WO1998027242A1 - Pieces en acier a grande resistance de charge et leurs procedes de production - Google Patents
Pieces en acier a grande resistance de charge et leurs procedes de production Download PDFInfo
- Publication number
- WO1998027242A1 WO1998027242A1 PCT/JP1997/004430 JP9704430W WO9827242A1 WO 1998027242 A1 WO1998027242 A1 WO 1998027242A1 JP 9704430 W JP9704430 W JP 9704430W WO 9827242 A1 WO9827242 A1 WO 9827242A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- steel
- surface pressure
- pressure resistance
- weight
- high surface
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- F—MECHANICAL ENGINEERING; LIGHTING; HEATING; WEAPONS; BLASTING
- F16—ENGINEERING ELEMENTS AND UNITS; GENERAL MEASURES FOR PRODUCING AND MAINTAINING EFFECTIVE FUNCTIONING OF MACHINES OR INSTALLATIONS; THERMAL INSULATION IN GENERAL
- F16C—SHAFTS; FLEXIBLE SHAFTS; ELEMENTS OR CRANKSHAFT MECHANISMS; ROTARY BODIES OTHER THAN GEARING ELEMENTS; BEARINGS
- F16C33/00—Parts of bearings; Special methods for making bearings or parts thereof
- F16C33/30—Parts of ball or roller bearings
-
- C—CHEMISTRY; METALLURGY
- C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
- C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
- C23C8/00—Solid state diffusion of only non-metal elements into metallic material surfaces; Chemical surface treatment of metallic material by reaction of the surface with a reactive gas, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals
- C23C8/06—Solid state diffusion of only non-metal elements into metallic material surfaces; Chemical surface treatment of metallic material by reaction of the surface with a reactive gas, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals using gases
- C23C8/28—Solid state diffusion of only non-metal elements into metallic material surfaces; Chemical surface treatment of metallic material by reaction of the surface with a reactive gas, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals using gases more than one element being applied in one step
-
- C—CHEMISTRY; METALLURGY
- C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
- C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
- C23C8/00—Solid state diffusion of only non-metal elements into metallic material surfaces; Chemical surface treatment of metallic material by reaction of the surface with a reactive gas, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals
- C23C8/06—Solid state diffusion of only non-metal elements into metallic material surfaces; Chemical surface treatment of metallic material by reaction of the surface with a reactive gas, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals using gases
- C23C8/28—Solid state diffusion of only non-metal elements into metallic material surfaces; Chemical surface treatment of metallic material by reaction of the surface with a reactive gas, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals using gases more than one element being applied in one step
- C23C8/30—Carbo-nitriding
- C23C8/32—Carbo-nitriding of ferrous surfaces
-
- C—CHEMISTRY; METALLURGY
- C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
- C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
- C23C8/00—Solid state diffusion of only non-metal elements into metallic material surfaces; Chemical surface treatment of metallic material by reaction of the surface with a reactive gas, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals
- C23C8/06—Solid state diffusion of only non-metal elements into metallic material surfaces; Chemical surface treatment of metallic material by reaction of the surface with a reactive gas, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals using gases
- C23C8/34—Solid state diffusion of only non-metal elements into metallic material surfaces; Chemical surface treatment of metallic material by reaction of the surface with a reactive gas, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals using gases more than one element being applied in more than one step
-
- C—CHEMISTRY; METALLURGY
- C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
- C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
- C23C8/00—Solid state diffusion of only non-metal elements into metallic material surfaces; Chemical surface treatment of metallic material by reaction of the surface with a reactive gas, leaving reaction products of surface material in the coating, e.g. conversion coatings, passivation of metals
- C23C8/80—After-treatment
-
- F—MECHANICAL ENGINEERING; LIGHTING; HEATING; WEAPONS; BLASTING
- F16—ENGINEERING ELEMENTS AND UNITS; GENERAL MEASURES FOR PRODUCING AND MAINTAINING EFFECTIVE FUNCTIONING OF MACHINES OR INSTALLATIONS; THERMAL INSULATION IN GENERAL
- F16C—SHAFTS; FLEXIBLE SHAFTS; ELEMENTS OR CRANKSHAFT MECHANISMS; ROTARY BODIES OTHER THAN GEARING ELEMENTS; BEARINGS
- F16C2204/00—Metallic materials; Alloys
- F16C2204/60—Ferrous alloys, e.g. steel alloys
- F16C2204/62—Low carbon steel, i.e. carbon content below 0.4 wt%
Definitions
- the present invention relates to a steel component for high surface pressure resistance applied to a driving force transmission component requiring contact fatigue strength and wear resistance such as a rolling element such as a gear and a bearing and races and cam components thereof, and a method of manufacturing the same. It is about. Background art
- High contact fatigue strength is also required for gears, bearings, etc. in power transmission components used in automobiles and construction machinery.
- gears are carburized and nitrided. It is usually practiced to harden the surface by using a method such as the one described above.
- material measures such as aggressive addition of Mo to steel to increase the surface hardness and increase the temper softening resistance have been adopted through the guidelines for increasing the surface pressure strength.
- the surface hardness is further increased, and the hardness is reduced due to heat generated based on micro-shear deformation due to rolling with sliding or simply rolling friction or contact stress (Hertz stress).
- various measures have been widely studied to increase the surface pressure strength by carburizing steel to which a higher tempering softening resistance element, for example, Mo, is added than in the past.
- a higher tempering softening resistance element for example, Mo
- the contact stress increases, the oil film thickness on the contact surface becomes thinner, and as a result, the wear force increases due to the deterioration of lubrication, and the heat generation and the greater contact stress increase.
- problems such as the occurrence of fracture shear stress, and a large and sufficient improvement in surface pressure strength cannot be expected.
- there is also a problem that the addition of a large amount of an element such as Mo that enhances the resistance to temper softening causes a remarkable increase in steel material cost.
- high carbon carburization in which the cementite phase is dispersed and deposited at a high density on the surface layer by carburizing, but examples of applying high-concentration carburizing to gear wheels, and fine cementitious spheroidization
- the Cr component concentration is increased to 2 to 8% by weight, and further, 0.5 to 4% by weight Ni, 0.01 to 0.5%.
- % By weight Nb, 0.1 to 2% by weight V, 0.05 to 1% by weight At least one of Mo is added to make the surface carbon concentration after carburizing 2.0% or more.
- Japanese Patent Application Laid-Open No. Hei 8-120438 discloses a technique relating to a material and a method for improving the design of an expensive alloy while suppressing the generation of an incompletely quenched layer during quenching.
- the surface carbon content is set to 1.5% by weight or less in order to prevent the precipitated carbide from growing and condensing over 5 m. Because the content is less than 5% by weight, the amount of carbide precipitation is set to be as low as less than 7% by volume, and the nitrogen that has been infiltrated is also effectively nitrided or carbonitrided. It is not used as a strengthening measure by precipitation, and most of the permeated nitrogen forms a solid solution in the austenite of the parent phase and only functions as a function to prevent the formation of an incomplete quenched layer during quenching. .
- a method similar to the above-mentioned publication is also disclosed in Japanese Patent Application Laid-Open No. H8-37020, in which a large amount of cementite is precipitated.
