WO2015146099A1 - イエロートナーおよびその製造方法 - Google Patents
イエロートナーおよびその製造方法 Download PDFInfo
- Publication number
- WO2015146099A1 WO2015146099A1 PCT/JP2015/001563 JP2015001563W WO2015146099A1 WO 2015146099 A1 WO2015146099 A1 WO 2015146099A1 JP 2015001563 W JP2015001563 W JP 2015001563W WO 2015146099 A1 WO2015146099 A1 WO 2015146099A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- group
- dispersion
- toner
- mass
- particles
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Images
Classifications
-
- G—PHYSICS
- G03—PHOTOGRAPHY; CINEMATOGRAPHY; ANALOGOUS TECHNIQUES USING WAVES OTHER THAN OPTICAL WAVES; ELECTROGRAPHY; HOLOGRAPHY
- G03G—ELECTROGRAPHY; ELECTROPHOTOGRAPHY; MAGNETOGRAPHY
- G03G9/00—Developers
- G03G9/08—Developers with toner particles
- G03G9/09—Colouring agents for toner particles
- G03G9/0906—Organic dyes
- G03G9/091—Azo dyes
-
- G—PHYSICS
- G03—PHOTOGRAPHY; CINEMATOGRAPHY; ANALOGOUS TECHNIQUES USING WAVES OTHER THAN OPTICAL WAVES; ELECTROGRAPHY; HOLOGRAPHY
- G03G—ELECTROGRAPHY; ELECTROPHOTOGRAPHY; MAGNETOGRAPHY
- G03G9/00—Developers
- G03G9/08—Developers with toner particles
- G03G9/0802—Preparation methods
- G03G9/0804—Preparation methods whereby the components are brought together in a liquid dispersing medium
- G03G9/0806—Preparation methods whereby the components are brought together in a liquid dispersing medium whereby chemical synthesis of at least one of the toner components takes place
-
- G—PHYSICS
- G03—PHOTOGRAPHY; CINEMATOGRAPHY; ANALOGOUS TECHNIQUES USING WAVES OTHER THAN OPTICAL WAVES; ELECTROGRAPHY; HOLOGRAPHY
- G03G—ELECTROGRAPHY; ELECTROPHOTOGRAPHY; MAGNETOGRAPHY
- G03G9/00—Developers
- G03G9/08—Developers with toner particles
- G03G9/09—Colouring agents for toner particles
- G03G9/0906—Organic dyes
- G03G9/0924—Dyes characterised by specific substituents
Definitions
- the present invention relates to a yellow toner used in a recording method such as an electrophotographic method, an electrostatic recording method, a magnetic recording method, a toner jet method, and a manufacturing method thereof.
- color image originals are color-separated with blue, green, and red color filters, and the latent image corresponding to the original image is developed using yellow, magenta, cyan, and black color developers. .
- the coloring power of the colorant in the developer of each color greatly affects the image quality.
- yellow colorants for toner compounds having isoindolinone, quinophthalone, isoindoline, anthraquinone, azo skeleton, and the like are known.
- a yellow dye C.I. which has high transparency and coloring power and excellent light resistance.
- a pyridone azo skeleton such as Solvent Yellow 162 are known (see Patent Documents 1 and 2).
- a pyridone azo compound having a phenyl group having two or more substituents is known as a color filter application (see Patent Document 3).
- An object of the present invention is to provide a toner having high coloring power and excellent light resistance.
- the present invention is a yellow toner containing at least a binder resin, a wax and a colorant, wherein the yellow toner contains a compound represented by the general formula (1) as a colorant. is there.
- R 1 represents an alkyl group, an aryl group, or an amino group.
- R 2 represents a hydrogen atom, a cyano group, a carbamoyl group, an alkoxycarbonyl group, or a carboxylic acid amide group.
- R 3 represents Represents a hydrogen atom, an alkyl group or an acyl group, A represents an alkoxycarbonyl group, an alkoxysulfonyl group, a carboxylic acid amide group or a sulfonic acid amide group, n represents an integer of 2 to 5, and n A May be the same or different.
- a toner having high coloring power and excellent light resistance can be provided.
- FIG. 2 is a diagram showing a 1 H-NMR spectrum of compound (1).
