WO2013061739A1 - 熱電変換複合材料、それを用いた熱電変換材料ペースト、およびそれを用いた熱電変換モジュール - Google Patents

熱電変換複合材料、それを用いた熱電変換材料ペースト、およびそれを用いた熱電変換モジュール Download PDF

Info

Publication number
WO2013061739A1
WO2013061739A1 PCT/JP2012/075593 JP2012075593W WO2013061739A1 WO 2013061739 A1 WO2013061739 A1 WO 2013061739A1 JP 2012075593 W JP2012075593 W JP 2012075593W WO 2013061739 A1 WO2013061739 A1 WO 2013061739A1
Authority
WO
WIPO (PCT)
Prior art keywords
thermoelectric conversion
semiconductor
glass
oxide
composite material
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2012/075593
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
正 藤枝
沢井 裕一
内藤 孝
拓也 青柳
山本 浩貴
秀明 鷹野
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Hitachi Ltd
Original Assignee
Hitachi Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Hitachi Ltd filed Critical Hitachi Ltd
Publication of WO2013061739A1 publication Critical patent/WO2013061739A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Images

Classifications

    • H—ELECTRICITY
    • H02—GENERATION; CONVERSION OR DISTRIBUTION OF ELECTRIC POWER
    • H02S—GENERATION OF ELECTRIC POWER BY CONVERSION OF INFRARED RADIATION, VISIBLE LIGHT OR ULTRAVIOLET LIGHT, e.g. USING PHOTOVOLTAIC [PV] MODULES
    • H02S40/00—Components or accessories in combination with PV modules, not provided for in groups H02S10/00 - H02S30/00
    • H02S40/40—Thermal components
    • H02S40/44—Means to utilise heat energy, e.g. hybrid systems producing warm water and electricity at the same time
    • C—CHEMISTRY; METALLURGY
    • C03—GLASS; MINERAL OR SLAG WOOL
    • C03C—CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS
    • C03C3/00—Glass compositions
    • C03C3/12—Silica-free oxide glass compositions
    • C03C3/122—Silica-free oxide glass compositions containing oxides of As, Sb, Bi, Mo, W, V, Te as glass formers
    • C—CHEMISTRY; METALLURGY
    • C03—GLASS; MINERAL OR SLAG WOOL
    • C03C—CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS
    • C03C3/00—Glass compositions
    • C03C3/12—Silica-free oxide glass compositions
    • C03C3/16—Silica-free oxide glass compositions containing phosphorus
    • C03C3/21—Silica-free oxide glass compositions containing phosphorus containing titanium, zirconium, vanadium, tungsten or molybdenum
    • C—CHEMISTRY; METALLURGY
    • C03—GLASS; MINERAL OR SLAG WOOL
    • C03C—CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS
    • C03C8/00—Enamels; Glazes; Fusion seal compositions being frit compositions having non-frit additions
    • C03C8/02—Frit compositions, i.e. in a powdered or comminuted form
    • C03C8/08—Frit compositions, i.e. in a powdered or comminuted form containing phosphorus
    • C—CHEMISTRY; METALLURGY
    • C03—GLASS; MINERAL OR SLAG WOOL
    • C03C—CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS
    • C03C8/00—Enamels; Glazes; Fusion seal compositions being frit compositions having non-frit additions
    • C03C8/14—Glass frit mixtures having non-frit additions, e.g. opacifiers, colorants, mill-additions
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10N—ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10N10/00—Thermoelectric devices comprising a junction of dissimilar materials, i.e. devices exhibiting Seebeck or Peltier effects
    • H10N10/01—Manufacture or treatment
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10N—ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10N10/00—Thermoelectric devices comprising a junction of dissimilar materials, i.e. devices exhibiting Seebeck or Peltier effects
    • H10N10/10—Thermoelectric devices comprising a junction of dissimilar materials, i.e. devices exhibiting Seebeck or Peltier effects operating with only the Peltier or Seebeck effects
    • H10N10/17—Thermoelectric devices comprising a junction of dissimilar materials, i.e. devices exhibiting Seebeck or Peltier effects operating with only the Peltier or Seebeck effects characterised by the structure or configuration of the cell or thermocouple forming the device
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10N—ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10N10/00—Thermoelectric devices comprising a junction of dissimilar materials, i.e. devices exhibiting Seebeck or Peltier effects
    • H10N10/80—Constructional details
    • H10N10/85—Thermoelectric active materials
    • H10N10/851—Thermoelectric active materials comprising inorganic compositions
    • H10N10/852—Thermoelectric active materials comprising inorganic compositions comprising tellurium, selenium or sulfur
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10N—ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10N10/00—Thermoelectric devices comprising a junction of dissimilar materials, i.e. devices exhibiting Seebeck or Peltier effects
    • H10N10/80—Constructional details
    • H10N10/85—Thermoelectric active materials
    • H10N10/851—Thermoelectric active materials comprising inorganic compositions
    • H10N10/855—Thermoelectric active materials comprising inorganic compositions comprising compounds containing boron, carbon, oxygen or nitrogen
    • Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y02—TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
    • Y02E—REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION
    • Y02E10/00—Energy generation through renewable energy sources
    • Y02E10/50—Photovoltaic [PV] energy
    • Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y02—TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
    • Y02E—REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION
    • Y02E10/00—Energy generation through renewable energy sources
    • Y02E10/60—Thermal-PV hybrids

