WO2015040936A1 - ラベル台紙、ラベルおよびラベル台紙の製造方法 - Google Patents
ラベル台紙、ラベルおよびラベル台紙の製造方法 Download PDFInfo
- Publication number
- WO2015040936A1 WO2015040936A1 PCT/JP2014/068440 JP2014068440W WO2015040936A1 WO 2015040936 A1 WO2015040936 A1 WO 2015040936A1 JP 2014068440 W JP2014068440 W JP 2014068440W WO 2015040936 A1 WO2015040936 A1 WO 2015040936A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- label
- resin
- forming
- toner
- emulsion
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Images
Classifications
-
- G—PHYSICS
- G09—EDUCATION; CRYPTOGRAPHY; DISPLAY; ADVERTISING; SEALS
- G09F—DISPLAYING; ADVERTISING; SIGNS; LABELS OR NAME-PLATES; SEALS
- G09F3/00—Labels, tag tickets, or similar identification or indication means; Seals; Postage or like stamps
- G09F3/08—Fastening or securing by means not forming part of the material of the label itself
- G09F3/10—Fastening or securing by means not forming part of the material of the label itself by an adhesive layer
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B31—MAKING ARTICLES OF PAPER, CARDBOARD OR MATERIAL WORKED IN A MANNER ANALOGOUS TO PAPER; WORKING PAPER, CARDBOARD OR MATERIAL WORKED IN A MANNER ANALOGOUS TO PAPER
- B31D—MAKING ARTICLES OF PAPER, CARDBOARD OR MATERIAL WORKED IN A MANNER ANALOGOUS TO PAPER, NOT PROVIDED FOR IN SUBCLASSES B31B OR B31C
- B31D1/00—Multiple-step processes for making flat articles ; Making flat articles
- B31D1/02—Multiple-step processes for making flat articles ; Making flat articles the articles being labels or tags
- B31D1/021—Making adhesive labels having a multilayered structure, e.g. provided on carrier webs
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B05—SPRAYING OR ATOMISING IN GENERAL; APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D—PROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D1/00—Processes for applying liquids or other fluent materials
- B05D1/02—Processes for applying liquids or other fluent materials performed by spraying
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B05—SPRAYING OR ATOMISING IN GENERAL; APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D—PROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D1/00—Processes for applying liquids or other fluent materials
- B05D1/18—Processes for applying liquids or other fluent materials performed by dipping
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B31—MAKING ARTICLES OF PAPER, CARDBOARD OR MATERIAL WORKED IN A MANNER ANALOGOUS TO PAPER; WORKING PAPER, CARDBOARD OR MATERIAL WORKED IN A MANNER ANALOGOUS TO PAPER
- B31D—MAKING ARTICLES OF PAPER, CARDBOARD OR MATERIAL WORKED IN A MANNER ANALOGOUS TO PAPER, NOT PROVIDED FOR IN SUBCLASSES B31B OR B31C
- B31D1/00—Multiple-step processes for making flat articles ; Making flat articles
- B31D1/02—Multiple-step processes for making flat articles ; Making flat articles the articles being labels or tags
- B31D1/027—Multiple-step processes for making flat articles ; Making flat articles the articles being labels or tags involving, marking, printing or coding
-
- G—PHYSICS
- G09—EDUCATION; CRYPTOGRAPHY; DISPLAY; ADVERTISING; SEALS
- G09F—DISPLAYING; ADVERTISING; SIGNS; LABELS OR NAME-PLATES; SEALS
- G09F3/00—Labels, tag tickets, or similar identification or indication means; Seals; Postage or like stamps
- G09F3/02—Forms or constructions
Definitions
- the present invention relates to a label mount, and more particularly to a label mount, a label and a method for producing the label mount used when producing a label of a desired dimension by an electrophotographic method.
- the present applicant proposed a method of producing a label by an electrophotographic method (Patent Document 1). Specifically, the toner for label formation is transferred in an arbitrary shape onto the label forming area of the label mount formed by applying the adhesive to the release sheet by an electrophotographic method. Then, heat treatment (fixing) is performed to form a label film on the label forming area to produce a label. In this method, it is possible to produce the label in any shape on demand.
- this method performs both label formation (forming a film for a label) and label printing (printing an image etc. on the formed film for a label to form an image) with an electrophotographic printer be able to. For this reason, the pressure-sensitive adhesive layer-attached label obtained by this method is discharged from the label producing apparatus (electrophotographic printer) in a state where the necessary pattern is printed.
- Patent Document 2 proposes that a UV curable resin be used as a binder resin as a material of a label forming toner.
- UV irradiation is performed simultaneously with or immediately after fixation to form a label film having high film strength.
- a resin having a high molecular weight is used to select the material of the label forming toner, the film strength is improved, but the pulverization at the time of toner production becomes difficult and the productivity of the toner is deteriorated.
- a resin having a low molecular weight and good crushability is used, the film strength becomes weak. For this reason, by using the UV curable resin as a label forming toner, it is possible to improve both the grindability and the film strength.
- Patent Document 3 proposes increasing the transfer density of the toner image of the toner for forming a label by decreasing the linear velocity of the transport belt that transports the label mount. According to this proposal, a desired thickness of the label film after fixing can be obtained.
- Patent Document 4 proposes using a toner for forming a label containing polylactic acid having a mass average molecular weight of 100,000 or more as a binder resin. According to this proposal, a label with high film strength can be provided.
- Patent Document 5 proposes a method for producing a label including a step of curing the margin portion of the pressure-sensitive adhesive layer other than the label formation region by ultraviolet irradiation. According to this proposal, when the label film is peeled from the release sheet, the excess pressure sensitive adhesive does not adhere to the label film. For this reason, a label easy to handle can be produced.