- the inventors of the present invention are yellow toners having toner particles containing a binder resin, a wax, and a colorant.
- the inventors have found that a compound represented by the general formula (1) can provide a toner having high coloring power and excellent light resistance.
- R 1 represents an alkyl group, an aryl group, or an amino group.
- R 2 represents a hydrogen atom, a cyano group, a carbamoyl group, an alkoxycarbonyl group, or a carboxylic acid amide group.
- R 3 represents Represents a hydrogen atom, an alkyl group or an acyl group, A represents an alkoxycarbonyl group, an alkoxysulfonyl group, a carboxylic acid amide group or a sulfonic acid amide group, n represents an integer of 2 to 5, and n A May be the same or different.
- the toner colorant In order to make the toner colorant highly colored and have excellent light resistance, the following matters are important. For coloring power (high colorability), the characteristics unique to the material due to the structure and substituent effects are important. In addition, since the toner contains at least a binder resin and a wax component, compatibility with the binder resin and wax component mixed with the dye (colorant) is also important. In particular, in a toner, if the compatibility with a binder resin or a wax component mixed with a dye is poor, association or aggregation occurs and the coloring power is reduced. Therefore, in order to suppress the association and aggregation of the colored bodies that cause a reduction in coloring power, it is necessary to increase the compatibility with the binder resin and the wax component.
- the compatibility between the dye and the wax component is inferior to the compatibility between the dye and the binder resin. And agglomeration occur, and coloring power decreases. Therefore, it is necessary to solve this problem together.
- the dye compound of the general formula (1) according to the present invention is at least disubstituted (two or more A in the formula (1)), the monosubstituted (one A in the formula (1) is one. ) And light resistance is superior. This is thought to be influenced by the state of the electron density of the diazo group portion of the pyridone azo skeleton. In the present invention, it is considered that the electron density of the diazo group can be lowered and the light resistance has been improved by using two electron withdrawing groups as A in the formula (1). .
- the alkyl group for R 1 in the general formula (1) is not particularly limited, but a methyl group, an ethyl group, an n-propyl group, an iso-propyl group, an n-butyl group, a sec-butyl group, Examples thereof include an iso-butyl group and a tert-butyl group.
- the amino group in R 1 in the general formula (1) is not particularly limited, amino group, dimethylamino group and the like.
- R 1 in the general formula (1) is preferably an alkyl group because of excellent light resistance, and more preferably a methyl group.
- the alkoxycarbonyl group in R 2 in the general formula (1) is not particularly limited, methoxycarbonyl group, ethoxycarbonyl group, butoxycarbonyl group, ethyl hexoxycarbonyl group, and the like.
- Examples of the carboxylic acid amide group in R 2 in the general formula (1) include a carboxylic acid dimethylamide group, a carboxylic acid diethylamide group, a carboxylic acid ethyl (2-ethylhexyl) amide group, and a carboxylic acid butyl (ethyl) amide group.
- carboxylic acid monoalkylamide groups such as carboxylic acid methylamide group, carboxylic acid ethylamide group, and carboxylic acid 2-ethylhexylamide.
- R 2 in the general formula (1) is preferably a cyano group because of excellent light resistance.
- the alkyl group for R 3 in the general formula (1) is not particularly limited, but a methyl group, an ethyl group, an n-propyl group, an iso-propyl group, an n-butyl group, a sec-butyl group, ethyl substituted with iso-butyl group, tert-butyl group, octyl group, dodecyl group, nonadecyl group, cyclobutyl group, cyclopentyl group, cyclohexyl group, methylcyclohexyl group, 2-ethylpropyl, 2-ethylhexyl group, cyclohexenyl group
- Examples thereof include saturated or unsaturated linear, branched, or cyclic primary to tertiary alkyl groups having 1 to 20 carbon atoms.
- the acyl group for R 3 in the general formula (1) is not particularly limited, and examples thereof include a formyl group, an acetyl group, an ethylhexinoyl group, and a benzoyl group.
- R 3 in the general formula (1) is preferably an ethyl group, an n-butyl group or a 2-ethylhexyl group because of excellent light resistance.
