WO2021132206A1 - セルフクリーニング剤 - Google Patents

セルフクリーニング剤 Download PDF

Info

Publication number
WO2021132206A1
WO2021132206A1 PCT/JP2020/047823 JP2020047823W WO2021132206A1 WO 2021132206 A1 WO2021132206 A1 WO 2021132206A1 JP 2020047823 W JP2020047823 W JP 2020047823W WO 2021132206 A1 WO2021132206 A1 WO 2021132206A1
Authority
WO
WIPO (PCT)
Prior art keywords
titanium oxide
copper
self
cleaning agent
responsive photocatalyst
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2020/047823
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
幸介 藤田
俊介 河中
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
DIC Corp
Original Assignee
DIC Corp
Dainippon Ink and Chemicals Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by DIC Corp, Dainippon Ink and Chemicals Co Ltd filed Critical DIC Corp
Priority to CN202080087441.3A priority Critical patent/CN114829007B/zh
Priority to JP2021567469A priority patent/JPWO2021132206A1/ja
Publication of WO2021132206A1 publication Critical patent/WO2021132206A1/ja
Anticipated expiration legal-status Critical
Priority to JP2023108711A priority patent/JP7533710B2/ja
Ceased legal-status Critical Current

Links

Classifications

    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
    • B01J23/00—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00
    • B01J23/70—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00 of the iron group metals or copper
    • B01J23/72—Copper
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
    • B01J23/00—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00
    • B01J23/70—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00 of the iron group metals or copper
    • B01J23/76—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00 of the iron group metals or copper combined with metals, oxides or hydroxides provided for in groups B01J23/02 - B01J23/36
    • B01J23/84—Catalysts comprising metals or metal oxides or hydroxides, not provided for in group B01J21/00 of the iron group metals or copper combined with metals, oxides or hydroxides provided for in groups B01J23/02 - B01J23/36 with arsenic, antimony, bismuth, vanadium, niobium, tantalum, polonium, chromium, molybdenum, tungsten, manganese, technetium or rhenium
    • B01J23/847—Vanadium, niobium or tantalum or polonium
    • C—CHEMISTRY; METALLURGY
    • C11—ANIMAL OR VEGETABLE OILS, FATS, FATTY SUBSTANCES OR WAXES; FATTY ACIDS THEREFROM; DETERGENTS; CANDLES
    • C11D—DETERGENT COMPOSITIONS; USE OF SINGLE SUBSTANCES AS DETERGENTS; SOAP OR SOAP-MAKING; RESIN SOAPS; RECOVERY OF GLYCEROL
    • C11D7/00—Compositions of detergents based essentially on non-surface-active compounds
    • C11D7/02—Inorganic compounds
    • C11D7/20—Water-insoluble oxides
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
    • B01J2235/00—Indexing scheme associated with group B01J35/00, related to the analysis techniques used to determine the catalysts form or properties
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
    • B01J2235/00—Indexing scheme associated with group B01J35/00, related to the analysis techniques used to determine the catalysts form or properties
    • B01J2235/15—X-ray diffraction
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
    • B01J2235/00—Indexing scheme associated with group B01J35/00, related to the analysis techniques used to determine the catalysts form or properties
    • B01J2235/30—Scanning electron microscopy; Transmission electron microscopy
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B01—PHYSICAL OR CHEMICAL PROCESSES OR APPARATUS IN GENERAL
    • B01J—CHEMICAL OR PHYSICAL PROCESSES, e.g. CATALYSIS OR COLLOID CHEMISTRY; THEIR RELEVANT APPARATUS
    • B01J35/00—Catalysts, in general, characterised by their form or physical properties
    • B01J35/70—Catalysts, in general, characterised by their form or physical properties characterised by their crystalline properties, e.g. semi-crystalline