- Patent No. 4765810 gazette JP, 2010-184470, A JP 2011-107418 A JP 2012-108300 A JP, 2012-139982, A
- the label coat layer of Patent Document 1 is a layer covering an adhesive layer, and is a transparent label base material on which a thermoplastic resin powder of vinylidene chloride is applied, melted and consolidated.
- the coating layer which coated the adhesive layer surface is provided.
- this coat layer is a thing with the good binding property of the film for labels, and an adhesive layer, respectively.
- the label film, the coat layer, and the pressure-sensitive adhesive layer all come together and be neatly peeled off when peeling off.
- a method for producing a coating layer a resin constituting the coating layer is dissolved in an organic solvent, and the solution is applied to a coater (a coating device for applying a coating liquid to a strip-like base material traveling continuously using a roller) It is conceivable to form a layer by applying with an applicator (application tool for applying a sample moving downward from a gap of a predetermined width).
- an applicator application tool for applying a sample moving downward from a gap of a predetermined width.
- this method requires recovery of the volatilized organic solvent.
- the problem to be solved by the present invention is that it is suitable for the conveyance of the backing sheet in the label producing apparatus, and the label shape following property is good when peeling the label from the release sheet, and further the binding property with the label film, It is an object of the present invention to provide a method for producing a label mount, a label and a label mount having a coating layer having a good binding property with the pressure-sensitive adhesive layer.
- the label mount of the present invention is the exfoliation sheet which has the exfoliation surface which can exfoliate the adhering adhesive on at least one side, the adhesive layer laminated on the exfoliation surface, and the above-mentioned adhesive layer And a coating layer laminated on the surface opposite to the surface on the release sheet side, and the resin forming the coating layer is on the opposite side to the surface on the pressure-sensitive adhesive layer side of the coating layer
- a resin having a structure common to the resin component constituting the label forming toner for producing a label by transferring and fixing on a surface and / or a resin having a structure common to the resin component constituting the pressure-sensitive adhesive is used Configured as.
- the label of this invention is a label with an adhesive layer formed by transferring and fixing the toner for label formation on the surface of label mount.
- the manufacturing method of the label mount of this invention laminates
- the method comprises: an emulsion preparation step of preparing an emulsion by dispersing a resin having a structure in water to prepare an emulsion; and an emulsion application step of applying the emulsion obtained in the emulsion preparation step on the pressure-sensitive adhesive layer.
- FIG. 2A It is a figure which shows the next process of FIG. 2A. It is a figure which shows the next process of FIG. 2B. It is a figure which shows the next process of FIG. 2C. It is a figure which shows the next process of FIG. 2D. It is a figure which shows the next process of FIG. 2E. It is a figure which shows the first process of dip coating. It is a figure which shows the next process of FIG. 3A. It is a figure which shows the next process of FIG. 3B. It is a figure which shows the next process of FIG. 3C.
- the label producing apparatus is an apparatus for transferring and fixing a label forming toner on a mount in a desired shape.
- an electrophotographic printer includes a toner for forming a label in addition to a toner for printing, and has a function of transferring and fixing the toner for forming a label on a desired area of a print medium (label mount described later). It is an apparatus which it has.
- the label forming toner is a toner transferred to a label forming area of a print medium (label mount) to form a film-like label.
- the transfer and fixing of the toner for forming a label are performed in the same process as the development and fixing of the electrophotographic system.
- the label forming toner may be abbreviated as label toner.
- the label mount is a printing medium of the label producing apparatus, and comprises a release sheet (separator), an adhesive layer formed thereon, and a coat layer covering the surface of the adhesive layer.
- the label mount having dimensions acceptable to the label producing apparatus is manufactured in advance in a factory or the like and delivered to the user of the label producing apparatus. It is assumed that the label mount is supplied to the label producing apparatus, transferred, fixed, and discharged. Then, a film-like label is formed only in the label forming area of the label mount, and a necessary pattern is printed on the film-like label.
- the toner is not transferred to the blank area other than the label forming area, and the coat layer is exposed. Further, the coat layer immediately below the film-like label formed in the label forming area enhances the binding between the film-like label immediately above it as the binder and the pressure-sensitive adhesive layer just below it.
- the label mount after the label preparation process is stored until use and transported if necessary.
- the core of the label is a label film. When using this label, it is attached to necessary places such as office equipment, shelves, lockers, etc. by the adhesive force of the adhesive layer. For this reason, an adhesive layer is bound to the back side of the label. In particular, when the adhesive layer is attached to the back of the label, it is referred to as an adhesive layer-attached label.
- a label with an adhesive layer regardless of whether it is in a state of being stuck at any place or in a state of not being stuck (for example, in a state of being stored until use and with a release sheet attached) Call it
- the resin having a common structure means that the chemical structure is common (for example, the skeleton is common).
- polyester resins have a common structure. The same applies to acrylic resins.
- FIG. 1 is a cross-sectional view showing an internal configuration of a label producing apparatus according to an embodiment of the present invention.
- the label producing apparatus 1 includes a sheet feeding unit 2, a label forming unit 3, a printing unit 4, a conveyance unit 5, a fixing unit 6, a feed back mechanism unit 7, and a discharge unit 8.
- the sheet feeding unit 2 is provided with a sheet feeding tray 9 provided so as to project obliquely upward from the side of the label producing apparatus 1, a sheet feeding roller 11 provided at a sheet feeding port of the sheet feeding tray 9, and the sheet feeding roller A standby roller pair 12 disposed in the paper feed direction 11 is provided.
- the label forming unit 3 includes a photosensitive drum 13, a cleaner 14 disposed so as to surround the circumferential surface of the photosensitive drum 13, an initialization charger 15, an optical writing head 16, a powder hopper 17, and a powder hopper
- the developing roller 18 rotatably held at the lower opening of the transfer belt 17, the transfer belt 19, and the transfer roller 21 pressed against the lower surface of the photosensitive drum 13 via the upper transfer surface of the transfer belt 19 Ru.
