WO1995028366A1 - Silicon nitride/silicon carbide composite powders, their preparation and densified materials prepared using the composite powders - Google Patents
Silicon nitride/silicon carbide composite powders, their preparation and densified materials prepared using the composite powders Download PDFInfo
- Publication number
- WO1995028366A1 WO1995028366A1 PCT/US1995/004573 US9504573W WO9528366A1 WO 1995028366 A1 WO1995028366 A1 WO 1995028366A1 US 9504573 W US9504573 W US 9504573W WO 9528366 A1 WO9528366 A1 WO 9528366A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- powder
- silicon carbide
- silicon nitride
- weight
- range
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B82—NANOTECHNOLOGY
- B82Y—SPECIFIC USES OR APPLICATIONS OF NANOSTRUCTURES; MEASUREMENT OR ANALYSIS OF NANOSTRUCTURES; MANUFACTURE OR TREATMENT OF NANOSTRUCTURES
- B82Y30/00—Nanotechnology for materials or surface science, e.g. nanocomposites
-
- C—CHEMISTRY; METALLURGY
- C01—INORGANIC CHEMISTRY
- C01B—NON-METALLIC ELEMENTS; COMPOUNDS THEREOF; METALLOIDS OR COMPOUNDS THEREOF NOT COVERED BY SUBCLASS C01C
- C01B21/00—Nitrogen; Compounds thereof
- C01B21/06—Binary compounds of nitrogen with metals, with silicon, or with boron, or with carbon, i.e. nitrides; Compounds of nitrogen with more than one metal, silicon or boron
- C01B21/068—Binary compounds of nitrogen with metals, with silicon, or with boron, or with carbon, i.e. nitrides; Compounds of nitrogen with more than one metal, silicon or boron with silicon
- C01B21/0685—Preparation by carboreductive nitridation
-
- C—CHEMISTRY; METALLURGY
- C04—CEMENTS; CONCRETE; ARTIFICIAL STONE; CERAMICS; REFRACTORIES
- C04B—LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE; CERAMICS; REFRACTORIES; TREATMENT OF NATURAL STONE
- C04B35/00—Shaped ceramic products characterised by their composition; Ceramics compositions; Processing powders of inorganic compounds preparatory to the manufacturing of ceramic products
- C04B35/515—Shaped ceramic products characterised by their composition; Ceramics compositions; Processing powders of inorganic compounds preparatory to the manufacturing of ceramic products based on non-oxide ceramics
- C04B35/58—Shaped ceramic products characterised by their composition; Ceramics compositions; Processing powders of inorganic compounds preparatory to the manufacturing of ceramic products based on non-oxide ceramics based on borides, nitrides, i.e. nitrides, oxynitrides, carbonitrides or oxycarbonitrides or silicides
- C04B35/584—Shaped ceramic products characterised by their composition; Ceramics compositions; Processing powders of inorganic compounds preparatory to the manufacturing of ceramic products based on non-oxide ceramics based on borides, nitrides, i.e. nitrides, oxynitrides, carbonitrides or oxycarbonitrides or silicides based on silicon nitride
-
- C—CHEMISTRY; METALLURGY
- C04—CEMENTS; CONCRETE; ARTIFICIAL STONE; CERAMICS; REFRACTORIES
- C04B—LIME, MAGNESIA; SLAG; CEMENTS; COMPOSITIONS THEREOF, e.g. MORTARS, CONCRETE OR LIKE BUILDING MATERIALS; ARTIFICIAL STONE; CERAMICS; REFRACTORIES; TREATMENT OF NATURAL STONE
- C04B35/00—Shaped ceramic products characterised by their composition; Ceramics compositions; Processing powders of inorganic compounds preparatory to the manufacturing of ceramic products
- C04B35/515—Shaped ceramic products characterised by their composition; Ceramics compositions; Processing powders of inorganic compounds preparatory to the manufacturing of ceramic products based on non-oxide ceramics
- C04B35/58—Shaped ceramic products characterised by their composition; Ceramics compositions; Processing powders of inorganic compounds preparatory to the manufacturing of ceramic products based on non-oxide ceramics based on borides, nitrides, i.e. nitrides, oxynitrides, carbonitrides or oxycarbonitrides or silicides
- C04B35/584—Shaped ceramic products characterised by their composition; Ceramics compositions; Processing powders of inorganic compounds preparatory to the manufacturing of ceramic products based on non-oxide ceramics based on borides, nitrides, i.e. nitrides, oxynitrides, carbonitrides or oxycarbonitrides or silicides based on silicon nitride
- C04B35/593—Shaped ceramic products characterised by their composition; Ceramics compositions; Processing powders of inorganic compounds preparatory to the manufacturing of ceramic products based on non-oxide ceramics based on borides, nitrides, i.e. nitrides, oxynitrides, carbonitrides or oxycarbonitrides or silicides based on silicon nitride obtained by pressure sintering
-
- C—CHEMISTRY; METALLURGY
- C01—INORGANIC CHEMISTRY
- C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- C01P2004/00—Particle morphology
- C01P2004/60—Particles characterised by their size
- C01P2004/62—Submicrometer sized, i.e. from 0.1-1 micrometer
-
- C—CHEMISTRY; METALLURGY
- C01—INORGANIC CHEMISTRY
- C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- C01P2004/00—Particle morphology
- C01P2004/60—Particles characterised by their size
- C01P2004/64—Nanometer sized, i.e. from 1-100 nanometer
-
- C—CHEMISTRY; METALLURGY
- C01—INORGANIC CHEMISTRY
- C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- C01P2006/00—Physical properties of inorganic compounds
- C01P2006/10—Solid density
-
- C—CHEMISTRY; METALLURGY
- C01—INORGANIC CHEMISTRY
- C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- C01P2006/00—Physical properties of inorganic compounds
- C01P2006/12—Surface area
Definitions
- the invention relates to synthesis of silicon nitride/silicon carbide (Si3N_ ⁇ SiC) composite powders via carbothermal reduction of a mixture of silica (Si0 2 ) and carbon (C) powders, particularlyto those composite powders wherein the silicon carbide portion contains an amount of nitrogen, and to resulting composite powders.
- the invention also relates to densified bodies, including self-reinforced silicon nitride (SRS) bodies, prepared from the composite powders, especially to those densified by pressureless sintering.
- SRS self-reinforced silicon nitride
- a known method of preparing Si 3 N 4 powder is carbothermal synthesis, a reaction of nitrogen with Si0 2 powder contained in an admixture of Si0 2 and carbon (especially powdered carbon).
- Komeya et al. (U.S. Patent No. 4,428,916) prepare alpha-Si3N 4 ( ⁇ -SJ3N 4 ) powder in a nonoxidizing atmosphere by adding a seed such as Si 3 N powder, SiC powder or silicon oxynitride (SiON) powder, to the admixture.
- a seed such as Si 3 N powder, SiC powder or silicon oxynitride (SiON) powder
- EP 206,795 teaches that addition of silicon (Si) metal increases ⁇ -Si 3 N 4 yield.
- Inoue et al. (U.S. Patent No. 4,514,370) use a Si 3 N 4 seed that is prepared by carbothermal synthesis at a temperature of 1350- 1550° Centigrade (°C).
- JP 63-176,301 uses a Si3N 4 seed having a beta-Si 3 N 4 ( ⁇ -Si 3 N 4 ) content of 5-50 weight percent (wt%), based on seed weight, to prepare Si 3 N 4 powder with a ⁇ -Si 3 N 4 content of 1-20 wt%, based on powder weight.
- JP 80-015,946 discloses use of a carbohydrate, such as sucrose or starch, as a binder for mixed metal oxide powders and calcining the binder to form a carbonaceous residue.
- a second method of preparing Si3 4 powder reacts silicon (Si) metal with nitrogen.
- the resulting powder may contain substantial impurity levels. Although hydrofluoric acid may be used to leach out at least some of these impurities, its use tends to lead to high residual fluorine contents.
- a third method of preparing Si 3 M 4 powder known as diimide synthesis, reacts a halogenated silane compound and a nitrogen compound such as ammonia.
- the resulting powder has a residual chlorine content of at least 10 parts per million (ppm) of powder.
- a f i rst aspect of the invention is a process for preparing a silicon nitride-silicon carbide composite powder, the silicon carbide portion containing nitrogen, which comprises heating an admixture that comprises crystalline silica powder, carbon powder, and, optionally, crystalline silicon nitride powder to a temperature of from 1350°C to 1600°C in the presence of a nitrogen-containing atmosphere, preferably flowing, for a period of time sufficient to convert the admixture to a composite ⁇ -silicon nitride/silicon carbide powder, the silicon carbide portion of the powder having a mean number diameter within a range of from 10 to 700 nanometers and containing an amount of nitrogen, as determined by parallel electron energy loss spectroscopy, within a range of from 2 to 10 percent by weight of the silicon carbide portion.
- Mean number diameter also known as mean equivalent circular diameter, is a calculated value determined as described by John C. Russ, in Computer-Assisted Microscopy: The Measurement and Analysis of Images, at pages 182 and 192 (1990).
- the admixture is, prior to heating to the temperature of from 1350°C to 1600°C, blended with a binder composition and formed into shaped masses of material that are then converted to calcined masses by heating them to a temperature sufficient to decompose components of the binder composition into a solid carbonaceous residue and maintaining that temperature until evolution of residual gases effectively ceases, the calcined masses having a carbon content that is greater than stoichiometrically required to reduce the silica via carbothermal reduction.
- Shaped masses of material are used interchangeably to refer to a mass or body that has a shape suitable for processing as described herein.
- the shape is not particularly critical and may take on any solid geometric configuration such as spherical, ellipsoidal, cylindrical or conical. Commonly used terms for such shapes include, without limitation, “aggregates”, “granules” and “pellets”. As such, these terms may also be used interchangeably with masses and its equivalents.
- a second aspect of the invention is a silicon nitride-silicon carbide composite powder comprising a silicon nitride phase that is at least 90 percent by weight, based upon phase weight, ⁇ -silicon nitride and a silicon carbide phase that is in the form of particles having a mean number diameter within a range of from 10 to 700 nanometers, the silicon carbide phase having a nitrogen content, as determined by parallel electron energy loss spectroscopy, within a range of from 2 to 10 percent by weight of the silicon carbide portion, the silicon carbide phase being present in an amount of from greater than zero to 50, preferably from 0.01 to 25, more preferably from 0.1 to 15, still more preferably from 1 to 10 percent by weight, based upon composite powder weight, the composite powder having a BET surface area of from 3 to 15 m /g.
- the second aspect also includes silicon nitride-silicon carbide composite powders wherein the silicon carbide phase is in the form of particles having a bimodal distribution, the bimodal distribution having a first distribution peak located at a mean number diameter within a range of from 10 to 200 nm and a second distribution peak located at a mean number diameter within a range of from 200 to 700 nm.
- BET surface area refers to powder or particle surface area as measured by a conventional adsorption method such as that taught by S. Brunauer, P. H. Emmett and E. Teller in Journal of the American Chemical Society, volume 60, page 309 (1938).
- a third aspect of the present invention is a process for preparing a self-reinforced silicon nitride ceramic body which comprises subjecting a powdered admixture of a carbothermal ly synthesized silicon nitride/silicon carbide composite powder, a densification aid, a conversion aid, at least one whisker growth enhancing aid and, optionally, a catalyst to conditions of temperature and pressure sufficient to yield a ceramic body having a density of at least 96 percent of theoretical density and form, in situ, ⁇ -silicon nitride whiskers having an average aspect ratio of at least 2.5, the body having both a granular and an intragranular distribution of residual silicon carbide grains and a fracture toughness of at least 7 MPa m 1 2 , the intragranular silicon carbide grains having a mean number diameter within a range of from 10 to 400 nanometers, at least a portion of the intragranular silicon carbide grains containing nitrogen, as determined by parallel electron energy loss spectroscopy, in an amount that is within
- a fourth aspect of the present invention is a self-reinforced silicon nitride/silicon carbide ceramic body having a density of at least 96 percent of theoretical density and comprising a crystalline phase of ⁇ -silicon nitride of which at least about 20 volume percent, as measured by viewing one plane of the body by scanning electron microscopy, is in the form of whiskers having an average aspect ratio of at least 2.5 and a glassy grain boundary phase in an amount not greater than 35 percent by weight of total body weight, the silicon carbide being distributed, with respect to the ⁇ -silicon nitride whiskers, as granular and intragranular submicrometer grains, the body having a fracture toughness of at least 7 MPa m 1 2 , the intra- granular silicon carbide grains having a mean number diameter within a range of from 10 to 400 nm, at least a portion of the intragranular silicon carbide grains containing nitrogen, as determined by parallel electron energy loss spectroscopy, in an amount that is within a range of from 2 to
- a fifth aspect of the present invention is a silicon nitride-silicon carbide composite powder having a silicon nitride phase and a silicon carbide phase, the silicon nitride phase having a phase purity of > 10% ⁇ -Si 3 N 4 and comprising rod-like ⁇ -Si3N 4 crystallites that have a mean number diameter of about 0.04 ⁇ m, the number diameter ranging from 0.01 to O. I O ⁇ m, and a mean aspect ratio of from 5/1 to 8/1 , ranging from 1.5/1 to 21/1 and ⁇ -Si 3 N crystallites that have a mean number diameter of from 0.1 to 0.2 ⁇ m, the number diameter ranging from 0.03 to 0.5 ⁇ m.
