WO2024063130A1 - 樹脂組成物、樹脂硬化物および樹脂硬化物の製造方法 - Google Patents
樹脂組成物、樹脂硬化物および樹脂硬化物の製造方法 Download PDFInfo
- Publication number
- WO2024063130A1 WO2024063130A1 PCT/JP2023/034252 JP2023034252W WO2024063130A1 WO 2024063130 A1 WO2024063130 A1 WO 2024063130A1 JP 2023034252 W JP2023034252 W JP 2023034252W WO 2024063130 A1 WO2024063130 A1 WO 2024063130A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- meth
- compound
- polymerization initiator
- resin composition
- acrylate
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
- C08G18/00—Polymeric products of isocyanates or isothiocyanates
- C08G18/06—Polymeric products of isocyanates or isothiocyanates with compounds having active hydrogen
- C08G18/28—Polymeric products of isocyanates or isothiocyanates with compounds having active hydrogen characterised by the compounds used containing active hydrogen
- C08G18/67—Unsaturated compounds having active hydrogen
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
- C08G59/00—Polycondensates containing more than one epoxy group per molecule; Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups
- C08G59/02—Polycondensates containing more than one epoxy group per molecule
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
- C08L63/00—Compositions of epoxy resins; Compositions of derivatives of epoxy resins
Definitions
- the present invention relates to a resin composition, a cured resin product, and a method for producing a cured resin product, and specifically relates to a resin composition, a cured resin product that is a cured product of the resin composition, and a method for producing the cured resin product. .
- Plastic substrates are used as substrates for flexible displays, and require mechanical properties such as bending strength, dimensional accuracy due to changes in temperature and humidity, and processing suitability such as resistance to plating liquid during wiring pattern formation and resistance to soldering heat. .
- Patent Document 2 a photosensitive prepolymer containing an epoxy resin with excellent heat resistance has been disclosed (see, for example, Patent Document 2).
- an ultraviolet curable resin composition containing an acrylate resin composition that undergoes photo-radical polymerization and an epoxy-based resin composition that undergoes photo-cationic polymerization is disclosed (for example, see Patent Document 3).
- the present invention provides a resin composition for obtaining a cured resin product having excellent bending strength and heat resistance, a cured resin product that is a cured product of the resin composition, and a method for producing the cured resin product.
- the present invention [1] comprises a compound (A) having a (meth)acryloyl group, a compound (B) having an epoxy group and/or an oxetanyl group, a radical polymerization initiator (C), and a cationic polymerization initiator (D ), wherein one of the compound (A) and the compound (B) has a hydrogen-bonding substituent value of 0.0001 mol/g or more and 0.1111 mol/g or less.
- the hydrogen bonding substituent value of the other hydrogen bonding substituent group is 2/3 or less with respect to the hydrogen bonding substituent value of the one
- the cured product of the resin composition has two or more peaks of loss coefficient tan ⁇ , and the peak includes a first peak with a peak top position of less than 100°C and a second peak with a peak top position of 100°C or more, and has a minimum value of loss coefficient tan ⁇ of 100°C or less of 0.1 or less, It is a resin composition.
- the present invention [2] provides the above-mentioned [1], wherein one of the radical polymerization initiator (C) and the cationic polymerization initiator (D) is a photopolymerization initiator and the other is a thermal polymerization initiator. It contains the resin composition described above.
- the present invention [3] includes the resin composition described in the above [1] or [2], wherein the compound (A) is urethane (meth)acrylate.
- the present invention [4] includes a cured resin product that is a cured product of the resin composition described in any one of [1] to [3] above.
- the present invention [5] is the method for producing a cured resin product according to the above [4], wherein in the resin composition, both the radical polymerization initiator (C) and the cationic polymerization initiator (D) are , a photopolymerization initiator, a peak top position on the long wavelength side of the light absorption wavelength of the radical polymerization initiator (C), and a peak top position on the long wavelength side of the light absorption wavelength of the cationic polymerization initiator (D).
- the absolute value of the difference is 30 nm or more, and the peak top position of the radical polymerization initiator (C) and the peak top position of the cationic polymerization initiator (D) are on the relatively longer wavelength side.
- the method includes irradiating light having a wavelength corresponding to the peak top position, and then irradiating light having a wavelength corresponding to the peak top position on the relatively short wavelength side.
- a cured resin product having excellent bending strength and heat resistance can be produced.
- the resin composition of the present invention it is possible to produce a cured resin product with excellent bending strength and heat resistance, which improves dimensional accuracy due to temperature changes and humidity changes, resistance to plating liquid during wiring pattern formation, resistance to soldering heat, etc. It is possible to easily produce a cured resin material that satisfies processing suitability.
- the hydrogen-bonding substituent value of either one of the compound (A) having a (meth)acryloyl group and the compound (B) having an epoxy group and/or an oxetanyl group is
- the hydrogen bonding substituent value is 0.0001 mol/g or more and 0.1111 mol/g or less, and the value of the other hydrogen bonding substituent group is 2/3 or less of the value of the one hydrogen bonding substituent group.
- One is a certain first peak, and the other peak is a second peak whose top position is 100° C. or higher.
- the minimum value of the loss coefficient tan ⁇ at 100° C. or less is 0.1 or less. Since the compound originating from the first peak becomes the soft segment and the compound originating from the second peak becomes the hard segment, both heat resistance and flexibility can be achieved. Furthermore, since the minimum value of the loss coefficient tan ⁇ at 100° C. or less is 0.1 or less, it exhibits a high recovery rate against deformation.
- the cured resin product of the present invention is a cured product of the resin composition of the present invention. Therefore, it has excellent bending strength and heat resistance. Therefore, the cured resin product is effective as a base material for liquid crystal displays and organic EL displays, and is particularly effective as a base material for foldable displays.
- both the radical polymerization initiator (C) and the cationic polymerization initiator (D) are photopolymerization initiators, and the radical polymerization initiator (C) has a wavelength of light absorption
- the absolute value of the difference between the peak top position on the wavelength side and the peak top position on the long wavelength side of the light absorption wavelength of the cationic polymerization initiator (D) is 30 nm or more, and the peak top position of the radical polymerization initiator (C) is position and the peak top position of the cationic polymerization initiator (D), after irradiating with light having a wavelength corresponding to the peak top position on the relatively long wavelength side, the peak top position on the relatively short wavelength side is irradiated. Irradiate light with a corresponding wavelength. Therefore, a cured resin product having excellent bending strength and heat resistance can be produced.
- FIG. 1 is a transmission electron microscope image of the resin composition obtained in Example 1, showing that it has a phase-separated structure.
- Resin composition The resin composition of the present invention comprises a compound (A) having a (meth)acryloyl group, a compound (B) having an epoxy group and/or an oxetanyl group, a radical polymerization initiator (C), and a cationic polymerization initiator (C). and an initiator (D).
- each substance below is described as an example. That is, each substance is not limited to the examples below. Any substance that exhibits the functions and effects of the present invention can be used as a raw material for the resin composition.
- Compound (A) having a (meth)acryloyl group Compound (A) is not particularly limited as long as it has a (meth)acryloyl group and does not have an epoxy group or an oxetanyl group.
