WO2019013136A1 - 半導体装置 - Google Patents

半導体装置 Download PDF

Info

Publication number
WO2019013136A1
WO2019013136A1 PCT/JP2018/025767 JP2018025767W WO2019013136A1 WO 2019013136 A1 WO2019013136 A1 WO 2019013136A1 JP 2018025767 W JP2018025767 W JP 2018025767W WO 2019013136 A1 WO2019013136 A1 WO 2019013136A1
Authority
WO
WIPO (PCT)
Prior art keywords
semiconductor
barrier
semiconductor device
region
electrode
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2018/025767
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
雅裕 杉本
勲 ▲高▼橋
仁志 神原
四戸 孝
俊実 人羅
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Flosfia Inc
Original Assignee
Flosfia Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Priority to EP18831783.8A priority Critical patent/EP3654387A4/en
Priority to KR1020237010290A priority patent/KR20230044336A/ko
Priority to KR1020207000628A priority patent/KR20200020785A/ko
Priority to SG11202000144YA priority patent/SG11202000144YA/en
Priority to JP2019529115A priority patent/JP7313609B2/ja
Priority to KR1020257007346A priority patent/KR102999308B1/ko
Application filed by Flosfia Inc filed Critical Flosfia Inc
Priority to US16/628,341 priority patent/US11450774B2/en
Priority to CN201880045648.7A priority patent/CN110870079B/zh
Publication of WO2019013136A1 publication Critical patent/WO2019013136A1/ja
Anticipated expiration legal-status Critical
Priority to JP2023050423A priority patent/JP7595966B2/ja
Ceased legal-status Critical Current

Links

Images

Classifications

    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10D—INORGANIC ELECTRIC SEMICONDUCTOR DEVICES
    • H10D8/00—Diodes
    • H10D8/60—Schottky-barrier diodes 
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10D—INORGANIC ELECTRIC SEMICONDUCTOR DEVICES
    • H10D62/00—Semiconductor bodies, or regions thereof, of devices having potential barriers
    • H10D62/10—Shapes, relative sizes or dispositions of the regions of the semiconductor bodies; Shapes of the semiconductor bodies
    • H10D62/102—Constructional design considerations for preventing surface leakage or controlling electric field concentration
    • H10D62/103—Constructional design considerations for preventing surface leakage or controlling electric field concentration for increasing or controlling the breakdown voltage of reverse-biased devices
    • H10D62/105—Constructional design considerations for preventing surface leakage or controlling electric field concentration for increasing or controlling the breakdown voltage of reverse-biased devices by having particular doping profiles, shapes or arrangements of PN junctions; by having supplementary regions, e.g. junction termination extension [JTE] 
    • H10D62/106—Constructional design considerations for preventing surface leakage or controlling electric field concentration for increasing or controlling the breakdown voltage of reverse-biased devices by having particular doping profiles, shapes or arrangements of PN junctions; by having supplementary regions, e.g. junction termination extension [JTE]  having supplementary regions doped oppositely to or in rectifying contact with regions of the semiconductor bodies, e.g. guard rings with PN or Schottky junctions
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10D—INORGANIC ELECTRIC SEMICONDUCTOR DEVICES
    • H10D62/00—Semiconductor bodies, or regions thereof, of devices having potential barriers
    • H10D62/10—Shapes, relative sizes or dispositions of the regions of the semiconductor bodies; Shapes of the semiconductor bodies
    • H10D62/102—Constructional design considerations for preventing surface leakage or controlling electric field concentration
    • H10D62/103—Constructional design considerations for preventing surface leakage or controlling electric field concentration for increasing or controlling the breakdown voltage of reverse-biased devices
    • H10D62/105—Constructional design considerations for preventing surface leakage or controlling electric field concentration for increasing or controlling the breakdown voltage of reverse-biased devices by having particular doping profiles, shapes or arrangements of PN junctions; by having supplementary regions, e.g. junction termination extension [JTE] 
    • H10D62/106—Constructional design considerations for preventing surface leakage or controlling electric field concentration for increasing or controlling the breakdown voltage of reverse-biased devices by having particular doping profiles, shapes or arrangements of PN junctions; by having supplementary regions, e.g. junction termination extension [JTE]  having supplementary regions doped oppositely to or in rectifying contact with regions of the semiconductor bodies, e.g. guard rings with PN or Schottky junctions
    • H10D62/107—Buried supplementary regions, e.g. buried guard rings 
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10D—INORGANIC ELECTRIC SEMICONDUCTOR DEVICES
    • H10D62/00—Semiconductor bodies, or regions thereof, of devices having potential barriers
    • H10D62/40—Crystalline structures
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10D—INORGANIC ELECTRIC SEMICONDUCTOR DEVICES
    • H10D62/00—Semiconductor bodies, or regions thereof, of devices having potential barriers
    • H10D62/80—Semiconductor bodies, or regions thereof, of devices having potential barriers characterised by the materials
    • H10D62/875—Semiconductor bodies, or regions thereof, of devices having potential barriers characterised by the materials being semiconductor metal oxide, e.g. InGaZnO
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10D—INORGANIC ELECTRIC SEMICONDUCTOR DEVICES
    • H10D64/00—Electrodes of devices having potential barriers
    • H10D64/60—Electrodes characterised by their materials
    • H10D64/64—Electrodes comprising a Schottky barrier to a semiconductor
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10D—INORGANIC ELECTRIC SEMICONDUCTOR DEVICES
    • H10D99/00—Subject matter not provided for in other groups of this subclass