- the composite powders of the fifth aspect are prepared via a modification of the process of the first aspect of the present invention. The modification comprises using a seed Si3 that has a ⁇ -Si3N 4 content in excess of 75 wt%.
- x is a real number within a range of from greater than O to 18 and y is a real number within a range of from O to 1.28.
- a stoichiometric amount of carbon (C) would require x to be 0.
- the real number for x is desirably from 0.6 to 12, preferably from 0.6 to 6.
- the real number for y is desirably from 0.05 to 1.1 , preferably from 0.15 to 0.9, more preferably from 0.2 to 0.8, still more preferably from 0.26 to 0.77, and most preferably from 0.26 to 0.52.
- SiC grains Three terms may be used to describe the distribution of SiC grains relative to Si 3 N 4 grains in sintered bodies containing both.
- Gramular refers to SiC grains dispersed in glassy grain boundary pockets located at triple points between Si3N 4 grains.
- Intragranular refers to SiC grains dispersed within Si3 4 grains.
- Intergranular refers to SiC grains disposed along grain boundaries between two adjacent Si 3 N 4 grains.
- Temperatures and temperature ranges disclosed herein are primarily intended as guidelines. With changes in measurement device, reactor or other apparatus, or location of temperature measurement, some variation is expected. A skilled artisan can readily determine appropriate adjustments of the temperatures or temperature ranges without undue experimentation.
- an admixture suitable for use in preparing silicon nitride-silicon carbide composite materials contains crystalline silica powder, carbon powder and optionally, crystalline silicon nitride powder. Components of the admixture are also referred to as starting materials. Proper selection of carbon and silica sources for use as starting materials and seeding with fine Si 3 N 4 crystallites allow control of the size of Si3 4 and SiC crystallites in resultant composite powders. The size of SiC crystallites depends, to some extent, on starting carbon crystallite size. With all other parameters being equal, as carbon crystallite size decreases so does composite powder SiC crystallite size. SiC crystallite size is largely unaffected by Si0 2 source or the presence or absence of seed.
- Si3 4 crystallites depends heavily upon the presence of seed and the surface area and crystal linity of the starting Si0 2 .
- the size of starting carbon powder has much less, if any, effect on the resulting Si3N 4 crystallite size.
- a high purity composite powder with a SiC grain size (MND) less than about 100 nm, preferably less than about 50 nm, and a Si3N 4 grain size (MND) of about 0.2 ⁇ m can be produced by reacting a seeded (0.2 seed/Si0 2 ratio and high purity ⁇ -phase Si3N ) acetylene carbon black/high purity quartz precursor.
- Si3N 4 crystalli .es tend to contain small pores described as "micropores".
- the starting carbon crystallite size also has an effect upon micropore size.
- an increase in carbon crystallite size leads to a corresponding increase in micropore size.
- Starting material (carbon and silica) purity has a measurable effect upon resultant composite powder purity.
- Each raw material or starting material has a purity that is desirably
- the silica is preferably provided by crystalline quartz that is at least 98.9, more preferably at least 99.5% and most preferably at least 99.8% pure.
- the quartz preferably has a surface area (S.A.) of greater than (>) 0.2 square meters per gram (m /g) and a mean particle
- d5o 15 size by weight percent (wt%), as determined by laser light scattering using a model SPA MICROTRACTM apparatus, of less than 15 micrometers ( ⁇ m). If a different subscript, such as d ⁇ o is used in conjunction with a specified particle size, it means that 10 weight percent of the particles have a particle size less than or equal to the specified size.
- Silica mean particle size may be reduced by milling using a jet mill wherein the wear parts are fabricated from Si3N 4 , SiC
- the Si0 mean particle size (dso) is more preferably less than about 10 ⁇ m.
- the carbon powder used as a starting material has a surface area that is preferably at least 20 m 2 /g, more preferably at least 25 m 2 /g, and most preferably at least 70 m 2 /g.
- Average particle sizes (MND) that correspond respectively to the surface areas are 0.10
- Silica purity and morphology also affect whether the composite powder has ⁇ -Si3N 4 whiskers or fibers protruding from ⁇ -Si3N 4 crystallites.
- the protruding ⁇ -Si3N whiskers occur when the Si0 2 is either amorphous, without regard to purity, or crystalline, but relatively impure.
- crystalline quartz yields ⁇ -Si3N 4 crystallites from which few, if any, ⁇ -SJ3 4 whiskers or fibers protrude.
- silicon nitride-silicon carbide composite powders can be prepared from admixtures that lack crystalline silicon nitride, it is a preferred admixture component.
- the crystalline silicon nitride serves as a seed material.
- One preferred seed material has an ⁇ -Si3N 4 phase content of at least about 90 wt%, preferably at least 95 wt% , based upon Si3N 4 weight, a SiC content of less than about 1.5 wt%, a Si0 2 content of less than about 10 wt%, the SiC and Si0 2 contents being based upon seed material weight, and a surface area of at least 7.5 m 2 /g, preferably at least 10 m 2 /g.
- the SiC and Si0 2 contents are calculated based upon an assumption that all carbon in the composite powder is in the form of SiC and all oxygen in the composite powder is present as Si0 2 . All subsequent references to SiC and Si0 2 content of a composite powder are based upon this assumption. Occasionally, however, other forms of carbon, such as graphite particles or carbon tubes, may be observed.
- a second preferred seed material is a high purity ⁇ -SJ3N 4 /SiC powder prepared by carbothermal synthesis, as described herein, and having a Si 3 N 4 content of at least 95 wt%, and a combination of an amount of SiC and an amount of a Si0 2 , each amount being greater than 0.0 wt%, that totals no more than 5 wt%, all percentages being based on powder weight.
- the seed also has: a surface area of from 3 to 15 m 2 /g, desirably 7.5 m /g; a d-io of from 0.1 to 0.5 ⁇ m, desirably 0.38 ⁇ m; a dso of l ess than 1 ⁇ m, desirably from 0.5 to 1 ⁇ m, and preferably 0.86 ⁇ m; and a dgo of from 1 to 4 ⁇ m, desirably 2.5 ⁇ m.
- the seed is desirably present in an amount sufficient to provide a ratio of seed/Si0 2 that falls within a range of from 0.05: 1 to 1 : 1.
- the ratio is preferably from 0.1 : 1 to 0.6: 1 , more preferably from 0.15: 1 to 0.4: 1 , and most preferably 0.2: 1.
- Athird preferred silicon nitride seed material has a ⁇ -Si 3 N 4 phase content of at least 75 wt% .
- the use of this seed material yields a SisN ⁇ SiC composite powder wherein the Si 3 N4 phase contains both ⁇ -Si3N4 and ⁇ -Si3N 4 , the ⁇ -Si 3 N 4 being present in an amount of at least 10 wt%, based upon total SJ3N 4 content.
- the ⁇ -Si3N 4 is in the form of rod-like ⁇ -SJ3N 4 crystallites that have a MND of about 0.04 ⁇ m, the number diameter ranging from 0.01 to 0.10 ⁇ m, and a mean aspect ratio of from 5/1 to 8/1 , ranging from 1.5/1 to 21/1 and ⁇ -Si3N 4 crystallites that have a MND of from 0.1 to 0.2 ⁇ m, the number diameter ranging from 0.03 to 0.5 ⁇ m.
- the admixture may also include an amount of silicon metal powder.
- the amount should be sufficient to provide a ratio of silicon metal powder to silicon dioxide powder that falls within a range of from 0.05: 1 to 1 : 1.
- the range is preferably from 0.1 : 1 to 0.5: 1.
- the admixtures used to prepare the silicon nitride-silicon carbide composite powders may be heated to a reaction temperature as is.
- the admixtures are, however, preferably blended with a binder composition prior to heating to the reaction temperature.
- the binder composition is desirably a product of a condensation reaction between at least one first reactant that has at least one reactive hydroxyl moiety and at least one second reactant having at least one reactive nitrogen-containing moiety.
- the first reactant is desirably selected from monosaccharides, disaccharides, polysaccharides, starches, modified starches, soy protein, cellulose ethers and cellulose ether derivatives.
- the second reactant is desirably an amine or an amide.
- the first reactant is preferably selected from sucrose, fructose, glucose, mannose, xylose, raffinose, dextrin, amylose, maltose, lactose, arabinose, dextrose, galactose, amylopectin, glucose polymers, xylose polymers, copolymers of glucose and xylose (gluco- xylans), invert sugar, partially invert sugar, molasses from sucrose refining, whey from milk processing, corn syrup, starch, modified starch, methylcellulose, ethylcellulose, hydroxypropyl- methylcellulose, hydroxyethylcellulose, sodium carboxymethylcellulose, carboxymethylcellulose and soy protein.
- the first reactant is more preferably at least one of corn starch, wheat starch, sucrose, fructose, soy protein, and cellulose ethers.
- the second reactant is preferably selected from cyanoguanadine, melamine, urea, hexamethylene tetramine, trimethylamine, diethanolamine, triethanolamine, tetramethylene diamine, acetoguanamine, benzyldimethylamine, methylolmelamine, alkylated methylol- melamine, hexamethoxymethyl melamine, N,N'-dimethyl-p-phenylene diamine, tetraaminobenzene, diaminobenzidine, thiourea, formamide, acetamide, benzamide, oxamide, succinamide, malonamide, guanidine, biuret, triuret, dicyandiamide, biurea, ethylene urea, ammelide, ammeline, aminoguanidine, semicarbazide, thiosemicarbazide and acrylamide.
- the second reactant is more preferably melamine, hexamethylene
- starch and "modified starch”, as used herein, are defined in Condensed Chemical Dictionary. Eleventh Edition, Van Nostrand Reinhold Company, Inc. (1987), at pages 1089-90. The definitions are as follows:
- amylose anhydroglucopyranose units joined by glucosidic bonds
- amylopectin a branched-chain structure.
- Properties White, amorphous, tasteless powder or granules; various crystalline forms may be obtained, including microcrystalline. Irreversible gel formation occurs in hot water; swelling of granules can be induced at room temperature with such compounds as formamide, formic acid, and strong bases and metallic salts.
- any of several water-soluble polymers derived from a starch (corn, potato, tapioca) by acetylation, chlorination, acid hydrolysis, or enzymatic action. These reactions yield starch acetates, esters, and ethers in the form of stable and fluid solutions and films.
- Modified starches are used as textile sizing agents and paper coatings. Thin-boiling starches have high gel strength, oxidized starches made with sodium hypochlorite have low gelling tendency. Introduction of carboxyl, sulfonate, or sulfate groups into starch gives sodium or ammonium salts of anionic starches, yielding clear, non-gelling dispersions of high viscosity. Cationic starches result from addition of amino groups.
- the glucose units of starch can be crosslinked with such agents as formaldehyde, soluble metaphosphates, and epichlorohydrin.
- the admixture of crystalline silica powder, carbon powder, and, optionally crystalline silicon nitride powder may, without any intermediate processing, be heated to a reaction temperature of from 1350°C to 1600°C in the presence of a nitrogen-containing atmosphere, preferably flowing, for a period of time sufficient to convert the admixture to a composite ⁇ -silicon nitride/silicon carbide powder.
- a preferred procedure includes intermediate processing steps prior to heating to the reaction temperature.
- the admixture is added to a binder composition, mixed with water, preferably deionized water, and converted into a blended material using conventional apparatus such as a ball mill that is partially filled with suitable media, preferably Si0 2 -based media.
- the pellets may be of any shape or configuration that does not interfere with further processing. A cylindrical shape provides satisfactory results.
- the nitrogen-containing atmosphere may be established by gaseous nitrogen, gaseous ammonia, gaseous mixtures of nitrogen and ammonia, gaseous mixtures of nitrogen, ammonia or both with an inert or noble gas such as argon, or gaseous mixtures of nitrogen, ammonia or both with hydrogen and, optionally, an inert or noble gas.
- an inert or noble gas such as argon
- gaseous mixtures of nitrogen, ammonia or both with hydrogen and, optionally, an inert or noble gas may be established by gaseous nitrogen, gaseous ammonia, gaseous mixtures of nitrogen and ammonia, gaseous mixtures of nitrogen, ammonia or both with an inert or noble gas.
- the presence of ammonia tends to increase the amount of silicon carbide formed in the composite powders.
- the nitrogen-containing atmosphere may be static or flowing, but is preferably flowing. If the atmosphere is static, it must have a volume sufficient to maintain carbon monoxide generated during carbothermal reduction at a
- a level of carbon monoxide of less than about 3 percent by volume, preferably less than about 1.5 percent by volume, based upon total atmosphere volume is believed to be satisfactory.
- the moist shaped masses are desirably placed in a container such as a quartz boat.
- the container and its contents are then placed in an apparatus, such as a tube furnace, and heated, under flowing nitrogen, inert gas or air, preferably nitrogen, to a temperature and maintained at that temperature for a period of time sufficient to dry the pellets and allow a condensation reaction between the first and second reactantsto occur.
- the time and temperature will vary somewhat depending upon size of the shaped masses, their moisture content, choice of binder composition components and relative amounts of all components of the shaped masses.
- a temperature of 150° Centigrade (°C) and a time of two hours is sufficient. Longer times are generally needed with lower temperatures. Suitable times and temperatures for other reactants, pellet sizes and component ratios are readily determined without undue experimentation.