- quenching From the viewpoint of ensuring high cement content, high concentrations of Ni, which facilitates the discharge of cement cement and enhances hardenability, and Mo, which reduces the degree of concentration in cementite and effectively enhances hardenability, are shown.
- bearing products such as bearings are designed to reduce oxide, nitride and sulfide inclusions in steel in order to improve rolling life. Desulfurization and desalination using gas and special slag are carried out in many stages and bearing steel with high cleanliness is often used, and generally oxides of 10 to 20 m size are used.
- the present invention has been made to solve such a problem, and has high strength and compactness of gears, cams, bearing parts, and the like that require rolling strength and abrasion resistance accompanied by rolling and sliding. It is an object of the present invention to provide a steel part for high surface pressure resistance suitable for steel parts and the production method thereof. Disclosure of the invention
- the steel part for high surface pressure resistance disperses at least one of fine nitrides, carbides and carbonitrides having an average grain size of 3 m or less in a surface structure, Phase martensite leaves It is characterized by having a composite tissue which is finely divided and finely divided by these dispersions.
- the martensite leaf of the parent phase is required.
- carbide (cement cement) of 3 m or less is dispersed to reinforce the hardness of the surface, and the residual austenite amount of 20 to 80% by volume is added as a structural factor toughness.
- processed products are carburized, nitrocarburized or nitrocarburized, and 0.5 to 4.5% by weight (about 2.4 times by volume) of A Quenching from the temperature range where the parent phase is austenite, including the step of precipitating N very finely and the step of precipitating cementite with an average particle size of 3 or less to 30% by volume
- the present invention has a gist in a component for high surface pressure resistance manufactured by performing quenching and tempering and a method for manufacturing the same.
- the nitrogen penetration depth is determined by the maximum contact surface pressure (the maximum It should be arbitrarily adjusted according to the distance from the surface to the position of the maximum shear stress generated by the Rutz surface pressure), but is generally within lmm, preferably 0% because of the economics of carburizing and nitriding. Applies to 5 mm or less.
- Mechanism is a type of response to contact stress that suppresses the occurrence of surface cracks. It has a common problem in that it cannot be an effective means for crack propagation.
- the lens-like martensite leaves with normal carburized and quenched structure are relatively large, ranging from several meters to several tenths of a meter, and low-hardness residual austenite exists around them, and stress concentration tends to occur. Therefore, miniaturization of martensite leaves is considered important.However, even in the case of usual refinement of martensite leaves by refining austenite grains, the limit is at most a few ⁇ m, It is not enough as a remarkable strength improvement measure. Therefore, in the present invention, the main component of the size is 0.1 m or less, and finely divided particles, rods, and needles, and Z or carbonitride are dispersed at a high density of 1 to 15% by volume.
- the width of the leaf is significantly reduced to about 1 m or less by incorporating it into the martensite leaf.
- the effect of the obstacle causes the martensite leaf to bend and bend, and the structure can be changed from a simple lens-shaped martensite leaf to a fine irregularly shaped martensite, thereby exhibiting resistance to crack propagation.
- This effect also exerts a fine dispersion effect on the distribution of residual austenite present around the martensite leaves, and the residual austenite is partially dispersed by the contact stress.
- the transformation to ultra-fine and irregular martensite during transformation also has the effect of substantially reducing the stress concentration when large lenticular martensite leaves collide with each other. This leads to the relaxation and dispersion of the concentration of tensile residual stress in the residual austenite existing in the surrounding area, so it is considered that it also acts as an anti-power against crack growth along the martensite leaf.
- the dispersion requires significantly finer precipitates than the previously disclosed cementite (as shown in Photo 1 below, depending on the precipitation of cementite grains, the fineness of martensite may be reduced). ),
- the solid solubility in the matrix austenite is remarkably small, and the free energy of forming a dispersion from the parent phase is significantly larger than that of cementite (more stable).
- the surface pressure strength and the abrasion resistance are improved. It is also possible to combine well-known techniques, for example, by dispersing cementite of several meters in high concentration by carburizing to secure surface hardness.
- a bearing steel such as SUJ2 has a structure in which granular cementite with an average particle size of 0.3 to 1.0 O ⁇ m is dispersed in a volume fraction of about 1 to 2.5% by volume.
- the martensite shape in the inserted tissue is a lens-like martensite leaf, and it can be seen that with such a size and amount of granular cementite, the shape improvement of the martensite leaf as in the present invention cannot be achieved.
- V is added at a maximum amount of 1% by weight in the disclosed range, it will About 0.5% by weight of the steel already precipitates as VC special carbide at the steel material stage, 0.28% by weight of V forms a solid solution in austenite, and the remaining 0.22% by weight is fine during carburizing. Although it is estimated that the carbide precipitates as a fine carbide, the amount of precipitation of the VC carbide is about 0.25% by volume, which is small compared to the amount of cementite precipitation in the example. It can be seen that there is no significant effect on the shape of the matrix martensite.
- the steel of the present invention is carburized and nitrocarburized and then quenched to reduce the amount of residual austenite in the surface layer to 10 to 15% by volume by shot peening.
- the residual austenite amount was set to 20% by volume or more, and the upper limit of the residual austenite was set to 80% by volume. If the content is more than 80% by volume, the wear resistance starts to deteriorate.
- the amount of residual austenite is preferably 20 to 60% by volume.
- Quantitative control of residual austenite is carried out by controlling the carbon potential and the nitrogen potential during carburizing / nitriding or nitriding, but also by applying physical pressing means such as a shot or roll to the surface.
- the residual austenite phase was transformed into martensite by thermal means such as heat treatment and sub-zero treatment, and finally adjusted from the viewpoint of optimizing the surface hardness.
- 81 is contained in an amount of 0.3 to 3.0% by weight, and nitrogen on the surface is contained in an amount of 0.4 to 2.5% by weight. However, it is preferable to contain 0.7 to 1.7% by weight from the relation of the amount of A1 to be described later.
- the addition amount of A 1 is 0.2% by weight or more, the fine effect of the martensite is confirmed, the effect of improving the surface pressure strength can be confirmed, and the upper limit of the addition amount is in a very strict range.
- nitride dispersion can be expected for V from the effect of the addition of A 1, but the effective V that can act on nitride dispersion as described above is substantially 0.2% by weight or less.
- A1 doesn't have as much functionality as expected.
- carbide cement cement
- carbide cement cement
- the average particle size of the precipitated cementite is adjusted to 3 zm or less, with a content of 0.5 to 5.0% by weight. .
- V addition is set to 110 ° C. (common sense) in the case where the main purpose is not to precipitate nitrides but to make the cementite finer on the surface as described above. Assuming high-temperature carburization in C, the addition of up to about several wt% is effective, but in the present invention, the upper limit was set to 2 wt% from the viewpoint of cost.
- the A 1 nitride, Z or carbonitride precipitates most finely even at the outermost surface, and the particle diameter increases almost in proportion to the distance as the depth increases. Typically 900 degrees.
- the average particle size is 0.3 m or less within 0.5 mm from the surface, and the shear stress generated by the contact stress is often from the contact surface. There is no problem since it is common to have a maximum value within 0.5 mm.
- the remarkably improved tempering softening resistance of martensite in which very fine A1 nitrides and Z or carbonitrides are dispersed at high density also contributes to the improvement of surface pressure strength. You can see that.