- a label forming toner is accommodated in the powder hopper 17, a label forming toner is accommodated.
- the powder supply roller 22 is disposed in contact with the developing roller 18 in a sliding manner so as to be embedded in the label forming toner.
- the doctor blade 23 is disposed in contact with the developing roller 18 in a sliding manner.
- a recovery pipe 24 is provided between the cleaner 14 and the powder hopper 17.
- the recovery pipe 24 incorporates a long transport screw, and recovers, in the powder hopper 17, the toner in the form of powder that is cleaned from the photosensitive drum 13 and deposited in the cleaner 14.
- the printing unit 4 has the same configuration as the label forming unit 3 except that the recovery pipe 24 is not provided and the powder hopper 17 contains black toner for printing rather than label forming toner. is there. Not only black toner, but also magenta toner, cyan toner, and yellow toner may be provided to form a color printing unit.
- the transport unit 5 includes the above-described transport belt 19, a drive roller 25 and a driven roller 26 on which the transport belt 19 is stretched, a tension roller 27 provided to stretch the transport belt 19, and the upstream side of the transport belt 19 in the sheet transport direction (
- the right side is constituted by a rotation mechanism or the like for bringing the photosensitive drum 13 of the printing unit 4 into contact (solid line portion) or separating (dotted line portion).
- the pivoting mechanism is formed of, for example, a combination of known mechanical members.
- the fixing unit 6 includes a heat insulating casing 28, and a heat generating roller 29 and a pressure roller 31 which are disposed opposite to each other by being surrounded by the heat insulating casing 28, and the downstream side of the heat generating roller 29 and the pressure roller 31 (left in FIG. And an unloading roller 32 disposed at the
- the feed-back mechanism unit 7 includes feed-back roller pairs 33 (33a to 33f) disposed at six locations at substantially equal distances between the carry-out roller 32 of the fixing unit 6 and the standby roller pair 12 of the sheet feeding unit 2. And a feed back guide path 34 (34a to 34f) disposed in each of the feed back roller pairs 33.
- the discharge unit 8 includes a switching flap 35 disposed immediately after the discharge roller 32 of the fixing unit 6, a pair of conveyance rollers 36 disposed on the downstream upper side of the switching flap 35, a sheet discharge guide path 37, and the sheet discharge guide path 37.
- a sheet discharge roller pair 38 disposed at the end of the sheet discharge tray 39, and a sheet discharge tray 39 formed on the upper surface of the main body of the label producing apparatus 1 by being inclined obliquely upward from the lower outside of the sheet discharge roller pair 38.
- FIGS. 2A to 2F are diagrams schematically showing steps of producing a label produced by the label producing apparatus 1 having the above-described structure. The steps of producing the label will be described below with reference to FIGS. 2A to 2F.
- FIG. 2A shows the first step of producing a label using a label mount in a label producing apparatus, that is, a label mount 50 (a release sheet with an adhesive) placed on the paper feed tray 9 of the label producing apparatus 1. ing.
- the adhesive layer 41 is provided on the release sheet 40
- the coat layer 51 is provided on the adhesive layer 41.
- the label mount has a structure in which the release sheet, the pressure-sensitive adhesive layer, and the coating layer are laminated.
- the coat layer 51 is formed of a monomer, dimer, trimer or tetramer of a resin smaller in viscosity than the adhesive forming the adhesive layer 41. Since the label mount 50 is conveyed in the above-described label producing apparatus 1, when the adhesive layer 41 is exposed, it adheres to various rollers, the conveyance belt 19 and the like to cause a problem. In order to avoid this, a resin having a viscosity smaller than that of the pressure-sensitive adhesive layer 41 is selected for the coat layer 51. The method of applying this resin will be described later.
- the label mount 50 is carried into the machine by the paper feed roller 11 and conveyed toward the standby roller pair 12.
- the standby roller pair 12 pauses its rotation and abuts the leading edge of the label mount 50 between the rollers. As a result, the label mount 50 stops its progress, and stands by until the conveyance timing comes.
- the printing unit 4 application of the developing bias to the developing roller 18 and application of the transfer bias to the transfer roller 21 are stopped (or a reverse potential bias is applied). Thereby, the printing function by the black toner by the printing unit 4 is stopped. Further, along with the stop of the printing function by the printing unit 4, the transport belt 19 is moved to the position shown by the broken line in FIG. 1 by the rotation mechanism. As a result, the conveyance surface of the conveyance belt 19 contacts only the photosensitive drum 13 of the label forming unit 3. In this state, in the label forming unit 3, the photosensitive drum 13 rotates in the clockwise direction.
- the initialization charger 15 applies uniform high negative charge to the circumferential surface of the photosensitive drum 13.
- the optical writing head 16 exposes the peripheral surface of the photosensitive drum 13 in accordance with the exposure signal to form a low potential portion.
- an electrostatic latent image composed of the high negative potential portion by initialization and the low negative potential portion by exposure is formed on the photosensitive drum 13.
- the powder supply roller 22 supplies the powdery label toner in such a manner as to be rubbed against the developing roller 18.
- the doctor blade 23 regulates the toner for label on the surface of the developing roller 18 to be a layer of a certain thickness.
- the label toner is charged to a weak negative potential due to friction and adheres to the surface of the developing roller 18.
- the developing roller 18 conveys the label toner attached in a layer of a certain thickness on the surface to the opposite portion to the photosensitive drum 13, that is, the developing portion while rotating.
- a development bias of “ ⁇ 250 V” is applied to the development roller 18 from a bias power supply. Further, the potential of the low potential portion of the electrostatic latent image of the photosensitive drum 13 is lowered to, for example, “ ⁇ 70 V” by exposure.