- the shaped masses are 5 heated to a higher temperature and maintained at that temperature for a period of time sufficient to calcine the shaped masses.
- "calcine” means that the shaped masses are heated under an inert atmosphere, such as that provided by nitrogen or an inert gas such as argon, at a temperature sufficient to decompose components of the binder composition into a carbonaceous residue and maintained at that temperature until evolution 0 of residual gases effectively ceases (approaches a rate of evolution of 0 liters per minute) at that temperature.
- air can be substituted for inert gas at temperatures below that at which carbon will oxidize.
- Calcination temperatures typically range from 250°C o 1000°C, preferably from 300°C to 350°C.
- the shaped masses are heated to a temperature of 330°C over a period of 30 minutes and maintained at that temper- 5 ature for a period of two hours.
- the tube furnace and its contents are then cooled to ambient temperature to yield calcined masses suitable for reaction to provide the composite powders.
- suitable times and temperatures for other reactants, shaped mass sizes and component ratios are readily determined without undue experimentation.
- the admixture or the calcined masses (where the preferred intermediate processing steps are used) is are heated to a reaction temperature of from 1350°C to 1600°C in the presence of a flowing nitrogen-containing atmosphere.
- the calcined masses may be added to a reactor and then heated to the reaction temperature (slow heating) or added directly to a preheated reactor (rapid heating).
- slow heating an aliquot of the calcined masses is suitably placed in a crucible adapted for mixing crucible contents that is then placed in a rotary reactor apparatus prior to heating to the reaction temperature.
- Other apparatus such as a pusher furnace, may also be used.
- the aliquot may be added to a preheated crucible through which a nitrogen- containing gas flows. Rapid heating preferably occurs at a rate of greater than about 100°C/sec and is believed to generate high local concentrations of volatile silicon monoxide (SiO) gas. These concentrations are believed to favor nucleation of ⁇ -Si3N particles over growth of ⁇ -Si3N4 particles. Heating rates of less than 100°C/second, also known as “slow heating", are believed to favor particle growth over particle nucleation.
- the apparatus used for either rapid heating or slow heating is not particularly critical and a skilled artisan can scale up from the apparatus used in succeeding examples to batch or continuous apparatus capable of handling larger quantities of starting material admixtures or calcined masses without undue experimentation.
- the foregoing process may be modified to produce a silicon nitride-silicon carbide composite powder wherein the silicon carbide portion is present as a bimodal distribution.
- the presence of the bimodal distribution may be detected by transmission electron microscopy.
- a suitable modification involves heating to two different reaction temperatures.
- a first reaction temperature, maintained for a first period of time is from 1350°C to less than 1500°C.
- the first period of time is preferably from 120 to 470 minutes and the first temperature is preferably from 1425 to 1490°C.
- a second reaction temperature, maintained for a second period of time that is shorter than the first period of time, is at least 1500°C, but less than about 1600°C.
- the second period of time is from preferably 10 to 120 minutes, and the second temperature is preferably from 1500 to 1600°C.
- Skilled artisans recognize that a multimodal (greater than bimodal) distribution of the silicon carbide portion is attainable by further apportioning of reaction temperatures and allocating appropriate periods of time.
- the bimodal distribution preferably has a first distribution peak and a second distribution peak as determined from transmission electron micrographs.
- the first distribution peak is preferably located at a MND within a range of from 10 to 200 nanometers (nm).
- the second distribution peak is preferably located at a MND within a range of from 200 to 700 nm.
- a second modification of the process provides for early preparation of at least some silicon carbide.
- the second modification like the modification to generate a bimodal distribution of the silicon carbide portion, involves use of more than one reaction temperature. In this modification, heating proceeds to an initial temperature that thermodynamically favors formation of silicon carbide over formation of silicon nitride for a first period of time to generate submicrometer SiC crystallites.
- the initial temperature and the first period of time are sufficient to provide the composite powder with a silicon carbide content that is greater than 0 wt%, but less than about 50 wt%, based upon composite powder weight.
- the silicon carbide is in the form of crystallites having a MND that ranges from 10 nm to 700 nm.
- the initial temperature is preferably within a range of 1500-1550°C and the first period of time is from 1 minute to 45 minutes.
- the second temperature is within a range of from 1350°C to less than 1500°C and the second period of time is from 375 minutes to 419 minutes.
- Modification of the process is not limited to manipulation of the reaction temperature.
- the silicon nitride-silicon carbide composite powder may be subjected to post synthesis procedures.
- One such procedure heats the composite powder to a temperature within a range of from 500°Cto 1000°C in an oxidizing atmosphere for a period of time sufficient to effect removal of excess free carbon.
- the oxidizing atmosphere is established by any gas that will oxidize free carbon into a gaseous phase such as carbon monoxide or hydrogen cyanide at that temperature.
- the gas is suitably air, mixtures of air and nitrogen, o ammonia, carbon dioxide, mixtures of carbon dioxide and carbon monoxide, hydrogen, mixtures of hydrogen and a hydrocarbon, or other oxidizing atmospheres known to those skilled in the art.
- the composite powder After removal of excess free carbon, the composite powder has a silicon nitride phase that is at least 90 percent by weight, based upon silicon nitride phase weight, ⁇ -silicon nitride and a silicon 5 carbide phase.
- the silicon carbide phase is in the form of particles having a MND within a range of from 10 to 700 nanometers.
- the silicon carbide phase is present in an amount of from greater than 0 to 50 percent by weight, based upon composite powder weight, the composite powder having a BET surface area of from 3 to 15 m /g.
- the silicon carbide phase has a nitrogen content, as determined by parallel electron energy loss spectroscopy, within a range 0 of from 2 to 10 percent by weight of the silicon carbide portion
- a second procedure which may be used in place of, or subsequent to, the procedure to remove excess carbon subjects the composite powderto a heat treatment in the presence of nitrogen or an inert gas such as argon (or mixtures thereof), preferably flowing, at a temperature within a range of from 1400°C to 1500°C in a nonoxidizing atmosphere for a 5 period of time sufficient to cause at least a portion of residual silicon dioxide to react with at least a portion of the silicon carbide.
- the heat treatment yields a composite powder with an increased silicon nitride content relative to the composite powder prior to the heat treatment.
- the period of time falls within a range that is desirably from more than five minutes to at least 24 hours, preferably from 4 hours to 12 hours.
- the composite powders may be subjected to additional post synthesis processing after the heat treatment.
- the additional processing may include washing, leaching, grinding or a combination thereof.
- starting materials that contain metallic impurities.
- Advantages may stem from economic considerations or a desire to control final product characteristics. Leaching, or removal of metallic impurities, may be accomplished by treating the heat treated powder with any of a variety of acids such as hydrochloric acid, hydrofluoric acid or nitric acid. Hydrofluoric acid also removes at least a portion of residual Si0 2 in the product.
- a grinding or milling step may be used to control particle size and particle size distribution of the composite powders. Conventional apparatuses, such as an attritor or a ball mill, may be used for grinding.
- the composite powders may be used as a seed for subsequent synthesis of composite powders. If used as a seed, they may be used as synthesized or subsequent to milling.
- Composite powders prepared with high purity starting materials and a high purity ⁇ -Si3N4 seed also have high purity: an ⁇ -Si3N 4 phase purity of at least 95% ; a Si 3 N 4 crystallite MND of less than 0.3 ⁇ m; a surface area that lies within a range of from 8 to 13 m 2 /g; a SiC content within a range of from greater than O to 50, preferably from 0.01 to 25, more preferably from 0.1 to 15, still more preferably from 1 to 10 wt%, based upon powder weight; and a SiC crystallite MND within a range of from 10 to 700 nm, desirably from 10 to 400 nm, and preferably less than 100 nm, more preferably less than 50 nm.
- the Si3 4/SiC composite also has: less than 2 wt% residual oxygen as monatomic O; and residual elemental impurities of less than 100 ppm calcium (Ca), less than 50 ppm iron (Fe), less than 200 ppm (preferably less than 50 ppm) aluminum (Al), less than 20 ppm sulfur (S), less than 50 ppm (preferably less than 10 ppm) fluorine (F), less than 10 ppm potassium (K) and less than 10 ppm chlorine (Cl).
- the ⁇ -Si3N 4 crystallites are substantially free of protruding ⁇ -Si3N 4 fibers.
- ⁇ -Si3 4 crystallites included as a seed in a starting powder mixture affect the size of ⁇ -Si3N 4 crystallites in a product.
- ⁇ -Si3N4 crystallites with a MND of less than 0.3 ⁇ m are prepared by reacting a precursor containing seed ⁇ -Si3N 4 crystallites that have a MND of less than 0.2 ⁇ m and are present in an amount sufficient to establish a precursor seed/Si 0 2 ratio of at least 0.15: 1.
- a unique rod-like ⁇ -Si3N 4 morphology results from a change in the seed material from a high (greater than 90 wt%) ⁇ -phase Si3 4 powder to a high (greater than 75 wt%) ⁇ -phase Si3N powder.
- the use of the latter powder as a seed yields a Si3N_j/SiC composite powder wherein the Si3N 4 phase comprises both ⁇ -Si 3 and ⁇ -SJ3N 4 , the ⁇ -Si3N 4 being present in an amount > 10 wt%, based upon total Si3 4 content.
- the ⁇ -Si 3 N 4 comprises rod-like ⁇ -SJ3N 4 crystallites that have a MND of about 0.04 ⁇ m, the number diameter ranging from 0.01 to 0.10 ⁇ m, and a mean aspect ratio of from 5/1 to 8/1 , ranging from 1.5/1 to 21/1 and ⁇ -Si3 4 crystallites that have a MND of from 0.1 to 0.2 ⁇ m, the number diameter ranging from 0.03 to 0.5 ⁇ m.
- “Powder si nterability” is a relative measure of time required to attain a desired density such as 97 percent of theoretical density.
- a first powder is termed more sinterable than a second powder if the first powder can be sintered to the desired density in a shorter time, under identical sintering conditions and seed/silica ratios, than the second powder.
- Composite powders wherein the Si3N 4 phase comprises both ⁇ -Si 3 N 4 and ⁇ -Si 3 4 , the ⁇ -Si3N 4 being in the form of rod-like crystallites are more sinterable than composite powders prepared with a high ⁇ -phase Si 3 N 4 seed and lacking the rod-like ⁇ -Si 3 N4 crystallites.
- the choice of binder, where used, also has an effect upon powder sinterability. As an illustration, a sucrose-based binder generally yields a more sinterable composite powder than an equivalent amount of a starch-based binder.
- Addition of an amount of silicon (Si) metal powder to a starting material composition provides a measure of control over SiC content of the composite powder without adversely affecting size of the Si 3 N component, especially the ⁇ -Si3 4 component, of the composite powder.
- the starting material composition typically includes Si0 2 , carbon powder, a seed material such as Si3N 4 powder, and a binder.
- a ratio of Si metal weight to total starting material composition weight is desirably from 0.01 : 1 to 1 : 1 , preferably from 0.1 : 1 to 0.5: 1.
- Rapid heating is one means of generating, in situ, fine SiC crystallites that serve as seeds for synthesis of ⁇ -Si 3 4 crystallites.
- the SiC crystallites have a MND that ranges from 10 nm to 700 nm, preferably from 30 nm to 100 nm. A particularly suitable MND is 50 nm.
- the SiC crystallites, particularly the fine crystallites result, at least in part, from initial, rapid heating of starting material compositions to temperatures that thermodynamically favor formation of SiC over formation of Si3N 4 . Temperatures within a range of 1500-1550°C provide acceptable results. Skilled artisans recognize that some SiC also forms at temperatures of less than 1500°C.
- the initial heating is of short duration, suitably from 1 minute to 45 minutes, desirably from 5 minutes to 30 minutes, preferably from 5 to 20 minutes.
- the temperature is preferably reduced to a level that favors formation of SJ3N over SiC. These times and temperatures are suitable for preparation of composite powders having SiC contents of no more than about 25 wt%, based upon composite powder weight. If greater SiC contents are desired, a higher initial temperature, a longer time at the initial temperature, or both should provide satisfactory results.
- a measure of control over composite powder surface area can be gained by varying excess carbon content, seed content or both in the shaped and calcined masses of starting materials (pellets). These parameters affect rates of nucleation and rates of growth of Si3 4 particles.
- a desired composite powder surface area can be attained by adjusting excess carbon content, seed/silica ratio or, preferably, both.
- Post synthesis heat treatment of composite powders may be used to alter powder SiC and Si0 2 contents. It is believed, without intending to be bound thereby, that at least a portion of residual SiC reacts with at least a portion of residual Si0 2 during heating in the presence of nitrogen or an inert gas such as argon (or mixtures thereof), preferably flowing, at a temperature of from 1400°C to 1500°C for a period of time that ranges from less than 4 hours to more than 12 hours.
- a heat treatment time of as few as 5 minutes produces negligible changes in residual SiC and Si0 2 contents and may be uneconomical. Times in excess of 12 hours, such as 24 hours or more, while usable, provide diminishing economic returns.
- Suitable times will vary depending upon the heat treatment temperature as well as upon other variables such as amount of SiC and Si0 2 as well as particle size.
