WO2000032847A2 - Aluminiumorganische elektrolyte und verfahren zur elektrolytischen beschichtung mit aluminium oder aluminium-magnesium-legierungen - Google Patents

Aluminiumorganische elektrolyte und verfahren zur elektrolytischen beschichtung mit aluminium oder aluminium-magnesium-legierungen Download PDF

Info

Publication number
WO2000032847A2
WO2000032847A2 PCT/EP1999/009236 EP9909236W WO0032847A2 WO 2000032847 A2 WO2000032847 A2 WO 2000032847A2 EP 9909236 W EP9909236 W EP 9909236W WO 0032847 A2 WO0032847 A2 WO 0032847A2
Authority
WO
WIPO (PCT)
Prior art keywords
aiet
magnesium
aluminum
electrolyte
toluene
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/EP1999/009236
Other languages
German (de)
English (en)
French (fr)
Other versions
WO2000032847A3 (de
Inventor
Herbert Lehmkuhl
Klaus-Dieter Mehler
Bertram Reinhold
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Studiengesellschaft Kohle gGmbH
Original Assignee
Studiengesellschaft Kohle gGmbH
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Studiengesellschaft Kohle gGmbH filed Critical Studiengesellschaft Kohle gGmbH
Priority to DE59901980T priority Critical patent/DE59901980D1/de
Priority to US09/857,013 priority patent/US6652730B1/en
Priority to CA002352800A priority patent/CA2352800A1/en
Priority to EP99962174A priority patent/EP1141447B1/de
Priority to JP2000585475A priority patent/JP2002531698A/ja
Priority to AT99962174T priority patent/ATE220129T1/de
Publication of WO2000032847A2 publication Critical patent/WO2000032847A2/de
Publication of WO2000032847A3 publication Critical patent/WO2000032847A3/de
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C25—ELECTROLYTIC OR ELECTROPHORETIC PROCESSES; APPARATUS THEREFOR
    • C25D—PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR
    • C25D3/00—Electroplating: Baths therefor
    • C25D3/02—Electroplating: Baths therefor from solutions
    • C25D3/42—Electroplating: Baths therefor from solutions of light metals
    • C25D3/44—Aluminium