- a potential difference of “ ⁇ 180 V” is formed between the photosensitive drum 13 and the developing roller 18. That is, the low potential portion of the electrostatic latent image forms a positive potential relative to the developing roller 18. Due to the potential difference, the toner for label formation charged to the negative polarity is transferred to the negative low potential portion of the positive polarity of the electrostatic latent image of the photosensitive drum 13. Then, a solid image of a desired shape by the label forming toner is formed on the photosensitive drum 13. The solid image of the desired shape formed by the label forming toner is conveyed to the transfer portion where the photosensitive drum 13 and the transfer roller 21 face each other by the rotation of the photosensitive drum 13. At the timing when the front end of the solid image on the photosensitive drum 13 is rotationally conveyed to the opposing portion to the transfer roller 21, the label mount 50 is conveyed to the opposing portion.
- the transfer roller 21 applies the transfer current output from the transfer bias power supply to the label mount 50 via the transport belt 19. Thereby, the solid image of the label forming toner on the photosensitive drum 13 is transferred to the label mount 50.
- the label forming toner for example, polyester type toner described later can be used.
- FIG. 2B shows the next step of FIG. 2A, that is, a state in which the solid image 42 of the label forming toner is transferred to the surface of the pressure-sensitive adhesive layer 41 of the release sheet 40.
- the toner for label formation remaining on the photosensitive drum 13 without being transferred is removed from the circumferential surface of the photosensitive drum 13 by the cleaner 14. Thereafter, the residual toner is collected by the collection pipe 24 into the powder hopper 17.
- the label mount 50 to which the solid image 42 of the label forming toner has been transferred is carried into the fixing unit 6, heated by the heat generating roller 29, and pressed by the pressing roller 31. As a result, the solid image 42 of the label forming toner that has become a film-like label is fixed on the surface of the adhesive layer 41.
- the coat layer 51 is composed of a monomer or an oligomer, the coat layer 51 is located between the pressure-sensitive adhesive layer 41 and the film-like label 42 f and forms a copolymer with the film-like label 42 f. It functions as a dressing.
- FIG. 2C shows a state subsequent to FIG. 2B, that is, a state in which the solid image 42 of the label forming toner is fixed as a film-like label 42f on the surface of the adhesive layer 41 of the label mount 50.
- the label mount 50 on which the film-like label 42 f is fixed to the surface of the adhesive layer 41 is fed to the feed back mechanism 7 because the switching flap 35 is at the diagonally upward solid position.
- the label mount 50 fed to the feed back mechanism 7 is fed back to the standby roller pair 12 by the six feed back roller pairs 33 (33a to 33f) and the feed back guide paths 34 (34a to 34f). .
- the application of the developing bias to the developing roller 18 of the label forming unit 3 and the application of the transfer bias to the transfer roller 21 are stopped (or a bias of reverse potential is applied), and the forming function of the film-like label is stopped. Ru.
- the printing unit 4 application of the developing bias to the developing roller 18 and application of the transfer bias to the transfer roller 21 are started, and the printing function by black toner is activated. Further, with the start of the printing function, the transport belt 19 is moved to the printing position shown by the solid line in the figure by the rotation mechanism, and the transport surface of the transport belt 19 contacts the photosensitive drum 13 of the printing unit 4.
- the image of the desired print data by the black toner of the printing unit 4 is transferred to the surface of the film-like label 42f. Ru.
- the formation of the image on the film-like label 42f is not limited to the electrophotographic method as described above, and can be performed by an inkjet method.
- FIG. 2D shows the state in which the image 43 of desired print data with black toner is transferred to the film-like label 42f formed on the surface of the pressure-sensitive adhesive layer 41 of the release sheet 40, that is, the next step of FIG. It shows.
- the label mount 50 on which the image 43 of the desired print data with black toner is transferred onto the film-like label 42 f is conveyed to the fixing unit 6. Then, the image 43 of the print data is fixed on the film-like label 42 f by heating and pressure by the fixing unit 6.
- FIG. 2E shows the next step of FIG. 2D, that is, the state in which the image 43 of print data becomes the fixed image 43g on the film-like label 42f.
- the label mount 50 on which the fixed image 43 g is fixed is at the position of the switching flap 35 in the substantially horizontal dotted line position, so that the discharge tray 39 via the conveyance roller pair 36, the discharge guide path 37, and the discharge roller pair 38. It is discharged to the top.
- FIG. 2F shows the next step of FIG. 2E, that is, the state where the film-like label 42 f is peeled off from the release sheet 40.
- the film-like label 42 f is bound to the pressure-sensitive adhesive layer 41 immediately below by the binding force of the coat layer 51.
- the label shape followability is good, and the adhesive layer 41 having the same shape as the shape 42f of the formed label film can be peeled off.
- the binding strength of the coat layer will be described later.
- the portion of the pressure-sensitive adhesive layer 41 which has not been removed together with the film-like label 42f is a margin 41e.
- the image 43 of print data is formed on the film-like label 42f. It is also possible to reverse the order of printing and film formation for the label. In that case, first, an image 43 of print data is formed on the surface of the coat layer 51 of the label mount 50, and then a film-like label 42f is formed. In this case, the film for labels has high transparency.
- the coat layer of the above-mentioned label mount was provided for transportability in the label producing apparatus. From the viewpoint of transportability in the label producing apparatus, it is required that the viscosity of the substance forming the coating layer is low, the softening point is sufficiently high, and the heat resistance is excellent. Furthermore, this coating layer is required to be easily cut following the shape of the label (label shape following property) when the user peels the label from the label mount after the label production. If the coat layer can be made thin, the label shape followability is high, and an effect can be expected in the mount design. Moreover, it is preferable that this coat layer is a thing with the good binding property of the film for labels, and an adhesive layer, respectively. It is desirable that the label film, the coat layer, and the pressure-sensitive adhesive layer all come together and be neatly peeled off when peeling off the label film after use.
- a low viscosity emulsion dispersed in water by using a method such as dip coating or spray coating using an emulsion, and a coat with a thickness of several ⁇ m (for example, 1 to 5 ⁇ m) Layers can also be made.
