WO2023234140A1 - シリコーン離型ポリエステルフィルム、及びその製造方法 - Google Patents

シリコーン離型ポリエステルフィルム、及びその製造方法 Download PDF

Info

Publication number
WO2023234140A1
WO2023234140A1 PCT/JP2023/019324 JP2023019324W WO2023234140A1 WO 2023234140 A1 WO2023234140 A1 WO 2023234140A1 JP 2023019324 W JP2023019324 W JP 2023019324W WO 2023234140 A1 WO2023234140 A1 WO 2023234140A1
Authority
WO
WIPO (PCT)
Prior art keywords
silicone
mass
parts
less
polyester film
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2023/019324
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
公典 西山
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Toyobo Co Ltd
Original Assignee
Toyobo Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toyobo Co Ltd filed Critical Toyobo Co Ltd
Priority to JP2024524776A priority Critical patent/JP7901304B2/ja
Priority to CN202380036088.XA priority patent/CN119110822A/zh
Priority to KR1020247031360A priority patent/KR20240144465A/ko
Publication of WO2023234140A1 publication Critical patent/WO2023234140A1/ja
Anticipated expiration legal-status Critical
Priority to JP2026068441A priority patent/JP2026123074A/ja
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J7/00—Chemical treatment or coating of shaped articles made of macromolecular substances
    • C08J7/04—Coating
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B05—SPRAYING OR ATOMISING IN GENERAL; APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
    • B05D—PROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
    • B05D5/00—Processes for applying liquids or other fluent materials to surfaces to obtain special surface effects, finishes or structures
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B05—SPRAYING OR ATOMISING IN GENERAL; APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
    • B05D—PROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
    • B05D7/00—Processes, other than flocking, specially adapted for applying liquids or other fluent materials to particular surfaces or for applying particular liquids or other fluent materials
    • B05D7/24—Processes, other than flocking, specially adapted for applying liquids or other fluent materials to particular surfaces or for applying particular liquids or other fluent materials for applying particular liquids or other fluent materials
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J5/00—Manufacture of articles or shaped materials containing macromolecular substances
    • C08J5/18—Manufacture of films or sheets
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
    • C09D183/00—Coating compositions based on macromolecular compounds obtained by reactions forming in the main chain of the macromolecule a linkage containing silicon, with or without sulfur, nitrogen, oxygen, or carbon only; Coating compositions based on derivatives of such polymers
    • C09D183/04—Polysiloxanes
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
    • C09D5/00—Coating compositions, e.g. paints, varnishes or lacquers, characterised by their physical nature or the effects produced; Filling pastes
    • C09D5/02—Emulsion paints including aerosols
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01G—CAPACITORS; CAPACITORS, RECTIFIERS, DETECTORS, SWITCHING DEVICES, LIGHT-SENSITIVE OR TEMPERATURE-SENSITIVE DEVICES OF THE ELECTROLYTIC TYPE
    • H01G13/00—Apparatus specially adapted for manufacturing capacitors; Processes specially adapted for manufacturing capacitors not provided for in groups H01G4/00 - H01G11/00
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J2367/00—Characterised by the use of polyesters obtained by reactions forming a carboxylic ester link in the main chain; Derivatives of such polymers