- Examples of compounds having a (meth)acryloyl group include 2-ethylhexyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, and lauryl (meth)acrylate.
- Polyurethane (meth)acrylate oligomers can be synthesized using various commercial products or by reacting a compound having an isocyanate group with a (meth)acrylate having an active hydrogen group to form a urethane.
- Commercially available products include, for example, AH-600; phenyl glycidyl ether acrylate hexamethylene diisocyanate urethane prepolymer manufactured by Kyoeisha Chemical Co., Ltd.; UA-306H; pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer; UA-306T; pentaerythritol triacrylate; Toluene diisocyanate urethane prepolymer, UA-306I; Pentaerythritol triacrylate isophorone diisocyanate urethane prepolymer, UA-510H; Dipentaerythritol pentaacrylate
- compounds having isocyanate groups that can be used for synthesis include, for example, ethylene diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, octamethylene diisocyanate, nonamethylene diisocyanate, 2, 2'-dimethylpentane diisocyanate, 2,2,4-trimethylhexane diisocyanate, decamethylene diisocyanate, butene diisocyanate, 1,3-butadiene-1,4-diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, 1,6 , 11-undecamethylene triisocyanate, 1,3,6-hexamethylene triisocyanate, 1,8-diisocyanate-4-isocyanatomethyloctane, 2,5,7-trimethyl-1,8-diisocyanate
- polyisocyanate derivatives include modified products obtained by modifying the above-mentioned polyisocyanate monomers by a known method. More specifically, examples of polyisocyanate derivatives include multimers, isocyanurate-modified products, allophanate-modified products, polyol-modified products, biuret-modified products, urea-modified products, oxadiazinetrione-modified products, and carbodiimide-modified products. It will be done. Moreover, polymethylene polyphenylene polyisocyanate is also mentioned as a polyisocyanate derivative.
- polyisocyanate derivatives can be used alone or in combination of two or more.
- polyisocyanate components can be used alone or in combination of two or more.
- isocyanates can also be synthesized by reacting a compound having an active hydrogen group with a compound having two or more isocyanate groups so that at least one isocyanate group remains.
- the active hydrogen group is a group capable of forming a hydrogen bond, such as a hydroxyl group, a mercapto group, and an amino group.
- Examples of compounds having hydroxyl groups include ethylene glycol, trimethylpyrrole, polyether polyol, polyester polyol, polycarbonate polyol, polyurethane polyol, epoxy polyol, vegetable oil polyol, polyolefin polyol, acrylic polyol, and vinyl monomer-modified polyol.
- Examples of compounds having a mercapto group include 1,2,6,10,11-pentamercapto-4,8-dithiaundecane, 1,2,9,10-tetramercapto-6-mercaptomethyl-4,7
- Examples of aliphatic mercaptan compounds such as -dithiadecane, aromatic mercaptan compounds such as thiophenol and mercaptotoluene, and polythiol compounds having two or more functional groups include 1,1-methanedithiol, 1,2-ethanedithiol, 1,1- Aliphatic polythiol compounds such as propanedithiol, 1,2-propanedithiol, 1,2-dimercaptobenzene, 1,3-dimercaptobenzene, 1,4-dimercaptobenzene, 1,2-bis(mercaptomethyl) Aromatic polythiols such as benzene, 1,3-bis(mercaptomethyl)benzene, 1,2-bis(mercaptoeth
- Examples of compounds having an amino group include ethylenediamine, 1,3-propanediamine, 1,3-butanediamine, 1,4-butanediamine, 1,6-hexamethylenediamine, 1,4-cyclohexanediamine, 3 -Aminomethyl-3,5,5-trimethylcyclohexylamine (isophoronediamine), 4,4'-dicyclohexylmethanediamine, 2,5-bis(aminomethyl)bicyclo[2.2.1]heptane, 2,6- Bis(aminomethyl)bicyclo[2.2.1]heptane, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, hydrazine, and tolylenediamine, triethylenetetramine, tetra Examples include ethylenepentamine.
- the isocyanate group-terminated prepolymer can be obtained by reacting the above polyisocyanate component and the above compound having an active hydrogen group by a known method. That is, in this method, a polyisocyanate component and a compound having an active hydrogen group are blended in a predetermined ratio and subjected to a urethanization reaction.
- the equivalent ratio of isocyanate groups in the polyisocyanate component to active hydrogen groups is, for example, more than 1, preferably 1.1 or more, more preferably 3. Above, more preferably 6 or more, preferably 20, more preferably 15 or less, still more preferably 10 or less.
- a known polymerization method is employed.
- polymerization methods include bulk polymerization and solution polymerization.
- bulk polymerization for example, the above components are blended under a nitrogen atmosphere and reacted at a reaction temperature of 75 to 85° C. for about 1 to 20 hours.
- solution polymerization for example, the above-mentioned components are added to a known organic solvent under a nitrogen atmosphere and reacted at a reaction temperature of 20 to 80° C. for about 1 to 20 hours.
- the average functionality of the isocyanate groups in the isocyanate-terminated prepolymer is, for example, 1.5 or more, preferably 2.0 or more.
- the average functionality of the isocyanate groups in the isocyanate-terminated prepolymer is, for example, 3.0 or less, preferably 2.5 or less.
- prepolymer crude product a composition (hereinafter referred to as prepolymer crude product) containing an isocyanate group-terminated prepolymer and an unreacted polyisocyanate component is obtained.
- the isocyanate group concentration of the prepolymer crude product is, for example, 0.3% by mass or more, preferably 0.5% by mass or more, more preferably, It is 1.0% by mass or more. Further, the isocyanate group concentration of the prepolymer crude product is, for example, 15% by mass or less, preferably 12% by mass or less, and more preferably 10% by mass or less.
- the prepolymer crude product is preferably purified by distillation. Distillation improves the mechanical strength and dimensional stability of the cured resin product (described later).
- the distillation method is not particularly limited, but includes, for example, a batch distillation method and a continuous distillation method.
- An example of the continuous distillation method is a thin film distillation method (Smith thin film distillation method).
- the distillation method is a thin film distillation method (Smith thin film distillation method).
- the distillation conditions are set depending on the purpose and use.
- the distillation temperature is, for example, 120°C or higher, preferably 150°C or higher. Further, the distillation temperature is, for example, 250°C or lower, preferably 200°C or lower.
- the distillation pressure absolute pressure
- the distillation pressure is, for example, 1 Pa or more, preferably 10 Pa or more, more preferably 50 Pa or more. Further, the distillation pressure is, for example, 300 Pa or less, preferably 200 Pa or less, more preferably 100 Pa or less.
- the feed rate of the prepolymer crude product is, for example, 0.1 g/min or more, preferably 1.0 g/min or more, and more preferably 2.0 g/min or more. Further, the feed rate of the prepolymer crude product is, for example, 100 g/min or less, preferably 50 g/min or less, more preferably 10 g/min or less.
- purified prepolymer product a purified product of the isocyanate group-terminated prepolymer (hereinafter referred to as a purified prepolymer product) is obtained.