Definitions

  • the present invention relates to a semiconductor device useful as a power device or the like and a semiconductor system provided with the same.
  • Patent Document 1 a metal having a small barrier height is disposed at the central portion on the semiconductor, and a Schottky contact between the metal and the semiconductor having a large barrier height is formed at the peripheral portion on the semiconductor to achieve reverse breakdown voltage. It is described to increase the size and further reduce the forward rise voltage.
  • Patent Document 2 discloses a wide band gap semiconductor in which a Schottky electrode and an ohmic electrode made of the same metal are formed on a substrate. The device is described, and it is described that such a configuration can improve the resistance to thermal destruction when a high current such as a surge current flows in the forward direction.
  • a high current such as a surge current flows in the forward direction.
  • the electrode material also needs to be restricted.
  • the barrier height changes depending on the temperature. There were problems, etc. and it was not always satisfactory. Therefore, a semiconductor device having a low rising voltage and excellent temperature stability has been desired.
  • Patent Document 3 describes a semiconductor device in which a conductive guard ring and a main junction joined to a Schottky electrode are connected to each other through a short circuit portion. It is described that the concentration of the electric field is alleviated, which contributes to the improvement of the withstand voltage. However, even if a large number of guard rings are installed, they are short-circuited with the main joint, so that there is a problem that the withstand voltage is deteriorated.
  • An object of the present invention is to provide a semiconductor device having excellent Schottky characteristics and semiconductor characteristics.
  • the present inventors have found that in the semiconductor device provided with at least a semiconductor region and a barrier electrode provided on the semiconductor region, the semiconductor region and the barrier electrode The rising voltage is lowered by embedding a plurality of barrier height adjusting regions, in which the barrier height with the barrier electrode is larger than the barrier height at the interface between the semiconductor region and the barrier electrode, between the semiconductor region and the barrier electrode. It has been found that the characteristics can be made excellent and the breakdown voltage can be made more excellent, and it has been found that such a semiconductor device can solve the above-mentioned conventional problems at once. In addition, after obtaining the above-mentioned findings, the present inventors repeated studies to complete the present invention.
  • a semiconductor device comprising at least a semiconductor region and a barrier electrode provided on the semiconductor region, wherein the semiconductor region and the barrier electrode are provided between the semiconductor region and the barrier electrode. And a plurality of barrier height adjusting regions are provided on the surface of the semiconductor region, wherein a barrier height adjusting region is provided such that a barrier height with the barrier electrode is larger than a barrier height at an interface of the semiconductor device.
  • a semiconductor device comprising at least a semiconductor region and a barrier electrode provided on the semiconductor region, wherein the semiconductor region and the barrier electrode are provided between the semiconductor region and the barrier electrode. And a plurality of barrier height adjusting regions are embedded in a surface of the semiconductor region.
  • the barrier height adjustment region contains a p-type oxide semiconductor as a main component.
  • the barrier height adjustment region contains a p-type oxide semiconductor having a corundum structure or a hexagonal crystal structure as a main component.
  • a semiconductor system comprising a semiconductor device, wherein the semiconductor device is the semiconductor device according to any one of the above [1] to [16].
  • the semiconductor device of the present invention is excellent in Schottky characteristics and semiconductor characteristics.
  • JBS junction barrier Schottky diode
  • mode of the junction barrier Schottky diode (JBS) of this invention It is a figure which shows typically the suitable one aspect
  • FIG. 1 It is a figure which shows typically a suitable example of the power supply circuit diagram of a power supply device. It is a schematic block diagram of the film-forming apparatus (mist CVD apparatus) used in the reference example. It is a figure which shows IV measurement result in a reference example, (a) shows a forward direction measurement result, (b) shows a reverse direction measurement result. It is a figure which shows typically the suitable one aspect
  • JBS junction barrier Schottky diode
  • JBS junction barrier Schottky diode
  • mode of the junction barrier Schottky diode (JBS) of this invention It is a figure which shows typically the suitable one aspect
  • the semiconductor device of the present invention is a semiconductor device including at least a semiconductor region and a barrier electrode provided on the semiconductor region, wherein the semiconductor region is provided between the semiconductor region and the barrier electrode.
  • a barrier height adjusting region is provided in which a barrier height with the barrier electrode is larger than a barrier height at the interface with the barrier electrode, and a plurality of the barrier height adjusting regions are provided on the surface of the semiconductor region.
  • a semiconductor device of the present invention is a semiconductor device including at least a semiconductor region and a barrier electrode provided on the semiconductor region, wherein the semiconductor is located between the semiconductor region and the barrier electrode.
  • a barrier height adjusting region is provided in which the barrier height with the barrier electrode is larger than the barrier height at the interface between the region and the barrier electrode, and a plurality of the barrier height adjusting regions are embedded in the surface of the semiconductor region. .
  • the barrier height adjusting region protrudes into the barrier electrode, and the barrier height adjusting region is embedded in the surface of the semiconductor region and further protrudes into the barrier electrode. preferable.
  • the concentration of the electric field can be further suppressed and the contact resistance can be further reduced.
  • the barrier electrode is not particularly limited as long as it forms a Schottky barrier having a predetermined barrier height at the interface with the semiconductor region.
  • the electrode material of the barrier electrode is not particularly limited as long as it can be used as a barrier electrode, and may be a conductive inorganic material or a conductive organic material.
  • the electrode material is preferably a metal.
  • the metal is not particularly limited, but preferably includes, for example, at least one metal selected from Groups 4 to 11 of the periodic table. Examples of the metal of Group 4 of the periodic table include titanium (Ti), zirconium (Zr), hafnium (Hf) and the like, among which Ti is preferable.
  • metal of periodic table group 5 for example, vanadium (V), niobium (Nb), tantalum (Ta) and the like can be mentioned.
  • the metal of Group 6 of the periodic table include one or more metals selected from chromium (Cr), molybdenum (Mo), tungsten (W) and the like, but in the present invention, Cr is preferable because semiconductor characteristics such as switching characteristics are further improved.
  • Cr is preferable because semiconductor characteristics such as switching characteristics are further improved.
  • metal of periodic table group 7 for example, manganese (Mn), technetium (Tc), rhenium (Re) and the like can be mentioned.
  • the metal of Group 8 of the periodic table include iron (Fe), ruthenium (Ru), osmium (Os) and the like.
  • Examples of the metal of Group 9 of the periodic table include cobalt (Co), rhodium (Rh), iridium (Ir) and the like.
  • a metal of periodic table group 10 for example, nickel (Ni), palladium (Pd), platinum (Pt) and the like can be mentioned, among which Pt is preferable.
  • a metal of periodic table 11 group copper (Cu), silver (Ag), gold (Au) etc. are mentioned, for example.
  • Examples of means for forming the barrier electrode include, for example, known means, and more specifically, for example, a dry method, a wet method, and the like. Examples of the dry method include known means such as sputtering, vacuum evaporation, and CVD. Examples of the wet method include screen printing and die coating.
  • the semiconductor region is not particularly limited as long as it contains a semiconductor as a main component, but in the present invention, the semiconductor region preferably contains a crystalline oxide semiconductor as a main component, and an n-type semiconductor as a main component.