Definitions

  • the present invention relates to a thermoelectric conversion material, and in particular, a thermoelectric conversion composite material in which a semiconductor thermoelectric conversion material and semiconductor glass are combined, a thermoelectric conversion material paste using the composite material, and a thermoelectric manufactured using the composite material. It concerns the conversion module.
  • Thermoelectric conversion materials are used as power generation elements and cooling elements because they exhibit the property of generating electricity when given a temperature difference (Seebeck effect) and conversely cooling when electricity flows (Peltier effect). Since the former property can directly convert heat into electricity, power generation using exhaust heat is possible, which is expected as one of clean energy technologies.
  • thermoelectric conversion materials Bi-Te materials, Bi-Sb materials, Bi-Te-Sb materials, etc. are known as thermoelectric conversion materials. Since the electromotive force due to the Seebeck effect is proportional to the temperature difference between the high-temperature part and the low-temperature part of the thermoelectric conversion element, a conventional thermoelectric conversion module must use a bulk-type thermoelectric conversion element to increase the temperature difference. There were many. However, the bulk-type thermoelectric conversion element has a problem in that microfabrication is not easy and the output density is low and the power generation unit price of the module is high. Therefore, development of a thermoelectric conversion element and a thermoelectric conversion module with high output density at low cost is strongly desired.
  • Patent Document 1 discloses ceramic thermoelectric conversion material particles having a diameter of 2 to 3 ⁇ m, ceramic thermoelectric conversion material particles having a diameter of 200 ⁇ m or less, and metal oxide fine particles as a binder.
  • a thermoelectric conversion element in which a paste composed of a solvent is formed by screen printing is disclosed. According to Patent Document 1, it is said that a highly efficient thermoelectric conversion element can be provided with good sinterability.
  • Patent Document 2 discloses a thermoelectric material in which an organic thermoelectric material and an inorganic thermoelectric material are integrated in a dispersed state, and the organic thermoelectric material is polyaniline or a derivative thereof, polypyrrole or a derivative thereof, polythiophene or a derivative thereof.
  • the inorganic thermoelectric material is Bi- (Te, Se) -based, Si-Ge-based, Pb-Te-based,
  • a thermoelectric material that is at least one selected from GeTe—AgSbTe, (Co, Ir, Ru) —Sb, and (Ca, Sr, Bi) Co 2 O 5 is disclosed.
  • an organic thermoelectric conversion material and an inorganic thermoelectric conversion material are hybridized to have both the workability of the organic thermoelectric conversion material and the thermoelectric characteristics of the inorganic thermoelectric conversion material, and according to the characteristics of the inorganic thermoelectric conversion material. It is said that a novel thermoelectric material capable of obtaining n-type thermoelectric characteristics can be provided.
  • Non-Patent Document 1 discloses a thin-film thermoelectric conversion module manufactured by using a semiconductor process such as a sputtering method. According to Non-Patent Document 1, by using a semiconductor process, for example, a thermoelectric conversion module having 540 35 ⁇ m square thermocouples on a 3.3 mm square chip of a silicon wafer can be manufactured. By using the thermoelectric conversion module, power generation using waste heat becomes possible, and a batteryless wireless sensor module is realized.
  • thermoelectric conversion material and the thermoelectric conversion element described in Patent Document 1 and Patent Document 2 can be used in a simple manufacturing process such as screen printing or coating by making the thermoelectric conversion material into a paste or liquid and have a desired pattern. A thick film can be formed easily (ie, at a low manufacturing cost).
  • the thermoelectric conversion material and the thermoelectric conversion element of Patent Document 1 use metal oxide fine particles as a binder of the inorganic thermoelectric conversion material, and the metal oxide fine particles do not have a thermoelectric conversion function. There was a problem that the thermoelectric conversion performance of was hindered. Further, the thermoelectric conversion material of Patent Document 2 has a problem in that the thermoelectric conversion performance as a whole is hindered because the thermoelectric conversion characteristics of the organic thermoelectric conversion material to be dispersed and mixed (hybridized) are low. .
  • thermoelectric conversion module described in Non-Patent Document 1 has a fine pattern and a dense film is formed, the element density per unit area of the module is high and the output (electromotive force) is high. It is expected to be obtained.
  • a thin film it is essentially difficult to take a temperature difference between the front and back surfaces of the element (the front and back surfaces of the module), and a very large cooling member (for example, a cooling fin) is used to create the temperature difference. I need. For this reason, there is a problem that the thermoelectric conversion module is enlarged as a whole.
  • a semiconductor process vacuum process
  • the manufacturing apparatus cost is high and the module price is high.
  • an object of the present invention is to provide a thermoelectric conversion composite material capable of producing a thermoelectric conversion element having high characteristics even using a low-cost process, and a thermoelectric conversion material paste using the composite material. It is another object of the present invention to provide a low-cost and highly efficient thermoelectric conversion module using the composite material.
  • thermoelectric conversion composite material in which a semiconductor thermoelectric conversion material and a binder are combined in order to achieve the above object, wherein the binder has the same polarity as the semiconductor thermoelectric conversion material.
  • the semiconductor glass is a lead-free glass containing vanadium oxide when the component is expressed by an oxide and having a softening point of 480 ° C. or lower.
  • “Lead-free” in the present invention refers to a prohibited substance (lead) in the RoHS Directive (Directive by the European Union (EU) on restrictions on the use of specific hazardous substances in electronic and electrical equipment, effective July 1, 2006). It shall be allowed to contain in the range below the specified value. The definition of the softening point of glass will be described later.
  • the present invention can be improved or changed as follows in the thermoelectric conversion composite material according to the present invention.
  • the concentration of pentavalent vanadium ions and the concentration of tetravalent vanadium ions are different.
  • the ratio of “pentavalent vanadium ion concentration: [V 5+ ]” to “tetravalent vanadium ion concentration: [V 4+ ]” is not “1” ([V 5+ ] / [V 4+ ] ⁇ 1).
  • the “valence and concentration of vanadium ion” in the present invention is defined as the valence and concentration measured by quantitative analysis by oxidation-reduction titration method based on JIS G1221.
  • the semiconductor glass further contains tellurium dioxide and / or diphosphorus pentoxide when the component is represented by an oxide, and when all of the vanadium oxide is converted into divanadium pentoxide, The total compounding ratio of vanadium (V 2 O 5 ), the tellurium dioxide (TeO 2 ) and the diphosphorus pentoxide (P 2 O 5 ) is 60% by mass or more.
  • the semiconductor thermoelectric conversion material is p-type, and the semiconductor glass has diarsenic trioxide (As 2 O 3 ), iron (III) oxide (Fe 2 O 3 ) when the component is expressed by an oxide.