Definitions

  • the present invention relates to a self-cleaning agent having a stain decomposition function.
  • Antifouling processing is a processing that makes it difficult for stains and dirt to adhere, and makes it easier to remove dirty things by washing, wiping, etc.
  • the antifouling treatment method is roughly classified into, for example, a water-repellent oil-repellent system and a water-absorbing oil-absorbing system.
  • the water-repellent oil-repellent system contains a fluorine compound, and a method for decomposing stains is photocatalytic oxidation.
  • a method using titanium is known (see, for example, Patent Document 1).
  • the photocatalytic titanium oxide has a problem that it requires a strong energy source called ultraviolet light and that the strong oxidizing action causes deterioration of the processed product and the base material itself.
  • the problem to be solved by the present invention is to provide a self-cleaning agent capable of decomposing dirt components under room light.
  • the present invention provides a self-cleaning agent containing a visible light responsive photocatalyst.
  • the self-cleaning agent of the present invention dirt components can be decomposed under practical room light. Further, by using a specific photocatalyst as the visible light responsive photocatalyst, a self-cleaning agent having further excellent antibacterial and antiviral properties can be obtained. Further, when a specific one is used as the visible light responsive photocatalyst, the handling is good even if the concentration of titanium oxide is increased.
  • the self-cleaning agent of the present invention preferably contains a visible light responsive photocatalyst in order to solve the problems of the present invention.
  • Examples of the visible light-responsive photocatalyst include a composition containing titanium oxide (a), and a metal compound is supported on titanium oxide (a) from the viewpoint of obtaining even more excellent antiviral properties. Is preferably mentioned.
  • titanium oxide (a) for example, rutile-type titanium oxide (a1), anatase-type titanium oxide, brookite-type titanium oxide, or the like can be used. These titanium oxides may be used alone or in combination of two or more. Among these, rutile-type titanium oxide (a1) is preferably contained because it has excellent photocatalytic activity in the visible light region.
  • the content rate (rutileization rate) of the rutile-type titanium oxide (a1) is preferably 15 mol% or more, more preferably 50 mol% or more, and further preferably 90 mol% or more.
  • any titanium oxide produced by either the vapor phase method or the liquid phase method can be used, but it is preferable to use the titanium oxide produced by the liquid phase method.
  • the liquid phase method and the gas phase method are generally known as the method for producing the titanium oxide.
  • the liquid phase method is a method for obtaining titanium oxide by hydrolyzing or neutralizing titanyl sulfate obtained from a liquid in which a raw material ore such as ilmenite ore is dissolved.
  • the vapor phase method is a method for obtaining titanium oxide by a vapor phase reaction between titanium tetrachloride obtained by chlorinating a raw material ore such as rutile ore and oxygen.
  • ilmenite ore may be used as the raw material ore for titanium oxide, or titanium slag obtained by metallizing the ilmenite ore to increase the titanium purity may be used.
  • the titanium oxide preferably contains a metal element such as zirconium or niobium. ..
  • the content ratio (Zr / Ti ratio) of zirconium to titanium 100 in titanium oxide is preferably 0.03 or more, more preferably 0.04 or more, still more preferably 0.05 or more, and preferably 0.8 or more. Below, it is more preferably 0.5 or less, still more preferably 0.3 or less. These upper and lower limits may be any combination.
  • the content ratio (Zr / Ti ratio) of zirconium to titanium 100 in titanium oxide is preferably 0.03 to 0.8, more preferably 0.04 to 0.5, and further preferably 0.05 to 0.3. is there.
  • the content ratio (Nb / Ti ratio) of niobium to titanium 100 in titanium oxide is preferably 0.05 or more, more preferably 0.08 or more, still more preferably 0.1 or more, and preferably 0.8 or more. Below, it is more preferably 0.5 or less, still more preferably 0.3 or less. These upper and lower limits may be any combination.