  • the n-type semiconductor region is more preferably included.
  • the crystalline oxide semiconductor preferably has a ⁇ -Galia structure or a corundum structure, and more preferably a corundum structure.
  • the semiconductor region preferably contains a gallium compound as a main component, more preferably an InAlGaO-based semiconductor, and most preferably ⁇ -Ga 2 O 3 or a mixed crystal thereof. .
  • main component means, for example, when the crystalline oxide semiconductor is ⁇ -Ga 2 O 3 , the atomic ratio of gallium in the metal element in the semiconductor region is 0.5 or more, and the ratio is ⁇ -Ga. That is fine if 2 O 3 is included.
  • the atomic ratio of gallium in the metal element in the semiconductor region is preferably 0.7 or more, more preferably 0.8 or more.
  • the semiconductor region is usually a single phase region, but may have a second semiconductor region composed of a different semiconductor phase or another phase as long as the object of the present invention is not impaired.
  • the semiconductor region is usually in the form of a film, and may be a semiconductor film.
  • the thickness of the semiconductor film in the semiconductor region is not particularly limited, and may be 1 ⁇ m or less, or 1 ⁇ m or more, but in the present invention, it is preferably 1 ⁇ m to 40 ⁇ m, and 1 ⁇ m to More preferably, it is 25 ⁇ m.
  • Surface area of the semiconductor film is not particularly limited, and may be 1 mm 2 or more, may be 1 mm 2 or less.
  • the crystalline oxide semiconductor is usually single crystal, it may be polycrystalline.
  • the semiconductor film may be a single layer film or a multilayer film.
  • the multilayer film preferably has a thickness of 40 ⁇ m or less, and is a multilayer film including at least a first semiconductor layer and a second semiconductor layer, In the case where a Schottky electrode is provided on the first semiconductor layer, it is also preferable that the multilayer film has a carrier concentration of the first semiconductor layer smaller than that of the second semiconductor layer.
  • the second semiconductor layer usually contains a dopant, and the carrier concentration of the semiconductor layer can be appropriately set by adjusting the doping amount.
  • the semiconductor film preferably contains a dopant.
  • the dopant is not particularly limited, and may be known. Examples of the dopant include n-type dopants such as tin, germanium, silicon, titanium, zirconium, vanadium or niobium, and p-type dopants. In the present invention, the dopant is preferably Sn, Ge or Si.
  • the content of the dopant in the composition of the semiconductor film is preferably 0.00001 at% or more, more preferably 0.00001 at% to 20 at%, and 0.00001 at% to 10 at% Is most preferred.
  • the dopant used in the first semiconductor layer is germanium, silicon, titanium, zirconium, vanadium or niobium, and the dopant used in the second semiconductor layer is tin. It is preferable because the semiconductor characteristics are further improved without loss.
  • the semiconductor film is formed, for example, by means of a mist CVD method, and more specifically, for example, the raw material solution is atomized or formed into droplets (atomization / droplet formation step), the obtained mist or liquid
  • the droplet is transported by carrier gas onto the substrate (transporting step), and then the mist or droplet is thermally reacted in the film forming chamber to form a semiconductor film containing a crystalline oxide semiconductor as a main component on the substrate. It is suitably formed by laminating (film forming process).
  • the raw material solution is atomized or formed into droplets.
  • the means for atomizing or dropletizing the raw material solution is not particularly limited as long as it can atomize or drop the raw material solution, and may be a known means, but in the present invention, ultrasonic waves are used.
  • the atomizing means or dropletizing means used is preferred.
  • the mist or droplet obtained by using ultrasonic waves is preferable because it has an initial velocity of zero and floats in the air, and for example, it is possible to float in a space and carry it as a gas rather than spraying it like a spray. As it is a possible mist, it is very suitable because it is not damaged by collision energy.
  • the droplet size is not particularly limited, and may be about several mm, but preferably 50 ⁇ m or less, more preferably 100 nm to 10 ⁇ m.
  • the raw material solution is not particularly limited as long as it can be atomized or formed into droplets, and contains a raw material capable of forming a semiconductor region, and may be an inorganic material or an organic material.
  • the raw material is preferably a metal or a metal compound, and gallium, iron, indium, aluminum, vanadium, titanium, chromium, rhodium, nickel, cobalt, zinc, magnesium, calcium, silicon, yttrium, strontium and the like More preferably, it contains one or more metals selected from barium.
  • the raw material solution one in which the metal is dissolved or dispersed in the form of a complex or a salt in an organic solvent or water can be suitably used.
  • the form of the complex include acetylacetonato complex, carbonyl complex, ammine complex, hydride complex and the like.
  • the salt form include organic metal salts (eg, metal acetates, metal oxalates, metal citrates, etc.), metal sulfides, metal nitrates, metal phosphates, metal halides (eg metal chlorides) Salts, metal bromide salts, metal iodide salts and the like) and the like.
  • hydrohalic acid examples include hydrobromic acid, hydrochloric acid, hydroiodic acid and the like, among which hydrobromic acid or hydroiodic acid because a better film can be obtained.
  • oxidizing agent examples include hydrogen peroxide (H 2 O 2 ), sodium peroxide (Na 2 O 2 ), barium peroxide (BaO 2 ), benzoyl peroxide (C 6 H 5 CO) 2 O 2 and the like.
  • the raw material solution may contain a dopant. Doping can be favorably performed by including the dopant in the raw material solution.
  • the dopant is not particularly limited as long as the object of the present invention is not impaired.
  • Examples of the dopant include n-type dopants such as tin, germanium, silicon, titanium, zirconium, vanadium or niobium, and p-type dopants.
  • the concentration of the dopant may generally be about 1 ⁇ 10 16 / cm 3 to 1 ⁇ 10 22 / cm 3 , and the concentration of the dopant may be low, for example, about 1 ⁇ 10 17 / cm 3 or less. May be Furthermore, according to the present invention, the dopant may be contained at a high concentration of about 1 ⁇ 10 20 / cm 3 or more. In the present invention, the carrier concentration is preferably 1 ⁇ 10 17 / cm 3 or more.
  • the solvent of the raw material solution is not particularly limited, and may be an inorganic solvent such as water, an organic solvent such as alcohol, or a mixed solvent of an inorganic solvent and an organic solvent.
  • the solvent preferably contains water, and more preferably water or a mixed solvent of water and an alcohol.
  • the mist or the droplets are transferred into the film forming chamber with a carrier gas.
  • the carrier gas is not particularly limited as long as the object of the present invention is not impaired.
  • oxygen, ozone, an inert gas such as nitrogen or argon, or a reducing gas such as hydrogen gas or a forming gas is preferable. It can be mentioned.
  • one kind of carrier gas may be used, two or more kinds may be used, and a dilution gas with a reduced flow rate (for example, 10-fold dilution gas etc.) is further used as a second carrier gas. It is also good.
  • the carrier gas may be supplied not only to one place, but also to two or more places.
  • the flow rate of the carrier gas is not particularly limited, but is preferably 0.01 to 20 L / min, and more preferably 1 to 10 L / min.
  • the flow rate of the dilution gas is preferably 0.001 to 2 L / min and more preferably 0.1 to 1 L / min.
  • the semiconductor film is formed on the substrate by thermally reacting the mist or the droplets in the film forming chamber.
  • the thermal reaction may be any reaction as long as the mist or the droplets react with heat, and the reaction conditions are not particularly limited as long as the object of the present invention is not impaired.
  • the thermal reaction is usually carried out at a temperature higher than the evaporation temperature of the solvent, preferably not higher than the temperature (eg 1000 ° C.), more preferably 650 ° C. or less, most preferably 300 ° C. to 650 ° C. preferable.
  • the thermal reaction may be carried out under any atmosphere of vacuum, non-oxygen atmosphere, reducing gas atmosphere and oxygen atmosphere, as long as the object of the present invention is not impaired. It is preferred to be carried out under an atmosphere. Moreover, although it may be performed under any pressure of atmospheric pressure, under pressure and under reduced pressure, in the present invention, it is preferable to carry out under atmospheric pressure. Note that the film thickness can be set by adjusting the film formation time.
  • the substrate is not particularly limited as long as it can support the semiconductor film.