Definitions

  • the invention relates to organoaluminum electrolytes which are suitable for the electrolytic deposition of aluminum or aluminum-magnesium alloys on electrically conductive materials, and to a process for this purpose using soluble aluminum anodes or soluble aluminum and magnesium anodes or an anode made of aluminum-magnesium alloy .
  • Organometallic complex compounds have been used for a long time for the electrolytic deposition of aluminum (dissertation H. Lehmkuhl, TH Aachen 1954, DE-PS 1047450; K. Ziegler, H. Lehmkuhl, Z. inorganic chemistry 283 (1956) 414; DE- PS 1056377; H. Lehmkuhl, Chem. Ing. Tech. 36 (1964) 616; EP-A 0084816; H. Lehmkuhl, K. Mehler and U. Landau in Adv. In electrochemical science and engineering (Ed. H. Gerischer , CW Tobias) Vol. 3, Weinheim 1994).
  • MX can be either alkali metal (Na, K, Rb, Cs) or onium halides, preferably their fluorides.
  • R are alkyl radicals with preferably one, two or four carbon atoms.
  • the conductivity of the electrolyte was of the order of 1 * 10 to 7 • 10 '3 S • cm "1.
  • the same authors described an electrolyte solution consisting of ethyl magnesium bromide and triethyl aluminum in THF / toluene 1: 1 the metal layers with a maximum of 10% Al were obtained.
  • magnesium anodes cannot be dissolved with the proposed electrolytes during the coating process. Continuous addition of the Mg content is not possible by dissolving the magnesium anode when using fluoride or generally halide-containing organoaluminum complexes as electrolytes.
  • dialkyl magnesium is used in ethereal solution to prepare the electrolyte. In a continuously operating coating process, the dialkyl magnesium would have to be supplied continuously in ethereal solution.
  • diethyl ether that some complexes e.g. B. Na [Et 3 AI-F-AIEt 3 ] can be split into Na [Et 3 AIF] + Et g Al - OEt 2 (K. Ziegler, R. Köster, H. Lehmkuhl, K. Reinert, Liebigs Ann. Chem 629, 33-49 (1960)).
  • dialkyl magnesium would first have to be made ether-free, which requires considerable effort and expense, or it would have to be prepared in ether-free form by reacting magnesium metal with dialkyl mercury, a very toxic compound.
  • An electrolyte of type I according to the invention is dissolved in 2.5-6 mol per mol of complex compound of an aromatic hydrocarbon which is liquid at 20 ° C., preferably in toluene or a liquid xylene.
  • the trialkyl aluminum is preferably triethyl aluminum (AIEt 3 ), alkali tetraalkyl aluminum is preferably a mixture of potassium and sodium tetraethyl aluminum.
  • the quantitative ratio of complex: AIEt 3 is 1: 0.5 to 1: 3, preferably 1: 2.
  • the proportion of Na [AIEt 4 ] is between 0 and 25 mol%, based on the total amount of K [AIEt 4 ] and NafAIEtJ, but is preferred between 5 and 20 mol%.
  • the addition of small amounts of Na [AIEt 4 ] is preferred because, in the absence of this component, the aluminum anodes can only be dissolved with moderate to poor current yields, e.g. 3 AlEt 3 were as in K [AlEt 4] / / what if prolonged electrolysis lead 6 toluene only at about 22% to a loss of triethylaluminum.
  • the electrolysis is carried out at temperatures between 80 and 105 ° C., preferably between 90 and 100 ° C.
  • An exemplary electrolyte I is: 0.8 mol K [AIEt 4 ] / 0.2 mol Na [AIEt 4 ] / 2.0 mol AIEt 3 / 3.3 mol toluene. No crystallization takes place from this electrolyte solution even when standing at room temperature for a long time; the specific conductivity at 95 ° C. is 13.8 mS-cm "1 .
  • Type II electrolytes preferably consist of mixtures of Na [Et 3 Al-H-AIEt 3 ], Na [AIEt 4 ] and AIEt 3 .
  • AIEt 3 ensures that Na [AIEt 4 ] no sodium metal (W. Grimme, dissertation TH Aachen (1960); DBP 11 14330 (1959); DBP 1 146258 (1961)), but aluminum metal is electrolytically deposited.
  • Na [Et 3 AI-H-AIEt 3 ] are very suitable as solutions in toluene for the electrolytic deposition and dissolution of aluminum at 90-105 ° C. In the electrolysis of this compound and in the absence of Na [AIEt 4 ] according to the invention, we have found that magnesium anodes are not dissolved.
  • the electrolyte II according to the invention is dissolved in 5-7 mol per mol Na [AlEt 4 ] of an aromatic hydrocarbon liquid at 20 ° C., preferably in toluene or a liquid xylene.
  • the quantitative ratio Na [Et 3 Al-H-AIEt 3 ] to Na [AIEt 4 ] is preferably 2: 1 to ensure homogeneous solubility in 6 mol toluene per mol Na [AIEt 4 ] and the molar ratio Na [AIEt 4 ] to AIEt 3 is preferably 1: 2 to ensure proper metal deposition by electrolysis.
  • An exemplary electrolyte is II: 1 mol of Na [Et 3 Al-H-AlEt 3] / 0.5 mol of Na [AlEt 4] / 1 mol of AlEt 3/3 mol of toluene. Even when standing at room temperature for a long time, this electrolyte solution does not crystallize, which would interfere with the technical usability of the electrolyte.
  • the specific conductivity at 95 ° C is 8.12 mS • cm " .
  • the electrolytic deposition of aluminum-magnesium alloy layers from the electrolytes according to the invention is carried out using a soluble aluminum and a likewise soluble magnesium anode or using an anode made of aluminum-magnesium alloy. In the case of two anodes, these are switched separately to ensure a continuous procedure and to control a selectable and desired alloy composition.
  • the electrolysis is expediently carried out in toluene solution at 90-100 ° C.
  • the anodic (AI 95-100%; Mg 93-100%) and cathodic current yields are practically quantitative. Since a finite and therefore necessary concentration of magnesium only builds up in the course of an electrolysis, this state must first be established before using a freshly prepared electrolyte. This can be done 1 .
  • the electrolytic deposition from the electrolytes according to the invention leads to aluminum-magnesium alloy layers which differ significantly in their electrochemical properties from previously known layer systems.
  • the electrochemical behavior of the alloy layers corresponds to the magnesium type in the cathodic partial reaction, to the aluminum type in the anodic partial reaction, combined with a pronounced passivity interval.