- the martensite divided by the fine A1 nitride, Z or carbonitride is divided into approximately 1 m in the length of the martensite leaf in the vicinity of the outermost surface, and is unclear by an optical microscope. It is considered that the structure becomes finer as it becomes a microstructure and has a remarkable effect on the occurrence of fatigue cracks on the surface.
- the carbon concentration on the surface during carburizing and nitriding or nitriding is set to at least 0.6% by weight to obtain surface hardness, but the nitrogen concentration is set to at least 20% by volume of residual austenite.
- the content was adjusted to 0.4% by weight or more for the purpose of adjustment.
- the upper limit of the nitrogen content was made to fluctuate greatly depending on the maximum addition amount of the A1 concentration, and was set within 2.5% by weight in order to adjust the residual austenite amount to the maximum of 80% by volume.
- the content is 0.7 to 1.7% by weight in view of the above-mentioned A 1 addition amount range.
- Cementite begins to precipitate as the carbon content exceeds about 1.1% by weight, but the average cementite particle size exceeds 3 m to prevent deterioration in roller pitting strength and rotational bending fatigue strength.
- the weight of the cementumite was set at 3.0% by weight at which the precipitation amount of the cementite was about 30% by volume.
- the carbon concentration is increased to 3.0% by weight or more, it becomes difficult to prevent the cementite from agglomerating even by adjusting the addition of Cr and V. As a result, the bending fatigue strength and the pitting strength decrease. Cannot be effectively prevented.
- the distribution coefficient Kr of Cr at 900 ° C is 6.4
- the distribution coefficient K of V is 12.3
- the distribution coefficient Mn of KM n is 2. 1.
- the partition coefficient of Mo, KM o was 3.5
- the partition coefficient of Ni, KN i was 0.22.
- the addition of A 1 has almost no solid solubility in cementite. Does not effectively reduce the cementite size, but the A1 needs to be forcibly discharged from the cementite during the growth of the cementite particles. This is effective when a large amount of A 1 is added as in the present invention.
- a 1 was remarkably concentrated in the matrix austenite, and A 1 nitride and Z or It acts on accelerating the precipitation of carbonitride and exerts a more effective coexistence effect.
- the upper limit of the amount of Cr added was set to 5% by weight or less in consideration of balance between hardenability and cost.
- the steel for machine structural use used in the present invention contains A1 as an essential component, and further adds one or more of V and Cr. In order to impart core strength, other components must be added in the following ranges,
- C is an indispensable element for providing the desired core hardness.
- carbon content of about 0.1 to 0.5% by weight as a steel material is used as a steel material.
- bearing steel is usually used after containing up to 1.2% by weight of carbon and spheroidizing.
- the amount of carbon contained as a material is desirably 0.1 to 1.2% by weight.
- Si is inevitably contained in an amount of about 0.2% by weight as an ordinary element.
- Si is conventionally used as an element for increasing the resistance to temper softening, but usually less than 1% by weight. Used within range.
- a martensite fine effect can be expected by nitriding, but in reality, it can be stopped within 1% by weight because it enhances grain boundary oxidizing property and imparts variation to carburizing property. It is good.
- Mn, Ni, and Mo each have an important role in carburizing / nitriding and Z or hardenability after nitriding, and are also commonly used in the present invention as steel for machine structural use.
- Nb, Ti, and Zr are added in trace amounts for the purpose of refining the crystal grain of the steel material, but it is preferable that they be used in a normal range. It is also expected to exert an effect on fine nitride precipitation as a nitride-forming element like A 1, but as described above, the reactivity with carbon contained in the steel material is high, and the amount of addition is small. Almost all of them are precipitated as carbides before the carbo-nitriding and / or nitriding treatment, and due to the actual penetration of nitrogen, a large amount of addition is required to precipitate nitrides, which is very costly. In the present invention, The addition amount is limited to the range of 0 to 0.1% by weight only for the purpose of use for grain refinement.
- C a, S and P b are usually added for the purpose of improving machinability.
- the amount of residual austenite in the vicinity of the surface layer after quenching is mainly controlled by controlling the amount of surface carbon and the amount of surface nitrogen by carbonitriding and Z or nitriding.
- the amount of residual austenite can be adjusted by physical or thermal means such as shot pinning and sub-zero treatment.
- the amount of residual austenite is reduced to approximately 10% by volume or less by X-ray analysis from the surface layer due to shot peening, the rolling life tends to increase, and the rolling life tends to increase by 20% by volume. Due to the above, there is a tendency that stable surface pressure strength can be obtained.
- the preferred volume% is 20 to 60% by volume in the region up to the outermost surface of 50 m, and 20 to 80% by volume at a depth of 0.5 mm.
- carburizing, carburizing and nitriding and Z or nitriding are applied to the present invention, they are generally carburized once at a temperature of 900 ° C or more, and then cooled to a temperature around 850 ° C. After cooling, ammonia gas is additionally added to form a carburizing or nitriding atmosphere to prevent decarburization or to perform nitriding under carburizing conditions.
- ammonia gas is additionally added to form a carburizing or nitriding atmosphere to prevent decarburization or to perform nitriding under carburizing conditions.
- the carburizing and nitriding treatment and the Z or nitriding treatment method applied to the present invention are not particularly limited, and include normal gas carburizing and nitriding, gas nitriding and carburizing and nitriding in a reduced-pressure gas atmosphere, and It is only necessary to be able to carry out the above-mentioned carburizing and nitriding, such as carburizing and nitriding in a plasma atmosphere, with appropriate changes so as to satisfy the above conditions.
- ultra-fine nitrides can be formed in the carbon or carbonitriding and Z or nitriding treatment to form a gear or a bearing rolling surface surface layer.
- a powerful nitriding element such as Al and V effectively, ultra-fine nitrides can be formed in the carbon or carbonitriding and Z or nitriding treatment to form a gear or a bearing rolling surface surface layer.
- the irregular needle-like martensite finely divided by the precipitated nitride or carbonitride is formed in the matrix, so that it is near the surface during rolling.
- the precipitate can be made extremely fine, and It was found that the steel had no reactivity with carbon originally contained therein, and that almost all of the added amount could efficiently utilize precipitates during the carbonitriding and Z or nitriding treatment reactions.
- the carburizing and nitriding by oil quenching, water quenching, etc., and quenching and hardening of the Z or the nitriding portion are performed to obtain the A 1 nitride and A hardened layer in which the carbonitrides are deposited very finely and the martensite leaves are refined is obtained, and the pitting resistance is excellent.
- the quenching method it is preferable to quench the steel from a temperature at or above the A1 point transformation of the steel, or to cool to a temperature below the A1 point and then reheat to a temperature above the A1 point to quench.
- the average crystal grains in the nitrided layer can be easily refined to about 5 m or less by reheating and quenching, and the rotational bending fatigue strength is reduced. Effectively works for improvement.
- FIG. 1 is a side view of a rotating bending test piece which is a steel part for high surface pressure resistance according to one embodiment of the present invention
- FIG. 2 shows a side view (a) of a small roller test piece and a side view (b) of a large roller test piece of a roller pitching test piece of the present embodiment.
- FIG. 3 is an explanatory diagram of the carburizing and nitriding treatment in which cementite is not precipitated during the carburizing period of the present embodiment.