  • the material of the substrate is also not particularly limited as long as the object of the present invention is not impaired, and the substrate may be a known substrate, may be an organic compound, or may be an inorganic compound.
  • the shape of the substrate may be any shape, and is effective for any shape, for example, plate-like such as flat plate or disc, fiber-like, rod-like, cylindrical, prismatic, Although cylindrical shape, helical shape, spherical shape, ring shape etc. are mentioned, a substrate is preferable in the present invention.
  • the thickness of the substrate is not particularly limited in the present invention.
  • the substrate is not particularly limited as long as it has a plate shape and serves as a support of the semiconductor film.
  • the substrate may be an insulator substrate, a semiconductor substrate, a metal substrate or a conductive substrate, but it is preferable that the substrate is an insulator substrate, and that a metal is used on the surface. It is also preferred that it is a substrate having a film.
  • the substrate includes, for example, a base substrate containing a substrate material having a corundum structure as a main component, a base substrate containing a substrate material having a ⁇ -gallia structure as a main component, and a substrate material having a hexagonal crystal structure as a main component
  • An underlying substrate may, for example, be mentioned.
  • main component means that the substrate material having the above-mentioned specific crystal structure is, in atomic ratio, preferably 50% or more, more preferably 70% or more, still more preferably 90% to all components of the substrate material. % Or more is included, and may be 100%.
  • the substrate material is not particularly limited as long as the object of the present invention is not impaired, and may be known.
  • the substrate material having a corundum structure of the for example, ⁇ -Al 2 O 3 (sapphire substrate) or ⁇ -Ga 2 O 3 is preferably mentioned, a plane sapphire substrate, m-plane sapphire substrate, r-plane sapphire substrate And c-plane sapphire substrates, ⁇ -type gallium oxide substrates (a-plane, m-plane or r-plane) and the like are more preferable examples.
  • a base substrate having a substrate material having a ⁇ -gallia structure as a main component for example, a ⁇ -Ga 2 O 3 substrate or containing Ga 2 O 3 and Al 2 O 3 and containing Al 2 O 3 in an amount of more than 0 wt%
  • a mixed crystal substrate having 60 wt% or less and the like can be mentioned.
  • a base substrate which has a substrate material which has a hexagonal crystal structure as a main component a SiC substrate, a ZnO substrate, a GaN substrate etc. are mentioned, for example.
  • an annealing treatment may be performed after the film forming step.
  • the treatment temperature for annealing is not particularly limited as long as the object of the present invention is not impaired, and is usually 300 ° C. to 650 ° C., preferably 350 ° C. to 550 ° C.
  • the annealing treatment time is usually 1 minute to 48 hours, preferably 10 minutes to 24 hours, and more preferably 30 minutes to 12 hours.
  • the annealing treatment may be performed under any atmosphere as long as the object of the present invention is not impaired, but preferably under non-oxygen atmosphere, more preferably under nitrogen atmosphere.
  • the semiconductor film may be provided directly on the substrate, or the semiconductor film may be provided through another layer such as a buffer layer (buffer layer) or a stress relaxation layer.
  • a buffer layer buffer layer
  • a stress relaxation layer a layer such as a stress relaxation layer.
  • the means for forming each layer is not particularly limited and may be a known means, but in the present invention, the mist CVD method is preferable.
  • the semiconductor film may be used as a semiconductor region in a semiconductor device or may be used as a semiconductor region as it is in a semiconductor device after using a known means such as peeling off the substrate or the like. Good.
  • the barrier height adjusting region is not particularly limited as long as the barrier height with the barrier electrode or the semiconductor region is larger than the barrier height at the interface between the semiconductor region and the barrier electrode.
  • the barrier height adjustment region generally contains a conductive material whose barrier height with the barrier electrode or the semiconductor region is larger than the barrier height at the interface between the semiconductor region and the barrier electrode.
  • the term "main component" means that the conductive material is contained in an atomic ratio of preferably 50% or more, more preferably 70% or more, still more preferably 90% or more based on all components of the barrier height adjusting region. May be 100%.
  • the conductive material is not particularly limited as long as the object of the present invention is not impaired, but is preferably a metal oxide or a metal.
  • the metal oxide examples include those exemplified as the main component of the semiconductor region.
  • the metal examples include those exemplified as the barrier electrode.
  • the adjustment of the barrier height may be performed by controlling oxygen concentration, impurity concentration, interface state density, termination structure, crystal structure or surface asperity, or modulating work function or electron affinity using known means. You may go by.
  • the barrier height adjusting region preferably contains a p-type semiconductor as a main component.
  • the p-type semiconductor include crystalline oxide semiconductors that are p-type doped using p-type dopants (preferably, Mg, Zn, Ca).
  • the p-type semiconductor preferably has a corundum structure or a hexagonal crystal structure, and more preferably a corundum structure.
  • the p-type semiconductor is preferably an oxide semiconductor containing gallium, more preferably an InAlGaO-based semiconductor as a main component, and mainly ⁇ -Ga 2 O 3 or a mixed crystal thereof. It is most preferable to include as a component.
  • the p-type semiconductor suitably used for the barrier height adjusting layer can be obtained, for example, by a mist CVD method by adding a p-type dopant and hydrobromic acid to a raw material solution containing a metal.
  • each means, and each condition it may be the same as that of the above-mentioned atomization * droplet formation process, a conveyance process, a film-forming process, each means, each condition etc.
  • the barrier height of the Schottky barrier between the barrier height adjusting layer and the barrier electrode is preferably adjusted to 1 eV or more.
  • semiconductor characteristics for example, switching characteristics etc.
  • the number of barrier height adjusting regions is not particularly limited as long as it is two or more. In the present invention, when the number of barrier height adjusting regions is three or more, the barrier height can be adjusted more effectively, and the semiconductor characteristics of the semiconductor device can be further improved. Preferably, it is 4 or more.
  • the means for forming the barrier height adjusting region is not particularly limited as long as the object of the present invention is not impaired, and may be a known means.
  • a means may be provided in which a plurality of trenches are provided in the surface of the semiconductor region on the side of the interface with the barrier electrode, and then a film made of the main component of the barrier height adjusting region is formed in the trenches.
  • surface modification is performed on a partial region of the semiconductor region using known surface treatment means such as dry etching, wet etching, plasma treatment, ultraviolet light treatment, heat treatment, or surface treatment with an organic solvent or organic acid or the like
  • a heat treatment for example, electron beam annealing, laser annealing or the like
  • an ultraviolet light treatment may be performed on the partial region after or at the time of interface formation to form a barrier height adjustment region.
  • the above-described means may be combined to form a barrier height adjustment region.
  • implementation of the formation means of these barrier height adjustment area may be performed in a vacuum atmosphere, may be performed in air
  • the semiconductor device of the present invention generally includes an ohmic electrode.
  • the ohmic electrode may be a known electrode material, and is not particularly limited as long as the object of the present invention is not impaired.
  • the ohmic electrode contains a metal of Group 4 or Group 11 of the periodic table.
  • the metal of periodic table group 4 or 11 used for the ohmic electrode may be similar to the metal contained in the Schottky electrode.
  • the ohmic electrode may be a single layer metal layer, or may include two or more metal layers. It does not specifically limit as a formation means of an ohmic electrode, For example, well-known means, such as a vacuum evaporation method and sputtering method, etc. are mentioned.
  • the metal that constitutes the ohmic electrode may be an alloy.
  • the ohmic electrode preferably contains Ti or / and Au.