  • the alloy layers have a quiescent current potential of about -1380 to -1500 mV at room temperature in a 5% aqueous NaCl solution with a pH of 9.0. SCE at Mg incorporation rates of 5 to 50% by weight. Due to the layer passivity (formation of intermetallic phases), the cathodic partial reaction in contact with more electronegative metals, such as magnesium, is additionally inhibited. The potential of the cathodic partial reaction is thereby shifted from the resting potential to even more negative potential values. The result of this is that the remaining potential difference between the cathodic partial reaction of the alloy layer (at pH 9 oxygen reduction) and the anodic partial reaction of the magnesium is greatly reduced.
  • the AlMg alloy layers therefore enable extensive adaptation to the quiescent current potential of the magnesium alloy AZ91 hp, which is approx. SCE is due to contact corrosion on magnesium is greatly reduced.
  • the alloy layers are therefore suitable for coating steel fasteners in contact with magnesite ⁇ .
  • the application potential here particularly concerns applications in the automotive industry in the transmission, engine and body area.
  • the developed alloy layers which are deposited from non-aqueous electrolytes, are also suitable as a high-quality surface coating for highly tempered steel parts with a tensile strength of> 1000 MPa and which cannot be coated with conventional galvanic processes - due to the risk of hydrogen embrittlement. This results in a potential field of application for the coating of tempered and spring steels with alkali-resistant and aluminum or magnesium-compatible coatings.
  • Example 17 an Rb [Al (Et) 4 ] electrolyte was used.
  • the cathode layer was uniform, shiny silver and contained 72.4% Al and 27.6% Mg, the cathodic layer weighed 34.3 mg and was approx. 12 ⁇ m thick.
  • the amount of toluene can gradually decrease due to evaporation, if it drops below 5 moles of toluene per mole of M [AIEt 4 ], the solution becomes inhomogeneous and a little AIEt 3 separates Form of oily droplets. In this case the amount of toluene must be increased to 6 mol toluene per mol M [AIEt 4 ].
  • Example 3 The electrolyte of Example 3 was electrolyzed again at 90-95 ° C after replacing the cathode with a new copper sheet.
  • the electrolyte of Examples 3 and 4 was electrolyzed four times in succession using only one magnesium anode.
  • the nature of the cathode layer and the Al and Mg content of the electrolyte are shown in Table 1. Table 1
  • An electrolyte with the composition K [AIEt 4 ] / AIEt 3/4 toluene with a specific conductivity of 17.3 mS • cm was between an anode consisting of aluminum sheet and magnesium sheet and a cathode made of TiAI 6 V 4 at 90- 95 ° C electrolyzed.
  • An electrolyte with the composition 0.8 mol K [AIEt 4 ] /0.2 mol Na [AIEt 4 ] / 2.0 AIEt 3 /3.3 mol toluene was between 2 anodes made of an aluminum-magnesium alloy with 25 wt .-% Mg and 75 wt .-% % AI and a rotating cylindrical screw M8 made of tempered steel (8.8) at 97-102 ° C with -2 cathodic current density of 0.8 A • dm and a current of 2.89 mF electrolyzed. Cathodic and anodic current yields were mif'99.5% quantitative. The approx. 9 ⁇ m thick alloy layer was uniform, shiny silver and adhered well to the base material.
  • Example 7 was repeated ten times after each time the cathodes were replaced by an uncoated screw at 98-100 ° C.
  • the respective thicknesses of the cathode layer were varied from 9 to 13 ⁇ m.
  • the anodic current yield over the ten tests was 99.5%.
  • Example 10 The electrolyte obtained in the course of Example 10 was electrolyzed at 93-98 ° C. between the Al and Mg anode and a slowly rotating cylindrical cathode made from tempered steel (8.8).
  • the anodic current density was on everyone
  • Example 11 The electrolyte of Example 11 was electrolyzed after replacing the cathode with a new one, also made from tempering steel, at 95-104 ° C.
  • the electrolyte of Example 11 was electrolyzed after replacing the cathode with a new one, also made from tempering steel, at 95-104 ° C.
  • anodic current densities were set to 0.45 A • dm for aluminum and 0.15 A • dm for magnesium.
  • the anodic current yields were 90%, the cathode layer was uniform and shiny silver; According to the analysis, the layer contained 71.8% Al and 28.2% Mg, the layer thickness was 13 ⁇ m.
  • Example 12 The electrolyte of Example 12 was electrolyzed after replacing the anodes made of Al and Mg with two alloy anodes of the composition 75% by weight Al and 25% by weight Mg and after using a new cylindrical cathode made of tempering steel 8.8 at 93 ° C. During the electrolysis, the cathode rotated slowly between the two anodes, the cathodic current density was
  • the cathode layer was 12 ⁇ m thick and was uniform and matt silver.
  • Example 13 was repeated three times after replacing the cathode with an uncoated one at 92-100 ° C.
  • the respective layer thicknesses were varied between 10 and 15 ⁇ m.
  • the anodic current yield over the 4 tests for the alloy anodes was 98.9%.
  • Example 15 Al deposition from Na [Et 3 Al-H-AIEt 3 ]
  • Example 16 Al deposition from K [Et 3 AIH-AIEt 3 ]
  • a test electrolysis was carried out at -2 -2 dm to 1.0 A dm. After passing through 7.73 mF, there was a uniform, silver-gray cathode layer. The current efficiency at the cathode was 100.0% and that at the anode was 99.6%.
  • the specific conductivity at 95 ° C is 12.9mS cm "1 .
  • the anodic current yield was 100% over 6 tests.
  • the initial composition of the layer with a fresh electrolyte was 90.96% Al and 9.04% Mg.
  • the system conditioned itself to a layer composition of 75.02% Al and 24.98% Mg.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Electrochemistry (AREA)
  • Materials Engineering (AREA)
  • Metallurgy (AREA)
  • Organic Chemistry (AREA)
  • Electrolytic Production Of Metals (AREA)
  • Electroplating Methods And Accessories (AREA)
  • Electroplating And Plating Baths Therefor (AREA)
PCT/EP1999/009236 1998-12-01 1999-11-27 Aluminiumorganische elektrolyte und verfahren zur elektrolytischen beschichtung mit aluminium oder aluminium-magnesium-legierungen Ceased WO2000032847A2 (de)