Definitions

  • the present invention relates to a silicone release polyester film. More specifically, for example, it has peelability and adhesion suitable for molding from light peeling to heavy peeling in ceramic green sheet molding used in the production of multilayer ceramic capacitors, and does not cause tearing or deformation of the sheets.
  • the present invention relates to a silicone release polyester film that can prevent this, and a method for producing the same.
  • a release film is used as a carrier film for ceramic green sheet molding.
  • polyester film is used as the base material of the release film in terms of dimensional stability and heat resistance.
  • the thickness of the sheet after drying is in the range of several ⁇ m or less. Therefore, carrier films are particularly required to have easy releasability. As the film becomes thinner, the rigidity of the ceramic green sheet decreases, and the peeling force of conventional release films causes the green sheet to tear or deform when peeled off, increasing the chip failure rate, so easy peelability is required. ing.
  • a release layer made of a silicone resin having a crosslinked structure and a silicone resin not having a crosslinked structure has been proposed (for example, Patent Document 2).
  • the solvent of the coating agent used to form the mold release layer is an organic solvent, which requires large-scale equipment to treat the organic solvent during coating and drying, and the running cost of treating the evaporated organic solvent. There is a problem in that the cost increases as a result.
  • Patent Document 3 a method that does not use an organic solvent has been proposed (for example, Patent Document 3), but this method has problems such as increased viscosity of the coating material, which makes handling complicated and makes uniform coating difficult.
  • the present invention has been devised to provide an appropriate lightweight film that can be suitably used as a carrier film in the production of multilayer ceramic capacitors, and which can be peeled off without causing damage such as tearing even a very thin film.
  • the purpose of the present invention is to provide a silicone releasable polyester film with excellent releasability, a method for producing the same, and the like.
  • the present invention provides the following silicone release polyester film (silicone release polyester film).
  • the present invention also provides the following method for producing a silicone release polyester film.
  • a method for producing a silicone release polyester film comprising: An aqueous dispersion (1) of silicone (A) having a number average molecular weight of 25,000 or more and containing 3 or more alkenyl groups in one molecule, An aqueous dispersion (2) of silicone (B) having a number average molecular weight of 25,000 or less and having alkenyl groups in one molecule only at both ends; An aqueous dispersion (3) of silicone (C) having a number average molecular weight of 10,000 or less and having a hydrogen atom directly bonded to a Si atom represented by a Si-H group, and platinum catalyst, The step of forming a coating layer formed using a mold release coating composition comprising; When the total solid content of the silicone (A), the silicone (B), and the silicone (C) is 100 parts by mass, the silicone (A) is 80 parts by mass or more, and the silicone (B) is 2 parts by mass. Contains 2 parts by mass or more and 20 parts by mass or less, and silicone (
  • the silicone release polyester film of the present invention can be used as a release film for sheet molding, and has a moderately low peel strength that allows it to be peeled off without tearing or other damage even if it is a very thin film. It is possible to provide a releasable polyester film having a mold release layer with excellent uniformity.
  • the releasable polyester film of the present invention having such characteristics can be suitably used, for example, as a carrier film for molding ceramic green sheets used in ceramic multilayer capacitors.
  • the method for producing a silicone release polyester film of the present invention makes it possible to efficiently and easily obtain a silicone release polyester film having the above characteristics.
  • the silicone release polyester film of the present invention is An aqueous dispersion (1) of silicone (A) having a number average molecular weight of 25,000 or more and containing 3 or more alkenyl groups in one molecule, An aqueous dispersion (2) of silicone (B) having a number average molecular weight of 25,000 or less and having alkenyl groups in one molecule only at both ends; An aqueous dispersion (3) of silicone (C) having a number average molecular weight of 10,000 or less and having a hydrogen atom directly bonded to a Si atom represented by a Si-H group, and platinum catalyst, A silicone release polyester film having a coating layer formed using a release coating composition comprising: When the total solid content of the silicone (A), the silicone (B), and the silicone (C) is 100 parts by mass, the silicone (A) is 80 parts by mass or more, and the silicone (B) is 80 parts by mass or more. The silicone (C) is contained in an amount of 2 parts by mass or
  • polyester film Known polyesters can be used as appropriate for the polyester film of the present invention, and for example, those shown below can be suitably used.
  • polyester The polyester constituting the polyester film used as the base film (hereinafter sometimes referred to as "base material") in the present invention is not particularly limited, and polyesters commonly used as base materials for release films can be used.
  • a film molded product can be used.
  • a polyester film formed from polyethylene terephthalate is particularly suitable.
  • the repeating units of ethylene terephthalate are preferably 90 mol% or more, more preferably 95 mol% or more, and a small amount of other dicarboxylic acid components and diol components may be copolymerized.
  • the polyester film is preferably a biaxially oriented polyester film for reasons such as high elastic modulus in both directions.
  • the intrinsic viscosity of the polyester film is preferably 0.50 dl/g or more and 0.70 dl/g or less, more preferably 0.52 dl/g or more and 0.65 dl/g or less.
  • the intrinsic viscosity is 0.50 dl/g or more, it is preferable because many breaks do not occur during the stretching process.
  • it is 0.70 dl/g or less it is preferable because the cutting properties are good when cutting into a predetermined product width and dimensional defects do not occur. Further, it is preferable that the raw material pellets be sufficiently vacuum dried.
  • polyester film when it is simply described as a "polyester film", it means a polyester film having (laminated) a surface layer A and a surface layer B.
  • the method for producing the polyester film in the present invention is not particularly limited, and conventionally commonly used methods can be used.
  • it can be obtained by melting the polyester in an extruder, extruding it into a film, cooling it in a rotating cooling drum to obtain an unstretched film, and then biaxially stretching the unstretched film.
  • a biaxially stretched film can be obtained by sequentially biaxially stretching a uniaxially stretched film in the longitudinal or transverse direction in the transverse or longitudinal direction, or by simultaneously biaxially stretching an unstretched film in the longitudinal and transverse directions. can.
  • the stretching temperature during stretching of the polyester film is preferably at least the secondary transition point (Tg) of the polyester. It is preferable to stretch the film by a factor of 1 to 8 times, particularly 2 times to 6 times, in both the longitudinal and transverse directions.
  • the thickness of the polyester film is preferably 12 ⁇ m or more and 100 ⁇ m or less, more preferably 16 ⁇ m or more and 50 ⁇ m or less, and even more preferably 19 ⁇ m or more and 33 ⁇ m or less. If the thickness of the film is 12 ⁇ m or more, there is no risk of deformation due to heat during film production, processing, and molding, which is preferable. On the other hand, if the thickness of the film is 100 ⁇ m or less, the amount of film to be discarded after use will not be excessively large, which is preferable in terms of reducing environmental burden.
  • the polyester film base material may be a single layer or a multilayer of two or more layers.
  • the base film may be a polyester film having a surface layer A that does not substantially contain particles having a particle size of 1.0 ⁇ m or more and a surface layer B that contains particles.
  • surface layer A does not substantially contain inorganic particles having a particle size of 1.0 ⁇ m or more.
  • particles having a particle size of less than 1.0 ⁇ m and 1 nm or more may be present in the surface layer A. Since the surface layer A does not substantially contain particles having a particle size of 1.0 ⁇ m or more, for example, inorganic particles, it is possible to reduce problems caused by transfer of the shape of particles in the base material to the resin sheet.
  • the surface layer A does not contain particles with a particle size of less than 1.0 ⁇ m, so that problems caused by transfer of the particle shape in the base material to the resin sheet can be more effectively suppressed.
  • the polyester film base material is preferably a laminated film having a surface layer A substantially free of inorganic particles on at least one side. Thereby, it is possible to more effectively suppress the transfer of the particle shape in the base material to the resin sheet and the occurrence of defects.