- the method for producing a label mount in the present invention is A method for producing a label mount used as the mount in a label producing apparatus for fixing a toner for forming a label on a mount in a state of being transferred to a desired shape, An adhesive layer forming step of forming an adhesive layer on the release sheet; An emulsion adjusting step of adjusting an emulsion by dispersing, in water, a resin having a structure in common with a resin component constituting the label forming toner and / or a resin having a structure in common with a resin component constituting the adhesive; An emulsion applying step of applying the emulsion obtained in the emulsion adjusting step on the pressure-sensitive adhesive layer formed on the release sheet; And d) drying the emulsion applied in the emulsion application step.
- the emulsion refers to a dispersion solution in which both the dispersoid and the dispersion medium are liquid.
- water ion-exchanged water
- Emulsion preparation is accomplished by adding the dispersing medium (eg, water) with stirring to the desired concentration.
- the dispersing medium eg, water
- the dispersoids to be mixed in advance are volatilized to obtain a non-volatile component.
- a dispersion medium is added little by little while stirring to obtain an emulsion dispersion of a desired concentration.
- the resin which is a dispersoid uses a monomer or an oligomer.
- a monomer is a monomer and is a substance that becomes a substrate when polymerization is performed.
- Polymerization is a group of chemical reactions that synthesizes polymers.
- Oligomers refer to dimers, trimers, tetramers, etc.
- dip coating or spray application can be used.
- the drying step may be any of natural drying, forced drying by heat (hot air), and the like. In the case of natural drying, for example, it is dried overnight.
- FIGS. 3A to 3D are diagrams showing the steps of dip coating.
- An emulsion for example, water in which resin monomers or oligomers are dispersed
- a label mount a release sheet coated with a pressure-sensitive adhesive
- FIG. 3B it is pulled up. At this time, it pulls up while adjusting the force and velocity by the viscous force, surface tension and gravity in the liquid.
- the film thickness (h) is known to have a predetermined relationship with the viscosity constant ⁇ (eta), the pulling speed (u), the density of the liquid (d), the gravitational acceleration (g), etc.
- ⁇ viscosity constant
- u the pulling speed
- g the density of the liquid
- g gravitational acceleration
- the film thickness is adjusted while the film thickness is adjusted by surface tension.
- drying naturally drying or forced drying with heat
- the dispersion medium here, water
- a coat layer having a thickness of about 1 to 5 ⁇ m can also be provided by using a spray coating method instead of the dip coating method.
- the thickness of the coating layer can be adjusted by adjusting the nozzle shape, the ejection pressure, the density of the dispersion, the viscosity of the dispersion, the length of the ejection time, etc. It is.
- Coating an emulsion using dip coating or spray coating is significantly different from coating a resin solution using a coater or applicator in that it is a coating means that does not use an organic solvent. Since the organic solvent is generally highly volatile, the concentration (or density) may change significantly over time after adjusting the concentration. On the other hand, since the dispersion of the emulsion uses water, the change with time of those numerical values after adjusting the density and viscosity of the dispersion is relatively small. Moreover, when using water as a dispersion liquid, unlike using an organic solvent, there is an advantage that it is not necessary to collect a solvent (dispersion medium).
- the density, viscosity, pulling speed and the like of the dispersion are controlled. Further, even in the spray coating method, the thickness, viscosity, ejection pressure and the like of the dispersion liquid are controlled to obtain a predetermined coating layer thickness. Therefore, it is advantageous to obtain the desired coat layer thickness that the smaller the change with time of those values after adjusting the dispersion. It will be apparent in the examples described later that obtaining a desired coat layer thickness is an important element in terms of label shape followability and binding properties.
- the toner for forming a label of the present invention contains a resin as its main component, and optionally, a charge control agent, a wax and a pigment are added and kneaded, and the kneaded product is pulverized under liquid nitrogen, and the powder is pulverized. It is obtained, and silica particles etc. are added as an external additive, and it uses and stirs.
- the resin component is not particularly limited, and examples thereof include polyester resins such as polylactic acid and polybutylene succinic acid, acrylic resins, ionomer resins, cellulose resins, polycarbonate resins, epoxy resins, epoxy resins, polyethylene resins, polypropylene resins, butadiene resins, Polybutylene resin, polystyrene resin, cyclic polyolefin resin, vinyl acetate resin, nitrile resin, polyacetal resin, phenol resin, polyamide resin, polyamide resin, polyimide resin, polyether resin, polyurethane resin, furan resin, polyketone resin, polyvinylidene resin, silicone resin, polyvinyl Alcohol resin, polyvinyl acetate resin, urea resin, melamine resin, polyallyl sulfone resin, xylene resin, various substituted resins of the above resins, or copolymers of monomers of the above resins Any such a combination of single or plural kinds may be used. However, good results are obtained
- a peeling sheet is paper (or resin on a sheet
- the coat layer is a layer of resin covering the top of the pressure-sensitive adhesive layer, and has a structure common to the resin component constituting the label forming toner and / or a resin common to the resin component constituting the pressure-sensitive adhesive. And.
- the thickness of the coat layer is preferably 1 to 5 ⁇ m. When it is too thick, the label shape following property (the adhesive layer peels off integrally as the label shape when the user peels the release sheet to use the label) is deteriorated.
- the resin used for the coat layer is preferably made of a resin having a structure in common with either or both of the resin contained in the label forming toner and the resin contained in the pressure-sensitive adhesive layer. This is to improve the bondability and the label shape followability.
- a polymer is partially formed between the resin contained in the toner for label formation and the resin contained in the adhesive layer. Or functions as a binder by forming a copolymer.
- resin which has a common structure means that the chemical structure is common (for example, frame is common).
- polyester resins have a common structure. The same applies to acrylic resins.
- the coating layer is required to have a strong bonding force with the label substrate (the substrate of the film-like label 42f) and the pressure-sensitive adhesive.
