naked eye, and a small number of bright spots were observed by loupe observation (3 to 20 in 5 cm ⁇ 5 cm). B: No bright spots were observed with the naked eye, but bright spots were found by loupe observation (more than 20 at 5 cm ⁇ 5 cm). X: Bright spots were observed with the naked eye, or no bright spots were found, but there was overall light leakage which was attributed to the presence of many bright spots observed by loupe observation.
- thermoplastic norbornene resin (ZEONOR1420R manufactured by Nippon Zeon Co., Ltd.) is dried, supplied to an extruder and melted at 215 ° C., and a stainless sintered body filter material (nominal filtration accuracy 10 ⁇ m particles 95% cut). And then extruded into a sheet on a casting roll. From the opposite side of the resin wrapped around the casting roll, the resin was pressed against the casting roll with a touch roll. The cooled film was peeled off from the casting roll and wound into a roll. The surface roughness of the casting roll and the touch roll is as shown in Table 1.
- the films A1 to A4 and A7 were manufactured at a touch linear pressure of 200 Kgf / cm, and the films A5 and A6 were manufactured at a touch linear pressure of 200 Kgf / cm.
- Example 1 The film A1 was used, and the above-mentioned physical properties were evaluated using the casting roll surface as the release layer surface. The evaluation results are shown in Table 2.
- Example 2 The film A2 was used, and the above-mentioned physical properties were evaluated using the casting roll surface as the release layer surface. The evaluation results are shown in Table 2.
- Example 3 The film A3 was used, and the above-mentioned physical properties were evaluated using the casting roll surface as the release layer surface. The evaluation results are shown in Table 2.
- Example 4 The film A2 was used, and the above-mentioned physical properties were evaluated using the touch roll surface as the release layer surface. The evaluation results are shown in Table 2.
- Example 5 The film A4 was used, and the above-mentioned physical properties were evaluated using the casting roll surface as the release layer surface. The evaluation results are shown in Table 2.
- Example 6 The film A5 was used, and the above-mentioned physical properties were evaluated using the casting roll surface as the release layer surface. The evaluation results are shown in Table 2.
- Example 7 The film A6 was used, and the above-mentioned physical properties were evaluated using the casting roll surface as the release layer surface. The evaluation results are shown in Table 2.
- Example 8 Using film A2, the casting roll surface was subjected to corona treatment, a coating agent having the following composition was applied as a release layer (surface flattening coating layer) thereon, and dried in a heating oven at 150 ° C. for 3 minutes. . The thickness of the coating layer was 2 ⁇ m.
- the coating agent was used after being filtered with a 2 ⁇ m filter.
- the above-mentioned physical properties were evaluated using the surface on which the surface-flattening coat layer was formed as the release layer surface. The evaluation results are shown in Table 2.
- Example 9 Using film A7, the touch roll surface was subjected to corona treatment, and a coating solution having the following composition was applied as a back surface easy-sliding coat layer thereon so that the coating amount after drying would be 0.07 g / m 2 . Then, it was introduced into a dryer and dried at 80 ° C. for 30 seconds.
- Example 10 Corrosion treatment is applied to the touch roll surface of the film A4, and the antistatic layer Pertron C-4402 (antimony-doped tin oxide particles) with MEK having a solid concentration of 5% is applied and heated. It was dried in an oven at 80 ° C. for 3 minutes. The thickness of the coating layer was 200 nm. The surface resistance was 7.5 ⁇ 10 7 ⁇ / ⁇ . The above-mentioned physical properties were evaluated using the casting roll surface of the obtained film as the release layer surface. The evaluation results are shown in Table 2.
- Pertron C-4402 antimony-doped tin oxide particles
- Example 11 A twin screw extruder in which a dried thermoplastic norbornene resin (ZEONOR1420R manufactured by Nippon Zeon Co., Ltd.) and silica particles (KE-P250 manufactured by Nippon Shokubai Co., Ltd.) having a particle size of 2.5 ⁇ m are mixed so that the particle content is 1000 ppm in terms of solid content. And pellet 1 was obtained.
- a dried thermoplastic norbornene resin ZONOR1420R manufactured by Nippon Zeon Co., Ltd.
- silica particles KE-P250 manufactured by Nippon Shokubai Co., Ltd.