- the purified prepolymer consists of an isocyanate group-terminated prepolymer, or an isocyanate group-terminated prepolymer and a very small amount (10,000 ppm or less) of an unreacted polyisocyanate component.
- the content of the isocyanate group-terminated prepolymer is, for example, 99.5% by mass or more, preferably 99.9% by mass or more, based on the total amount of the purified prepolymer, for example, 100% by mass or more. % by mass or less.
- the content thereof is, for example, 0.0001% by mass or more, preferably 0.0005% by mass, based on the total amount of the purified prepolymer (in terms of solid content). That's all.
- the content ratio of the unreacted polyisocyanate component is, for example, 0.020% by mass or less, preferably 0.013% by mass or less, more preferably , 0.010% by mass or less.
- a radical curable polyurethane resin is obtained by reacting the isocyanate group-terminated prepolymer (preferably a purified prepolymer) with a compound having a hydroxy group-containing (meth)acroyl group.
- a compound having a hydroxy group-containing (meth)acroyl group is a compound having one or more (meth)acroyl groups and one or more hydroxy groups.
- (meth)acryloyl refers to acryloyl and/or methacryloyl.
- (meth)acrylic refers to acrylic and/or methacrylic
- (meth)acrylate refers to acrylate and/or methacrylate.
- Examples of compounds containing a (meth)acryloyl group and a hydroxy group include hydroxy group-containing (meth)acrylates.
- hydroxy group-containing (meth)acrylate examples include monohydroxyl mono(meth)acrylate, polyhydroxyl mono(meth)acrylate, monohydroxyl poly(meth)acrylate, and polyhydroxyl poly(meth)acrylate.
- Monohydroxyl mono(meth)acrylate is a compound having one hydroxy group and one (meth)acryloyl group in one molecule.
- monohydroxyl mono(meth)acrylate include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl(meth)acrylate, 4-hydroxybutyl(meth)acrylate, 2-hydroxybutyl(meth)acrylate, 2- Phenoxypropyl (meth)acrylate, 4-hydroxycyclohexyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, 2-hydroxy-3-phenyloxypropyl (meth)acrylate, 2-(meth)acryloyloxy Ethyl-2-hydroxyethylphthalic acid, 2-hydroxyalkyl (meth)acryloyl phosphate, pentanediol mono(meth)acrylate, neopentyl glycol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, and polypropylene glyco
- Polyhydroxyl mono(meth)acrylate is a compound that has multiple hydroxy groups and one (meth)acryloyl group in one molecule.
- Examples of polyhydroxyl mono(meth)acrylates include trimethylolpropane mono(meth)acrylate, glycerin mono(meth)acrylate, and pentaerythritol mono(meth)acrylate.
- Monohydroxyl poly(meth)acrylate is a compound that has one hydroxy group and multiple (meth)acryloyl groups in one molecule.
- Examples of monohydroxyl poly(meth)acrylates include trimethylolpropane di(meth)acrylate, glycerin di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, and 2-hydroxy -3-(meth)acryloyloxypropyl (meth)acrylate.
- Polyhydroxyl poly(meth)acrylate is a compound that has multiple hydroxyl groups and multiple (meth)acryloyl groups in one molecule.
- Examples of polyhydroxyl poly(meth)acrylate include pentaerythritol di(meth)acrylate, dipentaerythritol tri(meth)acrylate, and dipentaerythritol tetra(meth)acrylate.
- the hydroxy group-containing unsaturated compound is preferably a hydroxy group-containing (meth)acrylate, more preferably a monohydroxyl mono(meth)acrylate, a monohydroxyl poly(meth)acrylate, and still more preferably a monohydroxyl mono(meth)acrylate.
- (meth)acrylates more preferably hydroxyalkyl (meth)acrylates, particularly preferably 2-hydroxyethyl (meth)acrylates.
- the above-mentioned isocyanate-terminated prepolymer and a hydroxyl-containing unsaturated compound are mixed in a predetermined equivalent ratio in an inert gas atmosphere to cause a urethane reaction.
- the equivalent ratio of the isocyanate group in the isocyanate group-terminated prepolymer to the hydroxy group in the hydroxy group-containing unsaturated compound is, for example, 0.7 or more, preferably 0.9 or more, For example, it is 1.5 or less, preferably 1.2 or less.
- reaction conditions are not particularly limited and are appropriately set depending on the purpose and use.
- the reaction temperature is, for example, 40°C or higher, preferably 50°C or higher, and more preferably 60°C or higher.
- the reaction temperature is, for example, 120°C or lower, preferably 100°C or lower, more preferably 80°C or lower.
- the reaction time is, for example, 0.5 hours or more, preferably 1.0 hours or more.
- the reaction time is, for example, 24 hours or less, preferably 10 hours or less.
- a known urethanization catalyst may be added as necessary.
- the addition ratio of the urethanization catalyst is appropriately set depending on the purpose and use.
- the radical curable polyurethane resin is obtained by a urethanization reaction between the isocyanate group of an isocyanate group-terminated prepolymer and the hydroxy group of a hydroxy group-containing (meth)acroyl compound, and the hydroxy group-containing (meth) It is a polyurethane resin having a (meth)acrylic group derived from an acroyl compound.
- Compound (B) having an epoxy group and/or oxetanyl group is a compound that has an epoxy group and/or an oxetanyl group and does not have a (meth)acryloyl group.
- compounds having an epoxy group include bisphenol epoxy compounds such as butyl glycidyl ether, phenyl glycidyl ether, bisphenol A type epoxy compounds, bisphenol F type epoxy compounds, bisphenol AD type epoxy compounds, and bisphenol S type epoxy compounds; naphthalene type epoxy compounds; Epoxy compounds; novolac-type epoxy compounds such as phenol novolak-type epoxy compounds and cresol novolac-type epoxy compounds; alcohol-type epoxy compounds such as hydrogenated bisphenol A-type epoxy compounds; halogenated epoxy compounds such as brominated epoxy compounds; polyfunctional epoxy Specific examples include bisphenol A type epoxy compounds such as EPICLON850, 850-S, and EXA-850CPR manufactured by DIC; bisphenol F type epoxy compounds such as EPICLON
- Aliphatic epoxy compounds include polyglycidyl ethers of polyhydric alcohols or their alkylene oxide adducts, and specific examples include ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, 1,9-nonanediol diglycidyl ether, 1,12-dodecanediol diglycidyl ether, glycerin triglycidyl ether, trimethylolpropane triglycidyl ether (Epolite 100MF manufactured by Kyoeisha Chemical Co., Ltd.), polyethylene glycol diglycidyl ether, etc.
- ethylene glycol diglycidyl ether diethylene glycol diglycidy
- Examples of the alicyclic epoxy compounds include hydrogenated products of the aromatic epoxy compounds, cyclohexane-based, cyclohexyl methyl ester-based, cyclohexyl methyl ether-based, spiro-based, and tricyclodecane-based epoxy compounds, and specific examples thereof include: Hydrogenated bisphenol A type epoxy compounds such as KRM-2408 manufactured by ADEKA and YX-8034 manufactured by JER; 3',4'-epoxycyclohexylmethyl 3,4-epoxycyclohexane carboxylate, 1,2:8,9 - Diepoxylimonene, 1,2-epoxy-4-vinylcyclohexane, 1,2-epoxy-4-(2-oxiranyl)cyclohexane adduct of 2,2-bis(hydroxymethyl)-1-butanol (manufactured by Daicel) EHPE3150) and alicyclic epoxy compounds such as the compound represented by the following formula (IV-1).