- heat treatment of a composite powder having a residual Si0 2 content of 4.4 wt% and a residual SiC content of 1.5 wt% for 12 hours at 1500°C yields a residual Si0 2 content of 2.03 wt% and a residual SiC content of 0.9 wt% whereas a heat treatment of the same powder for 4 hours at 1400°C yields a residual Si0 2 content of 3.4 wt% and a residual SiC content of 1.4 wt% .
- the heat treatment also decreases internal porosity of powder particles and causes the particles to take on a more spherical shape. The decrease in porosity is accompanied by a concurrent decrease in powder surface area and leads to a solid or near solid crystallite structure.
- the composite powders of the present invention are suitable for use in preparing
- SRS ceramic bodies are formed at elevated temperatures, either with applied pressure, as in hot pressing, or with little or no applied pressure, as in low pressure gas sintering or pressureless sintering.
- the composite powders are combined with suitable densification aids, conversion aids, whisker growth enhancing compounds and, optionally, preformed reinforcing materials.
- U.S. Patent Number 5,021 ,372 defines densification aids (column 5, lines 49-61), conversion aids (column 6, lines 19-27) and whisker growth enhancing compounds (column 7, lines 4-18).
- Patent Number 5,021 ,372 also includes suitable compounds and amounts for such densification aids (column 5, line 62 through column 6, line 18), conversion aids (column 6, lines 35-55) and whisker growth enhancing compounds (column 7, line 19 through column 8, line 52).
- densification aids column 5, line 62 through column 6, line 18
- conversion aids column 6, lines 35-55
- whisker growth enhancing compounds column 7, line 19 through column 8, line 52.
- a densification aid is a compound that forms a liquid phase into which ⁇ -S ' i3N 4 dissolves and in which mass transport rates of the silicon and nitrogen are quite rapid.
- the temperature at which the liquid phase forms varies with the densification aid.
- a conversion aid is a compound that forms a glassy phase through which mass transport is, in general, considerably slower than in the densification aid.
- ⁇ -Si 3 N 4 dissolves in the conversion aid on heating, but is not readily densified. Notwithstanding this lack of densification, the conversion aid promotes rapid, essentially complete conversion of ⁇ -Si3N 4 to ⁇ -Si3 4 . Whisker growth enhancing compounds promote formation of ⁇ -Si3N 4 whiskers.
- a self-reinforced silicon nitride/silicon carbide ceramic body is desirably prepared by subjecting a powdered admixture of the silicon nitride/silicon carbide composite powder (prepared as described herein), a densification aid, a conversion aid, at least one whisker growth enhancing aid and, optionally, a catalyst to conditions of temperature and pressure sufficient to yield a ceramic body having a density of at least 96 percent of theoretical density and form, in situ, ⁇ -silicon nitride whiskers having an average aspect ratio of at least 2.5.
- the body has both a granular and an intragranular distribution of residual silicon carbide grains and a fracture toughness of at least 7 MPa m" .
- the intragranular silicon carbide grains have a MND within a range of from 10 to 400 nanometers. At least a portion of the intragranular silicon carbide grains contain nitrogen, as determined by parallel electron energy loss spectroscopy, in an amountthat is within a range of from 2 to 10 percent by weight of the silicon carbide. If desired, the powdered admixture may be converted to a shaped body prior to being subjected to the conditions of temperature and pressure. The resulting ceramic body has a creep resistance that is greater than that obtained by substituting silicon nitride for the silicon nitride/silicon carbide composite powder.
- the resulting body includes a crystalline phase of ⁇ -silicon nitride of which at least about 20 volume percent, as measured by viewing one plane of the body by scanning electron microscopy, is in the form of whiskers having an average aspect ratio of at least 2.5 and a glassy grain boundary phase in an amount not greater than 35 percent by weight of total body weight.
- the resulting ceramic body also contains silicon carbide in an amount that is within a range of from greater than 0 percent by weight to 50 percent by weight, based upon combined weight of silicon nitride and silicon carbide.
- a raw material feed mixture by mixing 41.7 parts by weight (pbw) Si0 2 (a high purity crystalline quartz having an average particle size ⁇ 10 ⁇ r ⁇ ), 33.3 pbw acetylene carbon black (commercially available from Chevron Chemical Company under the trade designation SHAWINIGAN BLACKTM), and 25.0 pbw Si 3 N 4 (UBE Industries, Limited under the trade designation SN E-10) in a ball mill half filled with a Si0 2 -based media for five hours. Transfer the raw material feed mixture to a blender, add 8.2 pbw wheat starch, 3.5 pbw corn starch and 5.9 pbw melamine, all parts being based on 100 parts by weight of raw material feed mixture, and blend for 20 minutes.
- pbw Si0 2 a high purity crystalline quartz having an average particle size ⁇ 10 ⁇ r ⁇
- 33.3 pbw acetylene carbon black commercially available from Chevron Chemical Company under the trade designation SHAWINIGAN BLACKTM
- Six graphite lifts are attached to the inside of the crucible to aid in the mixing and turnover of the pellets.
- RF radio frequency
- the powder has a carbon content of 0.71 wt% (2.37 wt% as SiC) and an oxygen content of 2.1 1 wt%, all percentages being based upon powder weight.
- Transmission electron microscopy (TEM) shows that the carbon is in the form of nanosized SiC particles having a diameter ranging from 10 to 70 nm (0.01 to 0.07 ⁇ m).
- Examples 2-5 Repeat Example 1 , but vary the reaction temperature and time at that temperature as shown in Table I.
- Table I also shows the carbon content, equivalent SiC content, oxygen content and BET surface area of the powder after excess carbon removal (burnout).
- Table I includes comparable data for Example 1.
- Each powder has an ⁇ -Si3N 4 content in excess of 95 wt% with SiC being in the form of nanometer-sized (nanosized) particles.
- Example 1 repeat Example 1 , but vary the reaction temperature as shown in Table II and increase the time at reaction temperature to 390 minutes. Table II also shows the SiC content and size after carbon burnout.
- Example 3 Repeat Example 3, but increase the time at reaction temperature to 390 minutes.
- the pellets have a S ' i3N seed/Si0 2 ratio of 0.6: 1.
- the powder After carbon removal or burnout, the powder has a carbon content of 0.30 wt% (1.0 wt% as SiC) and an oxygen content of 1.78 wt%.
- the powder As in Example 1 , the powder has an ⁇ -Si3N 4 phase content in excess of 95 wt% and contains nanosized SiC particles having a diameter ranging from 10 to 70 nm.
- the powder has a BET surface area of 8.0 m 2 /g. Examples 12-15
- Example 1 1 repeats Example 1 1 , but change the amounts of Si0 2 , C and S ' i3N 4 and the value for y as shown in Table III.
- Table III also includes powder properties of the powders after carbon burnout for Examples 1 1-15. As in Example 1 1 , all powders have an ⁇ -SJ3N 4 phase content in excess of 95 wt% and contain nanosized SiC particles (10 to 70 nm). Table III
- Example 15 The data in Table III show that surface area (S.A.) increases as the seed to Si0 2 ratio decreases.
- the material with no seed (Example 15) has a higher S.A. than the other materials, but scanning electron microscopy (SEM) analysis shows that it has a blocky particle morphology.
- SEM scanning electron microscopy
- the blocky morphology leads to problems when the material is to be sintered.
- a material with a high S.A. and an equiaxed morphology is much more desirable than the blocky material from an ease of sintering point of view.
- At least a portion of the relatively high surface area for Example 15 is due to internal porosity.
- the material is, however, quite suitable for sintering if it is ground priorto sintering.
- Example 16 Example 16
- Example 1 1 Prepares three composite powder batches by replicating Example 1 1 save for changing the value for y as shown in Table IV.
- the carbon content, oxygen content and surface area for each powder are also shown in Table IV.
- total Si0 2 refers to a combination of Si0 2 contained in the composite powder and added Si0 2 . Attrit the composition for one hour in water using Si3N milling media. Use a roto-evaporator to dry the attrited combination into a formulated, sinterable powder.
- Table IV shows resulting densities in terms of percent of theoretical density.
- Sur ⁇ y bon gen face Con ⁇ Con ⁇ Area 3 Hours 9 Hours tent tent ( 2 /g) at 1750°C at 1750°C (wt%) (wt%)
- Example 16 Repeat Example 16, but change the recipe, use ethanol rather than water during attrition, a graphite crucible rather than a boron nitride crucible and a powder bed of the same composition as the recipe, and increase the sintering time to 12 hours.
- the recipe is: 92.77 wt% of the Si 3 N 4 composite powder of Example 1 , 1.25 wt% Y 2 0 3 , 1.45 wt% MgO, 3.85 wt% SiO 2 , 0.50 wt% ZrO 2 and 0.18 wt% Ta 2 0 5 .
- the resultant sintered part has a density of 99.5 percent of theoretical density.
- SiC is present and dispersed throughout the part (both intragranular and granular). There are no intergranular SiC particles.
- the intragranular SiC has a MND of 1 10 ⁇ 70 nm and the granular SiC has a MND of 140 ⁇ 40 nm. As such, the granular and intragranular SiC particles appear to be equivalent in size.
- Example 1 but substitute 1 1.7 pbw of sucrose for the 8.2 pbw wheat starch and 3.5 pbw corn starch used in that example, reduce the reaction temperature from 1500°Cto 1475°C, increase the time at temperature from 180 minutes to 390 minutes, and o i ncrease the carbon burnout tern peratu re from 700°C to 800°C.
- the powder has a carbon content of 0.52 wt% and an oxygen content of 2.06 wt%, all percentages being based upon powder weight.
- the powder carbon content equates to a SiC content of 1.73 wt% that, by TEM, is in the form of nanosized SiC particles (diameter ranging from 10 to 70 nm).
- the powder has a BET surface area of 12.2 m 2 /g. if the combination of starches used in Example 1 is 5 substituted for sucrose, the product powder has an oxygen content of 1.78 wt% , a carbon content of 0.30 wt% and a BET surface area of 8.0 m /g.
- Example 19 Repeat Example 16, but use a different recipe and sintering times of 3 and 12 hours rather than 3 and 9 hours to prepare sintered bodies using composite powders from
- the recipe is: 91.90 wt% composite powder; 1.97 wt% Y 2 ⁇ 3, 0.93 wt%
- Table V shows the composite powder source, binder type, composite powder surface area and percent theoretical density 5 under the given sintering conditions.
- Example 14 Repeat Example 14, but modify the procedure by heating to a first temperature of 1475°C, holding at that temperature for a period of 360 minutes, then heating to a temperature of 1520°C at a rate of 5°C/min and holding at that temperature for 30 minutes before cooling.
- the resultant powder has a carbon content of 1.42 wt% (4.74 wt% as SiC) and an oxygen content of 2.42 wt%, all percentages being based upon powder weight.
- TEM shows that the carbon is in the form of SiC particles having a bimodal size distribution with distribution peaks located at MND's 0.12 ⁇ 0.03 ⁇ m and at 0.44 ⁇ 0.10 ⁇ m. Duplicating this procedure save for omitting the increase in temperature to above 1500°C yields a monomodal distribution of SiC particle sizes. This example shows that modifications of SiC particle size distribution are possible via manipulation of combinations of reaction temperature and reaction time.
- Example 21 shows that modifications of SiC particle size distribution are possible via manipulation of combinations of reaction temperature and reaction time.
- Example 1 Use the procedure and raw materials of Example 1 , but reduce the amounts of wheat and corn starches respectively to 7.8 pbw and 3 pbw, to convert a raw material feed mixture of 47.2 pbw Si0 2 , 37.8 pbw acetylene carbon black, 9.4 pbw S ⁇ 3 4 and 5.6 pbw melamine into a product powder.
- the Si0 2 is a high purity quartz (Unimin Corp., lota Standard) that has, in part, a Fe content of 5 ppm, an Al content of less than 50 ppm and a Ca content of less than 5 ppm.
- the product powder has a surface area of 10.1 m 2 /g, a carbon content of 0.40 wt%, an oxygen content of 2.44 wt%, a Fe content of 31 ppm, an Al content of less than 50 ppm and a Ca content of 71 ppm, all parts and percentages being based upon powder weight.
- the Si0 2 After milling using a jet mill wherein the wear parts are fabricated from Si3N 4 , SiC or B 4 C and other non-wearing parts are lined with urethane, the Si0 2 has an average particle size of less than 10 ⁇ m.
- Example 17 for a combination of 91.89 wt% of the product powder, 1.97 wt% Y 2 0 3 , 0.94 wt% MgO, 4.43 wt% total Si0 2 , 0.56 wt% Zr0 2 and 0.21 wt% Ta 0 5 .
- the resultant sintered part has a density of 96.5 percent of theoretical density, a room temperature strength of 795 megapascals (MPa), a fracture toughness of 7.3 MPa m 1 2 and a Weibull modulus of 18.
- Jet milling the heat treated pellets after completing carbon removal yields a powder with a surface area of 10.4 m 2 /g, a carbon content of 0.41 wt% , an oxygen content of 2.4 wt% , a Fe content of 17 ppm, an Al content of less than 50 ppm and a Ca content of 67 ppm.
- the sintered part has a density of 96 % of theoretical density, a room temperature strength of 750 MPa, a fracture toughness of 7.3 MPa m 1 2 and a Weibull modulus of 15. If a lower purity quartz, such as Silica B (Table XII), is substituted for the high purity crystalline quartz, the product powder has correspondingly higher impurity levels. This powder converts to a sintered part having properties, such as room temperature strength and Weibull modulus, that are lower than those noted in this Example 21.