- the alkoxycarbonyl group in A in the general formula (1) is not particularly limited, but is a methoxycarbonyl group, an ethoxycarbonyl group, a butoxycarbonyl group, a hexoxycarbonyl group, or a 2-ethylhexoxycarbonyl group. Etc. In particular, a 2-ethylhexoxycarbonyl group is preferable because of excellent solubility and light resistance.
- the carboxylic acid amide group in A in the general formula (1) is not particularly limited, but carboxylic acid dimethylamide group, carboxylic acid diethylamide group, carboxylic acid butyl (ethyl) amide group, carboxylic acid di (ethylhexyl) ) Carboxylic acid dialkylamide groups such as amide groups and carboxylic acid di (2-ethylhexyl) amide groups; carboxylic acid methylamide groups, carboxylic acid ethylamide groups, carboxylic acid (ethylhexyl) amide groups, carboxylic acid (2-ethylhexyl) amide groups, etc. And carboxylic acid monoalkylamide groups.
- a carboxylic acid di (2-ethylhexyl) amide group is preferable because of excellent solubility and light resistance.
- the alkoxysulfonyl group in A in the general formula (1) is not particularly limited, but includes a methoxysulfonyl group, an ethoxysulfonyl group, a butoxysulfonyl group, a hexoxysulfonyl group, a 2-ethylhexoxysulfonyl group, and the like. Can be mentioned. In particular, a 2-ethylhexoxysulfonyl group is preferable because of excellent solubility and light resistance.
- the sulfonic acid amide group in A in the general formula (1) is not particularly limited, but sulfonic acid dimethylamide group, sulfonic acid diethylamide group, sulfonic acid butyl (ethyl) amide group, sulfonic acid di (2 A sulfonic acid dialkylamide group such as an ethylhexyl) amide group, and a sulfonic acid monoalkylamide group such as a sulfonic acid (2-ethylhexyl) amide group.
- a sulfonic acid di (2-ethylhexyl) amide group is preferable because of excellent solubility and light resistance.
- the compound represented by the general formula (1) used in the present invention can be synthesized with reference to a known method described in International Publication No. 2012/039361.
- the compounds (1) to (30) are shown below.
- the compound represented by the general formula (1) used in the present invention is particularly preferably the following compounds. It is not limited.
- the compound of the general formula (1) is expressed in an azo form.
- the compound of the general formula (1) has an azo-hydrazo tautomer, and the hydrazo is within the scope of the present invention.
- the content of the compound represented by the general formula (1) is preferably 1 to 20 parts by mass with respect to 100 parts by mass of the binder resin.
- the compounds represented by the general formula (1) can be used alone or in combination with known yellow dyes in order to adjust the color tone.
- the compound represented by the general formula (1) can be used in combination with a general yellow pigment.
- a general yellow pigment In particular, C.I. I. Pigment yellow 185, C.I. I. Pigment yellow 180 or C.I. I. Use in combination with Pigment Yellow 155 is effective in obtaining a good yellow color.
- These pigments may be used alone or in combination of two or more.
- the yellow toner of the present invention when produced, it may be in the form of a pigment dispersion in which a colorant is dispersed in a dispersion medium.
- the pigment dispersion is obtained by dispersing the compound represented by the general formula (1) in a dispersion medium that is an organic solvent or a mixture of an organic solvent and water.
- a dispersion medium that is an organic solvent or a mixture of an organic solvent and water.
- the method for preparing the dye dispersion include the following methods.
- the compound represented by the general formula (1) and a resin are dissolved as necessary, and the mixture is sufficiently mixed with the dispersion medium while stirring.
- the compound can be finely dispersed into uniform fine particles by applying mechanical shearing force with a dispersing machine such as a ball mill, paint shaker, dissolver, attritor, sand mill, or high speed mill.
- the content of the compound represented by the general formula (1) in the pigment dispersion is preferably 1.0 to 30.0 parts by mass, more preferably 100 parts by mass with respect to the dispersion medium.
- the amount is 2.0 to 20.0 parts by mass, particularly preferably 3.0 to 15.0 parts by mass.
- organic solvent used as the dispersion medium examples include the following. Methyl alcohol, ethyl alcohol, modified ethyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, tert-butyl alcohol, sec-butyl alcohol, tert-amyl alcohol, 3-pentanol, octyl alcohol, benzyl alcohol, cyclohexanol, etc.