- FIG. 4 is an explanatory view of the carburizing and nitriding treatment for precipitating cementite during the carburizing period of the present embodiment
- FIG. 5 is a diagram of the nitriding treatment of this embodiment
- Fig. 6 shows the results of pitting life surveyed using a small roller subjected to carburizing and nitriding without precipitation of cementite during the carburizing period of the present embodiment
- Fig. 7 shows No. 6 and N of the present embodiment.
- Gold near the surface of 10 Composition comparison photograph showing genus tissue
- FIG. 8 is a high-magnification photograph showing the metal structure at a position 100 m from the outermost surface of the present example
- FIG. 9 is a photograph of the results of nitrogen analysis showing the metal structure on the surface by the present Example EPMA,
- FIG. 10 is a graph showing the results of roller pitting life of a surface carburized portion formed by quenching after carburizing and nitriding of the present embodiment.
- Fig. 11 shows the results of pitting life surveyed using a small roller subjected to carburizing and nitriding to precipitate cementite during the carburizing period of this example.
- FIG. 13 is a graph showing the results of the fatigue strength of a rotary bending test piece subjected to a shot peening treatment after a heat treatment of a carburizing and nitriding treatment in which cementite is not precipitated during the carburizing period of the present example.
- Table 1 shows the component compositions of the steel within the composition range used in the present invention and the steel for the comparative material.
- the carbon content in the test steel ranges from 0.2% by weight, which is often used as an example of case hardened steel for gears, to 1.1% by weight, which is equivalent to SUJ 2 which is a representative of medium carbon steel and bearing steel.
- SUJ 2 which is a representative of medium carbon steel and bearing steel.
- test steels After being melted, hot forged and normalized, these test steels are processed into rotary bending test pieces and small roller pieces for roller pitching tests, as shown in Figs.
- large roller piece for roller pitting test, tempering quenching the SUJ 2 is used to adjust the H R C 6 4 hardness.
- the carburizing and nitriding treatments in this embodiment are performed by the methods shown in Figs. Incidentally, carbonitriding, carbon potential C p during immersion ⁇ management is carried out by adjusting the C_ ⁇ 2 gas concentration carburizing gas composition, nitrogen potential N p is adjusted by varying the ammonia Nia flow Is done.
- Fig. 3 shows that after carburizing at 930 ° C while adjusting Cp to 0.8% by weight, carburizing and nitriding at 850 ° C was performed. Under these conditions, the precipitation of cementite does not occur during carburization, and the A 1 nitride is precipitated during nitriding. However, for steels containing 1% by weight or more of Cr, one A small amount of cementite may precipitate. This is a result of avoiding the difficulty of controlling C 0 2% (0.25%) in the carburizing gas RX gas when controlling Cp, and reducing the substantial A 1 addition effect. There is no problem to confirm.
- Fig. 4 shows that Cp was set to 1.4% by weight to actively promote the precipitation of cementite even during the carburization period, and at the same time, to reduce the A1 nitride by nitriding at 850 ° C. Is intended to be deposited.
- Fig. 5 shows the results of nitriding at 830 ° C for No. 8,12 of high carbon bearing steel level.
- the tempering treatment at all levels was unified under the condition of 160 ° C x 2 hours.
- the infiltration nitrogen was unified so that the depth of permeated nitrogen was approximately 0.2 mm by the nitriding time at 850 ° C.
- the cross section of the test piece was calibrated.
- Timely analysis by EPMA X-ray microanalyzer-1 using the Optical microscopes and scanning electron microscopes are used at appropriate times to observe A1 nitride, Z or carbonitride deposited in the layer near the surface, and to observe martensite structure.
- the number of surface rotations is set higher than the number of rotations of the outer blade 3.
- the measurement of the amount of residual austenite / residual stress at each position near the surface bath was performed by electrolytic polishing from the surface.
- the conditions for the roller pitting fatigue test were as follows, while pressing a large piece of SUJ 2 on a small roller of the test steel as shown in Fig. 2, while rotating at a rotation speed of 100 rpm and a slip ratio of 40%. was fixed, and the surface pressure strength was evaluated while adjusting the surface pressure appropriately in the range of 250 to 3775 kg / mm 2 .
- the condition for determining the occurrence of pitching was evaluated by the number of rotations until one pitch defect occurred on the small roller. Incidentally, Ran'au preparative number of roller pitching was 2 0 ⁇ 3 0 X 1 0 6 times.
- the rotary bending fatigue strength was evaluated bending fatigue strength of 2 OX 1 0 6 times rotation speed 3 6 0 0 rpm as Ran'au preparative conditions.
- Fig. 6 shows the pitting life investigated using a small roller piece carburized and nitrided under the conditions shown in Fig. 3.
- the lower limit of the variance of the pitting life can be shown by the broken line in FIG.
- the roller pitting life of No. 1, 4, 5, 6 : 7, 8 containing 0.3% by weight or more clearly increases with the increase in the amount of A1 added.
- No. 4, 6 containing almost 1% by weight of A 1 has extremely high strength, which is almost completely run-out even at the maximum Hertzian surface pressure of 37.5 kg / mm 2 in this embodiment.
- FIG. 7 shows a composition comparison showing a metal structure near the surface of No. 10 of a comparative material with a typical A1 added material No. 6.
- martensite is precipitated extremely finely in the vicinity of the outermost surface of No. 6, and the average length of the martensite leaf is reduced to about 1 ⁇ or less.
- the martensite leaves seen in a needle shape under an optical microscope consist of a series of these fine and ultra-fine martensites, showing a clear difference in the morphology between the comparative material and the martensite leaves.
- FIG. 8 shows a high-magnification photograph showing the metallographic structure at a position of 100 m from the outermost surface.
- the average particles uniformly dispersed were less than 0.3 m. It was found that A1 nitrides were contained, and these fine A1 nitrides and dispersions of Z or carbonitride finely divided the martensite leaf to about 1 / xm or less in width, and as a result It can be seen that it is an irregularly shaped martensite leaf.
- a small amount of cementite with a particle size of about 0.1 to 0.2 is precipitated, but the shape of the martensite leaf is substantially a very linear lens-like martensite leaf.
- Fig. 9 shows the results of nitrogen analysis showing the metal structure on the surface by EPMA.
- the results are 1.2% by weight in No. 6 and 0.7% by weight in No. 11.
- the surface nitrogen concentration of each test piece varies greatly with the A1 concentration, but the amount of the change is based on the assumption that all the added A1 becomes A1N, and the stoichiometric composition of A1N Is almost equal to the amount of nitrogen calculated from The carbon content is almost as intended.
- the amount of residual austenite in the surface layer of No. 6, 11 is approximately in the range of 40 to 60% by volume.
- the amount of residual austenite at a position 20 m from the outermost surface is about 12% by volume larger in No. 6 to which A 1 is added than in No. 11.
- the amount of retained austenite is greatly affected by the amount of nitrogen infiltrated in the hardened structure after carburizing and nitriding. I have confirmed.
- Fig. 10 shows the results of the carburizing and nitriding treatment of No. 6 with 0.2 mm in order to confirm the effect on the roller pitting life of the surface nitriding portion formed by quenching after carburizing and nitriding.