- Example 17 using two different crucible environments and a mixture of 92.31 wt% of the omposite powder of Example 3, 2.35 wt% Y 2 0 3 , 1.16 wt% MgO, 3.50 wt% total Si0 2 , 0.50 wt% Zr0 2 and 0.18 wt% Ta 2 Os.
- One crucible environment (Environment A) is provided by a boron nitride (BN) crucible with no surrounding powder bed.
- the other (Environment B) is provided by a graphite crucible painted with a BN coating and filled with a powder bed of the same composition as the mixture.
- the part sintered in Environment A has a residual carbon content of 0.10 wt% and intragranular SiC with a MND of 80 ⁇ 40 nm and no granular SiC whereas the part sintered in Environment B has a residual carbon content of 0.39 wt% , intragranular SiC with a MND of 80 ⁇ 40 nm and granular SiC with a MND of 220 ⁇ 40 nm.
- Example 23 Repeat Example 1 , but use air rather than an air/nitrogen mixture to remove excess carbon.
- the resultant powder has a carbon content of 0.44 wt% (1.47 wt% as SiC), an oxygen content of 2.36 wt% (4.43 wt% as Si0 2 ) and a BET surface area of 6.8 m /g. The results, while not the same as those in Example 1, are believed to be within experimental error.
- the crucible has a diameter of 2.25 in (5.7 cm) and a depth of 3 in (7.6 cm).
- Analysis of the powder shows a carbon content of 0.26 wt% (0.87 wt% as SiC) and an oxygen content of 1.08 wt% (2.03 wt% as Si0 2 ).
- the powder has a Si3N 4 content of 97.1 wt%.
- X-ray diffraction (XRD) analysis shows that the
- Si3N 4 is greater than 95 wt% alpha phase.
- the powder has a BET surface area of 5.2 m /g. SEM and TEM analysis suggest that the reduction in surface area from 6.8 m /g to 5.2 m /g is a result of reduced internal powder particle porosity. Another way of expressing reduced internal porosity is to say that the particles take on a more solid crystallite form.
- Si0 2 sources Use three different grades (coarse, medium and fine) of high purity crystalline quartz as Si0 2 sources and acetylene carbon black as a carbon source to prepare three different precursor powder batches.
- the Si0 2 sources are shown in Table VII, wherein the fine grade is designated "A”, the medium grade is designated “B” , and coarse grade is designated "C”.
- Grades A and B are prepared by jet milling Grade C as described hereinabove.
- each precursor powder batch by placing 1 16.6 g of acetylene carbon black, 145.9 g of quartz (Table VII), and 15.9 g of melamine into a 6250 milliliter (ml) urethane lined milling jar half filled with Si3N 4 milling media (5 mm average diameter). Place the jar on a roller mill and dry mill for 2 hours before separating the precursor batch from the milling media. Add 700 ml deionized water to a large flask containing a stir bar, and heat the water, with stirring, to a temperature of 80°C.
- Example 23 Use the apparatus and procedure of Example 23, but reduce the time at reaction temperature from 12 hours to 5 hours and use a temperature of either 1470°C or 1500°C to convert 15.0 g of calcined pellets prepared from each precursor powder batch into a product. Remove excess carbon as in Example 1 , but increase the temperature from 700°C to 800°C and reduce the time at temperature from 3 hours to 2 hours.
- Example 32 Analysis of each product provides results shown in Table VIII. XRD analysis shows the S ⁇ 3N to be greater than 95% ⁇ -phase.
- the product of Example 32 has a SiC content of 1.7 wt% , a Si0 2 content of 18.2 wt% and a SJ3N 4 content of 80.1 wt% .
- the high purity quartz used as a starting material should be of a fine grade, preferably with a S.A. > 0.2 m /g and a mean particle size W50) ⁇ 15 ⁇ m in order to obtain high levels of conversion ( ⁇ 3 wt% residual monatomic O) and low levels of nanophase SiC ( ⁇ 2 wt% SiC, ⁇ 0.6 wt% C as SiC). If greater SiC contents are desired, higher temperatures should be used. If higher residual oxygen contents are desired, coarser grades of high purity quartz should be used. Examples 38-41
- X-Ray fluorescence (XRF) analysis of the resultant powders shows that they contain less than 100 ppm Ca, less than 50 ppm Al, less than 50 ppm Fe, less than 20 ppm S, less than 10 ppm Cl, less than
- Example 32 Prepare each precursor powder batch with a different carbon source using the component amounts and procedure outlined in Example 32. Convert the powder batches to product powder using the procedure of Example 32, but reduce the temperature to 1435°C. Analysis of each product provides results shown in Table XI. XRD analysis shows the Si 3 N to be greater than 95% alpha phase.
- Table XI demonstrate that SiC size depends, to some extent, upon starting carbon particle size.
- the amount of SiC may be influenced by other factors, such as the level of impurities in carbon type C (Table X) or temperature (Table II).
- Example 1 Prepare wet pellets as in Example 1 using 1 16.6 grams (g) of acetylene carbon black, 145.9 g of quartz (Grade B, Table VII), 29.2 g of Si 3 4 having a ⁇ -phase content of 81.2 wt% (commercially available from Shin Etsu Chemical Company as KSN80SP), 17.2 g of melamine, 24.0 g wheat starch, 10.3 g of corn starch and 200 g of deionized water. Place the wet pellets into a forced air convection oven and dry them overnight (14 hours) at 135°C. Place the dried pellets into a tube furnace with flowing nitrogen gas and heat for 5 hours at 330°C to calcine the starches and melamine. Convert 9.2 g of the calcined pellets into a powder using the procedure of
- Example 32 with a reaction temperature of 1500°C and a time at that temperature of 5 hours.
- Example 45 Place 10.3 g of the calcined pellets prepared in Example 45 into a feed tube maintained at room temperature (taken as 25°C) and located above a high temperature graphite crucible that is maintained at a temperature of 1435°C. Gaseous nitrogen flows through a perforated distributor in the crucible's base at a rate of 6 slpm. Open a ball valve in the feed tube to add the room temperature pellets to the heated crucible from above.
- Characterization of the powder of Example 45 reveals the presence of ⁇ -Si 3 N 4 and ⁇ -Si 3 N crystallites, the ⁇ -Si3N 4 crystallites having a MND of about 0.045 ⁇ m and a mean aspect ratio of 5.4/1 , the aspect ratio ranging between 1.5/1 and 9/1 (a length within a range of from 0.08 to 0.5 ⁇ m, with a mean of 0.24 ⁇ m).
- the ⁇ -Si3N 4 crystallites have a MND 0.17 ⁇ m, the MND ranging from 0.03 to 0.46 ⁇ m.
- Characterization of the powder of Example 46 reveals the presence of ⁇ -Si3N and ⁇ -S ⁇ 3 4 crystallites, the ⁇ -Si3N 4 crystallites having a MND of about 0.036 ⁇ m and a mean aspect ratio of 7.6/1 , the aspect ratio ranging between 3/1 and 21/1 (a length within a range of from 0.05 to 1.1 ⁇ m. with a mean of 0.27 ⁇ m).
- the ⁇ -Si3 4 crystallites have a MND 0.12 ⁇ m, the MND ranging from 0.05 to 0.22 ⁇ m.
- Example 13 0.26) and a composite powder prepared as in Example 45 with a y value of 0.26 are both sintered as in Example 16, the composite powder prepared as in Example 45 reaches a density of 97 percent of theoretical density in 3 hours whereas the composite powder prepared as in Example 13 requires nearly 9 hours to attain the same density.
- the composite powder containing bo h ⁇ -Si3N 4 and ⁇ -Si 3 N 4 crystallites (the ⁇ -Si3N 4 crystallites being rod-like) is therefore more sinterable than a composite powder lacking the rod-like ⁇ -SJ3N 4 crystallites.
- the product has an ⁇ -phase Si3N 4 content in excess of 95 wt%.
- the ⁇ -phase Si3 4 in such a product contains no rod-like crystallites.
- Changing the seed to a blend of 75 wt% of the seed used in Example 1 and 25 wt% of the seed used in Examples 45 and 46 yields a product having an ⁇ -phase Si3N 4 content of 90.5 wt% and a ⁇ -phase Si3N 4 that contains no rod-like crystallites.
- heating the seed used in Example 46 at 1500°C for 5 hours fails to produce any rod-like crystallites.
- Si3N4 powder (UBE Industries Ltd., as SN E-3).
- the quartz particle size is obtained in the same manner as silicas A and B in Table VII.
- the calcined pellets contain carbon at a level of 100% excess over that required to carbothermally reduce the Si0 2 .
- the pellets contain sufficient
- Si3N 4 to provide a seed/Si0 2 ratio of 0.2/1.
- FEG/SEM Field Emission Gun Scanning Electron Microscopy
- Example 47 Duplicate this Example, but use the slower heating procedure of Example 1 , to produce Si 3 4 crystallites that are larger than those of this Example 47 and contain few, if any, new, fine crystallites.
- Examples 32-37 prepare precursor powder batches from three different Si0 sources and acetylene carbon black.
- Table XII shows the Si0 2 sources.
- High purity crystalline quartz obtained in the same manner as A and B in Table VII
- low purity crystalline quartz is designated “B”
- high purity amorphous quartz is designated "C”.
- Example 45 but change the seed to that used in Example 47, to prepare a product powder having a carbon content of 0.72 wt% (2.4 wt% as SiC) and an oxygen content of 1.38 wt% (2.6 wt% as Si0 2 ).
- XRD analysis shows the Si 3 N 4 to be greater than 95% alpha phase.
- TEM/SEM analysis of the product indicates an ⁇ -Si3N 4 crystallite MND of 0.68 ⁇ m.
- TEM analysis shows a SiC crystallite MND of less than 50 nm.
- Example 51 but change the seed to that used in Example 1 , to prepare a product powder having a carbon content of 0.47 wt% (1.6 wt% as SiC) and an oxygen content of 1.28 wt% (2.4wt% as Si0 2 ).
- XRD analysis shows the Si 3 to be greater than 95% alpha phase.
- TEM/SEM analysis of the product indicates an ⁇ -Si3 4 crystallite MND of 0.25 ⁇ m.
- Examples 51 and 52 demonstrate that ⁇ -Si3N 4 seed MND strongly influences product ⁇ -Si 3 N4 crystallite MND.
- the smaller starting material MND in Example 52 leads to a product MND that is smaller than that of Example 51.
- a seed ⁇ -Si 3 N 4 crystallite MND of less than 0.15 ⁇ m favors synthesis of high purity (low metals and ⁇ 2 wt% monatomic oxygen) ⁇ -Si 3 4 powder with a crystallite MND of ⁇ 0.3 ⁇ m.
- Example 52 but vary the amount of ⁇ -Si 3 N 4 seed from no seed in Example
- Table XIV shows the seed/Si0 2 ratio and the product ⁇ -Si3N 4 crystallite MND.
- Table XIV includes comparable data from Example 52.
- Table XII both with and without the same Si3N 4 seed as in Example 1. Use the same apparatus and procedure as in Examples 32-37, but reduce the temperature to 1435°C, to convert 10.4 g of each batch of calcined pellets into a product powder.
- Table XV identifies the carbon and Si0 2 sources, states whether or not the precursor powder batch contains a seed, and specifies the crystallite MND for both Si3N 4 and SiC.
- Example 61 shows a carbon content of 1.1 wt% (3.7 wt% as SiC) and an oxygen content of 3.1 wt% (5.8 wt% as Si0 2 ).
- XRD analysis shows the Si3N 4 to be greater than 95% alpha phase.
- SEM/TEM analysis of the product shows that the Si3N 4 crystallites fall within a size range of 0.4to 1.1 ⁇ m with a crystallite MND of about ⁇ .7 ⁇ 0.2 ⁇ m.
- the SiC crystallites are within a range of 30 to 100 nm with a MND of about 50 nm.
- Example 62 which differs from Example 61 by containing seed Si3N 4 , reveals a carbon content of 0.5 wt% (1.7 wt% as SiC), an oxygen content of 2.0 wt% (3.8 wt% as Si0 2 ).
- the Si3N 4 crystallite size falls within a range of 0.1 to 0.5 ⁇ m with a crystallite MND of about ⁇ .2 ⁇ 0.1 ⁇ m.
- the SiC crystallites are within a range of 20 to 90 nm with a crystallite MND of about 40 nm.
- Example 59-64 Prepare six batches of calcined pellets using the procedure and component amounts of Examples 59-64, the carbon sources of Table X, and Silica A from Table XII. Use the 5 apparatus and procedure of Examples 59-64 to convert 10.5 g of each batch of calcined pellets into a product powder.
- Table XVI identifies the carbon (C) source, and provides product powder carbon and oxygen contents, with equivalent SiC and Si0 2 contents.
- XRD analysis shows the Si3N 4 to be greater than 95% ⁇ -phase.
- SEM/TEM analysis of the Si 3 N crystallites reveals micropores of a size approximating that of the carbon source.
- Example 47 using 10.6 g of calcined pellets prepared from a combination of 302 grams (g) of acetylene carbon black, 378 g of high purity quartz, 40 g of melamine, 56 g of wheat starch, 24 g of corn starch and 520 g of deionized water. All starting materials are the same as those used in Example 1.