  • the surface layer A that does not substantially contain particles with a particle size of less than 1.0 ⁇ m also substantially does not contain particles with a particle size of 1.0 ⁇ m or more.
  • substantially no particles means, for example, in the case of inorganic particles of less than 1.0 ⁇ m, the amount of inorganic elements determined by fluorescent X-ray analysis is 50 ppm or less, preferably 10 ppm. Hereinafter, it most preferably means a content that is below the detection limit. Even if particles are not actively added to the film, contaminants derived from foreign substances or dirt attached to the raw resin or the line or equipment in the film manufacturing process are peeled off and mixed into the film. This is because there is. Moreover, "substantially not containing particles with a particle size of 1.0 ⁇ m or more” means that particles with a particle size of 1.0 ⁇ m or more are not included.
  • a surface layer B which can contain inorganic particles, on the opposite side of the surface layer A, which does not substantially contain inorganic particles.
  • the layer on the side to which the release layer is applied is layer A
  • the layer on the opposite side is layer B
  • the other core layer is layer C
  • the layer structure in the thickness direction is release layer/A/ B, or a laminated structure such as release layer/A/C/B.
  • the C layer may have a plurality of layers.
  • the surface layer B may not contain inorganic particles. In that case, it is preferable to provide a coating layer containing at least inorganic particles and a binder on the surface layer B in order to provide slipperiness for winding up the film into a roll.
  • the surface layer B forming the opposite surface to the surface to which the release layer is applied preferably contains inorganic particles from the viewpoint of the slipperiness of the film and the ease with which air can escape.
  • inorganic particles from the viewpoint of the slipperiness of the film and the ease with which air can escape.
  • silica particles and/or calcium carbonate particles it is preferable to use silica particles and/or calcium carbonate particles.
  • the total amount of inorganic particles contained in the surface layer B is preferably 5,000 ppm or more and 15,000 ppm or less.
  • the area surface average roughness (Sa) of the film of the surface layer B is preferably in the range of 1 nm or more and 40 nm or less. More preferably, the range is 5 nm or more and 35 nm or less.
  • the total amount of silica particles and/or calcium carbonate particles is 5000 ppm or more and Sa is 1 nm or more, air can be released uniformly when the film is rolled up, resulting in a good rolled shape and good flatness. , it is suitable for producing ultra-thin ceramic green sheets.
  • the lubricant is less likely to aggregate and coarse protrusions are not formed, resulting in stable quality when producing ultra-thin ceramic green sheets. It is preferable.
  • inert inorganic particles and/or heat-resistant organic particles can also be used as the particles contained in layer B, but from the viewpoint of transparency and cost, silica particles and/or More preferably, calcium carbonate particles are used.
  • other inorganic particles that can be used include alumina-silica composite oxide particles, hydroxyapatite particles, and the like.
  • the heat-resistant organic particles include crosslinked polyacrylic particles, crosslinked polystyrene particles, and benzoguanamine particles.
  • porous colloidal silica is preferable, and when using calcium carbonate particles, light calcium carbonate whose surface is treated with a polyacrylic acid-based polymer compound is preferable from the viewpoint of preventing the lubricant from falling off. .
  • the average particle diameter of the inorganic particles added to the surface layer B is preferably 0.1 ⁇ m or more and 2.0 ⁇ m or less, particularly preferably 0.3 ⁇ m or more and 1.0 ⁇ m or less. It is preferable that the average particle diameter of the inorganic particles is 0.1 ⁇ m or more because the release film has good slip properties. Further, if the average particle diameter is 2.0 ⁇ m or less, there is no risk of adversely affecting the smoothness of the surface of the mold release layer, so there is no risk of pinholes occurring in the ceramic green sheet, which is preferable.
  • a film may be applied to the surface of the surface layer A and/or surface layer B before or after uniaxial stretching during the film forming process.
  • a coating layer may be provided on the substrate, and a corona treatment or the like may be applied.
  • the ceramic sheet releasability of the silicone release polyester film can be measured, for example, as follows.
  • the prepared slurry is uniformly coated onto the coating layer of the release polyester film to a thickness of 2 ⁇ m after drying, and then dried to form a ceramic sheet.
  • the release polyester film on which the ceramic sheet has been formed is cut into a size such as 25 mm x 150 mm, and an adhesive tape is attached to the ceramic sheet side to prepare a test piece.
  • the obtained test piece is conditioned for 24 hours at 23° C. and 50% humidity, and then peeled off using a tensile tester at a peeling angle of 90° and a peeling speed of 10 m/min to form a ceramic sheet (adhesive tape side). Peel off and measure the peel strength.
  • the peel strength of the ceramic sheet for example, in the case of the conditions of the example, a peel strength of less than 0.60 N/mm is preferable, and a peel strength of 0.55 or less can be evaluated as more preferable.
  • the mold release coating composition of the present invention includes: An aqueous dispersion (1) of silicone (A) having a number average molecular weight of 25,000 or more and containing 3 or more alkenyl groups in one molecule, An aqueous dispersion (2) of silicone (B) having a number average molecular weight of 25,000 or less and having alkenyl groups in one molecule only at both ends; An aqueous dispersion (3) of silicone (C) having a number average molecular weight of 10,000 or less and having a hydrogen atom directly bonded to a Si atom represented by a Si-H group, and platinum catalyst, including.
  • the alkenyl group-containing silicone component in the present invention is composed of at least two components having different molecular weights.
  • silicone (A) having a number average molecular weight of 25,000 or more and containing three or more alkenyl groups in one molecule (hereinafter referred to as "silicone (A)" or “alkenyl group-containing silicone (A)”) ) is used.
  • the alkenyl group-containing silicone (A) preferably has alkenyl groups at both ends and side chains in one molecule.
  • the alkenyl group-containing silicone (A) contains at least 3 or more alkenyl groups in one molecule, but may have 4 or more, 5 or more, 6 or more, etc., for example.
  • the upper limit of the number of alkenyl groups in the alkenyl group-containing silicone (A) may be any value as long as it achieves the effects of the present invention, and may be, for example, 30 or less, 20 or less, 15 or less, 10 or less, etc. . If the alkenyl group-containing silicone (A) has two or less alkenyl groups in one molecule, the crosslinking reactivity decreases and the peeling of the ceramic sheet becomes difficult.
  • alkenyl group-containing silicone (A) examples include organopolysiloxanes having a structure represented by the following general formula (I).
  • R 1 a R 2 b SiO (4-ab)/2 ...(I) (In formula (I), R 1 is an alkenyl group having 2 to 8 carbon atoms, R 2 is a monovalent saturated hydrocarbon group having 1 to 16 carbon atoms selected from an alkyl group or an aryl group, and a represents an integer from 0 to 3, b represents an integer from 0 to 2, and satisfies a+b ⁇ 3.)
  • the alkenyl group-containing silicone (A) may have either a linear structure or a branched structure, or may have a partially cross-linked structure, or may be a mixture thereof.
  • alkenyl group having 2 to 8 carbon atoms represented by R 1 examples include vinyl group, allyl group, butenyl group, pentenyl group, and hexenyl group. Among these, vinyl groups are particularly preferred.
  • Examples of the alkyl group represented by R 2 include a methyl group, ethyl group, propyl group, butyl group, and examples of the aryl group include a phenyl group and tolyl group. Among these, it is preferable that 80 mol % or more of the substituents of R 2 be methyl groups from the viewpoint of easy releasability.
  • the curing speed and pot life of the composition is improved by ensuring that the silicon atoms having an alkenyl group are in the range of 0.05 to 20 mol%, for example, based on the total silicon atoms in the alkenyl group-containing silicone (A). Preferable from this point of view.
  • the proportion of silicon atoms having alkenyl groups is less than the lower limit, the curing speed of the composition decreases, and it may become difficult to efficiently form a cured silicone film during film formation.
  • the proportion of silicon atoms having alkenyl groups exceeds the upper limit, the pot life of the composition may be shortened.
  • Examples of the alkenyl group-containing silicone (A) include silicones represented by the following formula (1-1). (In formula (1-1), m is 2.5 and n is 400.)
  • the alkenyl group-containing silicone (A) can be produced by a known method. Further, the alkenyl group-containing silicone in the present invention is preferably contained in the composition in the form of an aqueous dispersion (aqueous dispersion (1)).