- Other compounds having an epoxy group in the molecule include heterocyclic epoxy compounds, glycidyl ether type epoxy compounds, glycidyl ester type epoxy compounds, glycidylamine type epoxy compounds, rubber modified epoxy compounds, urethane modified epoxy compounds, and epoxidized polybutadiene. , epoxidized styrene-butadiene-styrene block copolymers, epoxy group-containing polyester compounds, epoxy group-containing polyurethane compounds, epoxy group-containing acrylic compounds, and the like.
- compounds having an oxetanyl group in the molecule include 3-ethyl-3-hydroxymethyloxetane (oxetane alcohol) (for example, OXT-101 manufactured by Toagosei Co., Ltd.), 2-ethylhexyloxetane (for example, OXT-101 manufactured by Toagosei Co., Ltd.) OXT-212), xylylene bisoxetane (XDO: e.g. OXT-121 manufactured by Toagosei Co., Ltd.), 3-ethyl-3 ⁇ [(3-ethyloxetan-3-yl)methoxy]methyl ⁇ oxetane (e.g.
- Toagosei Co., Ltd. OXT-212
- OXT-221 manufactured by Toagosei Co., Ltd. OXT-221 manufactured by Toagosei Co., Ltd.
- oxetanylsilsesquioxetane for example, OXT-191 manufactured by Toagosei Co., Ltd.
- phenol novolak oxetane for example, PHOX manufactured by Toagosei Co., Ltd.
- 3-ethyl-3-phenoxymethyloxetane POX: for example, OXT-211 manufactured by Toagosei Co., Ltd.
- 3-ethyl-3-allyloxymethyloxetane for example, AL-EOX manufactured by Yokkaichi Gosei Co., Ltd.
- radical polymerization initiators that generate radicals upon heating include organic peroxides such as ketone peroxides, peroxyketals, hydroperoxides, and dialkyl peroxides. , diacyl peroxide type, peroxy ester type, and peroxydicarbonate type.
- organic peroxides such as ketone peroxides, peroxyketals, hydroperoxides, and dialkyl peroxides.
- diacyl peroxide type, peroxy ester type, and peroxydicarbonate type One type or two or more types of these organic oxides can be used.
- One type or two or more types of these organic oxides can be used, and the amount thereof is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 3 parts by mass, based on the entire resin composition. be.
- the curing accelerator for the above organic peroxide naphthenic acid metal complexes, dimethylaniline, quaternary ammonium salts, and phosphoric acid esters can be used.
- radical initiators can be used as photoradical polymerization initiators that generate radicals upon light irradiation, such as 1-[4-(2-hydroxyethoxy)phenyl]-2 -Hydroxy-2-methyl-1-propan-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, benzophenone, 2,2-dimethoxy-1,2-diphenylethan-1-one, 2,4,6- Trimethylbenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylethoxyphosphine oxide, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone-1, 2-hydroxy-2-methyl-1- Phenyl-propan-1-one, 2-methyl-1-[4-methylthio]phenyl]-2-morpholinopropan-1-one, benzoin methyl ether, benzoin ethyl ether, benzoin isobutyl ether, benzoin methyl ether
- Cationic polymerization initiator (D) examples include TA-60, TA-60B, TA-100, and TA-120 manufactured by San-Apro; Adeka Opton CP-77 and Adeka Opton CP-66 manufactured by ADEKA. CI-2639, CI-2624 manufactured by Nippon Soda; CXC-1612, CXC-1738 manufactured by King Industries; Sun-Aid SI-45, San-Aid SI-60, San-Aid SI-80, Sun-Aid manufactured by Sanshin Chemical Industry Co., Ltd. Examples include SI-100, SunAid SI-110, SunAid SI-B3, SunAid SI-B3A, and SunAid SI-B4.
- a photosensitizer is a component for increasing sensitivity to light.
- the photosensitizer include thioxanthone derivatives, carbonyl compounds, organic sulfur compounds, persulfides, redox compounds, azo and diazo compounds, halogen compounds, photoreducible dyes, and thioxanthone derivatives are preferred.
- thioxanthone derivatives include isopropylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, thioxanthone ammonium salt, etc., and 2,4-diethylthioxanthone is preferable.
- radical polymerization initiator (C) and the cationic polymerization initiator (D) preferably one is a photopolymerization initiator and the other is a thermal polymerization initiator.
- the photosensitizers may be used alone or in combination of two or more.
- the resin composition of the present invention may contain a filler, an antistatic agent, a coupling agent, a stabilizer, a surfactant, a solvent, etc., as long as the object of the present invention is not impaired.
- Fillers such as inorganic fillers, organic fillers, and carbon diameter fillers may be included for the purpose of imparting thixotropy, improving mechanical strength by adding fillers, imparting flame retardancy, coloring, imparting conductivity, and/or imparting antistatic properties. can.
- Inorganic fillers include powders of metal oxides such as silica, zirconia, beryllia, magnesium oxide, titania, and iron oxide; sols such as colloidal silica, titania sol, and alumina sol; clay minerals such as talc, kaolinite, and smectite; carbonized Carbides such as silicon and titanium carbide; nitrides such as silicon nitride, aluminum nitride, and titanium nitride; borides such as boron nitride, titanium boride, and boron oxide; composite oxides such as mullite; aluminum hydroxide, water Hydroxides such as magnesium oxide and iron hydroxide; barium titanate, strontium carbonate, magnesium silicate, lithium silicate, sodium silicate, potassium silicate, glass, lithium cobaltate, olivine-type lithium iron phosphate, etc. salt, etc.
- metal oxides such as silica, zirconia, beryllia, magnesium oxide,
- organic filler examples include particles, fibers, and flakes of acrylic resin, epoxy resin, polyimide, and cellulose.
- Examples of carbon-based fillers include graphite, acetylene black, and carbon nanotubes.
- fillers may be used in the form of powder, in the form of water-dispersed colloids such as silica sol or aluminum sol, or in the form of dispersed in organic solvents such as organosol.
- the filler particles preferably have an average particle diameter of 0.005 to 500 ⁇ m, more preferably 0.01 to 100 ⁇ m.
- the average particle diameter and particle size distribution can be measured using, for example, a laser diffraction/scattering particle size distribution measuring device, and specifically, LA-920 manufactured by Horiba, Ltd. or the like can be used.
- the filler can be contained in an amount of, for example, 4,900 parts by mass or less per 100 parts by mass of the resin composition, preferably 0.1 to 1,900 parts by mass, and more preferably 10 to 900 parts by mass.
- antistatic agent imidazolium salts such as 1,3-dimethylimidazolium methyl sulfate, 1-ethyl-3-methylimidazolium bis(pentafluoroethylsulfonyl)imide, 1-ethyl-3-methylimidazolium bromide, etc.