- the results of pitching when the part was removed from the surface by 0.10 mm and 0.15 mm were shown. So in addition, the pitching result when the shot apnea was applied to the surface layer of No. 6 at an arc height of 0.9 to reduce the residual austenite amount on the surface to about 14% was also added. Shown.
- the pitching life was remarkably reduced as the amount of removal of the nitrided layer increased, and eventually became almost the same as the carbonitriding strength of the comparative material without the result of martensite refinement by A1 nitride. You can see it.
- reduction of the residual austenite amount of shots peening also are particularly reduces the pitching grayed life at the highest surface pressure 3 7 5 kg / mm 2 in the embodiment, not as pronounced as the effect of removing immersion ⁇ I understood that.
- shot peening has the effect of remarkably hardening the surface and the effect of generating high compressive residual stress, and is a factor that increases pitting strength, wear resistance, and bending fatigue strength. Since the effect of the positive surface can also be expected, it is preferable to use it within the range where the amount of residual austenite on the surface does not fall below about 20% by volume.
- Fig. 5 shows the results of pitting after nitriding treatment shown in Fig. 5 for bearing steel levels of No. 8 and 12 where the steel material has a high carbon concentration and has already precipitated cementite.
- the pitching life lower limit line shown by the broken line in Fig. 6 is also shown in Fig. 11 as a life evaluation standard.
- the surface carbon content of No. 2, 6, 11 is 1.5 to 1.8% by weight, and the structure is such that cementite having an average particle size of 2 to 5 // m is precipitated.
- the surface carbon content of Nos. 1 and 4 is in the range of 2.3 to 2.6% by weight, and is a structure in which cementite with an average particle size of 1.5 to 2.5 m is precipitated.
- the SCM4200H comparative material of No. 11 is 5 m and the one of No. 3 is 2.5 m, and as the Cr content increases, the precipitated cement particles become finer. This is consistent with the trend reported in the past, but the effect of further refinement of cementite was confirmed for steels to which A1 was added. Further, it can be understood that the improvement effect of the pitting life is almost rational from the viewpoint of the difference between the carbon content and the cementite particle size and the systematic effect of the precipitation effect of A 1 nitride.
- Figure 12 shows the rotational bending fatigue strength of N0.6, 11 after the heat treatment of Fig.3.
- the results in Fig. 12 show that there is no such concern. This is because the size of the deposited A 1 nitride is very small, less than 0.3 m.
- the figure also shows the rotational bending fatigue strength when shot beaning is performed at an arc height of 0.9, but the effect is almost the same as that of No.
- Fig. 13 shows the rotation of No. 3, 4, 6, 11 after the heat treatment of Fig. 4.
- the results of bending fatigue strength are compared and shown.
- cementite having an average particle size of about 5 m is precipitated on the surface of No.
- the rotational bending strength of No. 11 is about 10% compared to the case where no cementite is precipitated.
- a decrease in strength was observed.
- N0.6 in which the cementite particle size was reduced to about 2 m by the addition of A1
- the strength of the cementite hardly decreased, so that when cementite was deposited on the surface and used, cementite was not used.
- Fig. 13 also shows the fatigue strength when the rotating bending test piece after heat treatment of No. 6, 11 was subjected to shot peening with an arc height of 0.9. On the other hand, a large improvement effect cannot be achieved for No. 11 with a large cementite grain size, while the remarkable rotational bending fatigue strength of N0.6 with fine cementite precipitates. From the viewpoint of fatigue strength, it is important to reduce the average particle size of cementite to 3 m or less, but it is more important to eliminate cementite aggregates from the viewpoint of fatigue strength. I understood. Furthermore, Fig. 13 also shows the rotational bending fatigue strength after heat treatment of Fig. 4 for Nos.
- the ultrafine precipitates such as A1 nitrides are precipitated by carburizing and nitriding or nitriding, and then the martensite leaves formed by quenching are refined.
- fatigue fracture caused by contact stress was significantly improved.
- A1 is discharged from the cementite granules without impairing the hardenability of the mother phase, and the precipitated cementite is not impaired. It has the effect of making the evening grain finer and also has an effective effect on the precipitation of A1 nitride due to nitriding, making it possible to significantly improve the average life in rolling fatigue. ing.
- the present invention is suitable for steel parts for high strength, compactness, etc. of gears, cams, bearing parts and the like that require rolling strength and abrasion resistance involving rolling and sliding.
Landscapes
- Chemical & Material Sciences (AREA)
- Engineering & Computer Science (AREA)
- Mechanical Engineering (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Materials Engineering (AREA)
- Metallurgy (AREA)
- Organic Chemistry (AREA)