  • the content ratio (Nb / Ti ratio) of niobium to titanium 100 in titanium oxide is preferably 0.05 to 0.8, more preferably 0.08 to 0.5, and further preferably 0.10 to 0.3. is there. If the titanium oxide is within the above range, the dispersibility in the solvent is high, and the mixture can be handled well even if the concentration of titanium oxide is increased.
  • the content ratio of the metal element (zirconium and / or niobium) to titanium 100 in the visible light responsive photocatalyst is the same as the above range.
  • titanium oxide substantially contains a metal element means that the content ratio of the metal element in titanium oxide is 0.02 or more with respect to titanium 100.
  • Titanium oxide substantially containing a metal element (zirconium and / or niobium) in the present invention has a small cohesive force with respect to the specific surface area (BET value) caused by the primary particles and can suppress the viscosity of the mixed solution. It is possible, and it is presumed that it contributes to the improvement of the concentration of titanium oxide.
  • the BET specific surface area of the titanium oxide (a) is preferably in the range of 1 to 200 m 2 / g from the viewpoint of obtaining even more excellent antiviral properties and visible light responsiveness, and is preferably 3 to 100 m 2 / g.
  • the range of 4 to 70 m 2 / g is more preferable, the range of 8 to 50 m 2 / g is more preferable, and the productivity of the self-cleaning agent can be further increased.
  • the range is preferably 9.5 m 2 / g.
  • the method for measuring the BET specific surface area of the rutile-type titanium oxide (a1) will be described in Examples described later.
  • the primary particle size of the titanium oxide (a) is preferably in the range of 0.01 to 0.5 ⁇ m, preferably 0.03 to 0.5 ⁇ m, from the viewpoint of obtaining even more excellent antiviral properties and visible light responsiveness.
  • the range of 0.35 ⁇ m is more preferable, and the range of 0.06 to 0.35 ⁇ m is even more preferable.
  • the primary particle size of the titanium oxide (a) is measured by a method of directly measuring the size of the primary particles from an electron micrograph using a transmission electron microscope (TEM). .. Specifically, the minor axis diameter and the major axis diameter of each titanium oxide primary particle are measured, the average is taken as the particle size of the primary particle, and then for 100 or more titanium oxide particles, each particle is used. The volume (weight) of was obtained by approximating it to a cube having the obtained particle size, and the volume average particle size was defined as the average primary particle size.
  • the visible light responsive photocatalyst further improves the photocatalytic activity in the visible light region and easily exhibits an appropriate activity capable of decomposing dirt components under practical indoor light, and thus titanium oxide (a).
  • titanium oxide (a) With a metal compound supported (titanium oxide composition) is preferably used.
  • a transition metal such as copper, iron, tungsten, zirconium, or molybdenum
  • other metals such as zinc, aluminum, antimony, and tin can be used depending on the desired physical properties.
  • the titanium oxide an inorganic compound may be supported depending on desired physical properties, and for example, silicon may be used.
  • a copper compound is preferable, and a divalent copper compound is more preferable, from the viewpoint of obtaining even more excellent antibacterial property, antiviral property, and stain component degrading activity.
  • a method for supporting the metal compound on the titanium oxide (a) a known method can be used.
  • Examples of the method for supporting the divalent copper compound on the titanium oxide (a) include titanium oxide (a) containing rutile-type titanium oxide (a1), a divalent copper compound raw material (b), water (c), and water (c). , A method having a mixing step (i) of the alkaline substance (d) can be mentioned.
  • the concentration of the titanium oxide (a) in the mixing step (i) is preferably in the range of 3 to 40% by mass.
  • a mixing step with good handling can be performed even if the concentration of titanium oxide (a) is increased.
  • the mixing step can be satisfactorily performed even when the concentration of the titanium oxide (a) exceeds 25% by mass and is 40% by mass or less.
  • divalent copper compound raw material (b) for example, a divalent copper inorganic compound, a divalent copper organic compound, or the like can be used.