- Pyridinium salt derivatives such as 3-methyl-1-propylpyridimium bis(trifluoromethylsulfonyl)imide and 1-butyl-3-methylpyridinium bis(trifluoromethylsulfonyl)imide; Tetrabutylammonium heptadecafluorooctane Examples include alkylammonium derivatives such as sulfonate and tetraphenylammonium methanesulfonate; phosphonium salt derivatives such as tetrabutylphosphonium methanesulfonate; and composite conductivity imparting agents such as a complex of polyalkylene glycol and lithium perchlorate.
- the antistatic agent can be contained in an amount of, for example, 40 parts by mass or less, preferably 0.01 to 40 parts by mass, and more preferably 0.1 to 30 parts by mass, based on 100 parts by mass of the resin composition. More preferably, it is 0.5 to 5 parts by mass.
- [Coupling agent] As a coupling agent, (tridecafluoro-1,1,2,2-tetrahydrooctyl)triethoxysilane is used as a fluorine-based silane coupling agent, and a coupling agent manufactured by Shin-Etsu Chemical Co., Ltd. (as an epoxy-modified silane coupling agent) (Product name: KBM-403), a coupling agent manufactured by Toagosei Co., Ltd.
- TESOX oxetane-modified silane coupling agent
- triethanolamine titanate titanium acetylacetonate, titanium ethyl acetoacetate, titanium lactate, titanium lactate ammonium salt, tetrastearyl titanate, isopropyl tricumylphenyl titanate, isopropyl tri(N-aminoethyl-aminoethyl) titanate, dicumyl Phenyloxyacetate titanate, isopropyl trioctanor titanate, isopropyl dimethacryisostearoyl titanate, titanium lactate ethyl ester, octylene glycol titanate, isopropyl triisostearoyl titanate, triisostearyl isopropyl titanate, isopropyl tridodecylbenzenesulfonyl titanate, tetra(2) -ethylhexyl) titanate, butyl titanate dimer, isopropyl isostearoy
- coupling agents can be used alone or in an appropriate combination of two or more.
- a titanium-based coupling agent or a silane coupling agent is preferred.
- Such coupling agents can be used to improve adhesion when molding a resin composition onto another base material, but by coating the filler surface with these coupling agents, the resin composition It is also possible to improve mechanical strength by increasing affinity with the matrix.
- the coupling agent can be contained in an amount of, for example, 40 parts by mass or less, preferably 0.01 to 40 parts by mass, and more preferably 0.1 to 30 parts by mass, based on 100 parts by mass of the resin composition. More preferably, it is 0.5 to 5 parts by mass.
- the resin composition can include a stabilizer.
- stabilizers include, without particular limitation, 2,6-di-t-butylphenol, 2,4-di-t-butylphenol, 2,6-di-t-butyl-4-ethylphenol, Phenolic antioxidants such as 2,4-bis-(N-octylthio)-6-(4-hydroxy-3,5-di-t-butylanilino)-1,3,5-triazine; alkyldiphenylamine, N, Aromatic amine antioxidants such as N'-diphenyl-p-phenylenediamine, 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline, and N-phenyl-N'-isopropyl-p-phenylenediamine.
- Benzotriazole light stabilizers Hindered amine light stabilizers such as phenyl-4-piperidinyl carbonate, bis-[2,2,6,6-tetramethyl-4-piperidinyl sebacate]; [2,2'- Ni-based light stabilizers such as thio-bis(4-t-octylphenolate)]-2-ethylhexylamine-nickel (II); cyanoacrylate-based light stabilizers; oxalic acid anilide-based light stabilizers; fullerene, hydrogenated Examples include fullerene-based light stabilizers such as fullerene and fullerene hydroxide. These stabilizers may be used alone or in combination.
- the stabilizer may be contained in an amount of, for example, 10 parts by mass or less, preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.05 to 5 parts by mass, based on 100 parts by mass of the resin composition. is 0.1 to 1 part by mass.
- the resin composition can contain a surfactant for the purpose of adjusting wettability, antifoaming properties, and/or smoothness within a range that does not impair coatability.
- surfactant examples include anionic surfactants, double-sided surfactants, and nonionic surfactants.
- anionic surfactants include soap, lauryl sulfate, polyoxyethylene alkyl ether sulfate, alkylbenzene sulfonate (e.g., dodecylbenzene sulfonate), polyoxyethylene alkyl ether phosphate, polyoxyethylene alkyl Phenyl ether phosphate, N-acylamino acid salt, ⁇ -olefin sulfonate, alkyl sulfate salt, alkylphenyl ether sulfate salt, methyl taurate, trifluoromethane sulfonate, pentafluoroethane sulfonate, heptafluoro Examples include propane sulfonate and nonafluorobutane sulfonate, and sodium ion, lithium ion, etc. can be used as the counter cation.
- amphoteric surfactants include alkyldiaminoethylglycine hydrochloride, 2-alkyl-N-carboxymethyl-N-hydroxyethylimidazolinium betaine, lauryldimethylaminoacetic acid betaine, coconut oil fatty acid amidopropyl betaine, fatty acid alkyl betaine, Examples include sulfobetaine and amine oxide.
- nonionic (nonionic) surfactants examples include alkyl ester type compounds of polyethylene glycol, alkyl ether type compounds such as triethylene glycol monobutyl ether, ester type compounds such as polyoxysorbitan ester, alkylphenol type compounds, and fluorine type compounds. , silicone type compounds, and the like.
- the surfactants may be used alone or in combination.
- the surfactant can be contained in an amount of, for example, 50 parts by weight or less, preferably 0.01 to 50 parts by weight, more preferably 0.05 to 20 parts by weight, based on 100 parts by weight of the resin composition. , more preferably 0.1 to 10 parts by mass.
- the resin composition can be produced by mixing and stirring the above components. Stirring can be performed using a stirring device such as a propeller mixer, a planetary mixer, a hybrid mixer, a kneader, an emulsifying homogenizer, a three-roll mill, a bead mill, and an ultrasonic homogenizer. Moreover, stirring can be performed while heating or cooling as necessary.
- a stirring device such as a propeller mixer, a planetary mixer, a hybrid mixer, a kneader, an emulsifying homogenizer, a three-roll mill, a bead mill, and an ultrasonic homogenizer.
- Heating method For heating, various known methods can be used, such as hot air, a hot plate, an oven, infrared rays, microwaves, etc.
- cooling in addition to natural cooling, various known methods can be used, such as cooling gas, pressing against a heat sink, etc.
- the resin composition of the present invention may further contain a solvent.
- a solvent hydrocarbons (propane, n-butane, n-pentane, isohexane, cyclohexane, n-octane, isooctane, benzene, toluene, xylene, ethylbenzene, amylbenzene, turpentine, pinene, etc.), halogenated hydrocarbons (chlorinated Methyl, chloroform, carbon tetrachloride, ethylene chloride, methyl bromide, ethyl bromide, chlorobenzene, chlorobromomethane, bromobenzene, fluorodichloromethane, dichlorodifluoromethane, difluorochloroethane, etc.), alcohol (methanol, ethanol, 1-propanol, Isopropanol, 1-butanol, 1-pentan
- the resin composition is not particularly limited, and may include a compound (A) having a (meth)acryloyl group, a compound (B) having an epoxy group and/or an oxetanyl group, a radical initiator, a cationic initiator, and any components thereof. It is prepared by mixing in a known manner.