- General Engineering & Computer Science (AREA)
- Solid-Phase Diffusion Into Metallic Material Surfaces (AREA)
- Heat Treatment Of Articles (AREA)
Priority Applications (3)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| DE69723302T DE69723302T2 (de) | 1996-12-17 | 1997-12-03 | Stahlteile mit guter widerstandsfähigkeit gegen oberflächendruck und verfahren zur herstellung |
| EP97946091A EP0950723B1 (en) | 1996-12-17 | 1997-12-03 | High bearing-strength steel parts and processes for the production thereof |
| US09/319,999 US6413328B2 (en) | 1996-12-17 | 1997-12-03 | High surface pressure resistant steel parts and methods of producing same |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP8/354150 | 1996-12-17 | ||
| JP35415096A JP3909902B2 (ja) | 1996-12-17 | 1996-12-17 | 高耐面圧用鋼部品およびその製造方法 |
Related Child Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| US09/707,933 Division US6447619B1 (en) | 1996-12-17 | 2000-11-08 | High surface pressure resistant steel parts and methods of producing same |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO1998027242A1 true WO1998027242A1 (fr) | 1998-06-25 |
Family
ID=18435629
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP1997/004430 Ceased WO1998027242A1 (fr) | 1996-12-17 | 1997-12-03 | Pieces en acier a grande resistance de charge et leurs procedes de production |
Country Status (6)
| Country | Link |
|---|---|
| US (2) | US6413328B2 (enExample) |
| EP (2) | EP0950723B1 (enExample) |
| JP (1) | JP3909902B2 (enExample) |
| KR (1) | KR100504705B1 (enExample) |
| DE (2) | DE69736020T2 (enExample) |
| WO (1) | WO1998027242A1 (enExample) |
Families Citing this family (73)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US6474751B1 (en) | 1995-12-26 | 2002-11-05 | Denso Corporation | Hydraulic circuit having a rotary type pump and brake apparatus for a vehicle provided with the same |
| JP3909902B2 (ja) * | 1996-12-17 | 2007-04-25 | 株式会社小松製作所 | 高耐面圧用鋼部品およびその製造方法 |
| JP3894635B2 (ja) | 1997-08-11 | 2007-03-22 | 株式会社小松製作所 | 浸炭部材とその製造方法並びに浸炭処理システム |
| JP4100751B2 (ja) | 1998-01-30 | 2008-06-11 | 株式会社小松製作所 | 転動部材とその製造方法 |
| JP4022607B2 (ja) * | 1999-07-21 | 2007-12-19 | 日産自動車株式会社 | 耐高面圧部材の製造方法 |
| IT1309928B1 (it) * | 1999-12-01 | 2002-02-05 | Bundy S P A | Tubo per impianti di alimentazione di fluidi a pressione, inparticolare per l'alimentazione di carburante nei motori diesel, |
| WO2002038984A1 (fr) * | 2000-11-13 | 2002-05-16 | Nsk Ltd. | Transmission a variation continue toroidale et procede de production de la transmission |
| US20030075244A1 (en) * | 2001-05-17 | 2003-04-24 | Nissan Motor Co., Ltd. | Bearing pressure-resistant member and process for making the same |
| US7438477B2 (en) | 2001-11-29 | 2008-10-21 | Ntn Corporation | Bearing part, heat treatment method thereof, and rolling bearing |
| JP4812220B2 (ja) * | 2002-05-10 | 2011-11-09 | 株式会社小松製作所 | 高硬度高靭性鋼 |
| JP4166041B2 (ja) * | 2002-06-03 | 2008-10-15 | 株式会社椿本チエイン | 焼結スプロケット及びその製造方法 |
| JP2004076125A (ja) * | 2002-08-21 | 2004-03-11 | Komatsu Ltd | 転動部材 |
| JP3990254B2 (ja) * | 2002-10-17 | 2007-10-10 | Ntn株式会社 | 総ころタイプの転がり軸受 |
| DE60303849T2 (de) * | 2002-10-17 | 2006-11-02 | Ntn Corp. | Vollrolliger radial Wälzlager und Rollennockenfolger für Brennkraftmaschine |
| US7334943B2 (en) | 2003-02-28 | 2008-02-26 | Ntn Corporation | Differential support structure, differential's component, method of manufacturing differential support structure, and method of manufacturing differential's component |
| JP4573535B2 (ja) * | 2003-02-28 | 2010-11-04 | Ntn株式会社 | デファレンシャルの支持構造およびデファレンシャルの構成部品 |
| JP4718781B2 (ja) | 2003-02-28 | 2011-07-06 | Ntn株式会社 | トランスミッションの構成部品および円錐ころ軸受 |
| JP4390576B2 (ja) | 2003-03-04 | 2009-12-24 | 株式会社小松製作所 | 転動部材 |
| JP4390526B2 (ja) | 2003-03-11 | 2009-12-24 | 株式会社小松製作所 | 転動部材およびその製造方法 |
| JP2004301321A (ja) | 2003-03-14 | 2004-10-28 | Ntn Corp | オルタネータ用軸受およびプーリ用軸受 |
| JP4486411B2 (ja) * | 2003-06-05 | 2010-06-23 | Ntn株式会社 | ローラ付きカムフォロア |
| JP4152283B2 (ja) | 2003-08-29 | 2008-09-17 | Ntn株式会社 | 軸受部品の熱処理方法 |
| EP1516940B1 (en) * | 2003-09-18 | 2010-09-15 | Mahindra & Mahindra Ltd. | Method for producing gears and/or shaft components with superior bending fatigue strength and pitting fatigue life from conventional alloy steel |
| US7384488B2 (en) * | 2003-09-18 | 2008-06-10 | Mahindra & Mahindra Ltd | Method for producing gears and/or shaft components with superior bending fatigue strength and pitting fatigue life from conventional alloy steels |
| JP2005163173A (ja) * | 2003-11-14 | 2005-06-23 | Komatsu Ltd | 歯車部材およびその製造方法 |
| US7169238B2 (en) * | 2003-12-22 | 2007-01-30 | Caterpillar Inc | Carbide method and article for hard finishing resulting in improved wear resistance |
| US7594762B2 (en) | 2004-01-09 | 2009-09-29 | Ntn Corporation | Thrust needle roller bearing, support structure receiving thrust load of compressor for car air-conditioner, support structure receiving thrust load of automatic transmission, support structure for continuously variable transmission, and support structure receivin |
| JP4540351B2 (ja) * | 2004-01-15 | 2010-09-08 | Ntn株式会社 | 鋼の熱処理方法および軸受部品の製造方法 |
| JP4799006B2 (ja) * | 2004-03-01 | 2011-10-19 | 株式会社小松製作所 | Fe系シール摺動部材およびその製造方法 |
| JP4799004B2 (ja) * | 2004-03-08 | 2011-10-19 | 株式会社小松製作所 | Fe系シール摺動部材及びその製造方法 |
| JP4820562B2 (ja) * | 2004-04-05 | 2011-11-24 | 株式会社小松製作所 | Fe系耐摩耗摺動材料および摺動部材 |
| DE102004028667A1 (de) * | 2004-06-12 | 2005-12-29 | Ina-Schaeffler Kg | Hebelartiger Nockenfolger |