- the resulting powder has a carbon content of 0.8 wt% (2.7 wt% as SiC) and an oxygen content of 2.4 wt% (4.5 wt% as Si0 2 ), based on powder weight.
- XRD analysis shows the Si 3 N 4 to be greater than 95% ⁇ -phase.
- a TEM photomicrograph shows the powder contains nanophase SiC having a MND of about 50 nm. The powder has a BET surface area of 1 1.8 m 2 /g.
- Example 6 Repeat Example 6, but preheat the crucible to a temperature of 1500°C and maintain that temperature for a period of 10 minutes before reducing the temperature to that of Example 68 for a period of 7 hours.
- the resultant powder has a carbon content of 4.7 wt%
- Example 69 Repeat Example 69, but vary the initial preheat temperature and time at that temperature as shown in Table XVII.
- Table XVII also shows carbon and oxygen contents of the powder, equivalent weight percentages of SiC and Si0 2 , Si3N content and powder S.A. and includes comparable data for Examples 68 and 69.
- Example 73 15 1475 2.1 3.9 3.2 10.7 85.4 12.2
- a comparison of Example 68 with Examples 69-73 shows the elevated initial temperatures of Examples 69-71 promote the formation of SiC.
- Examples 72 and 73 show that preheating temperatures below 1500°C, e.g. 1475°C, also yield levels of SiC that exceed those attained in the absence of preheating. Lower preheating temperatures should provide similar results if preheating times are increased to compensate for slower rates of SiC production.
- the SiC formed at the initial high temperature should serve as a seed or catalyst for the subsequent carbothermal synthesis of ⁇ -Si3N 4 .
- Examples 74-83 Vehicle Amounts of Seed and Excess Carbon Content
- Example 47 Use the procedure of Example 47 to prepare five different precursor powder batches with varying amounts, all of which are shown in Table XVIII, of acetylene carbon black, high purity quartz (>99.8 wt% Si0 2 with a mean particle size (d 5 o) of 5.1 ⁇ m), and a crystalline ⁇ -phase Si 3 N powder (prepared as in Example 2 with a mean particle size (dso) of 0.86 ⁇ m and a BET surface area of 7.46 m 2 /g), together with 28.0 g wheat starch, 12.0 g corn starch and 20.0 g melamine. Convert each powder batch to calcined pellets as in Example 47, but increase the deionized water to 300 g. Table XVIII also shows % excess carbon and ratio of seed/Si0 2 ratio in each batch of calcined pellets.
- Table XIX presents data relating to each example.
- the powder of Example 74 has an equivalent SiC content of 2.84 wt% and an equivalent Si0 2 content of 2.78 wt% . Equivalents for the other examples are readily determined without undue experimentation.
- XRD analysis shows the Si3N 4 to be greater than 95% -phase. Table XIX
- Example 47 Use the procedure of Example 47 to prepare a primary batch powder from 302 g of acetylene carbon black, 378 g of the same quartz as in Example 1 and 40 g of melamine. Also as in Example 47, convert 220 g of the primary batch powder, 17.1 g wheat starch, 7.3 g corn starch and 173 g of deionized water into calcined pellets of a first precursor (P-1).
- a second precursor (P-2) by placing 250 g of the primary batch powder in the same milling jar used to prepare the primary batch powder together with the same size milling media and 15.8 g of Si metal (Elkem HQ SILGRAINTM, ⁇ 10 ⁇ m average particle size) and dry ball milling for two hours before separating the resulting powder mixture from the milling media. Convert this powder mixture, 20.7 g wheat starch, 8.9 grams corn starch and 181 g deionized water into calcined pellets using the same procedure as in preparing P-1. The calcined pellets have a Si/Si0 2 ratio of 0.12.
- Example 84 Prepare a third precursor (P-3) in the same manner as used for P-2, but increase the amount of Si metal to provide calcined pellets having a Si/Si0 2 ratio of 0.36.
- the powder has a carbon content of 1.2 wt% (4.0 wt% as SiC) and an oxygen content of 2.3 wt% (4.3 wt% as Si0 2 ), based on powder weight.
- XRD analysis shows the Si3N 4 to be greater than 95% ⁇ -phase.
- a SEM photomicrograph shows the powder contains crystallites having a diameter of about 1 ⁇ m.
- Example 84 but vary the ti me at temperature or the precursor or both, as shown in Table XX, to prepare Examples 85-92.
- Table XX shows selected data for Examples 84-
- Example 93 Prepare a pressureless sinterable composition using the powder of Example 3 and the following formulation, wherein all weight percentages are based upon composition weight and all components are in powder form: 95.6 wt% SJ3 ; 2.31 wt% Y2O3; 1.17 wt% MgO; 0.24 wt% Si0 2 ; 0.5 wt% Zr0 2 ; and 0.18 wt% Ta 2 0 5 .
- the amount of Si0 2 reflects the added amount rather than the amount of Si0 2 contributed by the Si3 4 powder of Example 3. If that amount is included, the composition has a total Si0 2 content of 3.5 wt%.
- Attritthe composition components for one hour in ethanol using zirconia milling media to prepare an attrited mixture. Dry the attrited mixture using a rotary evaporator and separate the attrited mixture from the milling media using a 35 mesh (425 ⁇ m sieve opening) stainless steel sieve. Convert the mixture into test pieces by uniaxial pressing at about 2500 pounds per square inch (psi) (about 17 megapascals (MPa)) followed by isostatic pressing at about 40,000 psi (about 276 MPa).
- psi pounds per square inch
- MPa megapascals
- test pieces Place the test pieces into a BN painted graphite crucible and surround them with a powder bed of the same composition as the test pieces. Sinter the pieces for 12 hours in a 4 inch (10 cm) ASTRO graphite furnace at 1750°C under a one atmosphere (about 100 kilopascals (KPa)) flowing nitrogen atmosphere.
- KPa kilopascals
- TEM analysis of the sintered pieces shows a SRS structure that contains residual SiC particles.
- the SiC particles are distributed throughout a SRS matrix and located in a glassy grain boundary phase at triple point junctions of Si 3 N 4 grains (granular) and within Si 3 N 4 grains (intragranular).
- the sintered pieces Based upon the Si3N 4 powder's carbon content, the sintered pieces contain about 1.4 wt% SiC reinforcement, based upon sintered piece weight.
- Example 94 Cut a section from a sintered piece and polish a surface to a mirror finish using, in succession, diamond pastes having an average particle size of 15 ⁇ m, 6 ⁇ m and 1 ⁇ m. Indent the polished surface with a 30.4 pound (lb) (about 14 kg) load using a diamond Vicker's indentor. From the indent, the Palmqvist toughness of the material is determined to be 44.2 kg/mm. If S ⁇ 3N 4 powder, such as that used as a seed in Example 1 , is used in place of the composite powder of the present invention, the resultant sintered body has a lower Palmqvist toughness even with the same total Si0 2 content, additions of SiC powder or both. Similar results are expected with other powders produced as described herein as well as with other physical properties.
- Example 94 Example 94
- Each material is prepared according to the following formulation wherein all percentages are based upon composition weight: 85.78 wt% of a combination of Si3N 4 and SiC powders; 5.84 wt% Y 2 ⁇ 3; 3.22 wt% MgO; 0.32 wt% CaO; and 4.84 wt% total Si0 2 (added powder plus Si0 2 introduced by the Si3 4 powder).
- Prepare four powders as in Example 1 but vary the temperature and increase the time at temperature to 390 minutes.
- the resulting powders, their SiC contents and their designation are, respectively: 1450°C, 1.38 wt%, and A-1 ; 1470°C, 3.89 wt%, and A-2; 1480°C, 5.28 wt%, and A-3; and 1490°C, 19.78 wt%, and A-4.
- Table XXII contrasts SiC content of several of the materials with average strain to failure, average fracture o toughness values and average room temperature fracture strength.
- Table XXIII summarizes TEM results fortwo of the materials.
- the nitrogen content is determined by parallel electron energy loss spectroscopy (parallel EELS) with a GATAN Model 666 spectrometer fitted to either a VG HB601 UX STEM operated at 100 kilovolts (kV) or an ABT EM-002B operated at 200 kV.
- R. F. Egerton, in Electron Energy Loss Spectroscopy in the Electron Microscope (1986) describes an 5 approach wherein the nitrogen and carbon EELS signals for each particle are integrated and the nitrogen/carbon atomic ratio is calculated.
- the GATAN software follows this approach.
- the nitrogen values (2-10 wt%) reported herein reflect the use of this computational approach.
- the wt% nitrogen in SiC is then calculated directly from the atomic ratios.
- SRS materials prepared with composite powders of the present invention have a greater retention of high temperature strength (MPa) at SiC contents of 3.89 wt% or 1.38 wt% than those prepared with physical mixtures of 3.5 wt% or 7.0 wt% submicrometer SiC powder and either diimide derived Si 3 N 4 powders or direct nitrided Si3N 4 powders.
- MPa high temperature strength
- Table XXII shows that SRS materials prepared with composite powders of the invention have greater creep resistance at a given SiC content than those prepared with physical mixtures of submicrometer SiC powder and either diimide derived Si 3 N 4 powders or direct nitrided Si3N 4 powders. Creep resistance is inversely proportional to strain at failure. A SiC addition of 7.0 wt% to a diimide derived SJ3N 4 powder is required to attain the same creep resistance as a composite powder having a SiC content of 1.38 wt% . Table XXII also shows that physical additions of SiC decrease fracture toughness and, to a lesser extent, room temperature strength of SRS materials.
- Table XXIII highlights microstructural differences between an SRS material prepared from a composite powder of the invention and an SRS material prepared by physically admixing SiC powder into a composition based upon a diimide derived Si 3 N 4 powder. These microstructural differences are believed, at least in part, to account for the differences disclosed by reviewing Tables XXI through XXIII.
- An additional difference is that at least a portion of the intragranular SiC in the SRS material prepared with powder A-2 (Table XXIII) contains about 3.3 wt% residual nitrogen (as measured by parallel EELS) whereas the intragranular SiC in the SRS material prepared with powder B-2 (physically mixed SiC) does not. This residual nitrogen presumably comes from the SiC portion of the composite powders prepared as described herein. As such, it is expected in all SRS bodies prepared from composite powders of the present invention. Similar results are expected with other composite powders prepared as described herein.
- Example 95 shows microstructural differences between an SRS material prepared from a composite powder
- Example 96 Repeat Example 5, but change the reaction temperature from 1475°Cto 1500°C.
- the resulting powder has a carbon content of 1.59 wt% (5.3 wt% as SiC), based upon powder weight.
- TEM analysis shows that the carbon is present as nanosized SiC.
- Parallel EELS analysis shows that the SiC has a nitrogen content of 2.3 wt%, based upon SiC weight.
- Example 96
- Example 95 Repeat Example 95, but eliminate the Si3 4 powder used as a seed and decrease the reaction temperature from 1500°C to 1485°C.
- the resulting powder has a carbon content of 1.1 wt% (3.7 wt% as SiC), based upon powder weight.
- TEM analysis shows that the carbon is present as nanosized SiC.
- Parallel EELS analysis shows that the SiC has a nitrogen content of 9.9 wt%, based upon SiC weight.
- Examples 95 and 96 demonstrate that composite powders of the invention contain SiC and that the SiC contains nitrogen. Similar results are expected with the composite powders of the other examples as well as with other composite powders prepared as described herein. By way of contrast, parallel EELS analysis of commercially available silicon carbide powder reveals no detectable level of nitrogen even after the powder has been subjected to a three hour heat treatment at 700°C in any one of air, nitrogen or a 50/50 (by volume) air/nitrogen mixture.