- the coat layer of the label mount becomes a binding layer of the label base and the adhesive. That is, the bonding strength of the coated layer to the label substrate and the adhesive affects the strength of the label. If the bonding strength is poor, only the label substrate (film-like label 42f) or only the label substrate and the coating layer may be peeled off when the label is attached and re-peeled off.
- the binding force provided by the coating layer also provides the label shape followability.
- the binding strength between the film-like label and the coating layer is exerted only in the label forming area. Therefore, the cohesion does not function in the margin other than the label forming area. Therefore, the user can peel off the label from the release sheet by following the shape of the label.
- a polyester resin for example, polybutylene succinic acid
- an acrylic adhesive for example, a pressure sensitive adhesive SK Dyne 1811 L made by Soken Chemical Co., Ltd.
- a TD- 75 a TD- 75
- the label property binding property, label shape following property
- a polyester-based resin monomer or oligomer is used as a constituent material of the coating layer, the binding property with the label base material after heat-fixing of the label forming toner is good.
- the binding strength with the acrylic pressure sensitive adhesive is excellent.
- the base sheet has excellent properties such as abrasion resistance, and by selecting a resin having a high softening point, the heat resistance is also excellent.
- a resin of the same system as the resin used as the label substrate (a resin having a common structure or skeleton) and a resin of the same system as the resin used as the adhesive are selected.
- the use of a mixture of the following in the coating layer results in strong binding.
- the bonding strength is polymerized at least in part between the resin forming the label base material and the resin forming the coating layer, and the resin forming the coating layer and the resin forming the pressure-sensitive adhesive layer when fixing the label toner. It is believed that this occurs as a result of the formation of a copolymer.
- the resin which forms a coating layer is good with combined use of a polyester resin and an acrylic resin. That is, these two resins are mixed and used.
- the mixing ratio may be 1: 9 to 9: 1 by mass ratio of non-volatile components. It is for the bondability and the label shape followability. Furthermore, 3: 7 to 7: 3 are more desirable. It is because the binding property was more remarkable.
- the mass of the non volatile component volatilized the solvent naturally over 2 hours, and measured it with the upper balance balance. The resin whose mass has been measured is further dispersed in water and dissolved as an emulsion for use.
- polybutylene succinic acid is used for the toner
- an acrylic adhesive is used for the adhesive layer
- a polyester emulsion and an acrylic resin emulsion are mixed for the coat layer.
- ⁇ Method of measuring each physical property value in the example >> The measuring method of each physical property value is shown.
- ⁇ Measurement of softening point Device Flow tester (made by Shimadzu, CFT-500D) Sample: 1 g Heating rate: 6 ° C / min Load: 20kg Nozzle: diameter 1 mm, length 1 mm Method 1/2: The temperature at which half of the sample flowed out was taken as the softening point.
- Measurement of toner particle size Device FPIA-2100 (made by Sysmex Corporation) Sample: A small amount of sample, purified water and surfactant were placed in a beaker and dispersed by an ultrasonic cleaner. Measurement: Volume average particle size was obtained.
- Preparation of label mounts >> -Preparation example 1 100 parts by mass of a pressure-sensitive adhesive SK dyne 181L manufactured by Soken Chemical Co., Ltd., which is an acrylic adhesive, and 0.2 parts by mass of a curing agent TD-75 manufactured by Soken Chemical Co., Ltd. were mixed and stirred at room temperature for 2 hours. The mixture was applied onto a separator (release sheet) using an applicator and subjected to an aging treatment at 100 ° C. for 2 minutes. Polyester emulsion; an emulsion dispersion was prepared by diluting Erichel KZT-8803 manufactured by Unitika with an ion-exchanged water four times at room temperature.
- the emulsion dispersion was filled in a stainless vat of a size sufficient to dip the entire A4 size, and the adhesive surface side of the backing coated with the above-mentioned adhesive was immersed therein. After slowly pulling it out, it was dried overnight at room temperature to obtain a backing 1.
- the size of the obtained backing sheet 1 is A4 size (width 210 mm, length 297 mm).
- the thickness of the pressure-sensitive adhesive was 6 ⁇ m, and the thickness of the coating layer was 4 to 5 ⁇ m.
- the mixing ratio is a mass ratio of non-volatile components, that is, solid components.
- -Preparation example 2 As the emulsion, a mixture of polyester emulsion; Eritel KZT-8803 and acrylic resin emulsion; 9: 1 (non-volatile content ratio) of Mitsui Chemicals Sumitomo Chemical's Barrier Star B-3000 was used, and the same procedure as in Preparation Example 1 was carried out, Was produced.
- -Preparation example 3 The same procedure as in Preparation Example 1 was repeated, except that a mixture of polyester emulsion; Eritel KZT-8803 and acrylic resin emulsion; barrier star B-3000 7: 2 (nonvolatile content ratio) was used as the emulsion. Was produced.
- -Preparation example 4 The same procedure as in Preparation Example 1 was repeated, except that a polyester emulsion; Eritel KZT-8803 and an acrylic resin emulsion; and a 5: 5 (non-volatile content ratio) mixture of Mitsui Star KZT 8803 and Acrylic resin; Was produced.
- Preparation Example 6 The same procedure as in Preparation Example 1 was repeated, except that a mixture of polyester emulsion; Eritel KZT-8803 and acrylic resin emulsion; 1: 9 (non-volatile content ratio) of Mitsui Star K-ZT 8803, and Mitsui Chemicals Chemical Barrier Star B-3000, was used as the emulsion.
- Preparation Example 7 A base paper 7 was produced in the same manner as in Production Example 1 except that an acrylic resin emulsion; Varistar B-3000 manufactured by Mitsui Chemicals, Inc. was used as the emulsion.