  • the semiconductor thermoelectric conversion material is n-type, and the semiconductor glass has silver oxide (I) (Ag 2 O), copper oxide (II) (CuO), alkali when the component is represented by an oxide. It further contains at least one of a metal oxide and an alkaline earth metal oxide.
  • the compounding ratio of the semiconductor glass is 10 to 50% by volume.
  • the semiconductor thermoelectric conversion material is a Bi- (Te, Se, Sn, Sb) material, Pb-Te material, Zn-Sb material, Mg-Si material, Si-Ge material, GeTe- At least one selected from AgSbTe materials, (Co, Ir, Ru) -Sb materials, (Ca, Sr, Bi) Co 2 O 5 materials, Fe-Si materials, and Fe-V-Al materials It is.
  • the thermoelectric conversion material paste according to the present invention includes the above-described thermoelectric conversion composite material and a solvent.
  • thermoelectric conversion material paste according to the present invention the solvent is butyl carbitol acetate or ⁇ -terpineol, and further contains ethyl cellulose or nitrocellulose as a resin binder.
  • the thermoelectric conversion element according to the present invention is made of the above-described thermoelectric conversion composite material, and at least a part of the semiconductor glass is crystallized.
  • the thermoelectric conversion element is defined as a semiconductor thermoelectric conversion material formed into a desired shape and size and fired (sintered).
  • the crystallized portion is a vanadium complex oxide crystal.
  • thermoelectric conversion module includes a substrate, a plurality of thermoelectric conversion elements arranged on the substrate, and a plurality of thermoelectric conversion elements formed on the substrate and adjacent to each other.
  • the thermoelectric conversion element is a thermoelectric conversion element made of the above-described thermoelectric conversion composite material, and is electrically connected in series so that the polarities of the adjacent thermoelectric conversion elements are alternated.
  • the thermoelectric conversion module is defined as a plurality of thermoelectric conversion elements electrically connected.
  • thermoelectric conversion composite material capable of producing a thermoelectric conversion element having high characteristics even using a low-cost process
  • thermoelectric conversion material paste using the composite material. Furthermore, by using the composite material, a low-cost and high-efficiency thermoelectric conversion module can be provided.
  • thermoelectric conversion module which concerns on this invention.
  • thermoelectric conversion module which concerns on this invention.
  • thermoelectric conversion module which concerns on this invention.
  • thermoelectric conversion module which concerns on this invention.
  • thermoelectric conversion module which concerns on this invention.
  • thermoelectric conversion module which concerns on this invention.
  • thermoelectric conversion module which concerns on this invention.
  • thermoelectric conversion module which concerns on this invention.
  • thermoelectric conversion module which concerns on this invention.
  • thermoelectric conversion module which concerns on this invention.
  • solar energy / solar heat combined power generation system using the thermoelectric conversion module according to the present invention It is a cross-sectional schematic diagram which shows the measuring method of the conversion efficiency of a thermoelectric conversion module.
  • thermoelectric conversion materials that enable the production of thermoelectric conversion elements that are more efficient than conventional methods even using low-cost processes such as screen printing and coating
  • present inventors have newly developed semiconductor thermoelectric conversion materials and new ones. It has been found that the above-described object can be achieved by compounding with a semiconductor glass.
  • thermoelectric conversion composite material As described above, the thermoelectric conversion composite material according to the present invention is obtained by compounding a semiconductor thermoelectric conversion material with a semiconductor glass having the same polarity as the semiconductor thermoelectric conversion material, and the semiconductor glass oxidizes components. It is a lead-free glass containing vanadium oxide and having a softening point of 480 ° C. or lower. More specifically, the semiconductor glass used in the present invention further contains and contains tellurium dioxide (TeO 2 ) and / or diphosphorus pentoxide (P 2 O 5 ) when the component is represented by an oxide. When all vanadium oxides are converted as divanadium pentoxide (V 2 O 5 ), the total blending ratio of divanadium pentoxide, tellurium dioxide and diphosphorus pentoxide is 60% by mass or more.
  • the semiconductor glass of the present invention becomes both a p-type semiconductor and an n-type semiconductor by adjusting the valence balance of vanadium ions in the glass.
  • the ratio of “pentavalent vanadium ion concentration: [V 4+ ]” to “pentavalent vanadium ion concentration: [V 5+ ]” is smaller than “1” ([V 5+ ] / [V 4+ ] ⁇ 1) is a p-type semiconductor, and if it is greater than “1” ([V 5+ ] / [V 4+ ]> 1), it is an n-type semiconductor.
  • the semiconductor glass By making the polarity of the semiconductor glass the same as that of the semiconductor thermoelectric conversion material, the semiconductor glass can be compounded without impairing the thermoelectric conversion characteristics as a whole.
  • the “valence and concentration of vanadium ions” can be measured by quantitative analysis by a redox titration method based on JIS G1221. Further, the conductivity of the semiconductor glass in an amorphous state is about 10 ⁇ 2 to 10 ⁇ 6 S / m.
  • the polarity (that is, [V 5+ ] / [V 4+ ]) of the semiconductor glass of the present invention can be controlled by an additive element.
  • an element having an effect of reducing divanadium pentoxide (V 2 O 5 ) may be added.
  • diarsenic trioxide As 2 O 3
  • iron (III) oxide Fe 2 O 3
  • antimony trioxide Sb 2 O 3
  • bismuth oxide At least one or more of (III) (Bi 2 O 3 ), tungsten trioxide (WO 3 ), molybdenum trioxide (MoO 3 ), and manganese oxide (MnO) may be added.
  • the polarity of the semiconductor glass is n-type ([V 5+ ] / [V 4+ ]> 1)
  • the component is represented by an oxide
  • the addition of these elements not only controls the polarity of the semiconductor glass but also has an effect of strengthening the glass structure (an effect of increasing the stability of the glass) and an effect of improving the water resistance.
  • the semiconductor glass used in the present invention is characterized by a low softening point of 480 ° C. or lower.
  • a low softening point of 480 ° C. or lower.
  • firing can be performed at a temperature lower than the sintering temperature of thermoelectric conversion materials in conventional bulk thermoelectric conversion elements (for example, 600 to 650 ° C for Bi-Te materials). It becomes possible.
  • Lowering the calcination temperature in addition to reducing the energy cost required for calcination, suppresses unwanted chemical reactions and thus prevents degradation of thermoelectric conversion characteristics.
  • FIG. 1 is an example of a chart obtained in the temperature rising process of differential thermal analysis (DTA) for a typical semiconductor glass in the present invention.
  • DTA measurement was performed using ⁇ -alumina as a reference sample at a temperature increase rate of 5 ° C./min in the atmosphere.
  • the mass of the reference sample and the measurement sample was 650 mg, respectively.
  • DTA differential thermal analysis
  • each temperature shall be the temperature calculated
  • the characteristic temperatures (eg, softening point T s ) described herein are based on the above definition.