  • FIG. 1 shows a junction barrier Schottky diode (JBS) which is one of the preferred embodiments of the present invention.
  • the semiconductor device of FIG. 1 includes a semiconductor region 3 and a barrier electrode 2 provided on the semiconductor region and capable of forming a Schottky barrier between the semiconductor region, and the barrier electrode 2 and the semiconductor region 3. And a barrier height adjusting layer capable of forming a Schottky barrier having a barrier height larger than the barrier height of the Schottky barrier of the barrier electrode 2 between the semiconductor region 3 and the semiconductor region 3.
  • the barrier height adjustment layer 1 is embedded in the semiconductor region 3.
  • barrier height adjusting layers be provided at regular intervals, and it is more preferable that the barrier height adjusting regions be provided between both ends of the barrier electrode and the semiconductor region.
  • the JBS is configured to be excellent in thermal stability and adhesion, to further reduce the leak current, and further to be excellent in semiconductor characteristics such as withstand voltage.
  • the semiconductor device of FIG. 1 includes the ohmic electrode 4 on the semiconductor region 3.
  • each layer of the semiconductor device of FIG. 1 is not particularly limited as long as the object of the present invention is not hindered, and may be a known means. For example, after forming a film by a vacuum evaporation method, a CVD method, a sputtering method, various coating techniques and the like, a means for patterning by a photolithography method, and a means for direct patterning using a printing technique and the like can be mentioned.
  • FIG. 2A shows a stacked body in which the ohmic electrode 4 is stacked on the semiconductor substrate as the semiconductor region 3 and a plurality of trenches are formed on the opposite surface.
  • the barrier height adjustment layer 1 is formed in the trench of the semiconductor region 3 as shown in FIG. 2B by using the photolithography method for the stacked body of FIG. 2A.
  • the barrier electrode 2 is formed on the barrier height adjusting layer 1 and the semiconductor region 3 by the above-mentioned dry method (preferably vacuum evaporation method or sputtering) or the above-mentioned wet method.
  • the laminated body shown in FIG. 2C has a structure in which the barrier height adjusting layer 1 is embedded in the semiconductor region 3 and thus is particularly excellent in withstand voltage.
  • FIG. 3 shows a junction barrier Schottky diode (JBS) which is one of the preferred embodiments of the present invention.
  • the semiconductor device of FIG. 3 differs from the semiconductor device of FIG. 1 in that a guard ring 5 is provided at the outer peripheral portion of the barrier electrode. With such a configuration, it is possible to obtain a semiconductor device that is further excellent in semiconductor characteristics such as withstand voltage. In the present invention, the breakdown voltage can be more effectively improved by embedding a part of the guard ring 5 on the surface of the semiconductor region 3. Furthermore, by using a metal having a high barrier height for the guard ring, the guard ring can be industrially advantageously provided in combination with the formation of the barrier electrode, without significantly affecting the semiconductor region and without deteriorating the on-resistance. Can be formed.
  • JBS junction barrier Schottky diode
  • a material having a high barrier height is used for the guard ring.
  • the material used for the guard ring include a conductive material having a barrier height of 1 eV or more, and may be the same as the electrode material.
  • the material used for the guard ring has a high degree of freedom in design of the pressure-resistant structure, can provide many guard rings, and can flexibly make the pressure resistance better, so Preferably there.
  • the shape of the guard ring is not particularly limited, and examples thereof include a square shape, a circular shape, a U shape, an L shape, and a strip shape. In the present invention, a square shape or a circular shape is preferable.
  • the number of guard rings is also not particularly limited, but is preferably three or more, and more preferably six or more.
  • FIG. 4A shows a stacked body in which the ohmic electrode 4 is stacked on the semiconductor substrate as the semiconductor region 3 and a plurality of trenches are formed on the opposite surface. Then, after the barrier height adjustment region 1 is formed on the semiconductor region 3 as shown in FIG. 4 (b) by the photolithographic method for the stacked body of FIG. 4 (a), the semiconductor as shown in FIG. 4 (c) The area 3 surface is exposed. In the laminated body of FIGS. 4B and 4C, a barrier height adjusting region 1, a semiconductor region 3 and an ohmic electrode 4 are laminated. After the laminate of FIG.
  • the barrier electrode 2 is formed on the barrier height adjusting layer 1 and the semiconductor region 3 by the above-mentioned dry method (preferably vacuum evaporation or sputtering) or the above-mentioned wet method.
  • a laminate of 4 (d) is obtained.
  • the laminated body shown in FIG. 4D is etched using a photolithography method, and as shown in FIG. 5E, a part of the barrier electrode 2 and a part of the semiconductor region 3 are removed.
  • a guard ring 5 is formed on the semiconductor region 3 exposed on the surface by the dry method (preferably vacuum evaporation or sputtering) or the wet method, etc.
  • the laminate of FIG. 5 (f) is obtained.
  • the guard ring 5, the barrier electrode 2, the barrier height adjusting layer 1, the semiconductor region 3 and the ohmic electrode 4 are laminated.
  • the barrier height adjustment layer 1 is embedded in the semiconductor region 3 and further includes the guard ring 5 of the embedded structure in the peripheral portion of the semiconductor region 3, so that the laminated body of FIG. ing.
  • the guard ring 5 is finally formed, but in the present invention, it is also preferable to form the guard ring 5 before forming the barrier electrode 2, and by forming in this way, the electrode is formed The influence of metal can be suppressed.
  • FIG. 11 shows a junction barrier Schottky diode (JBS) which is one of the preferred embodiments of the present invention.
  • the semiconductor device of FIG. 11 includes a semiconductor region 3 and a barrier electrode 2 provided on the semiconductor region and capable of forming a Schottky barrier between the semiconductor region, and the barrier electrode 2 and the semiconductor region 3.
  • a barrier height adjusting layer capable of forming a Schottky barrier having a barrier height larger than the barrier height of the Schottky barrier of the barrier electrode 2 between the semiconductor region 3 and the semiconductor region 3.
  • the barrier height adjusting layer 1 is embedded in the semiconductor region 3 and protrudes from the semiconductor region 3 into the barrier electrode 2.
  • barrier height adjusting layers be provided at regular intervals, and it is more preferable that the barrier height adjusting regions be provided between both ends of the barrier electrode and the semiconductor region.
  • JBS is more excellent in thermal stability and adhesion, leakage current is further reduced, electric field concentration is further suppressed, and semiconductor characteristics such as reduction in contact resistance are further improved.
  • the semiconductor device of FIG. 11 includes the ohmic electrode 4 on the semiconductor region 3 opposite to the barrier electrode 2 side.
  • each layer of the semiconductor device of FIG. 11 there may be mentioned means for forming each layer described above.
  • FIG. 12A shows a semiconductor substrate as the semiconductor region 3 in which a plurality of trenches are formed on the surface. Then, a gallium-containing p-type oxide semiconductor is formed as a barrier height adjusting layer 1 on the semiconductor substrate of FIG. 12A by mist CVD to obtain a laminate shown in FIG. 12B. The laminate obtained is subjected to etching using a photolithography method to remove unnecessary portions, and the laminate shown in FIG. 12C is obtained. After the laminate of FIG.
  • the barrier electrode 2 is formed on the barrier height adjusting layer 1 and the semiconductor region 3 by the above-mentioned dry method (preferably vacuum evaporation or sputtering) or the above-mentioned wet method.
  • a laminate of 12 (d) is obtained.
  • the barrier height adjusting layer 1 is embedded in the semiconductor region 3 and has a structure projecting into the barrier electrode 2. Therefore, the electric field concentration is suppressed and the contact resistance is reduced.
  • the present invention is useful for a semiconductor device which can be lowered and, in particular, excellent in withstand voltage.
  • FIG. 13 shows a junction barrier Schottky diode (JBS) which is one of the preferred embodiments of the present invention.