Priority Applications (6)

Application Number Priority Date Filing Date Title
DE59901980T DE59901980D1 (de) 1998-12-01 1999-11-27 Aluminiumorganische elektrolyte und verfahren zur elektrolytischen beschichtung mit aluminium oder aluminium-magnesium-legierungen
US09/857,013 US6652730B1 (en) 1998-12-01 1999-11-27 Aluminum organic electrolytes and method for electrolytic coating with aluminum or aluminum-magnesium-alloys
CA002352800A CA2352800A1 (en) 1998-12-01 1999-11-27 Aluminium organic electrolytes and method for electrolytic coating with aluminium or aluminium-magnesium-alloys
EP99962174A EP1141447B1 (de) 1998-12-01 1999-11-27 Aluminiumorganische elektrolyte und verfahren zur elektrolytischen beschichtung mit aluminium oder aluminium-magnesium-legierungen
JP2000585475A JP2002531698A (ja) 1998-12-01 1999-11-27 アルミニウム有機電解質、及びアルミニウム又はアルミニウム−マグネシウム合金を電気被覆する方法
AT99962174T ATE220129T1 (de) 1998-12-01 1999-11-27 Aluminiumorganische elektrolyte und verfahren zur elektrolytischen beschichtung mit aluminium oder aluminium-magnesium-legierungen

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
DE19855666A DE19855666A1 (de) 1998-12-01 1998-12-01 Aluminiumorganische Elektrolyte und Verfahren zur elektrolytischen Beschichtung mit Aluminium oder Aluminium-Magnesium Legierungen
DE19855666.7 1998-12-01

Publications (2)

Publication Number Publication Date
WO2000032847A2 true WO2000032847A2 (de) 2000-06-08
WO2000032847A3 WO2000032847A3 (de) 2000-11-16

Family

ID=7889774

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/EP1999/009236 Ceased WO2000032847A2 (de) 1998-12-01 1999-11-27 Aluminiumorganische elektrolyte und verfahren zur elektrolytischen beschichtung mit aluminium oder aluminium-magnesium-legierungen