- the compound (A) having a (meth)acryloyl group and the compound (B) having an epoxy group and/or oxetanyl group are each appropriately selected from the viewpoint of compatibility so that a phase-separated molded article can be obtained.
- the compound (A) having a (meth)acryloyl group and the compound (B) having an epoxy group and/or an oxetanyl group phase separate as a soft segment and a hard segment, preferably, (meth)
- the compound (A) having an acryloyl group and the compound (B) having an epoxy group and/or an oxetanyl group can be selected based on the hydrogen-bonding substituent value.
- the hydrogen-bonding substituent is a group capable of forming a hydrogen bond, and includes, for example, a hydroxyl group, a mercapto group, and an amino group.
- the compatibility of the hydrogen-bonding substituent group can be arbitrarily adjusted by hydrogen bonding.
- phase separation of the resin composition can be suppressed by bringing the hydrogen-bonding substituent values of the compound (A) having a (meth)acryloyl group and the compound (B) having an epoxy group and/or oxetanyl group close to each other.
- phase separation of the resin composition can be promoted by making the hydrogen-bonding substituent values of the compound (A) having a (meth)acryloyl group and the compound (B) having an epoxy group and/or oxetanyl group far apart.
- the hydrogen bond substituent value of either the compound (A) having a (meth)acryloyl group or the compound (B) having an epoxy group and/or an oxetanyl group is 0.0001 mol/g or more, preferably 0.0005 mol/g or more and 0.1111 mol/g or less, preferably 0.1000 mol/g or less.
- the valence of one hydrogen-bonding substituent to the valence of the other hydrogen-bonding substituent is 2/3 or less, preferably 1/2 or less, and, for example, 1/100 or more, preferably 1 /20.
- the other hydrogen-bonding substituent value is, for example, 0.000001 mol/g or more, preferably 0.000005 mol/g or more.
- the other hydrogen-bonding substituent value is, for example, 0.0741 mol/g or less, preferably 0.0667 mol/g or less.
- the hydrogen-bonding substituent valence can be calculated from the number of hydrogen-bonding substituent valences contained in one molecule using the following formula (1).
- Hydrogen-bonding substituent value (mol/g) number of hydrogen-bonding substituents in one molecule ⁇ molecular weight (1)
- the mixing ratio of the compound (A) having a (meth)acryloyl group and the compound (B) having an epoxy group and/or oxetanyl group is appropriately selected depending on the purpose and use.
- the contribution of the soft segment and the hard segment can be adjusted depending on the volume ratio of the compound (A) having a (meth)acryloyl group and the compound (B) having an epoxy group and/or an oxetanyl group.
- the physical properties of the resin composition can be adjusted as desired by increasing the amount of the soft segment to make it more flexible, or by decreasing it to make it more rigid.
- the compatibility changes depending on the mixing ratio, the type of compound (A), and the type of compound (B), it can be adjusted as desired from the viewpoint of generating a phase-separated structure and expressing desired characteristics.
- the content of compound (A) is, for example, 1 part by mass or more, preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and, for example, 55 parts by mass or less.
- the content ratio of compound (B) is, for example, 45 parts by mass or more and, for example, 99 parts by mass or less, preferably, with respect to 100 parts by mass of the total amount of compound (A) and compound (B). It is 95 parts by mass or less, more preferably 90 parts by mass or less.
- the content ratio of the compound (A) is For example, 1 part by mass or more, preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and preferably 50 parts by mass or less, based on 100 parts by mass of the total amount of (A) and compound (B). is 45 parts by mass or less.
- the content ratio of compound (B) is, for example, 50 parts by mass or more, preferably 55 parts by mass or more, and, for example, 99 parts by mass, based on 100 parts by mass of the total amount of compound (A) and compound (B). parts, preferably 95 parts by weight or less, more preferably 90 parts by weight or less.
- the content ratio of the compound (A) is, for example, , 1 part by mass or more, preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and, for example, 55 parts by mass or less.
- the content ratio of compound (B) is, for example, 45 parts by mass or more and, for example, 99 parts by mass or less, preferably, with respect to 100 parts by mass of the total amount of compound (A) and compound (B). It is 95 parts by mass or less, more preferably 90 parts by mass or less.
- Whether a phase separation structure has occurred can also be determined by whether two or more peaks of the loss modulus tan ⁇ are measured.
- the loss elastic modulus derived from the soft segment is tan ⁇ 1 and the loss elastic modulus derived from the hard segment is tan ⁇ 2 , the peak position of tan ⁇ 1 is less than 100°C (first peak), tan ⁇ If the peak position of 2 is 100°C or higher (second peak) and the minimum value of the loss modulus tan ⁇ 3 is 0.1 or lower at 100°C or lower, a flexible film with excellent heat resistance can be obtained. I found it.
- the mixing ratio of the compound (A) having a (meth)acryloyl group and the compound (B) having an epoxy group and/or oxetanyl group can be adjusted depending on the desired physical properties.
- Method for producing cured resin product A cured resin product is obtained by curing a resin composition.
- the curing method is appropriately selected depending on the type of radical polymerization initiator (C) and cationic polymerization initiator (D).
- the resin when the radical polymerization initiator (C) is a photoradical polymerization initiator and the cationic polymerization initiator (D) is a photocationic polymerization initiator, the resin is irradiated with active energy rays. Curing the composition. Moreover, when the radical polymerization initiator (C) is a thermal radical polymerization initiator and the cationic polymerization initiator (D) is a thermal cationic polymerization initiator, the resin composition is cured by heating.
- the radical polymerization initiator (C) is a photoradical polymerization initiator
- the cationic polymerization initiator (D) is a thermal cationic polymerization initiator
- the radical polymerization initiator (C) is When it is a thermal radical polymerization initiator and the cationic polymerization initiator (D) is a photocationic polymerization initiator, the resin composition is cured by irradiation with active energy rays and heating.
- the resin composition is cured only by irradiation with active energy rays, or by a combination of irradiation with active energy rays and heating.
- the active energy ray is appropriately selected depending on the type of the photoradical polymerization initiator and the photocationic polymerization initiator, but ultraviolet rays are preferably used.
- the heating temperature is, for example, 30°C or higher and, for example, 70°C or lower.
- the heating time is, for example, 10 minutes or more and, for example, 120 minutes or less.
- the peak top position on the long wavelength side of the light absorption wavelength of the photoradical polymerization initiator and the light absorption wavelength side of the photocationic polymerization initiator be
- the radical polymerization initiator (C) and the cationic polymerization initiator (D) are selected so that the absolute value of the difference from the peak top position on the longer wavelength side of the absorption wavelength is 30 nm or more.
- the peak top position corresponds to the peak top position on the longer wavelength side of the peak top position of the radical polymerization initiator (C) and the peak top position of the cationic polymerization initiator (D).