  • the semiconductor device of FIG. 13 includes a semiconductor region 3 and a barrier electrode 2 provided on the semiconductor region and capable of forming a Schottky barrier between the semiconductor region, and the barrier electrode 2 and the semiconductor region 3. And a barrier height adjusting layer capable of forming a Schottky barrier having a barrier height larger than the barrier height of the Schottky barrier of the barrier electrode 2 between the semiconductor region 3 and the semiconductor region 3.
  • the barrier height adjustment layer 1 is stacked on the semiconductor region 3 and protrudes into the barrier electrode 2.
  • barrier height adjusting layers be provided at regular intervals, and it is more preferable that the barrier height adjusting regions be provided between both ends of the barrier electrode and the semiconductor region.
  • JBS is more excellent in thermal stability and adhesion, leakage current is further reduced, electric field concentration is further suppressed, and semiconductor characteristics such as reduction in contact resistance are further improved.
  • the semiconductor device of FIG. 13 includes the ohmic electrode 4 on the semiconductor region 3 opposite to the barrier electrode 2 side.
  • each layer of the semiconductor device of FIG. 13 there may be mentioned means for forming each layer described above, and the like.
  • FIG. 12A shows a semiconductor substrate as the semiconductor region 3.
  • a p-type oxide semiconductor containing gallium is formed as a barrier height adjusting layer 1 on the semiconductor substrate of FIG. 14 (a) by mist CVD to obtain a laminate shown in FIG. 14 (b).
  • the laminate obtained is subjected to etching using a photolithographic method to remove an unnecessary part, and the laminate shown in FIG. 14C is obtained.
  • the barrier electrode 2 is formed on the barrier height adjusting layer 1 and the semiconductor region 3 by the above-mentioned dry method (preferably vacuum evaporation or sputtering) or the above-mentioned wet method Obtain a laminate of 14 (d).
  • the barrier height adjusting layer 1 is embedded in the semiconductor region 3 and has a structure projecting into the barrier electrode 2. Therefore, the electric field concentration is suppressed and the contact resistance is reduced.
  • the present invention is useful for a semiconductor device which can be lowered and, in particular, excellent in withstand voltage.
  • FIG. 15 shows a junction barrier Schottky diode (JBS) which is one of the preferred embodiments of the present invention.
  • the semiconductor device of FIG. 15 differs from the semiconductor device of FIG. 11 in that a guard ring 5 is provided at the outer peripheral portion of the barrier electrode. With such a configuration, it is possible to obtain a semiconductor device that is further excellent in semiconductor characteristics such as withstand voltage.
  • the breakdown voltage can be more effectively improved by embedding a part of the guard ring 5 on the surface of the semiconductor region 3.
  • the guard ring can be industrially advantageously provided in combination with the formation of the barrier electrode, without significantly affecting the semiconductor region and without deteriorating the on-resistance. Can be formed.
  • FIG. 16 shows a junction barrier Schottky diode (JBS) which is one of the preferred embodiments of the present invention.
  • the semiconductor device of FIG. 16 differs from the semiconductor device of FIG. 13 in that a guard ring 5 is provided at the outer peripheral portion of the barrier electrode. With such a configuration, it is possible to obtain a semiconductor device that is further excellent in semiconductor characteristics such as withstand voltage.
  • the breakdown voltage can be more effectively improved by embedding a part of the guard ring 5 on the surface of the semiconductor region 3.
  • the guard ring can be industrially advantageously provided in combination with the formation of the barrier electrode, without significantly affecting the semiconductor region and without deteriorating the on-resistance. Can be formed.
  • the semiconductor device is particularly useful for power devices.
  • Examples of the semiconductor device include, for example, a diode or a transistor (for example, MESFET or the like). Among them, a diode is preferable, and a junction barrier Schottky diode (JBS) is more preferable.
  • JBS junction barrier Schottky diode
  • the semiconductor device according to the present invention is suitably used as a power module, an inverter or a converter by further using known means, in addition to the above-mentioned matters, and further suitably used for a semiconductor system using a power supply device, for example. .
  • the power supply device can be manufactured from the semiconductor device or as the semiconductor device by connecting to a wiring pattern or the like using a known means.
  • An example of a power supply system is shown in FIG.
  • a power supply system is configured using a plurality of the power supply devices and a control circuit.
  • the power supply system can be used in a system device in combination with an electronic circuit as shown in FIG.
  • An example of a power supply circuit diagram of the power supply device is shown in FIG. FIG.
  • FIG. 8 shows a power supply circuit of a power supply device including a power circuit and a control circuit.
  • the mist CVD apparatus 19 used in the reference example will be described with reference to FIG.
  • the mist CVD apparatus 19 comprises a susceptor 21 for mounting the substrate 20, a carrier gas supply means 22a for supplying a carrier gas, and a flow rate control valve 23a for adjusting the flow rate of the carrier gas delivered from the carrier gas supply means 22a.
  • the susceptor 21 is made of quartz, and the surface on which the substrate 20 is placed is inclined from the horizontal surface.
  • the ultrasonic transducer 26 was vibrated at 2.4 MHz, and the vibration was propagated to the raw material solution 24 a through the water 25 a to atomize the raw material solution 24 a to generate mist.
  • the mist was introduced into the film forming chamber 27 by the carrier gas, and the mist reacted in the film forming chamber 27 at 510 ° C. under atmospheric pressure, whereby a semiconductor film was formed on the substrate 20.
  • the film thickness was 2.5 ⁇ m, and the film formation time was 180 minutes.
  • n + -type Semiconductor Layer 1.5% by volume ratio of hydrochloric acid and 0.2% of tin chloride are contained in a 0.05 M aqueous solution of gallium acetylacetonate, respectively, and the solution is used as a raw material solution except that it is used as a raw material solution.
  • a semiconductor film was formed on the n ⁇ -type semiconductor layer obtained in the above. The film obtained was subjected to film phase identification using an XRD diffractometer, and the obtained film was ⁇ -Ga 2 O 3 .
  • Ohmic Electrode Formation of Ohmic Electrode A Ti layer and an Au layer were respectively deposited by electron beam evaporation on the n + -type semiconductor layer. The thickness of the Ti layer was 35 nm, and the thickness of the Au layer was 175 nm.
  • a Pt layer was laminated on the n ⁇ -type semiconductor layer by electron beam evaporation. Then, annealing was performed at 400 ° C. for 30 seconds in a nitrogen atmosphere using a high-speed annealing apparatus (RTA) to form an annealed Pt layer. Further, a Pt layer which was subjected to photolithography and etching and was not annealed was also formed.
  • RTA high-speed annealing apparatus
  • Reference example 2 Adjustment of barrier height by p type semiconductor
  • Reference Example 2 the adjustment of the barrier height by the p-type semiconductor was evaluated.
  • 2-1 Formation of p-type semiconductor layer
  • a sapphire substrate having an n + -type semiconductor layer formed using mist CVD on the surface was used, and gallium bromide and magnesium bromide were mixed in ultrapure water as a raw material solution.
  • the aqueous solution is adjusted so that the atomic ratio of magnesium to gallium is 1: 0.01 and 0.1 mol / L of gallium bromide, and in this case, the one containing 20% by volume of hydrohalic acid What was used, except that the flow rate of the carrier gas was 1 L / min, the flow rate of the carrier gas (dilution) was 1 L / min, the deposition temperature was 520 ° C., and the deposition time was 60 minutes Above, 1-1.
  • a semiconductor film was formed in the same manner as in the above. The resulting per film, using an XRD diffractometer, was subjected to identification of the membrane phase, a film obtained using hydrobromic acid as hydrohalic acid was ⁇ -Ga 2 0 3.
  • the semiconductor device of the present invention can be used in all fields such as semiconductors (for example, compound semiconductor electronic devices etc.), electronic parts / electrical equipment parts, optical / electrophotographic related devices, industrial parts, etc., and is particularly useful for power devices is there.
  • mist CVD apparatus 20 substrate 21 susceptor 22a carrier gas supply means 22b carrier gas (dilution) supply means 23a flow control valve 23b flow control valve 24 mist generation source 24a Raw material solution 25 Container 25a Water 26 Ultrasonic transducer 27 Supply tube 28 Heater 29 Exhaust port