Landscapes
- Chemical & Material Sciences (AREA)
- Engineering & Computer Science (AREA)
- Ceramic Engineering (AREA)
- Organic Chemistry (AREA)
- Materials Engineering (AREA)
- Structural Engineering (AREA)
- Manufacturing & Machinery (AREA)
- Nanotechnology (AREA)
- Crystallography & Structural Chemistry (AREA)
- Physics & Mathematics (AREA)
- General Physics & Mathematics (AREA)
- Condensed Matter Physics & Semiconductors (AREA)
- Inorganic Chemistry (AREA)
- Composite Materials (AREA)
- Carbon And Carbon Compounds (AREA)
- Ceramic Products (AREA)
Priority Applications (3)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| DE69518746T DE69518746T2 (de) | 1994-04-14 | 1995-04-14 | Siliciumnitrid/siliciumcarbid kompositpulver, ihre herstellung und unter verwendung der kompositpulver hergestellte verdichtete werkstoffe |
| JP7527088A JPH09511981A (ja) | 1994-04-14 | 1995-04-14 | 窒化ケイ素/炭化ケイ素複合体粉末、それらの製造およびこの複合体粉末を用いて作られる高密度化材料 |
| EP95916972A EP0755367B1 (en) | 1994-04-14 | 1995-04-14 | Silicon nitride/silicon carbide composite powders, their preparation and densified materials prepared using the composite powders |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| US08/227,751 | 1994-04-14 | ||
| US08/227,751 US5538675A (en) | 1994-04-14 | 1994-04-14 | Method for producing silicon nitride/silicon carbide composite |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO1995028366A1 true WO1995028366A1 (en) | 1995-10-26 |
Family
ID=22854307
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/US1995/004573 Ceased WO1995028366A1 (en) | 1994-04-14 | 1995-04-14 | Silicon nitride/silicon carbide composite powders, their preparation and densified materials prepared using the composite powders |
Country Status (7)
| Country | Link |
|---|---|
| US (3) | US5538675A (enExample) |
| EP (1) | EP0755367B1 (enExample) |
| JP (1) | JPH09511981A (enExample) |
| CA (1) | CA2187333A1 (enExample) |
| DE (1) | DE69518746T2 (enExample) |
| ES (1) | ES2149359T3 (enExample) |
| WO (1) | WO1995028366A1 (enExample) |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN1061961C (zh) * | 1997-07-16 | 2001-02-14 | 国家建筑材料工业局山东工业陶瓷研究设计院 | 纳米碳化硅--氮化硅复相陶瓷的制备方法 |
Families Citing this family (51)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US5698156A (en) * | 1993-06-30 | 1997-12-16 | Sumitomo Electric Industries, Ltd. | Method of producing a silicon nitride based sintered body |
| US5767025A (en) * | 1994-03-30 | 1998-06-16 | Honda Giken Kogyo Kabushiki Kaisha | Composite powder comprising silicon nitride and silicon carbide |
| EP0676380B1 (en) * | 1994-03-30 | 1999-07-28 | Honda Giken Kogyo Kabushiki Kaisha | Composite powders of silicon nitride and silicon carbide |
| JPH1149572A (ja) * | 1997-08-01 | 1999-02-23 | Honda Motor Co Ltd | セラミックス複合粒子及びその製造方法 |
| US6214309B1 (en) * | 1997-09-24 | 2001-04-10 | University Of Connecticut | Sinterable carbides from oxides using high energy milling |
| US6793875B1 (en) | 1997-09-24 | 2004-09-21 | The University Of Connecticut | Nanostructured carbide cermet powders by high energy ball milling |
| EP1099077B1 (en) * | 1998-07-03 | 2003-10-01 | Toyota Jidosha Kabushiki Kaisha | Gas storage method and system, and gas occluding material |
| EP0994085B1 (en) * | 1998-10-13 | 2003-09-03 | Ngk Spark Plug Co., Ltd | Method of manufacturing spherical bodies |
| US6471931B1 (en) * | 1998-11-20 | 2002-10-29 | Clemson University | Process for recycling spent pot liner |
| US6221154B1 (en) * | 1999-02-18 | 2001-04-24 | City University Of Hong Kong | Method for growing beta-silicon carbide nanorods, and preparation of patterned field-emitters by chemical vapor depositon (CVD) |
| JP4589491B2 (ja) * | 1999-08-24 | 2010-12-01 | 株式会社ブリヂストン | 炭化ケイ素粉末、グリーン体の製造方法、及び炭化ケイ素焼結体の製造方法 |
| US6341747B1 (en) * | 1999-10-28 | 2002-01-29 | United Technologies Corporation | Nanocomposite layered airfoil |
| EP1116704A1 (en) * | 2000-01-11 | 2001-07-18 | Metalloceramica Vanzetti S.p.A. | Nanocomposite dense sintered silicon carbonitride ceramic cutting tool |
| JP4490816B2 (ja) | 2002-08-23 | 2010-06-30 | ジェームズ ハーディー インターナショナル ファイナンス ベスローテン フェンノートシャップ | 合成中空小球体 |
| US20070026171A1 (en) * | 2002-09-03 | 2007-02-01 | Extrand Charles W | High temperature, high strength, colorable materials for use with electronics processing applications |
| TW200408693A (en) * | 2002-09-03 | 2004-06-01 | Entegris Inc | High temperature, high strength, colorable materials for use with electronics processing applications |
| US7993570B2 (en) | 2002-10-07 | 2011-08-09 | James Hardie Technology Limited | Durable medium-density fibre cement composite |
| AU2003901529A0 (en) * | 2003-03-31 | 2003-05-01 | James Hardie International Finance B.V. | A durable high performance fibre cement product and method of making the same |
| JP2006507994A (ja) * | 2002-10-09 | 2006-03-09 | エンテグリス・インコーポレーテッド | デバイス処理システム用の高温高強度の着色可能な材料 |
| US20100192808A1 (en) * | 2003-08-25 | 2010-08-05 | Amlan Datta | Synthetic Microspheres and Methods of Making Same |
| JP3764157B2 (ja) * | 2003-10-10 | 2006-04-05 | 東洋炭素株式会社 | 高純度炭素系材料及びセラミックス膜被覆高純度炭素系材料 |
| US20050077226A1 (en) * | 2003-10-14 | 2005-04-14 | Bishop Bruce A. | Membrane devices using reaction bonded monolith supports |
| US7640936B2 (en) * | 2003-10-27 | 2010-01-05 | Philip Morris Usa Inc. | Preparation of mixed metal oxide catalysts from nanoscale particles |
| US20090156385A1 (en) * | 2003-10-29 | 2009-06-18 | Giang Biscan | Manufacture and use of engineered carbide and nitride composites |
| US20050261121A1 (en) * | 2004-05-19 | 2005-11-24 | Earthstone International Llc | Elimination of crystalline silica from white foam glass by chemical additions |
| US8916486B2 (en) * | 2004-05-19 | 2014-12-23 | Richard Lehman | Method of reducing the occurrence of crystalline silica in foamed glass by the introduction of chemical additives |
| US9963373B2 (en) | 2004-05-19 | 2018-05-08 | Earthstone International Llc | Method of reducing the occurrence of crystalline silica in foamed glass by the introduction of chemical additives |
| US9725350B2 (en) | 2004-05-19 | 2017-08-08 | Richard L. Lehman | Very low crystalline silica foamed glass and methods of using the same |
| US7998571B2 (en) * | 2004-07-09 | 2011-08-16 | James Hardie Technology Limited | Composite cement article incorporating a powder coating and methods of making same |
| US7314593B2 (en) * | 2004-10-27 | 2008-01-01 | Council Of Scientific And Industrial Research | Process for preparing improved silicon carbide powder |
| US7109138B2 (en) * | 2004-10-27 | 2006-09-19 | Council Of Scientific And Industrial Research | Composition for preparation of silicon carbide powder |
| CA2598708A1 (en) | 2005-02-24 | 2006-08-31 | James Hardie International Finance B.V. | Alkali resistant glass compositions |
| US8377419B2 (en) * | 2005-09-28 | 2013-02-19 | The President And Fellows Of Harvard College | Hyperpolarized solid materials with long spin relaxation times for use as imaging agents in magnetic resonance imaging |
| AU2006321786B2 (en) | 2005-12-06 | 2012-05-10 | James Hardie Technology Limited | Engineered low-density heterogeneous microparticles and methods and formulations for producing the microparticles |
| AU2007236561B2 (en) * | 2006-04-12 | 2012-12-20 | James Hardie Technology Limited | A surface sealed reinforced building element |
| KR100769695B1 (ko) * | 2006-08-10 | 2007-10-23 | 한양대학교 산학협력단 | 단결정 탄화규소 나노선, 이의 제조방법 및 이를 포함하는필터 |
| CA2603458C (en) * | 2006-09-21 | 2015-11-17 | Smith International, Inc. | Atomic layer deposition nanocoatings on cutting tool powder materials |
| KR100802182B1 (ko) * | 2006-09-27 | 2008-02-12 | 한국전자통신연구원 | 나노선 필터, 그 제조방법 및 흡착물 제거방법, 이를구비한 필터링 장치 |
| NO327122B1 (no) * | 2007-03-26 | 2009-04-27 | Elkem Solar As | Beleggingssystem |
| CN101289319B (zh) * | 2008-06-03 | 2010-06-30 | 浙江东新密封有限公司 | 一种反应烧结碳化硅陶瓷及其生产方法 |
| US20100092390A1 (en) * | 2008-10-09 | 2010-04-15 | President And Fellows Of Harvard College | Methods for Making Particles Having Long Spin-Lattice Relaxation Times |
| CN101880173A (zh) * | 2009-05-07 | 2010-11-10 | 宁波大学 | 一种碳化硅晶须原位增韧氧化铝陶瓷 |
| US20120171463A1 (en) | 2010-12-30 | 2012-07-05 | Saint-Gobain Cermaics & Plastics, Inc. | Silicon carbide body and method of forming same |
| US8741797B2 (en) * | 2011-09-30 | 2014-06-03 | Saint-Gobain Ceramics & Plastics, Inc. | Composite body including a nitride material, a carbide material, and an amorphous phase material |
| KR101976594B1 (ko) * | 2011-12-26 | 2019-05-09 | 엘지이노텍 주식회사 | 탄화규소 분말, 이의 제조 방법 및 단결정 성장 방법 |
| CN103318857B (zh) * | 2013-07-10 | 2015-11-25 | 石家庄经济学院 | 一种cvd法合成氮化硅纳米环的方法 |
| KR101899701B1 (ko) * | 2014-05-29 | 2018-09-17 | 가부시키가이샤 도요다 지도숏키 | 나노 실리콘 재료와 그 제조 방법 및 이차 전지의 부극 |
| RU2650976C1 (ru) | 2014-05-29 | 2018-04-18 | Кабусики Кайся Тойота Дзидосокки | Кремниевый материал и отрицательный электрод аккумуляторной батареи |
| US10164255B2 (en) | 2014-05-29 | 2018-12-25 | Kabushiki Kaisha Toyota Jidoshokki | Silicon material and negative electrode of secondary battery |
| KR102039085B1 (ko) * | 2015-10-30 | 2019-10-31 | 주식회사 하이원화이어 | 방열코팅용 조성물, 이 조성물을 함유하는 방열코팅, 및 조성물의 제조방법 |
| CN119874384B (zh) * | 2025-03-26 | 2025-07-18 | 山东工业陶瓷研究设计院有限公司 | 一种多孔氮化硅陶瓷的制备方法 |
Citations (2)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO1989007093A1 (en) * | 1988-01-27 | 1989-08-10 | The Dow Chemical Company | A self-reinforced silicon nitride ceramic of high fracture toughness and a method of preparing the same |
| EP0471568A2 (en) * | 1990-08-15 | 1992-02-19 | The Dow Chemical Company | A self-reinforced silicon nitride ceramic body and a method of preparing the same |
Family Cites Families (66)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| GB152160A (en) * | 1919-08-12 | 1920-10-14 | William John Stewart | Improvements in or relating to concrete floors |
| GB1121293A (en) * | 1963-10-28 | 1968-07-24 | Mini Of Technology | Improvements in the manufacture of silicon nitride |
| GB1528160A (en) * | 1975-08-08 | 1978-10-11 | Nat Res Dev | Silicon nitride based components |
| JPS5238500A (en) * | 1975-09-22 | 1977-03-25 | Toshiba Corp | Production of alpha-silicon nitride powder |
| JPS5290499A (en) * | 1976-01-27 | 1977-07-29 | Toshiba Ceramics Co | Process for preparing siliconnitride having high alphaaphase content |
| JPS5348373A (en) * | 1976-10-15 | 1978-05-01 | Hitachi Metals Ltd | Method for incinerating contaminated muds |
| SE427650B (sv) * | 1977-01-13 | 1983-04-25 | Tokyo Shibaura Electric Co | Kiselnitridpulvermaterial samt sett att framstella detsamma |
| JPS53102300A (en) * | 1977-02-18 | 1978-09-06 | Toshiba Corp | Preparation of type silicon nitride powders |
| JPS606884B2 (ja) * | 1977-05-07 | 1985-02-21 | 株式会社東芝 | α型窒化けい素粉末の製造方法 |
| JPS5515946A (en) * | 1978-07-19 | 1980-02-04 | Toray Ind Inc | Production of metal nitride fine powder |
| JPS5622611A (en) * | 1979-07-28 | 1981-03-03 | Sumitomo Electric Ind Ltd | Manufacture of alpha-type silicon nitride powder |