Country Status (7)

Country Link
US (1) US6652730B1 (enExample)
EP (1) EP1141447B1 (enExample)
JP (1) JP2002531698A (enExample)
AT (1) ATE220129T1 (enExample)
CA (1) CA2352800A1 (enExample)
DE (2) DE19855666A1 (enExample)
WO (1) WO2000032847A2 (enExample)

Cited By (7)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2003102276A1 (de) * 2002-05-31 2003-12-11 Aluminal Oberflächentechnik Gmbh & Co. Kg Verfahren zur herstellung von aluminiumorganischen komplexen und deren verwendung zur herstellung von elektrolytlösungen zur elektrochemischen abscheidung von aluminium-magnesium-legierungen
WO2004099218A1 (en) * 2003-04-30 2004-11-18 Akzo Nobel N.V. Production of mixed sodium and potassium tetraalkylaluminate solutions
WO2004053203A3 (de) * 2002-12-10 2004-12-23 Thyssenkrupp Stahl Ag Verfahren zur elektrolytischen abscheidung von magnesium oder magnesium-zink auf verzinktem blech
EP1518945A1 (de) * 2003-09-27 2005-03-30 Aluminal Oberflächtentechnik GmbH & Co. KG Elektrolyt für die galvanische Abscheidung von Aluminium-Magnesium-Legierungen
EP1524336A1 (de) * 2003-10-18 2005-04-20 Aluminal Oberflächtentechnik GmbH & Co. KG Mit einer Aluminium-/Magnesium-Legierung beschichtete Werkstücke
EP1624091A1 (de) * 2004-08-04 2006-02-08 Aluminal Oberflächentechnik GmbH & Co. KG Mit einer Aluminium/Magnesium-Legierung oder Aluminium beschichtete Werkstücke mit Zink-Zwischenschicht
RU2407090C1 (ru) * 2009-12-03 2010-12-20 Учреждение Российской академии наук Институт химии и технологии редких элементов и минерального сырья им. И.В. Тананаева Кольского научного центра РАН (ИХТРЭМС КНЦ РАН) СПОСОБ ПОЛУЧЕНИЯ ТВЕРДОГО ИОННОГО ЭЛЕКТРОЛИТА RbAg4I5

Families Citing this family (10)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2002088434A1 (en) * 2001-04-30 2002-11-07 Alumiplate Incorporated Aluminium electroplating formulations
US7250102B2 (en) 2002-04-30 2007-07-31 Alumiplate Incorporated Aluminium electroplating formulations
DE10134559B4 (de) * 2001-07-16 2008-10-30 Fraunhofer-Gesellschaft zur Förderung der angewandten Forschung e.V. Verfahren zur Beschichtung von Bauteilen, mit dem Verfahren herstellbare Dispersionsschichten und Verwendung
DE10226360A1 (de) 2002-06-13 2003-12-24 Crompton Gmbh Verfahren zur Herstellung von Alkalitetraalkylaluminaten und deren Verwendung
EP1403402A1 (de) * 2002-09-25 2004-03-31 Aluminal Oberflächtentechnik GmbH & Co. KG Verfahren zur elektrolytischen Beschichtung von Werkstoffen mit Aluminium, Magnesium oder Legierungen von Aluminium und Magnesium
DE102008051883A1 (de) 2008-10-16 2010-04-22 Nano-X Gmbh Beschichtung zum kathodischen Korrosionsschutz von Metall, Verfahren zum Herstellen der Beschichtung und Verwendung der Beschichtung.
CN103334132B (zh) * 2013-07-17 2016-05-25 沈阳大学 室温电沉积制备铝镁合金膜的方法
KR102544455B1 (ko) 2014-10-31 2023-06-19 베카에르트 빈장 스틸 코드 코., 엘티디. 굽힘부에서 제어된 곡률을 가지는 성형된 톱 와이어
CN104388998B (zh) * 2014-11-18 2016-08-24 沈阳大学 一种室温电沉积制备多孔纳米氧化铝的方法
CN116479475B (zh) * 2023-04-06 2026-03-20 安庆师范大学 一种双膜三室电解槽制备Mg-Al合金的方法和装置