  • the content of the alkenyl group-containing silicone (A) in 100 parts by mass of the aqueous dispersion (1) is, for example, , 1 part by mass to 80 parts by mass, 3 parts by mass to 75 parts by mass, 5 parts to 70 parts by mass, 10 parts by mass to 65 parts by mass, or 15 parts by mass to 60 parts by mass. It may be less than 100 yen. If the content is less than 10 parts by mass, the long-term stability of the emulsion may deteriorate, and if it is more than 80 parts by mass, the viscosity may increase and dispersibility may deteriorate.
  • the number average molecular weight of the alkenyl group-containing silicone (A) is 25,000 or more, and may be, for example, 26,000 or more, 27,000 or more, 28,000 or more, 30,000 or more.
  • the upper limit of the number average molecular weight of the alkenyl group-containing silicone (A) may be any value as long as it achieves the effects of the present invention, and may be, for example, 45,000 or less, 40,000 or less, etc. Moreover, if it exceeds 50,000, the emulsion of the aqueous dispersion may become unstable.
  • the content of the alkenyl group-containing silicone (A) is based on 100 parts by mass of the total solid content of the alkenyl group-containing silicone (A) and silicone (B) and the Si-H group-containing silicone (C). In this case, it is preferably 80 parts by mass or more and 96 parts by mass or less, for example, it may be 85 parts by mass or more and 95 parts by mass or less, 88 parts by mass or more and 94 parts by mass or less, 90 parts by mass or more and 92 parts by mass or less, etc. .
  • the above content is 96 parts by mass or more, the amount of polymeric silicone increases and the crosslinking density decreases.
  • the content is less than 80 parts by mass, the crosslinking points between the high molecular weight silicone and the low molecular weight silicone will decrease and the crosslinking density will decrease.
  • Silicone (B) having a number average molecular weight of 25,000 or less and having alkenyl groups only at both ends in one molecule (hereinafter sometimes referred to as “silicone (B)” or “alkenyl group-containing silicone (B)”) is used.
  • the alkenyl group-containing silicone (B) has alkenyl groups only at both ends in one molecule.
  • the above low molecular weight alkenyl group-containing silicone (B) enables a crosslinking reaction that complements the crosslinking network of the above high molecular weight alkenyl group containing silicone (A), maximizing the crosslink density as much as possible, and
  • the scope of rights is not limited to the above mechanism.
  • alkenyl group-containing silicone (B) examples include organopolysiloxanes having a structure represented by the following general formula (I').
  • R 1' is an alkenyl group having 2 to 8 carbon atoms
  • R 2' is a monovalent saturated hydrocarbon group having 1 to 16 carbon atoms selected from an alkyl group or an aryl group. (Yes, a' is 0 to 1, b' is 0 to 2, and represents an integer satisfying a'+b' ⁇ 3.)
  • the alkenyl group-containing silicone (B) may have either a linear structure or a branched structure, or may have a partially cross-linked structure, or may be a mixture thereof.
  • alkenyl group having 2 to 8 carbon atoms represented by R 1' examples include vinyl group, allyl group, butenyl group, pentenyl group, and hexenyl group. Among these, vinyl groups are particularly preferred.
  • the alkenyl group-containing silicone (B) has alkenyl groups only at both ends in one molecule.
  • Examples of the alkyl group represented by R 2' include a methyl group, ethyl group, propyl group, butyl group, and examples of the aryl group include a phenyl group and tolyl group. Among these, it is preferable that 80 mol% or more of the substituents of R 2' be methyl groups from the viewpoint of easy releasability.
  • the silicon atoms having an alkenyl group be in the range of 0.05 to 20 mol%, for example, with respect to the total silicon atoms in the alkenyl group-containing silicone (B), which will improve the curing speed and pot life of the composition. Preferable from this point of view.
  • Examples of the alkenyl group-containing silicone (B) include silicones represented by the following formula (1-2). (In formula (1-2), n is 200.)
  • the alkenyl group-containing silicone (B) can be produced by a known method. Further, the alkenyl group-containing silicone in the present invention is preferably contained in the composition in the form of an aqueous dispersion (aqueous dispersion (2)).
  • the number average molecular weight of the alkenyl group-containing silicone (B) is 25,000 or less, and may be, for example, 24,000 or less, 23,000 or less, 22,000 or less, 21,000 or less, 20,000, 19,000 or less, 18,000 or less, 17,000 or less.
  • the lower limit of the number average molecular weight of the alkenyl group-containing silicone (B) may be any value as long as it achieves the effects of the present invention, and may be, for example, 10,000 or more, 11,000 or more, 12,000 or more, etc.
  • the above molecular weight is 25,000 or more, the crosslinking density is not improved because it is almost the same as that of silicone A. On the other hand, when the above molecular weight is too small, it becomes difficult to form a crosslinked network between silicones A.
  • the alkenyl group-containing silicone (B) can be produced by a known method. Further, the alkenyl group-containing silicone (B) is preferably contained in the composition in the form of an aqueous dispersion (aqueous dispersion (2)).
  • the content of the alkenyl group-containing silicone (B) in 100 parts by mass of the aqueous dispersion (2) is, for example, , 1 part by mass or more and 80 parts by mass or less, 3 parts by mass or more and 70 parts by mass or less, 5 parts by mass or more and 65 parts by mass or less, 10 parts by mass or more and 60 parts by mass or less, or 15 parts by mass or more and 55 parts by mass or more. It may be less than parts by mass. If the content is less than 10 parts by mass, the long-term stability of the emulsion may deteriorate, and if it is more than 80 parts by mass, the viscosity may increase and dispersibility may deteriorate.
  • the content of the alkenyl group-containing silicone (B) is based on 100 parts by mass of the total solid content of the alkenyl group-containing silicone (A) and silicone (B) and the Si-H group-containing silicone (C). In this case, it is preferably 2 parts by mass or more and 20 parts by mass or less, for example, it may be 3 parts by mass or more and 18 parts by mass or less, 4 parts by mass or more and 15 parts by mass or less, 5 parts by mass or more and 10 parts by mass or less, etc. .
  • silicone (C) having a hydrogen atom directly bonded to an Si atom represented by a Si-H group (hereinafter referred to as "silicone (C)" or "Si-H group-containing silicone (C)”)
  • Si-H group-containing silicone (C) An example of the organohydrogenpolysiloxane having a structure represented by the following general formula (II) is exemplified.
  • R 3 c H d SiO (4-c-d)/2 ...(II)
  • R 3 is a monovalent saturated hydrocarbon group having 1 to 16 carbon atoms selected from an alkyl group or an aryl group, c is 0 to 2, d is 1 to 3, and Each represents an integer that satisfies c+d ⁇ 3.
  • the Si—H group-containing silicone (C) may have either a linear structure or a branched structure.
  • Examples of the alkyl group represented by R 3 include a methyl group, ethyl group, propyl group, butyl group, and examples of the aryl group include a phenyl group and tolyl group. Among these, it is preferable that 50 mol % or more of the substituents of R 3 be methyl groups from the viewpoint of easy releasability.
  • the Si--H group-containing silicone (C) preferably has at least 3, preferably 5 or more hydrogen atoms bonded to Si atoms in one silicone molecule.
  • Si--H group-containing silicone (C) examples include silicones represented by the following formula (2). (In formula (2), o is 30 and p is 35)
  • the above Si--H group-containing silicone (C) can be produced by a known method. Further, the Si--H group-containing silicone (C) in the present invention is preferably contained in the composition in the form of an aqueous dispersion (aqueous dispersion (3)).
  • the content of the alkenyl group-containing silicone (B) in 100 parts by mass of the aqueous dispersion (3) is For example, it can be 1 part by mass or more and 80 parts by mass or less, 3 parts by mass or more and 70 parts by mass or less, 5 parts by mass or more and 60 parts by mass or less, 8 parts by mass or more and 55 parts by mass or less, or 10 parts by mass or more. It may be 50 parts by mass or less. If the content is less than 10 parts by mass, the long-term stability of the emulsion may deteriorate, and if it is more than 80 parts by mass, the viscosity may increase and dispersibility may deteriorate.
  • the number average molecular weight of the Si—H group-containing silicone (C) is 10,000 or less, and may be, for example, 8,000 or less, 7,000 or less, 6,000 or less. When the number average molecular weight is 10,000 or more, the function as a crosslinking agent becomes insufficient and the crosslinking density decreases. Further, the lower limit of the number average molecular weight of the Si-H group-containing silicone (C) is not particularly limited as long as the effects of the present invention are achieved, but for example, it is 300 or more, 500 or more, 1000 or more, 2000 or more, etc. be able to.
  • the content of the Si-H group-containing silicone (C) is 100 parts by mass of the total solid content of the alkenyl group-containing silicone (A) and silicone (B) and the Si-H group-containing silicone (C).