- Preparation Example 8 Acrylic resin emulsion as emulsion; using calcium carbonate particles ⁇ -powder 3N manufactured by Shiroishi Calcium Co., Ltd. as additive particles in an amount of 2 times the mass ratio of non-volatile matter in the emulsion
- a label mount 8 was produced in the same manner as in Production Example 1.
- -Preparation example 9 BASF polyester resin Ecoflex FB-XF7011 was dissolved in THF (TetraHydroFuran: tetrohydrofuran) to prepare a 10% solution. The resin solution was applied onto a separator using an applicator to obtain a resin layer having a thickness of 10 ⁇ m. The obtained resin layer was attached to the pressure-sensitive adhesive layer produced in the same manner as in Production Example 1 to produce a backing sheet 9.
- Preparation Example 10 After producing a first coated layer with an acrylic emulsion on the pressure-sensitive adhesive layer, a second coated layer was produced in a polyester emulsion to obtain a laminated structure. The other conditions were the same as in Production Example 1 to produce a backing sheet 10. The polyester emulsion is used as a stock solution, and the acrylic emulsion is diluted four times with ion-exchanged water, which is common to Preparation Examples 1 to 7 and Preparation Example 10.
- -Preparation example 11 The polyester emulsion was used as a stock solution, and the acrylic emulsion was diluted twice with ion-exchanged water. The other conditions were the same as in Production Example 1 to produce a backing sheet 11.
- -Preparation example 12 The polyester emulsion was used as a stock solution, and the acrylic emulsion was diluted 1.5 times with deionized water. The other conditions were the same as in Production Example 1 to produce a backing sheet 12.
- Preparation Example 13 Both polyester emulsions and acrylic emulsions were used as stock solutions. The other conditions were the same as in Production Example 1 to produce a backing sheet 13.
- Synthesis of Polybutylene Succinic Acid Preparation for Production of Label Forming Toner >> ⁇ Synthesis example 1 5 parts by mass of an 88% aqueous solution of lactic acid in which 0.4 parts by mass of malic acid and 1 part by mass of germanium dioxide were dissolved with respect to 100 parts by mass of succinic acid and 89 parts by mass of 1,4-butanediol.
- the reaction system was changed to a nitrogen atmosphere, reacted at 220 ° C. for 1 hour, and then decompressed to 70 pa over 1.5 hours while raising the temperature to 230 ° C.
- the polymerization was allowed to proceed for another 2 hours to obtain polybutylene succinic acid.
- Toner production example 1 96.5 parts by mass of polybutylenesuccinic acid obtained in Synthesis Example 1 and 1 part by mass of Carnalyzer LR-147 as a charge control material and 2.5 parts by mass of carnauba wax (made by Yoko Yoko) are mixed, and 2 It knead
- the kneaded material was pulverized in a phosphorus rex mill manufactured by Hosokawa Micron under liquid nitrogen to obtain a powder of D50 (volume) of 37 ⁇ m.
- Example 1 Toner 1 as a label base material is developed on A4 size label mount 1 (preparation example 1) by an electrophotographic process, and the label mount 1 having the toner developed is passed through a 180 ° C. heat roll to make the label mount A film-like label having a thickness of 80 ⁇ m was obtained on 1 (Preparation Example 1). Thereafter, the image was developed / fixed on a film-like label by a Casio Computer N5300 printer.
- Examples 2 to 7, Examples 8 to 10, Comparative Example 3 Labels were produced in the same manner as in Example 1 using label mounts 2 to 7 (preparation examples 2 to 7) and label mounts 10 to 13 (production examples 10 to 13).
- Example 1 in which the constituent material is only polyester, the adhesive slightly remained on the SUS plate when the label was peeled off from the SUS plate. That is, this means that the adhesion between the adhesive and the coating layer is slightly weak. Further, in Examples 6 and 7 in which the content of the acrylic resin is high, the adhesive and the coat layer remained on the SUS plate similarly. That is, it means that the bond between the coat layer and the label is weak. In Comparative Example 1 in which calcium carbonate was added as a filler to the coating layer, the label and the adhesive layer were peeled off inside the coating layer when peeling off from the SUS plate.
- the comparative example 2 which produced the coating layer by the application by an applicator from the solution of polyester resin was obviously inferior in the tear-following property to a label.
- stock solution of the acrylic emulsion as it was was inferior in the tear-following property to a label.