  • the semiconductor thermoelectric conversion material compounded with the semiconductor glass is not particularly limited, and an optimum material can be selected according to the use temperature. For example, if it is used at 200 ° C. or lower, a Bi— (Te, Sb) -based material can be preferably used. In addition to the above, for example, Bi- (Te, Se, Sn, Sb) materials, Pb-Te materials, Zn-Sb materials, Mg-Si materials, Si-Ge materials, GeTe-AgSbTe -Based materials, (Co, Ir, Ru) -Sb based materials, (Ca, Sr, Bi) Co 2 O 5 based materials, Fe-Si based materials, Fe-V-Al based materials, etc. can be suitably used. . Furthermore, in order to cope with a wide temperature range, it is possible to combine thermoelectric conversion materials having different operating temperatures.
  • thermoelectric conversion material of the present invention is a composite of the semiconductor thermoelectric conversion material and the semiconductor glass described above, and the semiconductor thermoelectric conversion material powder and the semiconductor glass powder are mixed and applied and fired. (Details will be described later).
  • the particle diameters of the semiconductor thermoelectric conversion material powder and the semiconductor glass powder to be mixed are each preferably 5 ⁇ m or less in consideration of applicability in the application process.
  • the mixing ratio of the semiconductor glass to the semiconductor thermoelectric conversion material is preferably 10% by volume or more and 50% by volume or less (10 to 50% by volume).
  • the mixing ratio of the semiconductor glass is less than 10% by volume, the surface of the particles of the semiconductor thermoelectric conversion material is not sufficiently wetted by the softened / molten semiconductor glass, so that the liquid phase sintering of the semiconductor thermoelectric conversion material particles does not proceed sufficiently.
  • the mixing ratio of the semiconductor glass exceeds 50% by volume, the contact area between the semiconductor thermoelectric conversion material particles decreases, and the thermoelectric conversion characteristics as a whole deteriorate.
  • thermoelectric conversion material The performance of the thermoelectric conversion material will be briefly described.
  • the performance of thermoelectric conversion materials is often expressed using a dimensionless figure of merit (ZT) expressed by the following equation (1) as an index.
  • ZT dimensionless figure of merit
  • S Seebeck coefficient
  • ⁇ conductivity
  • ⁇ thermal conductivity
  • T operating temperature
  • the Seebeck coefficient is a physical property value of the thermoelectric conversion material, but when the thermoelectric conversion material is a sintered body, the conductivity and thermal conductivity are characteristic values.
  • formula (1) is applied to the thermoelectric conversion composite material (composite of semiconductor thermoelectric conversion material and semiconductor glass) according to the present invention, there are the following points to consider.
  • (A) Seebeck coefficient may decrease due to compounding.
  • (B) The effective conductivity may decrease due to the composite.
  • the effective thermal conductivity may decrease due to the composite. In other words, it can be said that it is important to suppress the decrease in the Seebeck coefficient (that is, the suppression of the chemical reaction between the semiconductor thermoelectric conversion material and the semiconductor glass) and the effective decrease in the electrical conductivity.
  • At least a part of the semiconductor glass combined with the semiconductor thermoelectric conversion material is crystallized.
  • M x V 2 O 5 M: copper, silver, alkali metal, alkaline earth metal, 0 ⁇ x ⁇ 1
  • LiV 2 O 4 CaVO
  • SrVO 3 La 1-x Sr x VO 3
  • Gd 1-x Sr x VO 3 V 2 O 3 , VO 2 and the like are preferably deposited.
  • FIG. 2 is a graph showing the temperature dependence of the electrical conductivity of the semiconductor glass on which Cu x V 2 O 5 is deposited and the semiconductor glass on which V 2 O 5 is deposited.
  • Conductivity at room temperature of the semiconductor glass before precipitating vanadium composite oxide crystals (crystallized glass) is because it was 10- 4 S / m order, as shown in FIG. 2, the present invention It has been confirmed that the electrical conductivity of the glass is dramatically improved (about 5 digits) by crystallizing the semiconductor glass.
  • thermoelectric conversion material paste includes the above-described thermoelectric conversion composite material and a solvent.
  • the paste may further contain a resin binder.
  • a resin binder As the solvent, butyl carbitol acetate or ⁇ -terpineol is preferably used.
  • the resin binder ethyl cellulose or nitrocellulose is preferably used.
  • a paste using ⁇ -terpineol as a solvent and not using a cellulose resin binder may be used.
  • thermoelectric conversion composite material By forming the thermoelectric conversion composite material according to the present invention into a paste, a desired shape (fine pattern) can be easily formed on the substrate using a low-cost process such as screen printing or coating. Thereafter, the semiconductor thermoelectric material in the paste is subjected to liquid phase sintering by firing at a temperature about 20 to 40 ° C. higher than the softening point T s of the semiconductor glass in the paste, thereby producing a thermoelectric conversion element and a thermoelectric conversion module. be able to.
  • thermoelectric conversion element is defined as a p-type semiconductor thermoelectric conversion material or an n-type semiconductor thermoelectric conversion material that is molded and fired (sintered) into a desired shape and size, and is a thermoelectric conversion module. Is defined as that a plurality of thermoelectric conversion elements are electrically connected.
  • FIG. 3 is a schematic cross-sectional view showing an example of the manufacturing process of the thermoelectric conversion module according to the present invention.
  • thermoelectric conversion module of the present invention and the manufacturing method thereof will be described with reference to FIG.
  • the substrate 101 may be any material having high thermal conductivity, and is not particularly limited.
  • aluminum can be used suitably.
  • alumina (Al 2 O 3 ), aluminum nitride (AlN), silicon carbide (SiC), beryllia (BeO), or the like having high thermal conductivity and high insulation may be used.
  • the insulating layer 102 only needs to have a high insulating property.
  • alumina or aluminum nitride may be formed by oxidizing or nitriding the substrate surface. It is more preferable that the insulating layer 102 has high thermal conductivity. Note that the insulating layer 102 is not necessarily formed when the substrate is highly insulating.
  • the electrode 103 is not particularly limited as long as it has an electric conductivity of the order of 10 5 S / m or more and a small difference in thermal expansion coefficient from the base material 101.
  • a metal film formed by a sputtering method or an electrode film coated and baked with a conductive paste may be used.
  • thermoelectric conversion material paste which concerns on this invention is prepared.
  • the p-type thermoelectric conversion material paste 104 is prepared by mixing p-type semiconductor thermoelectric conversion material particles 105, p-type semiconductor glass 106, and a solvent (for example, butyl carbitol acetate).
  • n-type thermoelectric conversion material paste 107 is prepared by mixing n-type semiconductor thermoelectric conversion material particles 108, n-type semiconductor glass 109, and a solvent (for example, butyl carbitol acetate).
  • thermoelectric conversion material pastes 104 and 107 are applied on the electrode 103 so that the polarities of the thermoelectric conversion material paste are alternated.
  • a coating method a screen printing method, an ink jet method, a stamp method, a photoresist film method, or the like can be suitably used. Thereafter, the solvent is removed by heating to about 150 ° C. to form a thermoelectric conversion material layer (precursor of thermoelectric conversion element).