- the dried pellets 1 were supplied to the extruder 1, and the dried thermoplastic norbornene resin (ZEONOR 1420R manufactured by Nippon Zeon Co., Ltd.) was supplied to the extruder 2, and the stainless steel sintered filter media (nominal filtration accuracy of 10 ⁇ m particles 95 % Cut), the mixture was laminated in a 2-kind 2-layer confluent block and extruded into a sheet shape on a casting roll in the same manner as the film A1 to obtain a film B1. At this time, the resin on the extruder 2 side was made to be the casting roll surface. The above-mentioned physical properties were evaluated using the casting roll surface of the obtained film as the release layer surface. The evaluation results are shown in Table 2.
- Example 12 Dried thermoplastic norbornene resin (ZEONOR 1420R manufactured by Nippon Zeon Co., Ltd.) and silica particles having a particle diameter of 100 nm (KE-P10 manufactured by Nippon Shokubai Co., Ltd.) were added to a twin-screw extruder so that the particle content was 600 ppm in terms of solid content. Then, pellet 2 was obtained. A film B2 was obtained in the same manner as in Example 11 except that the pellet 2 was supplied to the extruder 2. The above-mentioned physical properties were evaluated using the casting roll surface of the obtained film as the release layer surface. The evaluation results are shown in Table 2.
- Comparative Example 1 The film A3 was used, and the above-mentioned physical properties were evaluated using the touch roll surface as the release layer surface. The evaluation results are shown in Table 2.
- the specific measurement procedure of in-plane retardation is as follows. That is, a 4 cm ⁇ 2 cm rectangle was cut out from the base film used in Examples and Comparative Examples so that the long side was in the flow direction, and used as a measurement sample.
- the refractive index (flow direction nx, width direction ny) of this sample was measured using an Abbe refractometer (NAR-4T, manufactured by Atago Co., measurement wavelength 589 nm).
- the product was measured at 5 points in the width direction of the film (center portion, both end portions, intermediate portion between the center portion and the end portion), and the average was taken as the product ((nx-ny) ⁇ d) of the film thickness d (nm).
- the in-plane retardation (Re) was obtained.
- the liquid crystal compound alignment layer transfer film of the present invention uses a film whose surface roughness is controlled within a specific range as a transfer film for a retardation layer or a polarizing layer.
- the orientation state and retardation of the liquid crystal compound therein can be made as designed, and a retardation layer or a polarizing layer (liquid crystal compound orientation layer) in which occurrence of defects such as pinholes is reduced can be formed. Therefore, according to the present invention, a retardation layer laminated polarizing plate such as a circular polarizing plate can be stably manufactured with high quality.