| FR2883887B1 (fr) * | 2005-04-01 | 2009-02-20 | Snr Roulements Sa | Procede de renforcement par carbonitruration et realisation de deux etapes de transformation de l'austenite en martensite |
| JP2007046717A (ja) | 2005-08-10 | 2007-02-22 | Ntn Corp | ジョイント用爪付き転動軸 |
| CN100425736C (zh) * | 2005-11-30 | 2008-10-15 | 重庆长江轴承股份有限公司 | 高碳铬轴承零件表面化学热处理工艺 |
| JP5061478B2 (ja) * | 2006-03-15 | 2012-10-31 | 日本精工株式会社 | 転がり支持装置 |
| JP2007248397A (ja) * | 2006-03-17 | 2007-09-27 | Seiko Epson Corp | 装飾品および時計 |
| JP2007262506A (ja) * | 2006-03-29 | 2007-10-11 | Komatsu Ltd | 機械部品の製造方法 |
| US7846272B2 (en) * | 2006-04-28 | 2010-12-07 | Gm Global Technology Operations, Inc. | Treated austenitic steel for vehicles |
| DE102006029121A1 (de) * | 2006-06-22 | 2007-08-23 | Mahle International Gmbh | Hitzebeständiger Lagerwerkstoff |
| CN100425737C (zh) * | 2006-08-24 | 2008-10-15 | 李亚明 | 一种钢材表面化学热处理方法 |
| JP5212602B2 (ja) * | 2007-09-14 | 2013-06-19 | セイコーエプソン株式会社 | 機器およびハウジング材の製造方法 |
| US8596875B2 (en) * | 2008-12-12 | 2013-12-03 | Jtekt Corporation | Bearing constituent member and process for producing the same, and rolling bearing having bearing constituent member |
| US20120321503A1 (en) * | 2009-11-30 | 2012-12-20 | Minoru Honjo | Method for manufacturing ingot steel for bearings and bearing steel |
| CN102639736B (zh) * | 2009-11-30 | 2013-11-27 | 杰富意钢铁株式会社 | 轴承钢 |
| EP2514847B1 (en) * | 2010-03-19 | 2014-12-17 | Nippon Steel & Sumitomo Metal Corporation | Surface layer-hardened steel part and method of manufacturing the same |
| US20140041762A1 (en) * | 2011-04-13 | 2014-02-13 | Staffan Larsson | Method of heat treating a steel component |
| CN103597101B (zh) * | 2011-05-25 | 2016-10-12 | Skf公司 | 热处理钢构件的方法 |
| EP2739761B1 (en) | 2011-06-02 | 2017-05-24 | Aktiebolaget SKF | Carbo-nitriding process for martensitic stainless steel and stainless steel article having improved corrosion resistance |
| DE102012204618A1 (de) * | 2012-03-22 | 2013-09-26 | Schaeffler Technologies AG & Co. KG | Wälzlager mit einem Lagerring mit gehärteter Randzone |
| KR101269573B1 (ko) * | 2012-09-11 | 2013-06-05 | 동아대학교 산학협력단 | 고면압강도, 고강도 및 고내식성 철강부품의 제조방법 |
| EP2910657B1 (en) * | 2012-10-17 | 2019-05-01 | NTN Corporation | Bearing element, rolling bearing and process for producing bearing element |
| WO2015073094A2 (en) * | 2013-08-27 | 2015-05-21 | University Of Virginia Patent Foundation | Lattice materials and structures and related methods thereof |
| CN103556108A (zh) * | 2013-11-07 | 2014-02-05 | 山东新金发汽车零部件有限公司 | 一种提高低碳钢氮化产品硬度的方法 |
| KR101839166B1 (ko) * | 2013-12-25 | 2018-03-15 | 주식회사 포스코 | B 첨가강의 침탄질화 열처리 방법 |
| CN104152652A (zh) * | 2014-07-01 | 2014-11-19 | 江苏曙光华阳钻具有限公司 | 无磁钻铤内外壁及两端接头内外螺纹表面强化工艺 |
| KR20170033414A (ko) * | 2014-07-29 | 2017-03-24 | 신닛테츠스미킨 카부시키카이샤 | 침탄 질화 베어링 부품 |
| JP6827914B2 (ja) | 2017-12-18 | 2021-02-10 | Ntn株式会社 | 軸受部品及び転がり軸受 |
| JPWO2019026909A1 (ja) * | 2017-08-03 | 2020-06-25 | アイシン精機株式会社 | 鋼部品の製造方法および鋼部品 |
| JP6626918B2 (ja) | 2018-03-30 | 2019-12-25 | Ntn株式会社 | 軸受部品 |
| CN109182696B (zh) * | 2018-11-21 | 2021-11-05 | 中国航发哈尔滨东安发动机有限公司 | 一种三代渗碳钢材料氮化表面改性方法 |
| JP7681942B2 (ja) | 2019-10-01 | 2025-05-23 | Ntn株式会社 | 軸受部品 |
| US11624106B2 (en) | 2020-03-18 | 2023-04-11 | Caterpillar Inc. | Carburized steel component and carburization process |
| CN112030065B (zh) * | 2020-07-16 | 2021-08-03 | 钢铁研究总院 | 一种渗碳轴承钢及其制备方法 |
| JP7049490B2 (ja) * | 2021-01-19 | 2022-04-06 | Ntn株式会社 | 軸受部品及び転がり軸受 |
| JP7049492B2 (ja) * | 2021-01-19 | 2022-04-06 | Ntn株式会社 | 軸受部品及び転がり軸受 |
| JP7049491B2 (ja) * | 2021-01-19 | 2022-04-06 | Ntn株式会社 | 軸受部品及び転がり軸受 |
| CN114962460A (zh) | 2021-02-25 | 2022-08-30 | 斯凯孚公司 | 经热处理的滚子轴承圈 |
| FR3132720B1 (fr) * | 2022-02-11 | 2024-08-23 | Skf Aerospace France | Procédé de renforcement d’une pièce en acier par carbonitruration |
| JP7420855B2 (ja) * | 2022-03-29 | 2024-01-23 | Ntn株式会社 | 機械部品 |
| CN116334635A (zh) * | 2023-03-28 | 2023-06-27 | 江阴亿达机械制造有限公司 | 一种压裂泵阀箱的内螺纹强化处理工艺 |
| KR20240170090A (ko) * | 2023-05-26 | 2024-12-03 | 현대자동차주식회사 | 절연성능이 향상된 베어링용 강 |
| CN116926441B (zh) * | 2023-06-27 | 2026-07-31 | 河北河钢材料技术研究院有限公司 | 一种高旋转弯曲疲劳强度轴承钢 |
Citations (8)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH02277764A (ja) * | 1989-01-13 | 1990-11-14 | Nippon Seiko Kk | 転がり軸受 |
| JPH0488148A (ja) * | 1990-07-30 | 1992-03-23 | Kobe Steel Ltd | 迅速浸炭可能な高強度歯車用鋼及び高強度歯車 |
| JPH0570925A (ja) * | 1991-09-17 | 1993-03-23 | Nippon Steel Corp | 歪の小さい高強度歯車の浸炭窒化熱処理方法 |
| JPH05320822A (ja) * | 1992-05-22 | 1993-12-07 | Nippon Steel Corp | 接触疲労強度の高い駆動伝達系部品用鋼および駆動伝達系部品の製造方法 |
| JPH0617224A (ja) * | 1992-07-01 | 1994-01-25 | Kobe Steel Ltd | 高温転動疲労性に優れた浸炭軸受部品 |
| JPH073393A (ja) * | 1993-06-17 | 1995-01-06 | Sumitomo Metal Ind Ltd | 転動疲労寿命と製造性に優れた鋼器 |
| JPH083720A (ja) * | 1994-06-16 | 1996-01-09 | Sumitomo Metal Ind Ltd | 転動疲労寿命に優れた鋼製部品とその製造方法 |
| JPH0881734A (ja) * | 1994-09-12 | 1996-03-26 | Daido Steel Co Ltd | 窒化処理用鋼およびその製造方法 |
Family Cites Families (16)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US3928087A (en) * | 1972-11-14 | 1975-12-23 | Armco Steel Corp | Method of strengthening low carbon steel and product thereof |
| GB1471880A (en) * | 1973-10-26 | 1977-04-27 | Air Prod & Chem | Furnace atmosphere for the heat treatment of ferrous metal |
| JP2779170B2 (ja) * | 1988-07-25 | 1998-07-23 | マツダ株式会社 | 浸炭焼入方法 |
| JPH04160135A (ja) | 1990-10-22 | 1992-06-03 | Kobe Steel Ltd | 浸炭用鋼 |