  • thermoelectric Conversion Element / Thermoelectric Conversion Module Formation Step the substrate 101 on which the electrode 103 prepared in the above-described electrode formation step is formed is overlaid on the thermoelectric conversion material layer. At this time, it is preferable to arrange the substrate 101 on which the electrodes 103 are formed so that the polarities of the thermoelectric conversion materials are alternately connected in series. Thereafter, baking is performed at a temperature about 20 to 40 ° C. higher than the softening point T s of the semiconductor glasses 106 and 109, thereby forming a plurality of electrically connected thermoelectric conversion elements (that is, thermoelectric conversion modules).
  • thermoelectric conversion module it is preferable to seal the ends of the two substrates 101 to be paired with glass.
  • a glass paste 111 for sealing (or glass frit for sealing) may be applied to the end of the substrate 101, and then fired and sealed in an electric furnace. At this time, it is preferable to seal the inside of the thermoelectric conversion module while evacuating.
  • the glass paste 111 for sealing Although there is no special limitation as glass used for the glass paste 111 for sealing, it is desirable to use the glass which can be sealed in the temperature range which does not cause a chemical reaction between the semiconductor thermoelectric conversion material in the thermoelectric conversion element and the semiconductor glass. Moreover, it is preferable that the glass for sealing is glass excellent in water resistance.
  • FIG. 4 is a schematic cross-sectional view showing another example of the manufacturing process of the thermoelectric conversion module according to the present invention. Another example of the manufacturing process of the thermoelectric conversion module according to the present invention will be described with reference to FIG.
  • a highly insulating insulating layer 202 is formed on one surface of the substrate 201. After that, an electrode 203 is formed over the insulating layer 202. A pair of substrates 201 on which electrodes 203 are formed are prepared.
  • thermoelectric conversion material layer forming step a p-type thermoelectric conversion material paste 204 including p-type semiconductor thermoelectric conversion material particles 205 and p-type semiconductor glass 206 is applied on the electrode 203 of one substrate 201, and the other An n-type thermoelectric conversion material paste 207 containing n-type semiconductor thermoelectric conversion material particles 208 and n-type semiconductor glass 209 is applied on the electrode 203 of the substrate 201. Thereafter, each substrate is heated to about 150 ° C. to remove the solvent, thereby forming a thermoelectric conversion material layer (thermoelectric conversion element precursor).
  • thermoelectric conversion element / thermoelectric conversion module forming step the substrates on which the thermoelectric conversion material layers are formed are overlapped so that the polarities of the thermoelectric conversion materials are alternately connected in series. Thereafter, firing is performed at a temperature about 20 to 40 ° C. higher than the softening point T s of the semiconductor glasses 206 and 209, thereby forming a plurality of electrically connected thermoelectric conversion elements (that is, thermoelectric conversion modules).
  • the sealing process was abbreviate
  • FIG. 5 is a schematic perspective view showing an example of the thermoelectric conversion module according to the present invention.
  • a plurality of thermoelectric conversion elements p-type thermoelectric conversion element 304, n-type thermoelectric conversion element 305 are arranged between two opposing substrates 301.
  • the p-type thermoelectric conversion elements 304 and the n-type thermoelectric conversion elements 305 are electrically connected in series via the electrodes 302 formed on the substrate 301 so as to alternate.
  • Extraction electrodes 303 are attached to both ends of the thermoelectric conversion elements connected in series.
  • thermoelectric conversion element shown in the figure are examples, and the optimum shape and dimensions are the thermal conductivity of the thermoelectric conversion composite material to be used, the interfacial thermal resistivity between the thermoelectric conversion composite material and the electrode, It is designed as appropriate in consideration of the interface electrical resistivity and the use of the thermoelectric conversion module.
  • FIG. 6 is a schematic cross-sectional view showing an example of a combined solar / solar heat power generation system using the thermoelectric conversion module according to the present invention.
  • a combined solar / solar thermal power generation system 400 using a thermoelectric conversion module according to the present invention includes a solar cell module 401, a thermoelectric conversion module 402 according to the present invention, and a heat exchanger 403. It has a configuration.
  • the solar cell module 401 is disposed at a position facing sunlight, and has a structure in which a plurality of solar cells 406 connected through a lead frame 407 are fixed by a transparent resin 408 as an example.
  • the incident surface of sunlight is protected by tempered glass 405.
  • the thermoelectric conversion module 402 disposed on the back surface of the solar cell module 401 has a structure similar to that shown in FIGS. 3 to 5, and includes a plurality of thermoelectric conversion elements (p-type thermoelectric conversion elements) between two opposing substrates 409.
  • thermoelectric conversion elements 412, n-type thermoelectric conversion elements 413) are arranged, and electrodes formed on the substrate 409 via the insulating layer 410 so that the p-type thermoelectric conversion elements 412 and the n-type thermoelectric conversion elements 413 are alternately arranged.
  • 411 is electrically connected in series.
  • a heat exchanger 403 is disposed on the other surface of the thermoelectric conversion module 402. Further, a side plate 404 is attached to the side surface of the solar / solar heat combined power generation system 400 via a sealing glass 414.
  • the combined solar and solar power generation system 400 includes solar power generation by the solar cell module 401, solar power generation by the thermoelectric conversion module 402 using a temperature difference between the lower surface of the solar cell module 401 and the upper surface of the heat exchanger 403, and thermoelectric power generation.
  • Recovery for example, hot water supply
  • waste heat that could not be used in the conversion module 402 can be performed by the heat exchanger 403. That is, a cogeneration system of electric power and heat can be constructed.
  • the combined solar / solar heat power generation system 400 can suppress the decrease in efficiency due to the temperature increase of the solar battery cell 406 by actively removing the heat of the solar battery module 401 by the thermoelectric conversion module 402. Furthermore, the temperature difference between the upper and lower surfaces of the thermoelectric conversion module 402 is expanded by actively removing heat from the other surface of the thermoelectric conversion module 402 (surface opposite to the solar cell module 401) with the heat exchanger 403. The thermoelectric conversion efficiency can be improved.
  • Example 1 In this example, semiconductor glasses having various compositions were prepared, and the semiconductor glass was evaluated.