Landscapes
- Physics & Mathematics (AREA)
- Chemical & Material Sciences (AREA)
- General Physics & Mathematics (AREA)
- Optics & Photonics (AREA)
- Engineering & Computer Science (AREA)
- Manufacturing & Machinery (AREA)
- Health & Medical Sciences (AREA)
- Crystallography & Structural Chemistry (AREA)
- Analytical Chemistry (AREA)
- Polymers & Plastics (AREA)
- Materials Engineering (AREA)
- Organic Chemistry (AREA)
- Medicinal Chemistry (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Life Sciences & Earth Sciences (AREA)
- Biochemistry (AREA)
- General Health & Medical Sciences (AREA)
- Immunology (AREA)
- Pathology (AREA)
- Mechanical Engineering (AREA)
- Polarising Elements (AREA)
- Laminated Bodies (AREA)
- Shaping By String And By Release Of Stress In Plastics And The Like (AREA)
- Liquid Crystal (AREA)
- Investigating Materials By The Use Of Optical Means Adapted For Particular Applications (AREA)
- Coating Of Shaped Articles Made Of Macromolecular Substances (AREA)
- Manufacture Of Macromolecular Shaped Articles (AREA)
Priority Applications (3)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| CN201980064154.8A CN112771423B (zh) | 2018-10-26 | 2019-10-21 | 液晶化合物取向层转印用薄膜 |
| KR1020217007467A KR102789163B1 (ko) | 2018-10-26 | 2019-10-21 | 액정 화합물 배향층 전사용 필름 |
| JP2020553398A JP7539038B2 (ja) | 2018-10-26 | 2019-10-21 | 液晶化合物配向層転写用フィルム |
Applications Claiming Priority (14)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2018-201940 | 2018-10-26 | ||
| JP2018201940 | 2018-10-26 | ||
| JP2018-209663 | 2018-11-07 | ||
| JP2018209663 | 2018-11-07 | ||
| JP2018209662 | 2018-11-07 | ||
| JP2018-209662 | 2018-11-07 | ||
| JP2018219282 | 2018-11-22 | ||
| JP2018-219282 | 2018-11-22 | ||
| JP2018223878 | 2018-11-29 | ||
| JP2018-223878 | 2018-11-29 | ||
| JP2018231737 | 2018-12-11 | ||
| JP2018-231737 | 2018-12-11 | ||
| JP2019-000802 | 2019-01-07 | ||
| JP2019000802 | 2019-01-07 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2020085310A1 true WO2020085310A1 (ja) | 2020-04-30 |
Family
ID=70330512
Family Applications (4)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2019/041326 Ceased WO2020085310A1 (ja) | 2018-10-26 | 2019-10-21 | 液晶化合物配向層転写用フィルム |
| PCT/JP2019/041323 Ceased WO2020085307A1 (ja) | 2018-10-26 | 2019-10-21 | 液晶化合物配向層転写用配向フィルム |
| PCT/JP2019/041325 Ceased WO2020085309A1 (ja) | 2018-10-26 | 2019-10-21 | 液晶化合物配向層転写用フィルム |
| PCT/JP2019/041324 Ceased WO2020085308A1 (ja) | 2018-10-26 | 2019-10-21 | 液晶化合物配向層転写用配向フィルム |
Family Applications After (3)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2019/041323 Ceased WO2020085307A1 (ja) | 2018-10-26 | 2019-10-21 | 液晶化合物配向層転写用配向フィルム |
| PCT/JP2019/041325 Ceased WO2020085309A1 (ja) | 2018-10-26 | 2019-10-21 | 液晶化合物配向層転写用フィルム |