  • divalent copper inorganic compound examples include copper sulfate, copper nitrate, copper iodide, copper perchlorate, copper oxalate, copper tetraborate, copper ammonium sulfate, copper amide sulfate, copper ammonium chloride, and copper pyrophosphate.
  • Inorganic acid salts of divalent copper such as copper carbonate; halides of divalent copper such as copper chloride, copper fluoride, copper bromide; copper oxide, copper sulfide, azulite, malakite, copper azide and the like can be used. .. These compounds may be used alone or in combination of two or more.
  • divalent copper organic compound examples include copper formate, copper acetate, copper propionate, copper butyrate, copper valerate, copper caproate, copper enanthate, copper caprylate, copper pelargonate, copper capricate, and mistinic acid.
  • the divalent copper compound raw material (b) it is preferable to use the one represented by the following general formula (1) among the above-mentioned ones.
  • CuX 2 (1) In formula (1), X represents a halogen atom, CH 3 COO, NO 3 or (SO 4 ) 1/2 .
  • the X in the formula (1) is more preferably a halogen atom, and even more preferably a chlorine atom.
  • the amount of the divalent copper compound raw material (b) used in the mixing step (i) is preferably in the range of 0.01 to 20 parts by mass with respect to 100 parts by mass of the titanium oxide (a).
  • the range of 0.1 to 15 parts by mass is more preferable, and the range of 0.3 to 10 parts by mass is further preferable.
  • the water (c) is the solvent in the mixing step (i), and water alone is preferable, but other solvents may be contained if necessary.
  • the other solvent for example, an alcohol solvent such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol; a ketone solvent such as methyl ethyl ketone and methyl isobutyl ketone; dimethylformamide, tetrahydrofuran and the like can be used. These solvents may be used alone or in combination of two or more.
  • alkaline substance (d) for example, sodium hydroxide, potassium hydroxide, tetramethylammonium hydroxide, tetrabutylammonium hydroxide, triethylamine, trimethylamine, ammonia, a basic surfactant and the like can be used, and water can be used. It is preferable to use sodium oxide.
  • the alkaline substance (d) is preferably added as a solution from the viewpoint of easy control of the reaction, and the concentration of the alkaline solution to be added is preferably in the range of 0.1 to 5 mol / L.
  • the range of 3 to 4 mol / L is more preferable, and the range of 0.5 to 3 mol / L is even more preferable.
  • the titanium oxide (a), the divalent copper compound raw material (b), the water (c), and the alkaline substance (d) may be mixed.
  • examples thereof include a method in which titanium oxide (a) is mixed and stirred as necessary, then a divalent copper compound raw material (b) is mixed and stirred, and then an alkaline substance (d) is added and stirred. ..
  • the divalent copper compound derived from the divalent copper compound raw material (b) is supported on the titanium oxide (a).
  • the total stirring time in the mixing step (i) is, for example, 5 to 120 minutes, preferably 10 to 60 minutes.
  • Examples of the temperature in the mixing step (i) include a range of room temperature to 70 ° C.
  • the titanium oxide (a), the divalent copper compound raw material (b), and water (c) are mixed and stirred from the viewpoint of good support of the divalent copper compound on the titanium oxide (a), and then alkaline.
  • the pH of the mixture after mixing and stirring the substance (d) is preferably in the range of 8 to 11, and more preferably in the range of 9.0 to 10.5.
  • the mixed liquid can be separated as a solid content.
  • the method for performing the separation include filtration, sedimentation separation, centrifugation, evaporation drying and the like, but filtration is preferable.
  • the separated solid content may then be washed with water, crushed, classified, or the like, if necessary.
  • the divalent copper compound derived from the divalent copper compound raw material (b) supported on the titanium oxide (a) can be more firmly bonded to the solid content.
  • the heat treatment temperature is preferably in the range of 150 to 600 ° C, more preferably in the range of 250 to 450 ° C.
  • the heat treatment time is preferably 1 to 10 hours, more preferably 2 to 5 hours.
  • a titanium oxide composition containing titanium oxide in which a divalent copper compound is supported on titanium oxide (a) can be obtained.
  • the amount of the divalent copper compound supported on the titanium oxide (a) is in the range of 0.01 to 20 parts by mass with respect to 100 parts by mass of the titanium oxide (a). It is preferable from the viewpoint of photocatalytic activity including.