  • the platinum crucible containing the raw material mixed powder was placed in a glass melting furnace and heated and melted. The temperature was raised at a rate of 5 ° C./min, and the glass melted at the set temperature (900 to 1000 ° C.) was held for 1 hour with stirring. Thereafter, the platinum crucible was taken out of the glass melting furnace and cast into a graphite mold heated to 150 to 300 ° C. in advance. Next, the cast glass was moved to a strain relief furnace that had been heated to a strain relief temperature in advance, strain was removed by holding for 1 hour, and then cooled to room temperature at a rate of 1 ° C./min. The glass block cooled to room temperature was pulverized to prepare semiconductor glass SG-01 to SG-19 powders having the nominal compositions shown in the table.
  • the softening point T s was measured by differential thermal analysis (DTA) for each semiconductor glass powder obtained above.
  • the DTA measurement was performed with the reference sample ( ⁇ -alumina) and the measurement sample each having a mass of 650 mg and a temperature increase rate of 5 ° C / min in the atmosphere, and the peak temperature of the second endothermic peak was determined as the softening point T s (See FIG. 1).
  • the results are shown in Table 2.
  • As a result of DTA measurement it was confirmed that all of the semiconductor glasses SG-01 to SG-19 according to the present invention had a softening point of 480 ° C. or lower.
  • the fired molded body was pulverized in a mortar, and the reaction product was identified by a wide-angle X-ray diffraction measurement method (so-called ⁇ -2 ⁇ method).
  • a wide-angle X-ray diffraction measurement method for identification of detected peaks, an ICDD (International Center for Diffraction Data) card, which is a collection of X-ray diffraction standard data, was used.
  • a wide-angle X-ray diffractometer manufactured by Rigaku Corporation, model: RU200B was used as the measuring device.
  • the obtained X-ray diffraction pattern is composed only of a halo pattern derived from glass and a diffraction peak derived from Bi 2 Te 3 , it was determined that the mixed semiconductor glass did not chemically react with Bi 2 Te 3. Evaluated as “pass”.
  • the obtained X-ray diffraction pattern is a reaction product of semiconductor glass and Bi 2 Te 3 (for example, Bi 2 TeO 5 or Bi 4 TeO 8 ), and the volume fraction of the reaction product calculated from the diffraction peak intensity is less than 1/5 of the volume fraction of Bi 2 Te 3 ".
  • the volume fraction of the reaction product calculated from the diffraction peak intensity was more than 1/5 of the volume fraction of Bi 2 Te 3 , it was evaluated as “failed”.
  • the evaluation results are also shown in Table 2.
  • the semiconductor glasses SG-01 to SG-19 of the present invention all have low chemical reactivity with Bi 2 Te 3 when fired in an argon atmosphere.
  • SG-01, SG-02, SG-15, and SG-17 were confirmed to have low chemical reactivity with Bi 2 Te 3 even in firing in the atmosphere.
  • thermoelectric conversion element according to the present invention was produced and its characteristics were evaluated.
  • thermoelectric conversion material As a semiconductor thermoelectric conversion material, p-type Bi 0.3 Sb 1.7 Te 3 powder (manufactured by Toyoshima Seisakusho Co., Ltd., purity: 3N or more, particle size (D50): 3.2 ⁇ m) and n-type Bi 2 Te 3 powder (Co., Ltd.) Made by Toshima Seisakusho, purity: 3N or more, particle size (D50): 2.5 ⁇ m) were prepared. In addition, p-type SG-07 and n-type SG-15 were prepared as compound semiconductor glasses.
  • p-type Bi 0.3 Sb 1.7 Te 3 powder 70% by volume
  • p-type SG-07 (30% by volume)
  • EC ethyl cellulose
  • BCA butyl carbitol acetate
  • 15% by weight of the mixed solution was prepared to produce a p-type thermoelectric conversion material paste.
  • n-type Bi 2 Te 3 powder 70% by volume
  • n-type SG-15 (30% by volume) are mixed, and 15 masses of a mixed solution of EC and BCA is added to the mixed powder.
  • An n-type thermoelectric conversion material paste was prepared.
  • thermoelectric conversion element manufactured by Toshima Seisakusho Co., Ltd.
  • a thermoelectric conversion element manufactured by Toshima Seisakusho Co., Ltd.
  • the Seebeck coefficient and electrical conductivity of these thermoelectric conversion elements were measured with a thermoelectric property evaluation apparatus (manufactured by ULVAC-RIKO, model: ZEM-3). The measurement was performed three times in each of the temperatures of 323 K, 373 K, and 423 K in low-pressure helium gas, and the average value was obtained.
  • Table 3 The results are shown in Table 3.
  • thermoelectric conversion element according to the present invention maintained the same thermoelectric characteristics as compared with the conventional bulk type thermoelectric conversion element.
  • the semiconductor glass of the present invention and the thermoelectric conversion material paste using the same do not adversely affect the thermoelectric properties of the semiconductor thermoelectric conversion material.
  • a thermoelectric conversion element can be produced by firing at a lower temperature than in the case of a conventional bulk thermoelectric conversion element.
  • thermoelectric conversion module according to the present invention was produced, and its conversion efficiency was measured.
  • thermoelectric conversion module (Evaluation of thermoelectric conversion module) The thermoelectric conversion module shown in FIG. 5 was produced using the thermoelectric conversion material paste produced in Example 2. The dimensions and shape of the thermoelectric conversion elements 304 and 305 were made into a cubic shape with a side of about 100 ⁇ m, and 1.44 million thermoelectric conversion elements were integrated on a 70 cm square substrate 301. Table 4 shows an outline of the manufacturing conditions.
  • FIG. 7 is a schematic cross-sectional view showing a method for measuring the conversion efficiency of the thermoelectric conversion module.
  • the produced thermoelectric conversion module 502 was installed between the heater 501 and the copper block 504 having a known thermal conductivity. On the other end side of the copper block 504, a heat sink 505 for removing heat was disposed.
  • thermoelectric conversion module 502 One surface of the thermoelectric conversion module 502 was heated by the heater 501, and the module output P output from the extraction electrode 503 and the heat flux Q flowing through the copper block 504 were measured.
  • the thermoelectric conversion module 502 It was confirmed that a sufficiently high performance was obtained with a conversion efficiency ⁇ of about 2%.
  • thermoelectric conversion material paste 101, 201 ... substrate, 102, 202 ... insulating layer, 103, 203 ... electrode, 104, 204 ... p-type thermoelectric conversion material paste, 105, 205 ... p-type semiconductor thermoelectric conversion material particles, 106, 206... p-type semiconductor glass, 107, 207 ... n-type thermoelectric conversion material paste, 108, 208 ... n-type semiconductor thermoelectric conversion material particles, 109, 209 ... n-type semiconductor glass, 111 ... sealing glass paste, 300 ... thermoelectric conversion module, 301 ... substrate, 302 ... electrode, 303 ... extraction electrode, 304 ... p-type thermoelectric conversion element, 305 ... n-type thermoelectric conversion element, 400 ...
  • thermoelectric conversion module 403 ... heat exchanger, 404 ... side plate, 405 ... tempered glass, 406 ... Solar cell, 407 ... Lead frame, 408 ... Transparent resin, 409 ... Substrate, 410 ... insulating layer, 411 ... electrode, 412 ... p-type thermoelectric conversion element, 413 ... n-type thermoelectric conversion element, 414 ... sealing glass, 501 ... Heater, 502 ... Thermoelectric conversion module, 503 ... Lead electrode, 504 ... Copper block, 505 ... Heat sink.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Life Sciences & Earth Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • General Chemical & Material Sciences (AREA)
  • Geochemistry & Mineralogy (AREA)
  • Materials Engineering (AREA)
  • Organic Chemistry (AREA)
  • Inorganic Chemistry (AREA)
  • Manufacturing & Machinery (AREA)
  • Glass Compositions (AREA)
  • Inorganic Compounds Of Heavy Metals (AREA)
PCT/JP2012/075593 2011-10-25 2012-10-03 熱電変換複合材料、それを用いた熱電変換材料ペースト、およびそれを用いた熱電変換モジュール Ceased WO2013061739A1 (ja)