| PCT/JP2019/041324 Ceased WO2020085308A1 (ja) | 2018-10-26 | 2019-10-21 | 液晶化合物配向層転写用配向フィルム |
Country Status (5)
| Country | Link |
|---|---|
| JP (5) | JP7615489B2 (cg-RX-API-DMAC7.html) |
| KR (4) | KR102811735B1 (cg-RX-API-DMAC7.html) |
| CN (5) | CN112789531B (cg-RX-API-DMAC7.html) |
| TW (2) | TWI907337B (cg-RX-API-DMAC7.html) |
| WO (4) | WO2020085310A1 (cg-RX-API-DMAC7.html) |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2022117202A (ja) * | 2021-01-29 | 2022-08-10 | 三菱ケミカル株式会社 | プラスチックフィルム |
Families Citing this family (7)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN112789531B (zh) * | 2018-10-26 | 2023-10-27 | 东洋纺株式会社 | 液晶化合物取向层转印用取向薄膜 |
| WO2022070437A1 (ja) | 2020-10-02 | 2022-04-07 | 大日本印刷株式会社 | ぎらつきコントラストの補正方法、比較方法および比較装置、電子ディスプレイの製造方法、及び防眩層の製造方法 |
| JP7745340B2 (ja) * | 2020-11-16 | 2025-09-29 | 日東電工株式会社 | 光学フィルムの製造方法 |
| KR102387993B1 (ko) * | 2021-01-06 | 2022-04-19 | (주)엘프스 | 점착부재용 이형필름, 이를 포함하는 점착시트 및 이의 제조방법 |
| JP2022157822A (ja) * | 2021-03-31 | 2022-10-14 | 三菱ケミカル株式会社 | プラスチックフィルム |
| KR102912059B1 (ko) * | 2022-01-19 | 2026-01-15 | 마이크로웍스 주식회사 | 폴리에스테르계 이형필름 |
| TW202408816A (zh) * | 2022-07-21 | 2024-03-01 | 日商東洋紡股份有限公司 | 雙軸配向積層聚酯膜以及離型膜 |
Citations (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPS6363252B2 (cg-RX-API-DMAC7.html) * | 1980-07-29 | 1988-12-06 | ||
| JP2010120304A (ja) * | 2008-11-20 | 2010-06-03 | Fujifilm Corp | ノルボルネン系樹脂フィルム、ノルボルネン系樹脂フィルムの製造方法、偏光版、液晶表示板用光学補償フィルム及び反射防止フィルム |
| JP2017000039A (ja) * | 2015-06-08 | 2017-01-05 | キユーピー株式会社 | 凍結液卵白の製造方法 |
| JP2017146616A (ja) * | 2017-04-28 | 2017-08-24 | 大日本印刷株式会社 | 光学フィルム用転写体、光学フィルム、光学フィルム用転写体の製造方法、光学フィルムの製造方法 |
Family Cites Families (69)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2660601B2 (ja) | 1990-06-27 | 1997-10-08 | 日本石油株式会社 | 液晶表示素子用補償板の製造法 |
| JPH0756172A (ja) * | 1993-08-17 | 1995-03-03 | Seiko Epson Corp | 液晶表示体の製造方法 |
| JPH08334757A (ja) * | 1995-04-07 | 1996-12-17 | Sumitomo Chem Co Ltd | 液晶表示装置、偏光位相差複合フィルムおよびそれらの製造方法 |
| JP2001004837A (ja) | 1999-06-22 | 2001-01-12 | Fuji Photo Film Co Ltd | 位相差板および円偏光板 |
| JP2002328371A (ja) * | 2000-04-24 | 2002-11-15 | Nippon Kayaku Co Ltd | 液晶性化合物の配向方法 |
| JP2002062426A (ja) * | 2000-08-15 | 2002-02-28 | Fuji Photo Film Co Ltd | 配向膜、光学補償シート、楕円偏光板、およびそれを用いた液晶表示装置 |
| JP4691842B2 (ja) * | 2001-07-11 | 2011-06-01 | 東レ株式会社 | 偏光フィルム貼り合わせ用ポリエステルフィルム |
| CN1564951A (zh) * | 2002-06-27 | 2005-01-12 | 帝人株式会社 | 聚碳酸酯类取向膜以及相位差膜 |
| JP2004144943A (ja) | 2002-10-23 | 2004-05-20 | Fuji Photo Film Co Ltd | 円偏光板 |
| JP2004264345A (ja) * | 2003-02-03 | 2004-09-24 | Nitto Denko Corp | 位相差フィルムおよびその製造方法 |
| JP2004287416A (ja) * | 2003-03-06 | 2004-10-14 | Nitto Denko Corp | 傾斜配向フィルムの製造方法、傾斜配向フィルムおよびそれを用いた画像表示装置 |
| JP4344566B2 (ja) * | 2003-08-22 | 2009-10-14 | 富士フイルム株式会社 | 光学補償フィルムの製造方法 |
| JP4187594B2 (ja) | 2003-06-19 | 2008-11-26 | 帝人株式会社 | 円偏光板 |