| JPS5692109A (en) * | 1979-12-27 | 1981-07-25 | Sumitomo Electric Ind Ltd | Manufacture of alpha-type silicon nitride powder |
| JPS57106511A (en) * | 1980-12-24 | 1982-07-02 | Sumitomo Electric Ind Ltd | Manufacture of silicon nitride powder |
| JPS5891011A (ja) * | 1981-11-25 | 1983-05-30 | Toshiba Ceramics Co Ltd | α相含有率の高い窒化珪素粉末の製造方法 |
| JPS5891005A (ja) * | 1981-11-25 | 1983-05-30 | Toshiba Corp | 窒化ケイ素粉末の製造方法 |
| JPS5891007A (ja) * | 1981-11-26 | 1983-05-30 | Toshiba Corp | α型窒化けい素粉末の製造方法 |
| JPS5891006A (ja) * | 1981-11-26 | 1983-05-30 | Toshiba Corp | α型窒化ケイ素粉末の製造方法 |
| JPS58104006A (ja) * | 1981-12-11 | 1983-06-21 | Central Glass Co Ltd | 窒化珪素粉末の製造法 |
| JPS58199707A (ja) * | 1982-05-18 | 1983-11-21 | Ube Ind Ltd | 結晶質窒化ケイ素粉末の製法 |
| JPS5950617B2 (ja) * | 1982-06-10 | 1984-12-10 | 太平洋セメント株式会社 | 窒化珪素−炭化珪素組成物の製造法 |
| JPS5921506A (ja) * | 1982-07-27 | 1984-02-03 | Ube Ind Ltd | 結晶質窒化ケイ素粉末の製法 |
| JPS5939704A (ja) * | 1982-08-26 | 1984-03-05 | Asahi Glass Co Ltd | 窒化珪素の合成法 |
| JPS5997508A (ja) * | 1982-11-24 | 1984-06-05 | Toyota Central Res & Dev Lab Inc | 窒化珪素の製造方法 |
| JPS59107976A (ja) * | 1982-12-07 | 1984-06-22 | 東芝セラミツクス株式会社 | 易焼結性窒化ケイ素粉末の製造方法 |
| US4590053A (en) * | 1983-07-14 | 1986-05-20 | Sumitomo Chemical Company, Limited | Method for producing α-form silicon nitride fine powders |
| US4619905A (en) * | 1984-12-24 | 1986-10-28 | Gte Laboratories Incorporated | Process for the synthesis of silicon nitride |
| JPS61236604A (ja) * | 1985-04-11 | 1986-10-21 | Toshiba Ceramics Co Ltd | β−Si↓3N↓4の合成方法 |
| JPH0649565B2 (ja) * | 1985-04-19 | 1994-06-29 | 株式会社東芝 | α型窒化ケイ素粉末の製造方法 |
| DE3675590D1 (de) * | 1985-06-24 | 1990-12-20 | Kawasaki Steel Co | Verfahren zum herstellen von siliziumnitridpulvern. |
| DE3608352A1 (de) * | 1986-03-13 | 1987-09-17 | Bayer Ag | Verfahren zur herstellung von kohlenstoffarmem siliciumnitrid |
| US4851203A (en) * | 1986-04-03 | 1989-07-25 | Atochem | Metal carbide and nitride powders |
| DE3612162A1 (de) * | 1986-04-11 | 1987-10-15 | Bayer Ag | Verfahren zur herstellung von siliciumnitrid |
| JPH0723203B2 (ja) * | 1986-05-06 | 1995-03-15 | 小野田セメント株式会社 | α型窒化珪素粉末の製造方法 |
| JPS63239104A (ja) * | 1986-12-11 | 1988-10-05 | Sumitomo Chem Co Ltd | β相含有窒化ケイ素微粉末の製造方法 |
| JPS63162511A (ja) * | 1986-12-26 | 1988-07-06 | Toshiba Ceramics Co Ltd | 窒化ケイ素の製造方法 |
| JPS63162515A (ja) * | 1986-12-26 | 1988-07-06 | Toshiba Ceramics Co Ltd | 窒化ケイ素の製造方法 |
| JPH0791043B2 (ja) * | 1986-12-26 | 1995-10-04 | 東芝セラミツクス株式会社 | 窒化ケイ素の製造方法 |
| JPS63162513A (ja) * | 1986-12-26 | 1988-07-06 | Toshiba Ceramics Co Ltd | 窒化ケイ素の製造方法 |
| JPS63176301A (ja) * | 1987-01-19 | 1988-07-20 | Toshiba Ceramics Co Ltd | 窒化珪素粉末の製造方法 |
| US4919689A (en) * | 1988-01-27 | 1990-04-24 | The Dow Chemical Company | Self-reinforced silicon nitride ceramic of high fracture toughness |
| US5160508A (en) * | 1988-01-27 | 1992-11-03 | The Dow Chemical Company | Self-reinforced silicon nitride ceramic of high fracture toughness |
| US5120328A (en) * | 1988-01-27 | 1992-06-09 | The Dow Chemical Company | Dense, self-reinforced silicon nitride ceramic prepared by pressureless or low pressure gas sintering |
| US5021372A (en) * | 1988-01-27 | 1991-06-04 | The Dow Chemical Company | Method of preparing a self-reinforced silicon nitride ceramic of high fracture toughness |
| US5118645A (en) * | 1988-01-27 | 1992-06-02 | The Dow Chemical Company | Self-reinforced silicon nitride ceramic of high fracture toughness and a method of preparing the same |
| JP2646228B2 (ja) * | 1988-03-07 | 1997-08-27 | 東芝セラミックス株式会社 | 窒化ケイ素粉末の製造方法 |
| US4986972A (en) * | 1988-03-17 | 1991-01-22 | Toshiba Ceramics Co., Ltd. | Method for making silicon nitride powder |
| JPH01308231A (ja) * | 1988-06-03 | 1989-12-12 | Takeda Chem Ind Ltd | 安定化された医薬組成物および製造法 |
| EP0400650B1 (en) * | 1989-05-31 | 1996-10-09 | Kabushiki Kaisha Toshiba | Linearized differential amplifier |
| JPH035374A (ja) * | 1989-06-01 | 1991-01-11 | Mitsubishi Gas Chem Co Inc | 窒化ケイ素―炭化ケイ素複合焼結体およびその製造法 |
| JP2855460B2 (ja) * | 1990-02-07 | 1999-02-10 | 日本セメント株式会社 | 窒化けい素系複合粉末の製造方法 |
| JPH03237008A (ja) * | 1990-02-09 | 1991-10-22 | Shin Etsu Chem Co Ltd | 窒化ケイ素粉末の処理方法 |
| JPH04130063A (ja) * | 1990-09-17 | 1992-05-01 | Toshiba Ceramics Co Ltd | セラミック複合材料の製造方法 |
| JPH04209705A (ja) * | 1990-11-30 | 1992-07-31 | Sumitomo Chem Co Ltd | 窒化珪素質粉末の製造方法 |
| JP2842723B2 (ja) * | 1990-12-27 | 1999-01-06 | 京セラ株式会社 | 窒化珪素−炭化珪素質複合焼結体およびその製造方法 |
| DE4102628A1 (de) * | 1991-01-30 | 1992-08-06 | Bayer Ag | Verfahren zur herstellung eines werkstoffes auf si(pfeil abwaerts)3(pfeil abwaerts)n(pfeil abwaerts)4(pfeil abwaerts)-basis, so hergestellte werkstoffe sowie deren verwendung |
| JPH04294903A (ja) * | 1991-03-20 | 1992-10-19 | Riken Corp | 切削工具 |
| JPH05809A (ja) * | 1991-06-21 | 1993-01-08 | Toshiba Ceramics Co Ltd | 窒化けい素−炭化けい素複合粉末の製造方法 |
| JP2892186B2 (ja) * | 1991-07-17 | 1999-05-17 | 京セラ株式会社 | 窒化珪素−炭化珪素質複合焼結体の製造方法 |
| JPH0524924A (ja) * | 1991-07-19 | 1993-02-02 | Ngk Spark Plug Co Ltd | SiC被覆窒化珪素−炭化珪素複合焼結体 |
| EP0552381B1 (en) * | 1991-08-13 | 1998-04-29 | Sumitomo Electric Industries, Ltd. | Composite silicon nitride sinter and production thereof |
| FR2687393B1 (fr) * | 1992-02-18 | 1994-04-15 | Elf Atochem Sa | Procede continu de preparation de nitrure de silicium par carbonitruration et nitrure de silicium ainsi obtenu. |
| US5256610A (en) * | 1992-11-27 | 1993-10-26 | The United States Of America As Represented By The Administrator Of The National Aeronautics And Space Administration | Sintering silicon nitride |
| US5424256A (en) * | 1993-03-17 | 1995-06-13 | Sumitomo Electric Industries, Ltd. | Silicon nitride sintered body |
| US5384292A (en) * | 1993-04-14 | 1995-01-24 | Sumitomo Electric Industries, Ltd. | Silicon nitride composite sintered body and process for producing the same |
| US5523268A (en) * | 1993-12-22 | 1996-06-04 | Kabushiki Kaisha Toyota Chuo Kenkyusho | Silicon nitride sintered body |
| JPH0815945A (ja) * | 1994-07-04 | 1996-01-19 | Fuji Xerox Co Ltd | 多色画像形成装置 |
-
1994
- 1994-04-14 US US08/227,751 patent/US5538675A/en not_active Expired - Lifetime
-
1995
- 1995-04-14 WO PCT/US1995/004573 patent/WO1995028366A1/en not_active Ceased
- 1995-04-14 DE DE69518746T patent/DE69518746T2/de not_active Expired - Fee Related
- 1995-04-14 EP EP95916972A patent/EP0755367B1/en not_active Expired - Lifetime
- 1995-04-14 ES ES95916972T patent/ES2149359T3/es not_active Expired - Lifetime
- 1995-04-14 JP JP7527088A patent/JPH09511981A/ja not_active Ceased
- 1995-04-14 CA CA002187333A patent/CA2187333A1/en not_active Abandoned
- 1995-06-07 US US08/484,539 patent/US5525556A/en not_active Expired - Lifetime
-
1996
- 1996-07-12 US US08/678,199 patent/US5643843A/en not_active Expired - Lifetime
Patent Citations (2)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO1989007093A1 (en) * | 1988-01-27 | 1989-08-10 | The Dow Chemical Company | A self-reinforced silicon nitride ceramic of high fracture toughness and a method of preparing the same |
| EP0471568A2 (en) * | 1990-08-15 | 1992-02-19 | The Dow Chemical Company | A self-reinforced silicon nitride ceramic body and a method of preparing the same |
Non-Patent Citations (1)
| Title |
|---|
| T. LICKO ET AL.: "Synthesis of silicon nitride ...", JOURNAL OF THE EUROPEAN CERAMIC SOCIETY, vol. 9, 1992, GB, pages 219 - 230 * |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN1061961C (zh) * | 1997-07-16 | 2001-02-14 | 国家建筑材料工业局山东工业陶瓷研究设计院 | 纳米碳化硅--氮化硅复相陶瓷的制备方法 |
Also Published As
| Publication number | Publication date |
|---|---|
| EP0755367B1 (en) | 2000-09-06 |
| JPH09511981A (ja) | 1997-12-02 |
| US5643843A (en) | 1997-07-01 |
| US5525556A (en) | 1996-06-11 |
| CA2187333A1 (en) | 1995-10-26 |
| DE69518746T2 (de) | 2000-12-28 |
| ES2149359T3 (es) | 2000-11-01 |
| US5538675A (en) | 1996-07-23 |
| DE69518746D1 (de) | 2000-10-12 |
| EP0755367A1 (en) | 1997-01-29 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| EP0755367B1 (en) | Silicon nitride/silicon carbide composite powders, their preparation and densified materials prepared using the composite powders | |
| US4788167A (en) | Aluminum nitride/aluminum oxynitride/group IVB metal nitride abrasive particles derived from a sol-gel process | |
| Rajendran | Production of ultrafine alpha alumina powders and fabrication of fine grained strong ceramics | |
| EP0139793B1 (en) | A silicon nitride sintered body and a method for producing it | |
| US5342811A (en) | Composition and method for producing boron carbide/titanium diboride composite ceramic powders using a boron carbide substrate | |
| US5312785A (en) | Sintered self-reinforced silicon nitride | |
| JP2003040615A (ja) | 微粒αアルミナ粉末およびその製造方法 | |
| US5352641A (en) | Silicon nitride composite sintered body and process for producing same | |
| US4957886A (en) | Aluminum oxide/aluminum oxynitride/group IVB metal nitride abrasive particles derived from a sol-gel process | |
| US5182059A (en) | Process for producing high density SiC sintered bodies | |
| JPH0250076B2 (enExample) | ||
| US4855264A (en) | Aluminum oxide/aluminum oxynitride/group IVB metal nitride abrasive particles derived from a sol-gel process | |
| JPH11322433A (ja) | 窒化硼素含有複合セラミックス焼結体の製造方法及び同焼結体 | |
| US5294575A (en) | Silicon nitride ceramics containing crystallized grain boundary phases | |
| AU8018887A (en) | Aluminum oxide/aluminum oxynitride/group ivb metal nitride abrasive particles derived from a sol-gel process | |
| Amroune et al. | Synthesis of Al2O3–SiC from kyanite precursor | |
| KR20210088361A (ko) | 질화규소 소결체의 제조방법 및 이에 따라 제조된 질화규소 소결체 | |
| JP7862246B2 (ja) | 焼結用窒化ケイ素粉末 | |
| JP3268020B2 (ja) | 窒化珪素粉末の製造方法 | |
| JPH06219828A (ja) | ムライト・炭化珪素複合セラミックスの製造方法 | |
| AU566978B2 (en) | Producing beta- silicon aluminium oxynitride | |
| Dorn et al. | Particle size control during production of ceramic nitride powders | |
| JPH1129361A (ja) | 窒化ケイ素焼結体及びその製造方法 | |
| JP3251060B2 (ja) | 窒化珪素粉末 | |
| US5173459A (en) | Si3 N4 -A12 O3 composite sintered bodies and method of producing the same |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| AK | Designated states |
Kind code of ref document: A1 Designated state(s): CA JP |
|
| AL | Designated countries for regional patents |
Kind code of ref document: A1 Designated state(s): AT BE CH DE DK ES FR GB GR IE IT LU MC NL PT SE |
|
| DFPE | Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed before 20040101) | ||
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application | ||
| WWE | Wipo information: entry into national phase |
Ref document number: 2187333 Country of ref document: CA |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 1995916972 Country of ref document: EP |
|
| WWP | Wipo information: published in national office |
Ref document number: 1995916972 Country of ref document: EP |
|
| WWG | Wipo information: grant in national office |