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2011233584A JP5526104B2 (ja) 2011-10-25 2011-10-25 熱電変換複合材料、それを用いた熱電変換材料ペースト、およびそれを用いた熱電変換モジュール
JP2011-233584 2011-10-25

Publications (1)

Publication Number Publication Date
WO2013061739A1 true WO2013061739A1 (ja) 2013-05-02

Family

ID=48167574

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2012/075593 Ceased WO2013061739A1 (ja) 2011-10-25 2012-10-03 熱電変換複合材料、それを用いた熱電変換材料ペースト、およびそれを用いた熱電変換モジュール

Country Status (3)

Country Link
JP (1) JP5526104B2 (enExample)
TW (1) TWI505523B (enExample)
WO (1) WO2013061739A1 (enExample)

Cited By (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP2902518A3 (en) * 2014-01-29 2015-12-09 LG Innotek Co., Ltd. Thermoelectric material and thermoelectric element including the same
WO2018230031A1 (ja) * 2017-06-16 2018-12-20 三菱電機株式会社 太陽光発電パネル及びその製造方法
CN110770924A (zh) * 2017-06-29 2020-02-07 三菱综合材料株式会社 热电转换模块及热电转换模块的制造方法
CN111710775A (zh) * 2020-07-22 2020-09-25 中国科学院宁波材料技术与工程研究所 一种硒化锡基热电材料、其制备方法及应用
CN113161470A (zh) * 2021-04-09 2021-07-23 河南鸿昌电子有限公司 制造半导体致冷件所用的材料、半导体晶粒和致冷件
JP2022144073A (ja) * 2021-03-18 2022-10-03 国立研究開発法人産業技術総合研究所 熱電変換層を有する積層体とその製造方法、及び発電モジュール

Families Citing this family (9)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
KR101998697B1 (ko) * 2012-06-28 2019-07-10 엘지이노텍 주식회사 열전냉각모듈 및 이의 제조 방법
WO2015019871A1 (ja) * 2013-08-09 2015-02-12 リンテック株式会社 熱電変換材料及びその製造方法
JP6347025B2 (ja) * 2013-12-25 2018-06-27 株式会社小松プロセス 熱電変換材料、回路作製方法、及び、熱電変換モジュール
JP2015164393A (ja) * 2014-01-28 2015-09-10 学校法人日本大学 ヒートシンク及び複合型太陽エネルギー変換装置
WO2016104615A1 (ja) * 2014-12-26 2016-06-30 リンテック株式会社 ペルチェ冷却素子及びその製造方法
JP6791544B2 (ja) * 2015-06-24 2020-11-25 リンテック株式会社 熱電半導体組成物、並びに熱電変換材料及びその製造方法
CN105256161B (zh) * 2015-11-04 2017-09-29 武汉理工大学 一种Ag2Se块体热电材料的免烧致密化制备工艺
KR102088009B1 (ko) * 2016-12-27 2020-03-11 주식회사 엘지화학 열전 변환 복합재 및 이의 제조 방법
JP2019153664A (ja) * 2018-03-02 2019-09-12 株式会社ミクニ 熱電変換モジュールの製造方法

Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH0832123A (ja) * 1994-07-19 1996-02-02 Matsushita Electric Works Ltd 熱電変換素子の製造方法
JPH11251647A (ja) * 1998-02-27 1999-09-17 Ueki Corporation:Kk 熱電変換素子および熱電変換装置と、これらの製造方法
JP2008116445A (ja) * 2006-10-11 2008-05-22 Kitakyushu Foundation For The Advancement Of Industry Science & Technology 熱電対式温度センサ及びその製造方法
JP2011129832A (ja) * 2009-12-21 2011-06-30 Denso Corp 熱電変換素子及びその製造方法

Family Cites Families (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2008227178A (ja) * 2007-03-13 2008-09-25 Sumitomo Chemical Co Ltd 熱電変換モジュール用基板及び熱電変換モジュール
JP5414409B2 (ja) * 2009-01-16 2014-02-12 日立粉末冶金株式会社 低融点ガラス組成物、それを用いた低温封着材料及び電子部品

Patent Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH0832123A (ja) * 1994-07-19 1996-02-02 Matsushita Electric Works Ltd 熱電変換素子の製造方法
JPH11251647A (ja) * 1998-02-27 1999-09-17 Ueki Corporation:Kk 熱電変換素子および熱電変換装置と、これらの製造方法
JP2008116445A (ja) * 2006-10-11 2008-05-22 Kitakyushu Foundation For The Advancement Of Industry Science & Technology 熱電対式温度センサ及びその製造方法
JP2011129832A (ja) * 2009-12-21 2011-06-30 Denso Corp 熱電変換素子及びその製造方法

Non-Patent Citations (3)

* Cited by examiner, † Cited by third party
Title
B. I. SHARMA ET AL.: "Electrical properties of V2O5-CaO-P2O5 glasses exhibiting majority charge carrier reversal", JOURNAL OF MATERIALS SCIENCE, vol. 40, 2005, pages 5125 - 5131, XP019210770 *
SUMIO SAKKA ET AL., GLASS HANDBOOK, ASAKURA SHOTEN, 30 September 1975 (1975-09-30), pages 720 - 724 *
YOSHIHIRO KOUHARA ET AL.: "Particle optimize of the vanadium system low-melting lead-free glass", THE RESEARCH REPORTS OF THE FACULTY OF ENGINEERING, no. 49, 2007, pages 1 - 6, XP003031615 *

Cited By (10)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP2902518A3 (en) * 2014-01-29 2015-12-09 LG Innotek Co., Ltd. Thermoelectric material and thermoelectric element including the same
US9595652B2 (en) 2014-01-29 2017-03-14 Lg Innotek Co., Ltd. Thermoelectric material and thermoelectric element including the same
WO2018230031A1 (ja) * 2017-06-16 2018-12-20 三菱電機株式会社 太陽光発電パネル及びその製造方法
JPWO2018230031A1 (ja) * 2017-06-16 2019-06-27 三菱電機株式会社 太陽光発電パネル及びその製造方法
CN110770924A (zh) * 2017-06-29 2020-02-07 三菱综合材料株式会社 热电转换模块及热电转换模块的制造方法
CN110770924B (zh) * 2017-06-29 2023-11-14 三菱综合材料株式会社 热电转换模块及热电转换模块的制造方法
CN111710775A (zh) * 2020-07-22 2020-09-25 中国科学院宁波材料技术与工程研究所 一种硒化锡基热电材料、其制备方法及应用
JP2022144073A (ja) * 2021-03-18 2022-10-03 国立研究開発法人産業技術総合研究所 熱電変換層を有する積層体とその製造方法、及び発電モジュール
JP7627940B2 (ja) 2021-03-18 2025-02-07 国立研究開発法人産業技術総合研究所 熱電変換層を有する積層体とその製造方法、及び発電モジュール
CN113161470A (zh) * 2021-04-09 2021-07-23 河南鸿昌电子有限公司 制造半导体致冷件所用的材料、半导体晶粒和致冷件

Also Published As

Publication number Publication date
JP5526104B2 (ja) 2014-06-18
TW201332170A (zh) 2013-08-01
JP2013093397A (ja) 2013-05-16
TWI505523B (zh) 2015-10-21

Similar Documents

Publication Publication Date Title
JP5526104B2 (ja) 熱電変換複合材料、それを用いた熱電変換材料ペースト、およびそれを用いた熱電変換モジュール
US20110100410A1 (en) Thermoelectric converter element and conductive member for thermoelectric converter element
WO2011013529A1 (ja) 熱電変換材料及びそれを用いた熱電変換モジュール
JP2002151751A (ja) 熱電素子の製造方法及び熱電モジュール
EP4099411B1 (en) Thermoelectric conversion module
CN118614167A (zh) 热电转换组件和热电转换系统
CN102113141B (zh) 热电转换材料和热电转换元件
TWI469927B (zh) 新穎化合物半導體及其應用
JP6347025B2 (ja) 熱電変換材料、回路作製方法、及び、熱電変換モジュール
US20130126800A1 (en) Niobium oxide-based thermoelectric composites
JP5218285B2 (ja) 熱電変換材料
JP2006278997A (ja) 複合熱電モジュール
CN103173650B (zh) 热电材料与其制造方法、以及包含其的热电模组
JPWO2014073095A1 (ja) 熱電変換モジュール及びその製造方法
JP6358449B2 (ja) 熱電材料及びその製造方法
US20100327166A1 (en) Infrared sensor
KR101401078B1 (ko) 양봉분포하는 입자를 가진 열전분말의 제조방법
JP4876721B2 (ja) 熱電変換材料およびその製造方法
KR102621179B1 (ko) 열전소재 및 이를 포함하는 열전소자와 열전모듈
WO2022114239A1 (ja) 熱電材料、熱電変換素子、熱電発電モジュールおよびペルチェ冷却器
US7417186B2 (en) Thermoelectric conversion material, thermoelectric conversion element using the same, and electronic apparatus and cooling device comprising the element
KR20180100868A (ko) 고성능 화합물 반도체 및 그의 제조 방법
JP2018085415A (ja) 熱電変換素子およびその製造方法
Shi et al. Thermoelectric Power Generators and Their Applications
JP4477334B2 (ja) クラスレート化合物

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 12843002

Country of ref document: EP

Kind code of ref document: A1

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 12843002

Country of ref document: EP

Kind code of ref document: A1