Landscapes

  • Electrodes Of Semiconductors (AREA)
  • Chemical & Material Sciences (AREA)
  • Crystallography & Structural Chemistry (AREA)
  • Liquid Deposition Of Substances Of Which Semiconductor Devices Are Composed (AREA)
  • Bipolar Transistors (AREA)
  • Noodles (AREA)
  • Mechanical Treatment Of Semiconductor (AREA)
PCT/JP2018/025767 2017-07-08 2018-07-06 半導体装置 Ceased WO2019013136A1 (ja)

Priority Applications (9)

Application Number Priority Date Filing Date Title
KR1020237010290A KR20230044336A (ko) 2017-07-08 2018-07-06 반도체 장치
KR1020207000628A KR20200020785A (ko) 2017-07-08 2018-07-06 반도체 장치
SG11202000144YA SG11202000144YA (en) 2017-07-08 2018-07-06 Semiconductor device
JP2019529115A JP7313609B2 (ja) 2017-07-08 2018-07-06 半導体装置
KR1020257007346A KR102999308B1 (ko) 2017-07-08 2018-07-06 반도체 장치
EP18831783.8A EP3654387A4 (en) 2017-07-08 2018-07-06 SEMICONDUCTOR COMPONENT
US16/628,341 US11450774B2 (en) 2017-07-08 2018-07-06 Semiconductor device including two or more adjustment regions
CN201880045648.7A CN110870079B (zh) 2017-07-08 2018-07-06 半导体装置
JP2023050423A JP7595966B2 (ja) 2017-07-08 2023-03-27 半導体装置

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2017-134243 2017-07-08
JP2017134243 2017-07-08

Publications (1)

Publication Number Publication Date
WO2019013136A1 true WO2019013136A1 (ja) 2019-01-17

Family

ID=65002661

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2018/025767 Ceased WO2019013136A1 (ja) 2017-07-08 2018-07-06 半導体装置

Country Status (8)

Country Link
US (1) US11450774B2 (enExample)
EP (1) EP3654387A4 (enExample)
JP (2) JP7313609B2 (enExample)
KR (3) KR20230044336A (enExample)
CN (1) CN110870079B (enExample)
SG (1) SG11202000144YA (enExample)
TW (1) TWI783003B (enExample)
WO (1) WO2019013136A1 (enExample)

Cited By (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2020204006A1 (ja) * 2019-03-29 2020-10-08 株式会社Flosfia 結晶、結晶性酸化物半導体、結晶性酸化物半導体を含む半導体膜、結晶および/または半導体膜を含む半導体装置および半導体装置を含むシステム
EP3823045A1 (en) 2019-11-14 2021-05-19 Flosfia Inc. Semiconductor device and system including semiconductor
EP3823043A4 (en) * 2018-07-12 2022-04-13 Flosfia Inc. SEMICONDUCTOR DEVICE
WO2022075218A1 (ja) * 2020-10-07 2022-04-14 株式会社タムラ製作所 ショットキーダイオード
EP3823044A4 (en) * 2018-07-12 2022-04-20 Flosfia Inc. SEMICONDUCTOR DEVICE
EP3823041A4 (en) * 2018-07-12 2022-04-20 Flosfia Inc. SEMICONDUCTOR DEVICE

Families Citing this family (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP7279587B2 (ja) * 2018-09-25 2023-05-23 豊田合成株式会社 半導体装置の製造方法
JP7391297B2 (ja) * 2019-06-28 2023-12-05 株式会社Flosfia エッチング処理方法およびエッチング処理装置
KR20220134639A (ko) * 2020-02-07 2022-10-05 가부시키가이샤 플로스피아 반도체 소자 및 반도체 장치
CN113066870B (zh) * 2021-03-25 2022-05-24 电子科技大学 一种具有终端结构的氧化镓基结势垒肖特基二极管

Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS52101970A (en) 1976-02-20 1977-08-26 Sumitomo Electric Ind Ltd Semiconductor element having schottoky barriercontact
JP2013522876A (ja) * 2010-03-08 2013-06-13 クリー インコーポレイテッド ヘテロ接合障壁領域を含む半導体デバイス及びその製造方法
JP2014078660A (ja) 2012-10-12 2014-05-01 Sumitomo Electric Ind Ltd ワイドギャップ半導体装置およびその製造方法
JP2014107408A (ja) 2012-11-28 2014-06-09 Sanken Electric Co Ltd 半導体装置
WO2017111173A1 (ja) * 2015-12-25 2017-06-29 出光興産株式会社 積層体
JP2017118090A (ja) * 2015-12-21 2017-06-29 株式会社Flosfia 積層構造体および半導体装置