  • the amount of the divalent copper compound carried can be adjusted by adjusting the amount of the divalent copper compound raw material (b) used in the mixing step (i). The method for measuring the amount of the divalent copper compound supported will be described in Examples described later.
  • Examples of the above-mentioned embodiment include kneading into fibers and the like, a spray agent, and a coating agent.
  • Examples of the method of kneading into the fibers and the like include a method of kneading fibers such as polyester and the self-cleaning agent using an extruder or the like and spinning them.
  • spray agent examples include the self-cleaning agent and a mixture of solvents such as water and alcohol.
  • the coating agent examples include the self-cleaning agent, a solvent such as water and alcohol, and a mixture of a binder resin and the like.
  • a binder resin for example, an acrylic resin, a urethane resin, a phenol resin, a polyester resin, an epoxy resin or the like can be used. These binder resins may be used alone or in combination of two or more.
  • the dirt component can be decomposed under practical indoor light in the aspect of the organic material such as fiber and the inorganic material such as slate plate. Further, by using a specific photocatalyst as the visible light responsive photocatalyst, a self-cleaning agent having further excellent antibacterial and antiviral properties can be obtained.
  • the self-cleaning agent according to the present invention is excellent in antiviral property, antibacterial property, safety to human body, heat resistance, weather resistance, and water resistance.
  • Preparation Example 2 A titanium oxide composition was obtained in the same manner as in Preparation Example 1 except that the amount of copper (ii) chloride dihydrate used was changed from 8 parts by mass to 3.3 parts by mass in Preparation Example 1. Moreover, the change test of the titanium oxide concentration was carried out in the same manner as in Preparation Example 1.
  • a titanium oxide composition was obtained in the same manner as in Preparation Example 1 except that the type of titanium oxide was changed to the titanium oxide in Preparation Example 1. Moreover, the change test of the titanium oxide concentration was carried out in the same manner as in Preparation Example 1.
  • a titanium oxide composition was obtained in the same manner as in Preparation Example 1 except that the type of titanium oxide was changed to the titanium oxide in Preparation Example 1. Moreover, the change test of the titanium oxide concentration was carried out in the same manner as in Preparation Example 1.
  • the titanium oxide composition was prepared in the same manner as in Preparation Example 1 except that the type of titanium oxide was changed to the titanium oxide and the amount of water used was changed from 900 parts by mass to 4,000 parts by mass. Obtained. Moreover, the change test of the titanium oxide concentration was carried out in the same manner as in Preparation Example 1.
  • Preparation Example 6 A titanium oxide composition was obtained in the same manner as in Preparation Example 5 except that the amount of copper (ii) chloride dihydrate used was changed from 8 parts by mass to 3.3 parts by mass in Preparation Example 5. Moreover, the change test of the titanium oxide concentration was carried out in the same manner as in Preparation Example 1.
  • a titanium oxide composition was obtained in the same manner as in Preparation Example 5 except that the type of titanium oxide was changed to the titanium oxide in Preparation Example 5. Moreover, the change test of the titanium oxide concentration was carried out in the same manner as in Preparation Example 1.
  • a titanium oxide composition was obtained in the same manner as in Preparation Example 5 except that the type of titanium oxide was changed to the titanium oxide in Preparation Example 5. Moreover, the change test of the titanium oxide concentration was carried out in the same manner as in Preparation Example 1.
  • a titanium oxide composition was obtained in the same manner as in Preparation Example 5 except that the type of titanium oxide was changed to the titanium oxide in Preparation Example 5. Moreover, the change test of the titanium oxide concentration was carried out in the same manner as in Preparation Example 1.