- the peak top position corresponds to the peak top position on the longer wavelength side of the peak top position of the radical polymerization initiator (C) and the peak top position of the cationic polymerization initiator (D).
- Such cured resin products have excellent bending strength and heat resistance, and are therefore particularly suitable for use as substrates for foldable displays used in liquid crystal displays and organic EL displays.
- Manufacturing example 1 (1) Synthesis of isocyanate group-terminated prepolymer In a nitrogen atmosphere, in a separable glass flask, 100 parts of polyoxypropylene polyol (manufactured by Mitsui Chemicals SKC Polyurethane; DL 10,000, average number of functional groups 2, number average molecular weight 10,000) was placed as a polyol component. was introduced. Next, in a separable flask, 1,3-bis(isocyanatomethyl)cyclohexane (manufactured by Mitsui Chemicals; 1,3-H 6 XDI) was added as a polyisocyanate component in a proportion such that the equivalent ratio (NCO/OH) was 8.0. I put it in.
- polyoxypropylene polyol manufactured by Mitsui Chemicals SKC Polyurethane; DL 10,000, average number of functional groups 2, number average molecular weight 10,000
- 1,3-bis(isocyanatomethyl)cyclohexane manufactured by Mitsu
- Production example 4 100 parts of bisphenol A type epoxy resin (product name: EPICLON-850) manufactured by DIC Corporation, 0.07 parts of triphenylphosphine, 0.03 parts of hydroquinone, and 100 parts of toluene were placed in a 500 ml three-necked flask and heated at 100°C under an argon atmosphere. Then, 16 parts of acetic acid was added dropwise over 1 hour, and the mixture was further heated for 4 hours. Thereafter, 0.2 part of xylene sulfonic acid was added, and the mixture was further stirred at 40°C for 1 hour. Toluene was distilled off using an evaporator to obtain partially esterified epoxy resin 5.
- EPICLON-850 bisphenol A type epoxy resin manufactured by DIC Corporation
- Comparative manufacturing example 1 100 parts of bisphenol A type epoxy resin manufactured by Yuka Shell Epoxy Co., Ltd. (product name: Epicote 1004, epoxy equivalent 900), 0.07 parts of triphenylphosphine, 0.03 parts of hydroquinone, and 100 parts of toluene were placed in a 500 ml three-necked flask and placed in an argon atmosphere. Then, 4.0 parts of acetic acid was added dropwise at 100° C. over 1 hour, and the mixture was further heated for 4 hours. Thereafter, 0.2 part of xylene sulfonic acid was added, and the mixture was further stirred at 40°C for 1 hour. Toluene was distilled off using an evaporator to obtain a partially acrylated epoxy resin.
- Comparative manufacturing example 2 (1) Synthesis of isocyanate group-terminated prepolymer In a nitrogen atmosphere, 100 parts of polyester diol (manufactured by Kuraray; P-1010, average functional group number 2, number average molecular weight 1000) as a polyol component was charged into a glass separable flask. . Next, tolylene diisocyanate (manufactured by Mitsui Chemicals; Cosmonate T-100) as a polyisocyanate component was charged into the separable flask at a ratio such that the equivalent ratio (NCO/OH) was 2.0. Thereafter, the mixture was heated to 80°C.
- polyester diol manufactured by Kuraray; P-1010, average functional group number 2, number average molecular weight 1000
- tolylene diisocyanate manufactured by Mitsui Chemicals; Cosmonate T-100
- the above resin composition was formed into a PET film using a doctor blade to obtain a coating film with a thickness of 100 ⁇ m. Next, the above coating film was irradiated with active energy rays.
- the output of the active energy rays was 100 mW/cm 2 (measured with a luminometer (3664 optical power meter manufactured by Hioki Electric Co., Ltd. (measurement wavelength: 405 nm)), and irradiation was performed so that the cumulative light amount was 6000 mJ/cm 2 . Then, heat aging was performed at 40° C. for 30 minutes.
- the resin composition was cured (polymerized) and a cured resin product was obtained.
- Example 2 A cured resin product was obtained in the same manner as in Example 1 except that the ratio of the urethane acrylate resin in Production Example 1 was increased.
- Example 3 A cured resin product was obtained in the same manner as in Example 2, except that the ratio of the urethane acrylate resin in Production Example 1 was increased.
- Example 4 A cured resin product was obtained in the same manner as in Example 3 except that the ratio of the urethane acrylate resin in Production Example 1 was increased.
- Comparative example 1 A cured resin product was obtained in the same manner as in Example 4, except that the urethane acrylate resin of Production Example 1 was not blended.
- Comparative examples 2 to 7 A cured resin product was obtained in the same manner as in Example 4, except that the ratio of the urethane acrylate resin in Production Example 1 was increased.
- Comparative example 8 A cured resin product was produced in the same manner as in Example 4, except that the urethane acrylate resin of Production Example 1 was not blended, and Osaka Gas Chemical Co., Ltd., fluorene-based epoxy resin, OGSOL PG-100 (epoxy resin 3) was used. Obtained.
- Example 10 The same method as in Example 9 was used, except that a peroxide (manufactured by NOF Corporation; Percure O, benzoyl peroxide) was used instead of the UV radical initiator, and after UV curing, it was cured at 120 ° C. x 30 minutes. A cured resin product was obtained.
- a peroxide manufactured by NOF Corporation; Percure O, benzoyl peroxide
- Example 11 A cured resin was obtained in the same manner as in Example 9, except that after UV curing at 405 nm x 1000 mJ/cm 2 , further UV curing was performed at 365 nm x 6000 mJ/cm 2 .
- Example 12 A cured resin was obtained in the same manner as in Example 1, except that the urethane acrylate resin of Production Example 1 was changed to the urethane acrylate resin of Production Example 2.
- Example 13 A cured resin product was obtained in the same manner as in Example 12, except that Epoxy Resin 1 was changed to Epoxy Resin 4 (epoxy resin of Production Example 3).
- Example 14 A cured resin product was obtained in the same manner as in Example 1, except that Epoxy Resin 1 was changed to Epoxy Resin 5 (epoxy resin of Production Example 4).
- Comparative Example 14 (based on Example 3 of JP-A-7-199359) Each component was mixed at 25° C. according to the following recipe to obtain a resin composition, and a cured resin product was obtained in the same manner as in Example 1.
- Example 1 Furthermore, the resin composition of Example 1 was subjected to transmission electron microscopy. The results are shown in Figure 1.
- the resin composition, cured resin product, and method for producing a cured resin product of the present invention are suitably used in foldable display substrates used in liquid crystal displays and organic EL displays.