Landscapes
- Physics & Mathematics (AREA)
- General Physics & Mathematics (AREA)
- Engineering & Computer Science (AREA)
- Theoretical Computer Science (AREA)
- Making Paper Articles (AREA)
- Fixing For Electrophotography (AREA)
Priority Applications (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| US14/889,539 US20160086519A1 (en) | 2013-09-20 | 2014-07-10 | Label substrate and method for producing label and label substrate |
| CN201480033041.9A CN105308665A (zh) | 2013-09-20 | 2014-07-10 | 标签衬纸、标签及标签衬纸的制造方法 |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2013195154A JP6167793B2 (ja) | 2013-09-20 | 2013-09-20 | ラベル台紙、ラベル、ラベル台紙の製造方法およびラベルの作製方法 |
| JP2013-195154 | 2013-09-20 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2015040936A1 true WO2015040936A1 (ja) | 2015-03-26 |
Family
ID=52688596
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2014/068440 Ceased WO2015040936A1 (ja) | 2013-09-20 | 2014-07-10 | ラベル台紙、ラベルおよびラベル台紙の製造方法 |
Country Status (4)
| Country | Link |
|---|---|
| US (1) | US20160086519A1 (enExample) |
| JP (1) | JP6167793B2 (enExample) |
| CN (1) | CN105308665A (enExample) |
| WO (1) | WO2015040936A1 (enExample) |
Families Citing this family (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN112590386B (zh) * | 2020-12-24 | 2022-06-21 | 湖南恒创新材料有限公司 | 一种防水不干胶标签制备覆膜加工处理系统 |
Citations (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH11174959A (ja) * | 1997-12-15 | 1999-07-02 | Nitto Denko Corp | ラベル基材、ラベル及びその製造方法と製造装置 |
| JP2001341264A (ja) * | 2000-06-05 | 2001-12-11 | Toyobo Co Ltd | ポリエステル系被覆フィルム |
| JP2002169470A (ja) * | 2000-11-27 | 2002-06-14 | Three M Innovative Properties Co | 印刷表示シートおよび印刷表示体 |
| JP2005345793A (ja) * | 2004-06-03 | 2005-12-15 | Fuji Seal International Inc | つや消し用コーティング剤、プラスチックラベル及びラベル付き容器 |
| JP2010184470A (ja) * | 2009-02-13 | 2010-08-26 | Casio Electronics Co Ltd | ラベル作製方法、ラベル作製装置、及びラベル用トナー |
Family Cites Families (3)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US4216283A (en) * | 1977-05-23 | 1980-08-05 | Ani-Live Film Service Inc. | Dry transfer of electrophotographic images |
| US7105225B2 (en) * | 2001-10-05 | 2006-09-12 | 3M Innovative Properties Company | Water contract indicator |
| WO2005023953A1 (ja) * | 2003-08-28 | 2005-03-17 | Yushi-Seihin Co., Ltd. | 高温貼り付け可能な耐熱ラベル |
-
2013
- 2013-09-20 JP JP2013195154A patent/JP6167793B2/ja not_active Expired - Fee Related
-
2014
- 2014-07-10 WO PCT/JP2014/068440 patent/WO2015040936A1/ja not_active Ceased
- 2014-07-10 CN CN201480033041.9A patent/CN105308665A/zh not_active Withdrawn
- 2014-07-10 US US14/889,539 patent/US20160086519A1/en not_active Abandoned
Patent Citations (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH11174959A (ja) * | 1997-12-15 | 1999-07-02 | Nitto Denko Corp | ラベル基材、ラベル及びその製造方法と製造装置 |
| JP2001341264A (ja) * | 2000-06-05 | 2001-12-11 | Toyobo Co Ltd | ポリエステル系被覆フィルム |
| JP2002169470A (ja) * | 2000-11-27 | 2002-06-14 | Three M Innovative Properties Co | 印刷表示シートおよび印刷表示体 |
| JP2005345793A (ja) * | 2004-06-03 | 2005-12-15 | Fuji Seal International Inc | つや消し用コーティング剤、プラスチックラベル及びラベル付き容器 |
| JP2010184470A (ja) * | 2009-02-13 | 2010-08-26 | Casio Electronics Co Ltd | ラベル作製方法、ラベル作製装置、及びラベル用トナー |
Also Published As
| Publication number | Publication date |
|---|---|
| CN105308665A (zh) | 2016-02-03 |
| JP2015060152A (ja) | 2015-03-30 |
| JP6167793B2 (ja) | 2017-07-26 |
| US20160086519A1 (en) | 2016-03-24 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP4765810B2 (ja) | ラベル作成方法及び装置 | |
| JP6044121B2 (ja) | 画像転写シート、および画像記録体 | |
| US10828923B2 (en) | Pressure-printed material preparing apparatus | |
| JP5472409B2 (ja) | ラベル基材用組成物、ラベル基材、ラベル、及びそれらの製造方法 | |
| JP5287877B2 (ja) | ラベル作製方法及びラベル作製装置 | |
| JP6167793B2 (ja) | ラベル台紙、ラベル、ラベル台紙の製造方法およびラベルの作製方法 | |
| JP5163674B2 (ja) | シート作成方法及びシート作成装置 | |
| JP5509580B2 (ja) | 画像転写シート、画像記録体および画像記録体の作製方法 | |
| JP4685900B2 (ja) | 剥離部材、剥離部材の製造方法、画像除去装置、画像除去方法、画像形成・除去システム、及び画像形成・除去システムの画像除去方法 | |
| JP6593204B2 (ja) | 貼付ラベル、及び貼合せ物 | |
| KR101525307B1 (ko) | 중간 전사 매체 및 위변조 방지 매체 작성 장치 | |
| CN103034080B (zh) | 标签基材用组合物、标签基材的制作方法及标签 | |
| JP5477439B2 (ja) | ラベル作製方法およびラベル作製装置 | |
| JP2016068292A (ja) | 再剥離性粘着シート製造用の画像転写シート、再剥離性粘着シート製造用の画像記録シート、再剥離性粘着シート、画像記録シートの製造方法および再剥離性粘着シートの製造方法 | |
| US20160176214A1 (en) | Toner for thermal transfer printing sheet, thermal transfer printing sheet, and production method thereof | |
| JP2015184507A (ja) | フイルム形成用電子写真トナー | |
| JP2018034309A (ja) | 記録媒体の再生方法および記録媒体再生装置 | |
| JP2017062323A (ja) | 画像形成装置及び画像形成方法 | |
| JP2010078992A (ja) | 電子写真用の画像転写シート、画像記録体の作製方法および画像記録体 | |
| US20140295120A1 (en) | Label mount, label with mount, and production method thereof | |
| JP5473361B2 (ja) | 電子写真用弾性ローラの製造方法 | |
| CN105579224A (zh) | 带衬纸标签的制造方法、带衬纸标签及标签衬纸 | |
| JP2006123422A (ja) | ラミネート用部材 | |
| JP2015036792A (ja) | 電子写真用画像転写シート、画像記録体、および画像記録体の製造方法 | |
| JP2008068505A (ja) | 圧着はがき作成装置 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| WWE | Wipo information: entry into national phase |
Ref document number: 201480033041.9 Country of ref document: CN |
|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 14846297 Country of ref document: EP Kind code of ref document: A1 |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 14889539 Country of ref document: US |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| 122 | Ep: pct application non-entry in european phase |
Ref document number: 14846297 Country of ref document: EP Kind code of ref document: A1 |