Family Cites Families (7)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
BE540052A (enExample) * 1955-06-13
US3672965A (en) * 1970-06-29 1972-06-27 Continental Oil Co Electroplating of aluminum
US3672964A (en) * 1971-03-17 1972-06-27 Du Pont Plating on aluminum,magnesium or zinc
DE2338063A1 (de) * 1973-07-26 1975-04-03 Siemens Ag Verfahren zum beschichten von hochfrequenz-heizspulen aus kupfer, messing, silber oder aluminium
US4778575A (en) * 1988-01-21 1988-10-18 The United States Of America As Represented By The United States Department Of Energy Electrodeposition of magnesium and magnesium/aluminum alloys
DE3919068A1 (de) * 1989-06-10 1990-12-13 Studiengesellschaft Kohle Mbh Aluminiumorganische elektrolyte zur elektrolytischen abscheidung von hochreinem aluminium
US5015750A (en) * 1990-10-31 1991-05-14 Texas Alkyls, Inc. Preparation of trimethylaluminum

Cited By (11)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2003102276A1 (de) * 2002-05-31 2003-12-11 Aluminal Oberflächentechnik Gmbh & Co. Kg Verfahren zur herstellung von aluminiumorganischen komplexen und deren verwendung zur herstellung von elektrolytlösungen zur elektrochemischen abscheidung von aluminium-magnesium-legierungen
US7235681B2 (en) 2002-05-31 2007-06-26 Aluminal Oberflachentechnik Gmbh & Co. Kg Method for producing organoaluminum complexes and the use thereof for producing electrolyte solutions for the electrochemical deposition of aluminum-magnesium alloys
WO2004053203A3 (de) * 2002-12-10 2004-12-23 Thyssenkrupp Stahl Ag Verfahren zur elektrolytischen abscheidung von magnesium oder magnesium-zink auf verzinktem blech
WO2004099218A1 (en) * 2003-04-30 2004-11-18 Akzo Nobel N.V. Production of mixed sodium and potassium tetraalkylaluminate solutions
EP1518945A1 (de) * 2003-09-27 2005-03-30 Aluminal Oberflächtentechnik GmbH & Co. KG Elektrolyt für die galvanische Abscheidung von Aluminium-Magnesium-Legierungen
WO2005033374A1 (de) * 2003-09-27 2005-04-14 Aluminal Oberflächentechnik Gmbh & Co. Kg Elektrolyt für die galvanische abscheidung von aluminium-magnesium-legierungen
RU2347857C2 (ru) * 2003-09-27 2009-02-27 Алюминал Оберфлехентехник Гмбх Унд Ко. Кг Электролит для гальванического осаждения алюминий-магниевых сплавов
EP1524336A1 (de) * 2003-10-18 2005-04-20 Aluminal Oberflächtentechnik GmbH & Co. KG Mit einer Aluminium-/Magnesium-Legierung beschichtete Werkstücke
WO2005035835A3 (de) * 2003-10-18 2005-06-23 Aluminal Oberflaechentechnik Mit einer aluminium/magnesium-legierung beschichtete werkstücke
EP1624091A1 (de) * 2004-08-04 2006-02-08 Aluminal Oberflächentechnik GmbH & Co. KG Mit einer Aluminium/Magnesium-Legierung oder Aluminium beschichtete Werkstücke mit Zink-Zwischenschicht
RU2407090C1 (ru) * 2009-12-03 2010-12-20 Учреждение Российской академии наук Институт химии и технологии редких элементов и минерального сырья им. И.В. Тананаева Кольского научного центра РАН (ИХТРЭМС КНЦ РАН) СПОСОБ ПОЛУЧЕНИЯ ТВЕРДОГО ИОННОГО ЭЛЕКТРОЛИТА RbAg4I5

Also Published As

Publication number Publication date
US6652730B1 (en) 2003-11-25
CA2352800A1 (en) 2000-06-08
DE19855666A1 (de) 2000-06-08
EP1141447A2 (de) 2001-10-10
WO2000032847A3 (de) 2000-11-16
DE59901980D1 (de) 2002-08-08
JP2002531698A (ja) 2002-09-24
ATE220129T1 (de) 2002-07-15
EP1141447B1 (de) 2002-07-03