  • titanium oxide As shown in Preparation Examples 1 to 4, if titanium oxide is obtained by the liquid phase method, it can be stably mixed even if the concentration of titanium oxide (a) in the mixture in the mixing step (i) is increased, and it has antiviral properties. It was found that an excellent antiviral agent can be efficiently produced.
  • Example 1 25 parts by mass of the titanium oxide composition obtained in Adjustment Example 1, 73.5 parts by mass of water, and 1.5 parts by mass of a dispersant (“DISPERBIK 190” manufactured by Big Chemie) were dispersed with a sand grinder to obtain an aqueous slurry. It was.
  • the stain component (A) (0.5 parts by mass of oil red, 49.75 parts by mass of ethanol, and 49.75 parts by mass of oleic acid) was added dropwise to the obtained sample using a micropipette, and 500 lux was added.
  • the a * value was measured with a colorimeter (“CR-200 D65 light source” manufactured by Konica Minolta Co., Ltd.) 1 hour (0 days later), 1 day and 2 days after the dropping.
  • Example 2 In Example 1, the a * value was measured in the same manner as in Example 1 except that the stain component (A) was changed to the stain component (B) (chili oil manufactured by S & B Co., Ltd.). In addition, ⁇ a * was obtained by the difference from Comparative Example 4.
  • Example 3 In Example 1, the stain component (A) was changed to the stain component (C) (1 part by mass of S & B curry powder granules and 99 parts by mass of ethanol) in the same manner as in Example 1. The a * value was measured. In addition, ⁇ a * was obtained by the difference from Comparative Example 6.
  • Example 4 In Example 1, the a * value was measured in the same manner as in Example 1 except that the cotton broad cloth was changed to a slate plate (manufactured by Nozawa Corporation). In addition, ⁇ a * was obtained by the difference from Comparative Example 8.
  • Example 1 The a * value was measured in the same manner as in Example 1 except that the stain component (A) was directly dropped onto the cotton broad cloth used in Example 1. Further, this a * value was used as a reference for the amount of color change ( ⁇ a *) of Example 1, Comparative Example 2, and Comparative Example 3.
  • Comparative Example 4 In Comparative Example 1, the a * value was measured in the same manner as in Comparative Example 1 except that the stain component (A) was changed to the stain component (B). Further, this a * value was used as a reference for the amount of color change ( ⁇ a *) in Example 2 and Comparative Example 5.
  • Comparative Example 5 In Comparative Example 2, the a * value was measured in the same manner as in Comparative Example 2 except that the stain component (A) was changed to the stain component (B).
  • Comparative Example 6 In Comparative Example 1, the a * value was measured in the same manner as in Comparative Example 1 except that the stain component (A) was changed to the stain component (C). Further, this a * value was used as a reference for the amount of color change ( ⁇ a *) in Example 3 and Comparative Example 7.
  • Comparative Example 7 In Comparative Example 2, the a * value was measured in the same manner as in Comparative Example 2 except that the stain component (A) was changed to the stain component (C).
  • Comparative Example 9 In Comparative Example 2, the a * value was measured in the same manner as in Comparative Example 2 except that a slate plate (manufactured by Nozawa Corporation) was used instead of the cotton broad cloth.
  • the stain decomposition effect was determined by the difference ⁇ a * based on the a * value of the comparative example in which only the stain component was dropped on the base material (cotton broad cloth, slate plate).
  • the amount of color change is evaluated from ⁇ a * after n days and ⁇ a * at the initial stage (after 0 days), and the more the amount of color change becomes negative, the more the dye, which is a stain component, is decomposed.
  • the self-cleaning agent of the present invention has an excellent stain decomposition function under room light.
  • Comparative Examples 1 to 9 did not contain a visible light responsive photocatalyst, but were inferior in stain decomposability under room light.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Organic Chemistry (AREA)
  • Inorganic Chemistry (AREA)
  • Life Sciences & Earth Sciences (AREA)
  • Oil, Petroleum & Natural Gas (AREA)
  • Wood Science & Technology (AREA)
  • Materials Engineering (AREA)
  • Catalysts (AREA)
  • Paints Or Removers (AREA)
PCT/JP2020/047823 2019-12-23 2020-12-22 セルフクリーニング剤 Ceased WO2021132206A1 (ja)