  • the content of the Si-H group-containing silicone (C) is 100 parts by mass of the total solid content of the alkenyl group-containing silicone (A) and silicone (B) and the Si-H group-containing silicone (C).
  • 2 parts by mass or more and 20 parts by mass or less for example, 3 parts by mass or more and 18 parts by mass or less, 4 parts by mass or more and 15 parts by mass or less, 5 parts by mass or more and 10 parts by mass or less, etc. Good too.
  • the above content is less than 2 parts by mass, the curing reaction will be difficult to proceed and sufficient coating hardness may not be obtained.
  • Si-H will be excessively deposited on the surface. It precipitates on the green sheet and adheres strongly to the green sheet, which may result in heavy peeling.
  • the ratio (number of Si-H groups/number of alkenyl groups) between the number of Si-H groups and the number of alkenyl groups (number of alkenyl groups in silicone (A) and silicone (B)) in the mold release coating composition of the present invention is 1.0.
  • a range of 2.0 to 2.0 is preferable. If the above ratio is less than the lower limit, excess alkenyl groups will remain in the formed coating layer, making it easy to change the peel strength over time and reducing the crosslinking density, which will reduce the uniformity of the peel force and the residual adhesion. rate may decrease. Furthermore, if the above ratio exceeds the upper limit, highly reactive Si--H groups may remain in the formed coating layer, causing an increase in peeling force.
  • the alkenyl group-containing silicone solid content (the total amount of solid content of silicone (A) and silicone (B)) and the Si-H group content are based on the solid content mass of the above composition.
  • the total amount of silicone (C) solid content is preferably 70% by mass or more.
  • the more preferable content of each silicone solid content is 80% by mass or more and 97% by mass or less.
  • the silicone solid content refers to the amount excluding the aqueous solvent
  • the solid content mass of the composition refers to the total amount of solid content of each additive. If the total amount of silicone solid content is less than the lower limit, the area covered with silicone on the film surface on which the coating film is formed will decrease, the peeling force will become heavy, and the peeling force may become uneven. There is.
  • aqueous solvent Water is preferably used as the aqueous solvent for forming each silicone aqueous dispersion of the present invention.
  • a silicone mold release layer can be formed without using explosion-proof equipment and organic solvent recovery equipment that are required for organic solvents during the process of manufacturing a mold release film.
  • emulsifier Each water dispersion is made using an emulsifier to increase the stability and shear resistance of the water dispersion.
  • emulsifier a nonionic emulsifier that does not affect the curing reaction of silicone is preferred.
  • An ionic emulsifier may affect the curing reaction of silicone, and may also be localized in the coating film, for example, may bleed out to the surface and affect mold releasability.
  • the nonionic emulsifier preferably has an HLB value in the range of 8 or more and 18 or less, such as higher alcohols or alkylene oxide adducts of higher fatty acids, esters of alkylene oxide adducts of higher fatty acids and alcohols, and alkylene alkanolamides.
  • HLB value is a value calculated using the Griffin calculation formula.
  • the alkylene oxide examples include ethylene oxide, propylene oxide, and butylene oxide, and one or more of these may be used.
  • the HLB value is preferably in the range of 8 or more and 18 or less, and more preferably in the range of 10 or more and 15 or less, although it does not matter whether the addition format is block or random.
  • preferred examples include polyoxyethylene lauryl ether and polyoxyethylene tridecyl ether. If a nonionic emulsifier with an HLB value outside the above range is used as an emulsifier for a silicone aqueous dispersion, the emulsifying dispersion power and stability of the aqueous dispersion may decrease.
  • the nonionic emulsifier is preferably used in a range of 0.1% by mass or more and 20% by mass or less, more preferably 0.2% by mass or more and 15% by mass or less, based on the total solid content, and Preferably it is in the range of 0.5% by mass or more and 10% by mass or less. If it is below this range, emulsification tends to be poor, and if it is above this range, heavy exfoliation may occur.
  • a catalyst may be used in the release coating composition constituting the coating layer of the present invention in order to cause an addition reaction between the silicone (A) and/or the silicone (B) and the silicone (C).
  • platinum-based catalysts are particularly preferred.
  • Platinum-based catalyst Known platinum catalysts can be used, such as platinum chloride and chloroplatinic acid.
  • a 1,3-divinyl-1,1,3,3-tetramethyldisiloxane platinum complex (Karstedt catalyst) may be used in consideration of dispersibility in silicone. Uniform dispersibility can be ensured by simultaneously dispersing the components. These may be used alone or in combination of two or more.
  • the amount of platinum-based catalyst is based on the total mass of the water dispersion (1) of silicone (A), the water dispersion (2) of silicone (B), and the water dispersion (3) of silicone (C).
  • the mass of the platinum element is contained in a range of 120 ppm or more and 800 ppm or less. By setting it as the said range, silicone can be fully hardened. Moreover, the generation of silicone aggregates can be suppressed, and a release polyester film with excellent surface properties can be obtained.
  • the mass ratio of the platinum element exceeds the upper limit, the addition reaction between the alkenyl group and the Si--H group tends to be accelerated, resulting in the generation of silicone aggregates.
  • the amount of platinum-based catalyst is, for example, 600 ppm or less, 500 ppm or less, 300 ppm or less, 250 ppm or less. Furthermore, if the mass ratio of the platinum element is below the lower limit, the addition reaction does not proceed, which tends to cause poor curing of silicone. From the above viewpoint, the amount of platinum catalyst is, for example, 130 ppm or more, 140 ppm or more, 150 ppm or more, 200 ppm or more.
  • the aqueous coating composition contains a crosslinking reaction inhibitor.
  • the crosslinking reaction inhibitor is preferably a crosslinking reaction inhibitor having an alkynyl group.
  • the crosslinking reaction inhibitor having an alkynyl group is not particularly limited as long as it has an alkynyl group, but specifically, 1-ethynyl-1-cyclohexanol, 4-ethyl-1-octyn-3-ol, 3-Methyl-1-dodecyn-3-ol, 3,7,11-trimethyl-1-dodecyn-3-ol, 1,1-diphenyl-2-propyn-3-ol, 3-ethyl-6-ethyl- Examples include 1-nonyn-3-ol, 3-methyl-1-pentadecyn-3-ol, 2,5-dimethyl-3-hexyne-2,5-diol, and 3-phenyl-1-butyn-3-ol.
  • an ethynyl group can be mentioned as a preferable one. These may be used alone or in combination of two or more. Since the present invention employs an aqueous emulsion coating composition, a crosslinking reaction inhibitor having an alkynyl group and a hydroxyl group as exemplified may be used in view of the balance between affinity and solubility in water, coordination ability to platinum, and boiling point. is preferred.
  • the content of the crosslinking reaction inhibitor is preferably 5 ppm or more and 1000 ppm or less, more preferably 10 ppm or more and 700 ppm or less, and even more preferably 20 ppm or more and 500 ppm or less, based on the amount of the aqueous coating composition used to form the release layer.
  • the content of the crosslinking reaction inhibitor is at least the lower limit, the pot life becomes long, the addition curing reaction of silicone is difficult to proceed at room temperature, and silicone aggregates tend to be difficult to generate.
  • silicone will be difficult to transfer to the other material after the other material is peeled off, and the amount of reaction inhibitor that evaporates during heat treatment will decrease, resulting in contamination inside the oven. is less likely to occur.
  • the content of the crosslinking reaction inhibitor relative to the mass of platinum element is, for example, preferably 6 times or less, more preferably 5 times or less, particularly preferably 4 times or less.
  • the crosslinking reaction inhibitor having an ethynyl group is not particularly limited as long as it has an ethynyl group, but since a water-based coating composition is used in the present invention, it has a high solubility in water and coordination ability to platinum. In terms of balance and volatility, it is preferable to use a crosslinking reaction inhibitor having an ethynyl hydroxyl group, typified by 1-ethynylcyclohexanol.
  • the release coating composition of the present invention may further contain, for example, an adhesion imparting agent to a substrate, a coloring agent, an ultraviolet absorber, particles, an antistatic agent, etc., within a range that does not impair the objects of the present invention. May be added.
  • each silicone aqueous dispersion of the present invention a method of emulsifying the silicone component, an aqueous solvent, and an emulsifier described above may be mentioned.
  • These components can be emulsified using a known method.
  • silicone and emulsifier prepared in advance, and other components as necessary, are mixed using a stirring device such as a homogenizer, ajihomo mixer, or an ultra planetary mixer. Examples include a method of mechanical emulsification in an aqueous medium.