| JP2005092114A (ja) * | 2003-09-19 | 2005-04-07 | Fuji Photo Film Co Ltd | 光学補償シート、それを用いた偏光板、及び液晶表示装置 |
| JP3822198B2 (ja) | 2003-09-08 | 2006-09-13 | 日東電工株式会社 | 液晶配向フィルムの製造方法 |
| JP2005313467A (ja) * | 2004-04-28 | 2005-11-10 | Konica Minolta Opto Inc | セルロースエステルフィルムの製造方法、及びセルロースエステルフィルム |
| JP2006058540A (ja) * | 2004-08-19 | 2006-03-02 | Jsr Corp | 光学フィルム、偏光板および液晶ディスプレイ |
| JP4604661B2 (ja) * | 2004-11-05 | 2011-01-05 | ウシオ電機株式会社 | 光配向用偏光光照射装置 |
| JP2006201746A (ja) * | 2004-12-22 | 2006-08-03 | Nitto Denko Corp | 楕円偏光板およびそれを用いた画像表示装置 |
| CN101419305A (zh) * | 2004-12-22 | 2009-04-29 | 日东电工株式会社 | 椭圆偏光板及使用该椭圆偏光板的图像显示装置 |
| TWI413809B (zh) * | 2004-12-27 | 2013-11-01 | Dainippon Ink & Chemicals | 光學薄膜、橢圓偏光板、圓偏光板、液晶顯示元件、及該光學薄膜之製法 |
| JP2006195293A (ja) * | 2005-01-14 | 2006-07-27 | Fuji Photo Film Co Ltd | 液晶表示装置、光学補償フィルムおよび偏光板 |
| JP2006220716A (ja) * | 2005-02-08 | 2006-08-24 | Dainippon Printing Co Ltd | 配向膜用組成物、及び光学素子 |
| JP2006240034A (ja) * | 2005-03-03 | 2006-09-14 | Nissha Printing Co Ltd | ダイクロイック意匠付きインサート成形品の製造方法及びダイクロイック意匠付きインサート成形品 |
| JP2006243653A (ja) | 2005-03-07 | 2006-09-14 | Nitto Denko Corp | 楕円偏光板の製造方法および楕円偏光板を用いた画像表示装置 |
| JP2007001198A (ja) * | 2005-06-24 | 2007-01-11 | Fujifilm Holdings Corp | セルロースエステルフィルム積層体、偏光板、光学補償フィルム、反射防止フィルムおよび液晶表示装置 |
| CN100432799C (zh) * | 2005-07-20 | 2008-11-12 | 台湾薄膜电晶体液晶显示器产业协会 | 氢离子束应用于液晶分子配向的方法 |
| JP2007290342A (ja) * | 2005-09-12 | 2007-11-08 | Fujifilm Corp | セルロースアシレートフィルムの製造方法、偏光板および液晶表示装置 |
| JP4113547B2 (ja) * | 2005-12-12 | 2008-07-09 | インターナショナル・ビジネス・マシーンズ・コーポレーション | 配向層形成装置および配向層形成方法 |
| US7764339B2 (en) * | 2005-12-14 | 2010-07-27 | Dai Nippon Printing Co., Ltd. | Liquid crystal display device |
| JP2007241037A (ja) * | 2006-03-10 | 2007-09-20 | Toppan Printing Co Ltd | 偏光素子およびその製造方法ならびに液晶表示素子 |
| JP5209223B2 (ja) * | 2006-03-29 | 2013-06-12 | 住友化学株式会社 | フィルムおよびフィルムの製造方法、並びにその利用 |
| JP2008026824A (ja) * | 2006-07-25 | 2008-02-07 | Fujifilm Corp | 光学補償フィルムの製造方法、光学補償フィルム、偏光板、及び液晶表示装置 |
| JP2008126461A (ja) * | 2006-11-20 | 2008-06-05 | Mitsubishi Polyester Film Copp | 離型フィルム |
| JP5076810B2 (ja) * | 2007-10-31 | 2012-11-21 | Dic株式会社 | 光配向膜用組成物、光配向膜、及び光学異方体 |
| JP2009181104A (ja) * | 2008-02-01 | 2009-08-13 | Dic Corp | 光配向性基板、光学異方体及び液晶表示素子 |
| JP2009251288A (ja) * | 2008-04-07 | 2009-10-29 | Nitto Denko Corp | 楕円偏光板並びにその製造方法 |
| JP5446369B2 (ja) * | 2008-04-30 | 2014-03-19 | 東洋紡株式会社 | 粘着フィルム |
| JP5097623B2 (ja) * | 2008-06-09 | 2012-12-12 | 富士フイルム株式会社 | ラビング処理方法および光学フィルムの製造方法 |
| US8619204B2 (en) * | 2009-06-19 | 2013-12-31 | Nec Corporation | Liquid crystal shutter and liquid crystal shutter eyeglass |
| JP2011048025A (ja) * | 2009-08-25 | 2011-03-10 | Fujifilm Corp | フィルム、フィルムの製造方法、偏光板および液晶表示装置 |
| JP5451672B2 (ja) * | 2011-03-25 | 2014-03-26 | 富士フイルム株式会社 | 光反射性フィルムの製造方法 |
| WO2013031511A1 (ja) * | 2011-08-30 | 2013-03-07 | 東レ株式会社 | 偏光板離型フィルム用二軸配向ポリエステルフィルムおよびそれを用いた積層体、ならびに、偏光板の製造方法 |