Priority Applications (3)

Application Number Priority Date Filing Date Title
CN202080087441.3A CN114829007B (zh) 2019-12-23 2020-12-22 自清洁剂
JP2021567469A JPWO2021132206A1 (cg-RX-API-DMAC7.html) 2019-12-23 2020-12-22
JP2023108711A JP7533710B2 (ja) 2019-12-23 2023-06-30 セルフクリーニング剤

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2019231480 2019-12-23
JP2019-231480 2019-12-23

Publications (1)

Publication Number Publication Date
WO2021132206A1 true WO2021132206A1 (ja) 2021-07-01

Family

ID=76574132

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2020/047823 Ceased WO2021132206A1 (ja) 2019-12-23 2020-12-22 セルフクリーニング剤

Country Status (3)

Country Link
JP (2) JPWO2021132206A1 (cg-RX-API-DMAC7.html)
CN (1) CN114829007B (cg-RX-API-DMAC7.html)
WO (1) WO2021132206A1 (cg-RX-API-DMAC7.html)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN115820119A (zh) * 2021-09-16 2023-03-21 Dic株式会社 树脂组合物、涂布剂及物品

Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2004082088A (ja) * 2001-10-15 2004-03-18 Jfe Steel Kk 光触媒および光触媒材料
JP2004322052A (ja) * 2003-04-28 2004-11-18 Toagosei Co Ltd 可視光応答型光触媒
JP2004344863A (ja) * 2003-05-19 2004-12-09 Masanori Hirano 光触媒担持多孔性ゲル及びその製造法
WO2013094573A1 (ja) * 2011-12-22 2013-06-27 昭和電工株式会社 銅及びチタン含有組成物並びにその製造方法
JP2017155368A (ja) * 2016-03-03 2017-09-07 Dic株式会社 繊維加工用樹脂組成物、それを用いた布帛

Family Cites Families (11)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2005138008A (ja) * 2003-11-05 2005-06-02 National Institute For Materials Science 可視光応答型酸化チタン複合系光触媒およびその製造法
JP2007196182A (ja) * 2006-01-30 2007-08-09 Toray Ind Inc バグフィルター用濾布およびバグフィルター
JP5358433B2 (ja) * 2007-05-25 2013-12-04 石原産業株式会社 複合体及びその製造方法並びにそれを含む組成物
JP2011020033A (ja) * 2009-07-14 2011-02-03 Ishihara Sangyo Kaisha Ltd 可視光応答型光触媒およびその製造方法並びにそれを用いた光触媒コート剤、光触媒分散体
WO2011049068A1 (ja) * 2009-10-19 2011-04-28 国立大学法人 東京大学 ウィルスを不活化する方法及び抗ウィルス性付与物品
JP5567828B2 (ja) * 2009-11-30 2014-08-06 パナソニック株式会社 可視光応答型光触媒コーティング材、コーティング処理物及びアレルゲン不活性化方法
JP6040021B2 (ja) * 2012-12-13 2016-12-07 昭和電工株式会社 抗菌抗ウイルス性組成物及びその製造方法
WO2014141812A1 (ja) * 2013-03-15 2014-09-18 昭和電工株式会社 抗菌抗ウイルス性光触媒酸化チタン、及び中性領域で分散した抗菌抗ウイルス性光触媒酸化チタンスラリー並びにそれらの製造方法
CN103852481B (zh) * 2014-03-12 2016-03-02 攀钢集团攀枝花钢铁研究院有限公司 一种测定包膜钛白中元素成分的方法
JP7238877B2 (ja) * 2020-11-10 2023-03-14 Dic株式会社 金属化合物を担持した酸化チタンの水性組成物
CN116568398A (zh) * 2020-12-22 2023-08-08 Dic株式会社 氧化钛组合物