  • the particle size of the aqueous dispersion can be adjusted by adjusting the size of the stirring blade, stirring speed, and stirring time.
  • the average particle size of each silicone aqueous dispersion of the present invention is preferably 200 nm or less, more preferably 100 nm or more and 200 nm or less.
  • a coating layer is formed on at least one surface of a polyester film using the release coating composition of the present invention.
  • the coating layer (release layer) of the present invention is formed by applying the coating composition for mold release onto the polyester film, followed by drying.
  • the thickness of the coating layer after drying is preferably 5 nm or more and 70 nm or less. If the thickness of the coating layer is less than the lower limit, the release properties may be insufficient, and if it exceeds the upper limit, the peel strength will increase, and it may be necessary to increase the concentration of the coating liquid or increase the amount of coating. Therefore, it tends to be difficult to apply.
  • an aqueous coating solution containing the above composition is prepared, and the solid content concentration of the aqueous coating solution is 20% by mass or less based on the mass of the above coating solution.
  • the content is preferably 1% by mass or more and 10% by mass or less. If the solid content concentration in the aqueous coating liquid is less than the lower limit, the coating properties on the polyester film may be insufficient. Furthermore, if the solid content concentration exceeds the upper limit, the stability of the coating liquid and the appearance of the coating layer may deteriorate. Water is preferably used as the aqueous solvent to adjust the solid content concentration.
  • the aqueous coating solution can be applied to the polyester film at any stage, it is preferable to apply it during the manufacturing process of the polyester film. is preferred.
  • the polyester film before the completion of crystal orientation refers to an unstretched film, an unstretched film in the longitudinal direction (hereinafter sometimes referred to as continuous film forming direction, longitudinal direction, MD direction) or transverse direction (hereinafter referred to as continuous film forming direction, longitudinal direction, MD direction). , a direction perpendicular to the machine direction, a width direction, or a TD direction), and a film oriented by low-magnification stretching in two directions, the machine direction and the transverse direction (sometimes called the TD direction).
  • in-line coating in which an aqueous coating solution of the above composition is applied to an unstretched film or a uniaxially stretched film oriented in one direction, and the film is directly subjected to longitudinal stretching and/or transverse stretching and heat setting.
  • the coated layer may be dried by a stretching process or a heat setting process after coating, and a drying process may be added if necessary.
  • the curing can be performed by a stretching process or a heat setting process, but a curing process may be added as necessary.
  • the film surface is subjected to physical treatment such as corona surface treatment, flame treatment, plasma treatment, etc. as a preliminary treatment to improve coating properties, or the above-mentioned composition is applied together with the composition. It is preferable to use an emulsifier as a wetting agent.
  • any known coating method can be used as the coating method.
  • a roll coating method, a gravure coating method, a roll brushing method, a spray coating method, an air knife coating method, an impregnation method, a curtain coating method, etc. can be used alone or in combination.
  • the method for producing a silicone release polyester film of the present invention includes: An aqueous dispersion (1) of silicone (A) having a number average molecular weight of 25,000 or more and containing 3 or more alkenyl groups in one molecule, An aqueous dispersion (2) of silicone (B) having a number average molecular weight of 25,000 or less and having alkenyl groups in one molecule only at both ends; An aqueous dispersion (3) of silicone (C) having a number average molecular weight of 10,000 or less and having a hydrogen atom directly bonded to a Si atom represented by a Si-H group, and platinum catalyst, The step of forming a coating layer formed using a mold release coating composition comprising; When the total solid content of the silicone (A), the silicone (B), and the silicone (C) is 100 parts by mass, the silicone (A) is 80 parts by mass or more, and the silicone (B) is 2 parts by mass. The content of silicone (C) is from 2 parts
  • the method for producing a silicone release polyester film of the present invention makes it possible to efficiently and easily obtain a silicone release polyester film having the above characteristics. Note that the manufacturing method shown here is an example, and the present invention is not limited thereto.
  • the step of forming a coating layer using an aqueous dispersion mold release coating composition may be a method of forming a coating layer on a film using an aqueous dispersion mold release coating composition.
  • a known method can be used as appropriate.
  • barium titanate BaTiO 3
  • polyvinyl butyral 7 parts by mass of polyvinyl butyral
  • dioctyl phthalate 3 parts by mass of dioctyl phthalate
  • the obtained slurry was uniformly applied onto the coating layer of the release polyester film so that the thickness after drying was 2 ⁇ m, and then dried to form a ceramic sheet.
  • the release polyester film on which the ceramic sheet was formed was cut into 25 mm x 150 mm, and an adhesive tape (manufactured by Nitto Denko Corporation, trade name "31B Tape") was attached to the ceramic sheet side to prepare a test piece.
  • the obtained test piece was conditioned at 23°C and 50% humidity for 24 hours, and then the ceramic sheet (31B tape side) was peeled off using a tensile tester at a peeling angle of 90° and a peeling speed of 10 m/min. , the peel strength was measured.
  • the peel strength of the ceramic sheet was evaluated based on the following index. ⁇ : Peel strength is less than 0.60 N/mm ⁇ : Peel strength is 0.60 N/mm or more
  • this coated film was dried at 115°C for about 5 seconds, stretched 4.5 times in the transverse direction at 145°C, and further heat-set at 230°C for about 5 seconds to form a 25um coated film having the coated layer shown in Table 1.
  • a biaxially stretched polyester film was obtained.
  • Aqueous dispersion (A) of alkenyl group-containing silicone (1) Using an emulsifying device (manufactured by NP Lab Co., Ltd., device name "Ultra Planetary Mixer”) that can stir the entire inside of the container, silicone having an alkenyl group represented by the following formula (1-1) (number average A raw material consisting of 98% by mass (molecular weight: 28000) and 2% by mass of polyoxyethylene lauryl ether (trade name "Emulgen 109P” manufactured by Kao Corporation) as a surfactant was mechanically emulsified in an aqueous medium to reduce the solid content. A silicone aqueous dispersion containing 20% by mass of alkenyl groups was obtained. Furthermore, the emulsion particle size was adjusted by adjusting the stirring speed and stirring time during emulsification.
  • n 200.
  • Platinum-based catalyst Reaction inhibitor-containing platinum-based catalyst: isopropyl alcohol solution of chloroplatinic acid (an amount such that platinum metal is 500 ppm by mass in this composition), polyoxyethylene lauryl ether as a surfactant (manufactured by Kao Corporation, product) An aqueous dispersion with a solid content of 10% by mass was prepared using 99.75% by mass of Emulgen 109P, 0.2% by mass of a crosslinking reaction inhibitor (1-ethynylcyclohexanol), and pure water.
  • This platinum-based catalyst Since the crosslinking reaction inhibitor is preferentially coordinated, the catalytic effect can be delayed until the reaction inhibitor volatilizes.
  • a release coating composition a composition composed of alkenyl group-containing silicone aqueous dispersion/Si-H group-containing silicone aqueous dispersion/platinum catalyst was used according to the formulation shown in Table 1, and a 50 nm layer was used. A coating solution was prepared by diluting it with water so that the solid content concentration of the coating solution was 10%.
  • the films of the examples of the present invention had excellent releasability even from ceramic sheets as thin as 2 ⁇ m. This is presumed to be because a film with excellent releasability is obtained by using a specific composition containing a predetermined crosslinkable high-molecular-weight silicone, low-molecular-weight silicone, and Si-H group-containing silicone. .
  • the crosslinking was insufficient, resulting in uncured properties, and appropriate easy peelability could not be obtained.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Organic Chemistry (AREA)
  • Materials Engineering (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Wood Science & Technology (AREA)
  • Life Sciences & Earth Sciences (AREA)
  • Manufacturing & Machinery (AREA)
  • Health & Medical Sciences (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Power Engineering (AREA)
  • Dispersion Chemistry (AREA)
  • Microelectronics & Electronic Packaging (AREA)
  • Compositions Of Macromolecular Compounds (AREA)
  • Laminated Bodies (AREA)
PCT/JP2023/019324 2022-05-30 2023-05-24 シリコーン離型ポリエステルフィルム、及びその製造方法 Ceased WO2023234140A1 (ja)