Similar Documents

Publication Publication Date Title
EP1141447B1 (de) Aluminiumorganische elektrolyte und verfahren zur elektrolytischen beschichtung mit aluminium oder aluminium-magnesium-legierungen
DE69808415T2 (de) Elektroplattierung von nickel-phosphor-legierungsbeschichtungen
DE69210435T2 (de) Verfahren zur elektrolytischen Verzinkung von Aluminiumband
EP1301656B1 (de) Verfahren zur oberflächenbehandlung von aluminium oder aluminium-legierungen mittels alkansulfonsäurehaltigen formulierungen
EP2116634B1 (de) Modifizierter Kupfer-Zinn-Elektrolyt und Verfahren zur Abscheidung von Bronzeschichten
DE1062079B (de) Cyanidisches Bad und Verfahren zur galvanischen Abscheidung von Kupferueberzuegen
US2750334A (en) Electrodeposition of chromium
DE60020431T2 (de) Zink-Magnesium-elektroplattiertes metallisches Blech und Verfahren zu seiner Herstellung
DE3428277A1 (de) Waessriges bad und ein verfahren zur galvanischen abscheidung einer zink-eisen-legierung
DE832982C (de) Elektrolyt und Verfahren zur elektrolytischen Abscheidung von Kupfer
DE69106522T2 (de) Elektroplattierung.
DE3447813A1 (de) Waessriges saures bad sowie ein verfahren zur galvanischen abscheidung von zink oder zinklegierungen
DE3919069A1 (de) Aluminiumorganische elektrolyte und verfahren zur elektrolytischen abscheidung von aluminium
CH629541A5 (de) Verfahren zur elektrolytischen abscheidung einer eisenlegierung.
US4778575A (en) Electrodeposition of magnesium and magnesium/aluminum alloys
DE69007341T2 (de) Organoaluminium-Elektrolyte für die elektrolytische Absetzung von hochfeinem Aluminium.
DE68905429T2 (de) Verfahren fuer das zinn-elektroplattieren von metallischem material.
DE69205612T2 (de) Korrosionsbeständige Reinzink- oder Teilzinkplattierte Stahlbleche sowie Verfahren zu ihrer Herstellung.
DE1771116B1 (de) Galvanisches Bad zur Abscheidung von Aluminium
DE19716495C1 (de) Elektrolyt für die elektrolytische Abscheidung von Aluminium und dessen Verwendung
WO2005033374A1 (de) Elektrolyt für die galvanische abscheidung von aluminium-magnesium-legierungen
DE3619386C2 (enExample)
DE19649000C1 (de) Elektrolyt zur galvanischen Abscheidung von Aluminium und dessen Verwendung
EP0607119B1 (de) Verfahren zur abscheidung von blei- und bleihaltigen schichten, elektrolyte zur durchführung des verfahrens sowie verwendung von tensiden in sauren blei-elektrolyten
DE815882C (de) Verfahren zur Erzeugung von Niederschlaegen auf Metallflaechen durch Elektrolyse

Legal Events

Date Code Title Description
AK Designated states

Kind code of ref document: A2

Designated state(s): CA JP US

AL Designated countries for regional patents

Kind code of ref document: A2

Designated state(s): AT BE CH CY DE DK ES FI FR GB GR IE IT LU MC NL PT SE

121 Ep: the epo has been informed by wipo that ep was designated in this application
DFPE Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed before 20040101)
AK Designated states

Kind code of ref document: A3

Designated state(s): CA JP US

AL Designated countries for regional patents

Kind code of ref document: A3

Designated state(s): AT BE CH CY DE DK ES FI FR GB GR IE IT LU MC NL PT SE

ENP Entry into the national phase

Ref document number: 2352800

Country of ref document: CA

Ref country code: CA

Ref document number: 2352800

Kind code of ref document: A

Format of ref document f/p: F

WWE Wipo information: entry into national phase

Ref document number: 1999962174

Country of ref document: EP

WWE Wipo information: entry into national phase

Ref document number: 09857013

Country of ref document: US

ENP Entry into the national phase

Ref country code: JP

Ref document number: 2000 585475

Kind code of ref document: A

Format of ref document f/p: F

WWP Wipo information: published in national office

Ref document number: 1999962174

Country of ref document: EP

WWG Wipo information: grant in national office

Ref document number: 1999962174

Country of ref document: EP