Landscapes
- Chemical & Material Sciences (AREA)
- Health & Medical Sciences (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Medicinal Chemistry (AREA)
- Polymers & Plastics (AREA)
- Organic Chemistry (AREA)
- Epoxy Resins (AREA)
- Macromonomer-Based Addition Polymer (AREA)
Priority Applications (1)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2024548308A JP7848341B2 (ja) | 2022-09-22 | 2023-09-21 | 樹脂組成物、樹脂硬化物および樹脂硬化物の製造方法 |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2022151806 | 2022-09-22 | ||
| JP2022-151806 | 2022-09-22 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2024063130A1 true WO2024063130A1 (ja) | 2024-03-28 |
Family
ID=90454701
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2023/034252 Ceased WO2024063130A1 (ja) | 2022-09-22 | 2023-09-21 | 樹脂組成物、樹脂硬化物および樹脂硬化物の製造方法 |
Country Status (3)
| Country | Link |
|---|---|
| JP (1) | JP7848341B2 (cg-RX-API-DMAC7.html) |
| TW (1) | TW202428675A (cg-RX-API-DMAC7.html) |
| WO (1) | WO2024063130A1 (cg-RX-API-DMAC7.html) |
Citations (7)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH06102693A (ja) * | 1992-09-21 | 1994-04-15 | Canon Inc | 電子写真感光体 |
| JPH07258388A (ja) * | 1994-03-16 | 1995-10-09 | Air Prod And Chem Inc | ポリ−n−メチル化第2級アミンを含む可撓化されたポリエポキシド樹脂 |
| WO2005037876A1 (ja) * | 2003-10-15 | 2005-04-28 | Toagosei Co., Ltd. | オキセタニル基を有するポリマー、及びこれを含むカチオン硬化性樹脂組成物 |
| JP2005227367A (ja) * | 2004-02-10 | 2005-08-25 | Sekisui Chem Co Ltd | 液晶表示素子用硬化性樹脂組成物、液晶滴下工法用シール剤、上下導通材料及び液晶表示素子 |
| JP2020078547A (ja) * | 2018-11-12 | 2020-05-28 | アクシュネット カンパニーAcushnet Company | 熱可塑性ブレンドを組み込んだゴルフボール |
| WO2021200794A1 (ja) * | 2020-03-30 | 2021-10-07 | 三井化学株式会社 | 活性エネルギー線硬化性ポリウレタン樹脂、硬化性樹脂組成物、および、活性エネルギー線硬化性ポリウレタン樹脂の製造方法 |
| WO2023090230A1 (ja) * | 2021-11-16 | 2023-05-25 | 三井化学株式会社 | パターン形成方法、パターン、パターン付成形物の製造方法、および、パターン付成形物 |
-
2023
- 2023-09-21 JP JP2024548308A patent/JP7848341B2/ja active Active
- 2023-09-21 WO PCT/JP2023/034252 patent/WO2024063130A1/ja not_active Ceased
- 2023-09-22 TW TW112136174A patent/TW202428675A/zh unknown
Patent Citations (7)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH06102693A (ja) * | 1992-09-21 | 1994-04-15 | Canon Inc | 電子写真感光体 |
| JPH07258388A (ja) * | 1994-03-16 | 1995-10-09 | Air Prod And Chem Inc | ポリ−n−メチル化第2級アミンを含む可撓化されたポリエポキシド樹脂 |
| WO2005037876A1 (ja) * | 2003-10-15 | 2005-04-28 | Toagosei Co., Ltd. | オキセタニル基を有するポリマー、及びこれを含むカチオン硬化性樹脂組成物 |
| JP2005227367A (ja) * | 2004-02-10 | 2005-08-25 | Sekisui Chem Co Ltd | 液晶表示素子用硬化性樹脂組成物、液晶滴下工法用シール剤、上下導通材料及び液晶表示素子 |
| JP2020078547A (ja) * | 2018-11-12 | 2020-05-28 | アクシュネット カンパニーAcushnet Company | 熱可塑性ブレンドを組み込んだゴルフボール |
| WO2021200794A1 (ja) * | 2020-03-30 | 2021-10-07 | 三井化学株式会社 | 活性エネルギー線硬化性ポリウレタン樹脂、硬化性樹脂組成物、および、活性エネルギー線硬化性ポリウレタン樹脂の製造方法 |
| WO2023090230A1 (ja) * | 2021-11-16 | 2023-05-25 | 三井化学株式会社 | パターン形成方法、パターン、パターン付成形物の製造方法、および、パターン付成形物 |
Also Published As
| Publication number | Publication date |
|---|---|
| TW202428675A (zh) | 2024-07-16 |
| JPWO2024063130A1 (cg-RX-API-DMAC7.html) | 2024-03-28 |
| JP7848341B2 (ja) | 2026-04-20 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP5527871B2 (ja) | 紫外線硬化型ハードコート樹脂組成物 | |
| JP2010138393A (ja) | 光学レンズシート用エネルギー線硬化型樹脂組成物及びその硬化物 | |
| JP7022033B2 (ja) | 硬化性組成物及びその硬化物 | |
| JP6468355B2 (ja) | 樹脂組成物及びそれを用いた立体造形物 | |
| JP2012092307A (ja) | 光学レンズシート用エネルギー線硬化型樹脂組成物及びその硬化物 | |
| JPWO2015198787A1 (ja) | 活性エネルギー線硬化型樹脂組成物、塗料、塗膜、及び積層フィルム | |
| JP5307511B2 (ja) | 被膜形成用ラジカル重合性樹脂組成物 | |
| JP5059538B2 (ja) | 硬化性組成物、その硬化物 | |
| WO2023074601A1 (ja) | 嫌気硬化性組成物 | |
| JP6381318B2 (ja) | 光学レンズ用活性エネルギー線硬化性樹脂組成物 | |
| US20240101752A1 (en) | Silicone urethane (meth)acrylates and their use in 3d printing resins and coating compositions | |
| JP4935648B2 (ja) | フィルム状光導波路 | |
| WO2018212263A1 (ja) | フッ素系重合体含有光硬化性組成物 | |
| JP7848341B2 (ja) | 樹脂組成物、樹脂硬化物および樹脂硬化物の製造方法 | |
| WO2019230537A1 (ja) | 光硬化性組成物およびその硬化物 | |
| JP7324939B2 (ja) | 活性エネルギー線硬化性ポリウレタン樹脂、硬化性樹脂組成物、および、活性エネルギー線硬化性ポリウレタン樹脂の製造方法 | |
| JP2018199805A (ja) | 硬化性組成物及び硬化物 | |
| JP5222156B2 (ja) | カルボキシレート樹脂及びそれを含有する樹脂組成物 | |
| JP7210844B2 (ja) | 賦形フィルム及び光硬化型組成物 | |
| WO2024214490A1 (ja) | 樹脂組成物、樹脂硬化物、樹脂硬化物の製造方法、電子装置、電子装置の製造方法、および、樹脂シート | |
| WO2024095925A1 (ja) | 爪または人工爪用光硬化性組成物 | |
| TW202424031A (zh) | 片狀的光硬化性組成物、光硬化性組成物、片狀的光硬化性組成物之製造方法及積層體 | |
| JP2019065309A (ja) | 光湿気硬化型樹脂組成物硬化体 | |
| JP7243070B2 (ja) | 硬化性樹脂成形体、機能性フィルム、硬化性樹脂成形体の製造方法、及び硬化性樹脂フィルムの製造方法 | |
| JP2008260898A (ja) | 硬化性樹脂組成物及びその硬化物 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 23868251 Country of ref document: EP Kind code of ref document: A1 |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 2024548308 Country of ref document: JP |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| 122 | Ep: pct application non-entry in european phase |