Priority Applications (4)

Application Number Priority Date Filing Date Title
JP2024524776A JP7901304B2 (ja) 2022-05-30 2023-05-24 シリコーン離型ポリエステルフィルム、及びその製造方法
CN202380036088.XA CN119110822A (zh) 2022-05-30 2023-05-24 有机硅脱模聚酯薄膜和其制造方法
KR1020247031360A KR20240144465A (ko) 2022-05-30 2023-05-24 실리콘 이형 폴리에스테르 필름, 및 그 제조 방법
JP2026068441A JP2026123074A (ja) 2022-05-30 2026-04-17 シリコーン離型ポリエステルフィルム、及びその製造方法

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2022087332 2022-05-30
JP2022-087332 2022-05-30

Publications (1)

Publication Number Publication Date
WO2023234140A1 true WO2023234140A1 (ja) 2023-12-07

Family

ID=89024826

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2023/019324 Ceased WO2023234140A1 (ja) 2022-05-30 2023-05-24 シリコーン離型ポリエステルフィルム、及びその製造方法

Country Status (5)

Country Link
JP (2) JP7901304B2 (cg-RX-API-DMAC7.html)
KR (1) KR20240144465A (cg-RX-API-DMAC7.html)
CN (1) CN119110822A (cg-RX-API-DMAC7.html)
TW (1) TWI904440B (cg-RX-API-DMAC7.html)
WO (1) WO2023234140A1 (cg-RX-API-DMAC7.html)

Citations (17)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS6153326A (ja) * 1984-07-05 1986-03-17 ミネソタ マイニング アンド マニユフアクチユアリング コンパニ− 有機コーティングをポリエステルフィルム基材へ接着する方法
JPH07300774A (ja) * 1994-02-28 1995-11-14 Shin Etsu Chem Co Ltd シリコーンコーティング加工基材及びエアバッグ基材
JPH09216963A (ja) * 1995-10-17 1997-08-19 Hoechst Diafoil Co シリコーン剥離層被覆ポリエステルフィルム及びフィルムの被覆方法
JP2003026925A (ja) * 2001-07-12 2003-01-29 Shin Etsu Chem Co Ltd シリコーン組成物及びこれを用いた剥離フィルム
JP2009249570A (ja) * 2008-04-09 2009-10-29 Shin Etsu Chem Co Ltd フィルム用無溶剤型シリコーン剥離剤組成物およびそれを用いた剥離フィルム
JP2010195015A (ja) * 2009-02-27 2010-09-09 Teijin Dupont Films Japan Ltd セラミックシート製造用離型フィルム
JP2011207106A (ja) * 2010-03-30 2011-10-20 Lintec Corp セラミックグリーンシート成型用剥離フィルムおよびその製造方法
JP2011230469A (ja) * 2010-04-30 2011-11-17 Mitsubishi Plastics Inc 離型フィルム
JP2013525572A (ja) * 2010-04-28 2013-06-20 スリーエム イノベイティブ プロパティズ カンパニー シリコーン系材料
JP2013202831A (ja) * 2012-03-27 2013-10-07 Lintec Corp 剥離シート
CN103694892A (zh) * 2013-12-05 2014-04-02 深圳市冠恒新材料科技有限公司 一种含氟聚硅氧烷离型剂及其制备方法
JP2014083697A (ja) * 2012-10-19 2014-05-12 Teijin Dupont Films Japan Ltd シリコーン離型ポリエステルフィルム
JP2017025172A (ja) * 2015-07-18 2017-02-02 三菱樹脂株式会社 積層ポリエステルフィルム
US20170037210A1 (en) * 2015-08-05 2017-02-09 Nan Ya Plastics Corporation Release film and process for producing the same
WO2017200056A1 (ja) * 2016-05-20 2017-11-23 三菱ケミカル株式会社 離型フィルム
JP2021011081A (ja) * 2019-07-09 2021-02-04 東洋紡フイルムソリューション株式会社 シリコーン離型ポリエステルフィルム
JP2022037482A (ja) * 2020-08-25 2022-03-09 住友ベークライト株式会社 離型フィルム