| JPH05148535A (ja) * | 1991-06-07 | 1993-06-15 | Kobe Steel Ltd | 熱処理歪が少なく曲げ疲労強度の優れた表面硬化部品の製造方法 |
| US5427457A (en) * | 1991-07-18 | 1995-06-27 | Nsk Ltd. | Rolling bearing |
| DE4139975C2 (de) * | 1991-12-04 | 2001-02-22 | Ald Vacuum Techn Ag | Verfahren zur Behandlung von legierten Stählen und Refraktärmetallen und Anwendung des Verfahrens |
| JP3232664B2 (ja) * | 1992-07-08 | 2001-11-26 | 日本精工株式会社 | 転がり軸受 |
| DE69314438T2 (de) * | 1992-11-30 | 1998-05-14 | Sumitomo Electric Industries | Niedrig legierter Sinterstahl und Verfahren zu dessen Herstellung |
| NL9300901A (nl) * | 1993-05-26 | 1994-12-16 | Skf Ind Trading & Dev | Werkwijze voor het carbonitreren van staal. |
| JP3593668B2 (ja) * | 1994-06-21 | 2004-11-24 | Ntn株式会社 | 転がり軸受 |
| JP3538995B2 (ja) * | 1994-09-29 | 2004-06-14 | 日本精工株式会社 | 転がり軸受 |
| JPH08120438A (ja) | 1994-10-19 | 1996-05-14 | Kobe Steel Ltd | 機械構造用部品の製造方法 |
| KR100208151B1 (ko) * | 1996-11-14 | 1999-07-15 | 정몽규 | 강의 열처리 방법 |
| JP3909902B2 (ja) * | 1996-12-17 | 2007-04-25 | 株式会社小松製作所 | 高耐面圧用鋼部品およびその製造方法 |
| JP3894635B2 (ja) * | 1997-08-11 | 2007-03-22 | 株式会社小松製作所 | 浸炭部材とその製造方法並びに浸炭処理システム |
-
1996
- 1996-12-17 JP JP35415096A patent/JP3909902B2/ja not_active Expired - Fee Related
-
1997
- 1997-12-03 EP EP97946091A patent/EP0950723B1/en not_active Expired - Lifetime
- 1997-12-03 DE DE69736020T patent/DE69736020T2/de not_active Expired - Fee Related
- 1997-12-03 US US09/319,999 patent/US6413328B2/en not_active Expired - Fee Related
- 1997-12-03 EP EP02014033A patent/EP1273672B1/en not_active Expired - Lifetime
- 1997-12-03 WO PCT/JP1997/004430 patent/WO1998027242A1/ja not_active Ceased
- 1997-12-03 DE DE69723302T patent/DE69723302T2/de not_active Expired - Fee Related
- 1997-12-13 KR KR1019970068571A patent/KR100504705B1/ko not_active Expired - Fee Related
-
2000
- 2000-11-08 US US09/707,933 patent/US6447619B1/en not_active Expired - Lifetime
Patent Citations (8)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH02277764A (ja) * | 1989-01-13 | 1990-11-14 | Nippon Seiko Kk | 転がり軸受 |
| JPH0488148A (ja) * | 1990-07-30 | 1992-03-23 | Kobe Steel Ltd | 迅速浸炭可能な高強度歯車用鋼及び高強度歯車 |
| JPH0570925A (ja) * | 1991-09-17 | 1993-03-23 | Nippon Steel Corp | 歪の小さい高強度歯車の浸炭窒化熱処理方法 |
| JPH05320822A (ja) * | 1992-05-22 | 1993-12-07 | Nippon Steel Corp | 接触疲労強度の高い駆動伝達系部品用鋼および駆動伝達系部品の製造方法 |
| JPH0617224A (ja) * | 1992-07-01 | 1994-01-25 | Kobe Steel Ltd | 高温転動疲労性に優れた浸炭軸受部品 |
| JPH073393A (ja) * | 1993-06-17 | 1995-01-06 | Sumitomo Metal Ind Ltd | 転動疲労寿命と製造性に優れた鋼器 |
| JPH083720A (ja) * | 1994-06-16 | 1996-01-09 | Sumitomo Metal Ind Ltd | 転動疲労寿命に優れた鋼製部品とその製造方法 |
| JPH0881734A (ja) * | 1994-09-12 | 1996-03-26 | Daido Steel Co Ltd | 窒化処理用鋼およびその製造方法 |
Non-Patent Citations (1)
| Title |
|---|
| See also references of EP0950723A4 * |
Also Published As
| Publication number | Publication date |
|---|---|
| KR100504705B1 (ko) | 2005-11-08 |
| US6413328B2 (en) | 2002-07-02 |
| EP1273672A1 (en) | 2003-01-08 |
| US6447619B1 (en) | 2002-09-10 |
| EP0950723A1 (en) | 1999-10-20 |
| EP1273672B1 (en) | 2006-05-31 |
| US20010001396A1 (en) | 2001-05-24 |
| EP0950723A4 (en) | 2001-05-09 |
| KR19980064122A (ko) | 1998-10-07 |
| DE69736020D1 (de) | 2006-07-06 |
| JP3909902B2 (ja) | 2007-04-25 |
| DE69723302T2 (de) | 2004-06-17 |
| JPH10176219A (ja) | 1998-06-30 |
| EP0950723B1 (en) | 2003-07-02 |
| DE69736020T2 (de) | 2006-12-14 |
| DE69723302D1 (de) | 2003-08-07 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP3909902B2 (ja) | 高耐面圧用鋼部品およびその製造方法 | |
| JP4390526B2 (ja) | 転動部材およびその製造方法 | |
| JP4659139B2 (ja) | 高周波焼入れ用鋼 | |
| JP4956146B2 (ja) | 鍛造性と結晶粒粗大化防止特性に優れた肌焼鋼およびその製造方法並びに浸炭部品 | |
| US5427457A (en) | Rolling bearing | |
| CN104220621B (zh) | 耐咬合性优异的齿轮 | |
| JP4964063B2 (ja) | 冷間鍛造性および結晶粒粗大化防止特性に優れた肌焼鋼およびそれから得られる機械部品 | |
| JP2011094169A (ja) | 結晶粒粗大化防止特性に優れた肌焼鋼 | |
| JP2001073072A (ja) | 耐ピッチング性に優れた浸炭窒化部品 | |
| JP5886119B2 (ja) | 肌焼鋼鋼材 | |
| JP2006161144A (ja) | 高温浸炭特性と熱間鍛造性に優れた浸炭用圧延鋼材 | |
| JP4923776B2 (ja) | 転がり、摺動部品およびその製造方法 | |
| JP4413769B2 (ja) | 転がり軸受用鋼 | |
| JP4502929B2 (ja) | 転動疲労特性および結晶粒粗大化防止特性に優れた肌焼用鋼 | |
| JP2006299296A (ja) | 疲労特性と耐結晶粒粗大化特性に優れた肌焼用圧延棒鋼およびその製法 | |
| JP5198765B2 (ja) | 転動部材及びその製造方法 | |
| JP2003113445A (ja) | カム部材およびカムシャフト | |
| JP4940849B2 (ja) | 減圧浸炭部品およびその製造方法 | |
| JP3855418B2 (ja) | 軟窒化用鋼材の製造方法及びその鋼材を用いた軟窒化部品 | |
| JP3849296B2 (ja) | 軟窒化用鋼材の製造方法及びその鋼材を用いた軟窒化部品 | |
| JP3353698B2 (ja) | 軟窒化用鋼材の製造方法及びその鋼材を用いた軟窒化部品 | |
| JP7929355B2 (ja) | 窒化高周波焼入れ用鋼材及び鋼部品 | |
| JP3879251B2 (ja) | 強度と靱性に優れた表面硬化部品の製造方法 | |
| JP2002339039A (ja) | 高硬度鋼部品 | |
| JP2026033923A (ja) | 機械構造用部品 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| AK | Designated states |
Kind code of ref document: A1 Designated state(s): US |
|
| AL | Designated countries for regional patents |
Kind code of ref document: A1 Designated state(s): DE FR GB IT |
|
| DFPE | Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed before 20040101) | ||
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application | ||
| WWE | Wipo information: entry into national phase |
Ref document number: 09319999 Country of ref document: US |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 1997946091 Country of ref document: EP |
|
| WWP | Wipo information: published in national office |
Ref document number: 1997946091 Country of ref document: EP |
|
| WWG | Wipo information: grant in national office |
Ref document number: 1997946091 Country of ref document: EP |