| JP2013050572A (ja) * | 2011-08-31 | 2013-03-14 | Fujifilm Corp | 光学フィルム、偏光板、液晶表示装置及び配向制御剤 |
| JP2013097277A (ja) | 2011-11-02 | 2013-05-20 | V Technology Co Ltd | フィルム露光装置 |
| TW201314384A (zh) * | 2011-09-16 | 2013-04-01 | V Technology Co Ltd | 膜片曝光裝置 |
| JP2013088713A (ja) * | 2011-10-20 | 2013-05-13 | Fujifilm Corp | 配向フィルムの製造方法 |
| JP5257505B2 (ja) | 2011-12-09 | 2013-08-07 | 日本ゼオン株式会社 | 延伸フィルムの製造方法及び円偏光板の製造方法 |
| JP5607673B2 (ja) * | 2012-03-09 | 2014-10-15 | 日東電工株式会社 | 光学的表示装置 |
| JP2014071381A (ja) | 2012-09-28 | 2014-04-21 | Dainippon Printing Co Ltd | 光学フィルム用転写体、光学フィルム、画像表示装置及び光学フィルムの製造方法 |
| WO2014185322A1 (ja) * | 2013-05-14 | 2014-11-20 | 東洋紡株式会社 | 液晶表示装置、偏光板及び偏光子保護フィルム |
| JP6171707B2 (ja) * | 2013-08-07 | 2017-08-02 | 大日本印刷株式会社 | 光学フィルム用転写体、光学フィルム、光学フィルム用転写体の製造方法、光学フィルムの製造方法 |
| TWI645962B (zh) * | 2013-08-09 | 2019-01-01 | 住友化學股份有限公司 | 光學異向性薄片 |
| JP6303544B2 (ja) * | 2014-01-29 | 2018-04-04 | 東洋紡株式会社 | 液晶表示装置及び偏光板 |
| JP5968943B2 (ja) * | 2014-03-31 | 2016-08-10 | 日東電工株式会社 | 延伸積層体の製造方法および延伸積層体、ならびに偏光膜の製造方法および偏光膜 |
| CN106488839B (zh) * | 2014-07-18 | 2019-11-12 | 富士胶片株式会社 | 单轴取向聚酯薄膜、硬涂层薄膜、触摸面板用传感器薄膜、防飞散膜、防反射膜、触摸面板及单轴取向聚酯薄膜的制造方法 |
| KR102581852B1 (ko) * | 2015-01-28 | 2023-09-21 | 니폰 제온 가부시키가이샤 | 복층 필름, 광학 이방성 적층체, 원편광판, 유기 일렉트로 루미네선스 표시 장치, 및 제조 방법 |
| JP6724297B2 (ja) * | 2015-05-27 | 2020-07-15 | 日本ゼオン株式会社 | 光学積層体の製造方法、円偏光板の製造方法及び有機エレクトロルミネッセンス表示装置の製造方法 |
| JP6816942B2 (ja) * | 2015-09-01 | 2021-01-20 | 大日本印刷株式会社 | 光学フィルム用転写体、光学フィルムの製造方法及び画像表示装置の製造方法 |
| WO2017069133A1 (ja) * | 2015-10-20 | 2017-04-27 | 日産化学工業株式会社 | 液晶配向剤、液晶配向膜および液晶表示素子 |
| JP2017122864A (ja) | 2016-01-08 | 2017-07-13 | 大日本印刷株式会社 | 光学フィルム、画像表示装置、及び光学フィルムの製造方法 |
| JP6589657B2 (ja) * | 2016-01-21 | 2019-10-16 | Jnc株式会社 | 液晶配向剤、液晶配向膜およびこれを用いた液晶表示素子 |
| JP6565730B2 (ja) * | 2016-02-18 | 2019-08-28 | Jnc株式会社 | ジアミン、ポリアミック酸またはその誘導体、液晶配向剤、液晶配向膜および液晶表示素子 |
| KR102481313B1 (ko) * | 2016-07-21 | 2022-12-23 | 스미또모 가가꾸 가부시끼가이샤 | 타원 편광판 |
| JP2018028641A (ja) * | 2016-08-19 | 2018-02-22 | コニカミノルタ株式会社 | セルロースエステルフィルムの製造方法 |
| JP6331167B2 (ja) * | 2016-11-30 | 2018-05-30 | 大日本印刷株式会社 | 液晶セル |
| JP7000677B2 (ja) * | 2016-12-07 | 2022-01-19 | 東レ株式会社 | ポリエステルフィルム |
| JP6363252B1 (ja) | 2017-04-24 | 2018-07-25 | 日東電工株式会社 | ホメオトロピック配向液晶フィルムの製造方法 |
| CN112789531B (zh) * | 2018-10-26 | 2023-10-27 | 东洋纺株式会社 | 液晶化合物取向层转印用取向薄膜 |
-
2019
- 2019-10-21 CN CN201980064543.0A patent/CN112789531B/zh active Active
- 2019-10-21 WO PCT/JP2019/041326 patent/WO2020085310A1/ja not_active Ceased
- 2019-10-21 JP JP2020553395A patent/JP7615489B2/ja active Active
- 2019-10-21 WO PCT/JP2019/041323 patent/WO2020085307A1/ja not_active Ceased
- 2019-10-21 CN CN202310646255.4A patent/CN116804778A/zh active Pending
- 2019-10-21 JP JP2020553398A patent/JP7539038B2/ja active Active
- 2019-10-21 KR KR1020217007310A patent/KR102811735B1/ko active Active