Family Cites Families (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2003192987A (ja) 2001-12-26 2003-07-09 Toray Ind Inc 無溶剤型ポリシロキサン系塗剤及び離型フィルム
JP2006007689A (ja) 2004-06-29 2006-01-12 Toray Advanced Film Co Ltd 離型フィルム
JP4837613B2 (ja) 2007-03-30 2011-12-14 リンテック株式会社 剥離フィルムおよび剥離フィルムの製造方法
JP2018059001A (ja) * 2016-10-06 2018-04-12 信越化学工業株式会社 剥離紙用又は剥離フィルム用シリコーン組成物

Patent Citations (17)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS6153326A (ja) * 1984-07-05 1986-03-17 ミネソタ マイニング アンド マニユフアクチユアリング コンパニ− 有機コーティングをポリエステルフィルム基材へ接着する方法
JPH07300774A (ja) * 1994-02-28 1995-11-14 Shin Etsu Chem Co Ltd シリコーンコーティング加工基材及びエアバッグ基材
JPH09216963A (ja) * 1995-10-17 1997-08-19 Hoechst Diafoil Co シリコーン剥離層被覆ポリエステルフィルム及びフィルムの被覆方法
JP2003026925A (ja) * 2001-07-12 2003-01-29 Shin Etsu Chem Co Ltd シリコーン組成物及びこれを用いた剥離フィルム
JP2009249570A (ja) * 2008-04-09 2009-10-29 Shin Etsu Chem Co Ltd フィルム用無溶剤型シリコーン剥離剤組成物およびそれを用いた剥離フィルム
JP2010195015A (ja) * 2009-02-27 2010-09-09 Teijin Dupont Films Japan Ltd セラミックシート製造用離型フィルム
JP2011207106A (ja) * 2010-03-30 2011-10-20 Lintec Corp セラミックグリーンシート成型用剥離フィルムおよびその製造方法
JP2013525572A (ja) * 2010-04-28 2013-06-20 スリーエム イノベイティブ プロパティズ カンパニー シリコーン系材料
JP2011230469A (ja) * 2010-04-30 2011-11-17 Mitsubishi Plastics Inc 離型フィルム
JP2013202831A (ja) * 2012-03-27 2013-10-07 Lintec Corp 剥離シート
JP2014083697A (ja) * 2012-10-19 2014-05-12 Teijin Dupont Films Japan Ltd シリコーン離型ポリエステルフィルム
CN103694892A (zh) * 2013-12-05 2014-04-02 深圳市冠恒新材料科技有限公司 一种含氟聚硅氧烷离型剂及其制备方法
JP2017025172A (ja) * 2015-07-18 2017-02-02 三菱樹脂株式会社 積層ポリエステルフィルム
US20170037210A1 (en) * 2015-08-05 2017-02-09 Nan Ya Plastics Corporation Release film and process for producing the same
WO2017200056A1 (ja) * 2016-05-20 2017-11-23 三菱ケミカル株式会社 離型フィルム
JP2021011081A (ja) * 2019-07-09 2021-02-04 東洋紡フイルムソリューション株式会社 シリコーン離型ポリエステルフィルム
JP2022037482A (ja) * 2020-08-25 2022-03-09 住友ベークライト株式会社 離型フィルム

Also Published As

Publication number Publication date
KR20240144465A (ko) 2024-10-02
JP7901304B2 (ja) 2026-08-06
JPWO2023234140A1 (cg-RX-API-DMAC7.html) 2023-12-07
TWI904440B (zh) 2025-11-11
TW202405097A (zh) 2024-02-01
CN119110822A (zh) 2024-12-10
JP2026123074A (ja) 2026-07-29

Similar Documents

Publication Publication Date Title
JP5964718B2 (ja) シリコーン離型ポリエステルフィルム
JP7473865B2 (ja) シリコーン離型ポリエステルフィルム
JP5251315B2 (ja) 離型フィルムの製造方法
JP5840996B2 (ja) シリコーン離型ポリエステルフィルム
JP5319329B2 (ja) セラミックシート製造用離型フィルム
JP6077327B2 (ja) 離型用コーティング組成物およびそれからなるシリコーン離型ポリエステルフィルム
JP7626974B2 (ja) 離型フィルム
WO2022202588A1 (ja) 樹脂シート成型用離型フィルム
JP6178108B2 (ja) シリコーン離型フィルム
JP7842967B2 (ja) 離型フィルム
JP7828047B2 (ja) シリコーン離型ポリエステルフィルム、及びその製造方法
TWI887772B (zh) 離型膜及其製造方法
TWI904440B (zh) 聚矽氧離型聚酯膜、及其製造方法
JP7803407B2 (ja) シリコーン離型ポリエステルフィルム、及びその製造方法
JP5495324B2 (ja) 離型性ポリエステルフィルム
JP7769896B1 (ja) 離型フィルム
JP7842966B2 (ja) 離型フィルム
WO2024162200A1 (ja) 離型フィルム
WO2025023168A1 (ja) 離型フィルム
JP7856160B2 (ja) 離型フィルム
JP2023147243A (ja) 離型フィルム
WO2026004801A1 (ja) 離型フィルム
WO2023190169A1 (ja) 離型フィルム
TW202539890A (zh) 離型膜
JP2026005002A (ja) 離型フィルム

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 23815899

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2024524776

Country of ref document: JP

Kind code of ref document: A

ENP Entry into the national phase

Ref document number: 20247031360

Country of ref document: KR

Kind code of ref document: A

WWE Wipo information: entry into national phase

Ref document number: 1020247031360

Country of ref document: KR

WWE Wipo information: entry into national phase

Ref document number: 12024552420

Country of ref document: PH

WWE Wipo information: entry into national phase

Ref document number: 202380036088.X

Country of ref document: CN

WWE Wipo information: entry into national phase

Ref document number: 2401007549

Country of ref document: TH

WWE Wipo information: entry into national phase

Ref document number: 11202407169S

Country of ref document: SG

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 23815899

Country of ref document: EP

Kind code of ref document: A1