Patent Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2004082088A (ja) * 2001-10-15 2004-03-18 Jfe Steel Kk 光触媒および光触媒材料
JP2004322052A (ja) * 2003-04-28 2004-11-18 Toagosei Co Ltd 可視光応答型光触媒
JP2004344863A (ja) * 2003-05-19 2004-12-09 Masanori Hirano 光触媒担持多孔性ゲル及びその製造法
WO2013094573A1 (ja) * 2011-12-22 2013-06-27 昭和電工株式会社 銅及びチタン含有組成物並びにその製造方法
JP2017155368A (ja) * 2016-03-03 2017-09-07 Dic株式会社 繊維加工用樹脂組成物、それを用いた布帛

Cited By (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN115820119A (zh) * 2021-09-16 2023-03-21 Dic株式会社 树脂组合物、涂布剂及物品
JP2023043393A (ja) * 2021-09-16 2023-03-29 Dic株式会社 樹脂組成物、コーティング剤、及び物品
JP7809935B2 (ja) 2021-09-16 2026-02-03 Dic株式会社 樹脂組成物、コーティング剤、及び物品

Also Published As

Publication number Publication date
JP2023130423A (ja) 2023-09-20
JP7533710B2 (ja) 2024-08-14
CN114829007B (zh) 2024-03-12
JPWO2021132206A1 (cg-RX-API-DMAC7.html) 2021-07-01
CN114829007A (zh) 2022-07-29

Similar Documents

Publication Publication Date Title
JP5343176B1 (ja) 銅及びチタン含有組成物並びにその製造方法
JP6040021B2 (ja) 抗菌抗ウイルス性組成物及びその製造方法
JP5812488B2 (ja) 抗菌抗ウイルス性組成物及びその製造方法
JP5157561B2 (ja) 可視光応答型光触媒とその製造方法
EP2133311B1 (en) Zirconium oxalate sol
WO2015125367A1 (ja) 抗ウイルス性組成物、抗ウイルス剤、光触媒およびウイルス不活性化方法
JP7533710B2 (ja) セルフクリーニング剤
JP2016113332A (ja) BiVO4が担持された酸化チタン、その製造方法および抗ウイルス性組成物
CN104998664B (zh) 光触媒组合物及含有该光触媒组合物的光触媒涂料组合物
JP5510521B2 (ja) 光触媒粒子の分散液及びその製法
JP2020182918A (ja) 酸化チタン組成物の製造方法
JP7235162B2 (ja) 酸化チタン組成物
JP2011079713A (ja) 銅イオン修飾酸化チタン及びその製造方法、並びに光触媒
JP2016113331A (ja) BiVO4が担持された酸化チタンの製造方法および抗ウイルス性組成物
KR20230079058A (ko) 코팅용 조성물
JP6485464B2 (ja) 光触媒材料、光触媒材料の製造方法、抗ウイルス剤、抗菌剤、光触媒コーティング組成物、及び光触媒塗装体
JP6368926B2 (ja) 光触媒コーティング組成物
JP2015205254A (ja) 光触媒組成物、抗ウイルス剤及び抗菌剤
JP2015134726A (ja) 抗ウイルス性組成物、その製造方法及びウイルス不活化方法
JP4763492B2 (ja) 光触媒分散体およびその製造方法
WO2016158920A1 (ja) 二酸化バナジウム含有微粒子の製造方法、二酸化バナジウム含有微粒子及び分散液
JP2023006883A (ja) 銅担持酸化チタンスラリー、銅担持酸化チタンスラリーの製造方法および塗料組成物の製造方法
JP2022076642A (ja) 水性塗料、及び該水性塗料が塗装された物品
JP2005187313A (ja) チタニア溶液の製造方法

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 20905333

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2021567469

Country of ref document: JP

Kind code of ref document: A

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 20905333

Country of ref document: EP

Kind code of ref document: A1