- 2019-10-21 CN CN201980064152.9A patent/CN112771422B/zh active Active
- 2019-10-21 WO PCT/JP2019/041325 patent/WO2020085309A1/ja not_active Ceased
- 2019-10-21 KR KR1020217007116A patent/KR102929899B1/ko active Active
- 2019-10-21 WO PCT/JP2019/041324 patent/WO2020085308A1/ja not_active Ceased
- 2019-10-21 CN CN201980064549.8A patent/CN112805136B/zh active Active
- 2019-10-21 KR KR1020217007467A patent/KR102789163B1/ko active Active
- 2019-10-21 KR KR1020217007311A patent/KR102789162B1/ko active Active
- 2019-10-21 JP JP2020553396A patent/JP7539036B2/ja active Active
- 2019-10-21 CN CN201980064154.8A patent/CN112771423B/zh active Active
- 2019-10-21 JP JP2020553397A patent/JP7539037B2/ja active Active
- 2019-10-25 TW TW108138546A patent/TWI907337B/zh active
- 2019-10-25 TW TW108138545A patent/TWI824046B/zh active
-
2024
- 2024-09-10 JP JP2024155516A patent/JP2024170606A/ja active Pending
Patent Citations (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPS6363252B2 (cg-RX-API-DMAC7.html) * | 1980-07-29 | 1988-12-06 | ||
| JP2010120304A (ja) * | 2008-11-20 | 2010-06-03 | Fujifilm Corp | ノルボルネン系樹脂フィルム、ノルボルネン系樹脂フィルムの製造方法、偏光版、液晶表示板用光学補償フィルム及び反射防止フィルム |
| JP2017000039A (ja) * | 2015-06-08 | 2017-01-05 | キユーピー株式会社 | 凍結液卵白の製造方法 |
| JP2017146616A (ja) * | 2017-04-28 | 2017-08-24 | 大日本印刷株式会社 | 光学フィルム用転写体、光学フィルム、光学フィルム用転写体の製造方法、光学フィルムの製造方法 |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2022117202A (ja) * | 2021-01-29 | 2022-08-10 | 三菱ケミカル株式会社 | プラスチックフィルム |
Also Published As
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP7539038B2 (ja) | 液晶化合物配向層転写用フィルム | |
| JP7187764B2 (ja) | 液晶表示装置 | |
| JP2003121641A (ja) | 積層位相差板、偏光部材及び液晶表示装置 | |
| JP2023081987A (ja) | 偏光板の製造方法 | |
| JP7385380B2 (ja) | 位相差層およびハードコート層付偏光板の製造方法 | |
| WO2021192933A1 (ja) | 薄膜層転写用積層体 | |
| WO2020241704A1 (ja) | 画像表示装置の製造方法及び偏光子転写用積層体 | |
| WO2023276611A1 (ja) | 偏光板の製造方法、有機エレクトロルミネッセンス表示装置の製造方法、偏光板、有機エレクトロルミネッセンス表示装置、液晶表示装置 | |
| WO2017051844A1 (ja) | 光学積層体、偏光板、偏光板の製造方法および画像表示装置 | |
| JP7404635B2 (ja) | 配向液晶化合物層積層体の製造方法 | |
| JP7392278B2 (ja) | 液晶化合物積層体の製造方法、及び液晶化合物層の検査方法 | |
| JP7727541B2 (ja) | 転写用フィルム積層体及びその製造方法 | |
| KR102856585B1 (ko) | 원편광 소자 전사용 적층체 및 이것을 이용한 광학 물품의 제조 방법 | |
| WO2025028229A1 (ja) | 偏光板、表示装置 | |
| WO2025154790A1 (ja) | 偏光板、表示装置 | |
| WO2025062969A1 (ja) | 光学積層体の製造方法、偏光板の製造方法、光学積層体、偏光板、有機エレクトロルミネッセンス表示装置 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 19876887 Country of ref document: EP Kind code of ref document: A1 |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 2020553398 Country of ref document: JP |
|
| ENP | Entry into the national phase |
Ref document number: 20217007467 Country of ref document: KR Kind code of ref document: A |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| 122 | Ep: pct application non-entry in european phase |
Ref document number: 19876887 Country of ref document: EP Kind code of ref document: A1 |