Family Cites Families (24)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH0642541B2 (ja) 1988-04-22 1994-06-01 サンケン電気株式会社 ショットキバリア半導体装置
JPH05326925A (ja) * 1992-05-14 1993-12-10 Shindengen Electric Mfg Co Ltd ショットキバリア半導体装置
JPH1084120A (ja) * 1996-09-09 1998-03-31 Toshiba Corp 半導体装置
JP2006318956A (ja) 2005-05-10 2006-11-24 Sumitomo Electric Ind Ltd ショットキーダイオードを有する半導体装置
JP2006352028A (ja) * 2005-06-20 2006-12-28 Sumitomo Electric Ind Ltd 整流素子およびその製造方法
JP2008172035A (ja) 2007-01-12 2008-07-24 Univ Of Fukui ショットキーダイオード
JP5414019B2 (ja) * 2008-04-01 2014-02-12 独立行政法人産業技術総合研究所 バリアハイト制御をしたダイヤモンド電子デバイス
JP5382763B2 (ja) * 2008-04-09 2014-01-08 独立行政法人産業技術総合研究所 半導体素子及びその製造方法と、該半導体素子を備えた電子デバイス
JP2010225914A (ja) 2009-03-24 2010-10-07 Sanyo Electric Co Ltd ショットキーバリアダイオード
US8816468B2 (en) 2010-10-21 2014-08-26 Vishay General Semiconductor Llc Schottky rectifier
JP2012175090A (ja) * 2011-02-24 2012-09-10 Panasonic Corp ショットキーバリア型半導体装置
JP5306392B2 (ja) * 2011-03-03 2013-10-02 株式会社東芝 半導体整流装置
US20140217470A1 (en) * 2011-09-08 2014-08-07 Tamura Corporation Ga2O3 SEMICONDUCTOR ELEMENT
US9455326B2 (en) * 2012-02-15 2016-09-27 Fuji Electric Co., Ltd. Wide bandgap semiconductor device
JP6053103B2 (ja) * 2012-04-12 2016-12-27 富士電機株式会社 ワイドバンドギャップ半導体装置およびその製造方法
JP2014053393A (ja) 2012-09-06 2014-03-20 Sumitomo Electric Ind Ltd ワイドギャップ半導体装置およびその製造方法
JP6284140B2 (ja) * 2013-06-17 2018-02-28 株式会社タムラ製作所 Ga2O3系半導体素子
US9691910B2 (en) * 2013-08-19 2017-06-27 Idemitsu Kosan Co., Ltd. Oxide semiconductor substrate and schottky barrier diode
JP6242724B2 (ja) * 2014-03-20 2017-12-06 株式会社東芝 半導体装置およびその製造方法
KR102125822B1 (ko) * 2014-07-22 2020-06-23 가부시키가이샤 플로스피아 결정성 반도체막 및 판상체 및 반도체장치
JP6411258B2 (ja) 2015-03-19 2018-10-24 新電元工業株式会社 半導体装置
WO2016198388A1 (en) 2015-06-09 2016-12-15 Abb Schweiz Ag Method for manufacturing an edge termination for a silicon carbide power semiconductor device
JP6767705B2 (ja) * 2016-04-28 2020-10-14 パナソニックIpマネジメント株式会社 半導体素子
JP6967238B2 (ja) 2017-02-28 2021-11-17 株式会社タムラ製作所 ショットキーバリアダイオード

Patent Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS52101970A (en) 1976-02-20 1977-08-26 Sumitomo Electric Ind Ltd Semiconductor element having schottoky barriercontact
JP2013522876A (ja) * 2010-03-08 2013-06-13 クリー インコーポレイテッド ヘテロ接合障壁領域を含む半導体デバイス及びその製造方法
JP2014078660A (ja) 2012-10-12 2014-05-01 Sumitomo Electric Ind Ltd ワイドギャップ半導体装置およびその製造方法
JP2014107408A (ja) 2012-11-28 2014-06-09 Sanken Electric Co Ltd 半導体装置
JP2017118090A (ja) * 2015-12-21 2017-06-29 株式会社Flosfia 積層構造体および半導体装置
WO2017111173A1 (ja) * 2015-12-25 2017-06-29 出光興産株式会社 積層体

Cited By (15)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP3823041A4 (en) * 2018-07-12 2022-04-20 Flosfia Inc. SEMICONDUCTOR DEVICE
EP3823043A4 (en) * 2018-07-12 2022-04-13 Flosfia Inc. SEMICONDUCTOR DEVICE
US12148804B2 (en) 2018-07-12 2024-11-19 Flosfia Inc. Semiconductor device including one or more p-type semiconductors provided between an n-type semiconductor layer and an electrode
US11495695B2 (en) 2018-07-12 2022-11-08 Flosfia Inc. Semiconductor device
EP3823044A4 (en) * 2018-07-12 2022-04-20 Flosfia Inc. SEMICONDUCTOR DEVICE
JPWO2020204006A1 (enExample) * 2019-03-29 2020-10-08
JP7624136B2 (ja) 2019-03-29 2025-01-30 株式会社Flosfia 結晶、結晶性酸化物半導体、結晶性酸化物半導体を含む半導体膜、結晶および/または半導体膜を含む半導体装置および半導体装置を含むシステム
WO2020204006A1 (ja) * 2019-03-29 2020-10-08 株式会社Flosfia 結晶、結晶性酸化物半導体、結晶性酸化物半導体を含む半導体膜、結晶および/または半導体膜を含む半導体装置および半導体装置を含むシステム
US11088242B2 (en) 2019-03-29 2021-08-10 Flosfia Inc. Crystal, crystalline oxide semiconductor, semiconductor film containing crystalline oxide semiconductor, semiconductor device including crystal and/or semiconductor film and system including semiconductor device
JP2021082812A (ja) * 2019-11-14 2021-05-27 株式会社Flosfia 半導体装置
EP3823045A1 (en) 2019-11-14 2021-05-19 Flosfia Inc. Semiconductor device and system including semiconductor
JP7690157B2 (ja) 2019-11-14 2025-06-10 株式会社Flosfia 半導体装置
JP2022061884A (ja) * 2020-10-07 2022-04-19 株式会社タムラ製作所 ショットキーダイオード
WO2022075218A1 (ja) * 2020-10-07 2022-04-14 株式会社タムラ製作所 ショットキーダイオード
JP7599644B2 (ja) 2020-10-07 2024-12-16 株式会社タムラ製作所 ショットキーダイオード

Also Published As

Publication number Publication date
US20200152805A1 (en) 2020-05-14
JPWO2019013136A1 (ja) 2020-06-18
EP3654387A1 (en) 2020-05-20
TWI783003B (zh) 2022-11-11
CN110870079A (zh) 2020-03-06
KR20250035048A (ko) 2025-03-11
EP3654387A4 (en) 2021-03-31
KR102999308B1 (ko) 2026-07-31
JP7313609B2 (ja) 2023-07-25
KR20230044336A (ko) 2023-04-03
TW201907572A (zh) 2019-02-16
CN110870079B (zh) 2024-01-09
KR20200020785A (ko) 2020-02-26
US11450774B2 (en) 2022-09-20
JP7595966B2 (ja) 2024-12-09
JP2023068204A (ja) 2023-05-16
SG11202000144YA (en) 2020-02-27

Similar Documents

Publication Publication Date Title
JP7595966B2 (ja) 半導体装置
TWI830750B (zh) 半導體裝置及半導體系統
JP7751786B2 (ja) 半導体装置
JP2018129500A (ja) 半導体装置
JP2018060992A (ja) 半導体装置
JP6999106B2 (ja) 半導体装置
JP7612144B2 (ja) 半導体装置
JP6999103B2 (ja) 半導体装置
JP6999105B2 (ja) 半導体装置の製造方法
JP7733285B2 (ja) 半導体装置
JP6999104B2 (ja) 半導体装置
JP2018032699A (ja) 半導体装置
HK40023886A (en) Semiconductor device
HK40023886B (en) Semiconductor device
CN114207831A (zh) 半导体装置

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 18831783

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2019529115

Country of ref document: JP

Kind code of ref document: A

ENP Entry into the national phase

Ref document number: 20207000628

Country of ref document: KR

Kind code of ref document: A

NENP Non-entry into the national phase

Ref country code: DE

ENP Entry into the national phase

Ref document number: 2018831783

Country of ref document: EP

Effective date: 20200210

WWD Wipo information: divisional of initial pct application

Ref document number: 1020257007346

Country of ref document: KR

WWP Wipo information: published in national office

Ref document number: 1020257007346

Country of ref document: KR