- Alcohols such as methyl cellosolve, ethyl cellosolve, glycols such as diethylene glycol and diethylene glycol monobutyl ether; ketones such as acetone, methyl ethyl ketone and methyl isobutyl ketone; esters such as ethyl acetate, butyl acetate, ethyl propionate and cellosolve acetate; hexane , Octane, petroleum ether, cyclohexane, benzene, toluene, xylene and other hydrocarbon solvents; Halogenated hydrocarbon solvents such as carbonized carbon, trichloroethylene and tetrabromoethane; ethers such as diethyl ether, dimethyl glycol, trioxane and tetrahydrofuran; acetals such as methylal and diethyl acetal; organic acids such as formic acid, acetic acid and propionic acid Organic compounds
- a polymerizable monomer as an organic solvent used as a dispersion medium.
- the polymerizable monomer is preferably an addition polymerizable monomer.
- styrene monomers such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o-ethylstyrene, m-ethylstyrene, p-ethylstyrene; methyl acrylate, acrylic acid
- styrene acrylate monomers, or methacrylate monomers are preferable, and these are preferably used alone or in combination.
- styrene is preferred as the dispersion medium because of ease of handling.
- a resin may be added to the pigment dispersion.
- the resin to be contained in the pigment dispersion is determined according to the intended use and is not particularly limited. However, when the toner is produced by the dissolution suspension method, the resin to be the binder resin can be dissolved. Good.
- the resin used as the binder resin include polystyrene resins, polyacrylic acid resins, polymethacrylic acid resins, polyacrylic acid ester resins, polymethacrylic acid ester resins, and styrene acrylic copolymers (for example, styrene -Acrylic acid ester copolymer, styrene-methacrylic acid ester copolymer, styrene-acrylic acid ester-methacrylic acid ester copolymer), polyester resin, polyvinyl ether resin, polyvinyl methyl ether resin, polyvinyl alcohol resin, polyvinyl butyral resin Etc. These resins can be used alone or in admixture of two or more.
- the pigment dispersion can be dispersed in water using an emulsifier.
- an emulsifier used in this case include a cationic surfactant, an anionic surfactant, and a nonionic surfactant.
- the cationic surfactant include dodecyl ammonium chloride, dodecyl ammonium bromide, dodecyl trimethyl ammonium bromide, dodecyl pyridinium chloride, dodecyl pyridinium bromide, hexadecyl trimethyl ammonium bromide and the like.
- anionic surfactant examples include sodium stearate, fatty acid soap of sodium dodecanoate, sodium dodecyl sulfate, sodium dodecylbenzene sulfate, sodium lauryl sulfate and the like.
- Nonionic surfactants include dodecyl polyoxyethylene ether, hexadecyl polyoxyethylene ether, nonylphenyl polyoxyethylene ether, lauryl polyoxyethylene ether, sorbitan monooleate polyoxyethylene ether, monodecanoyl sucrose, etc. It is done.
- the binder resin used in the yellow toner of the present invention is not particularly limited, and examples thereof include a thermoplastic resin.
- Specific examples include vinyl resins that are homopolymers or copolymers of the following polymerizable monomers.
- the polymerizable monomer include styrene or styrene derivatives such as styrene, parachlorostyrene, and ⁇ -methylstyrene; methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, Acrylic acid esters such as lauryl acrylate and 2-ethylhexyl acrylate; Methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, lauryl methacrylate and 2-ethylhexyl methacrylate; Acrylonitrile, methacrylonitrile, etc.
- Vinyl nitriles vinyl ethers such as vinyl ethyl ether and vinyl isobutyl ether; ketones such as vinyl methyl ketone, vinyl ethyl ketone and vinyl isopropenyl ketone; ethylene, propylene, butadiene and isoprene
- the resin used as the binder resin is not limited to the vinyl resin.
- non-vinyl condensation resins such as epoxy resins, polyester resins, polyurethane resins, polyamide resins, cellulose resins, and polyether resins can also be used. Further, graft polymers of these non-vinyl condensation resins and vinyl monomers can also be used. These resins may be used alone or in combination of two or more.
- the polyester resin is synthesized from a divalent or higher valent acid component and a divalent or higher valent alcohol component.
- the acid component is not particularly limited, and examples thereof include aliphatic dicarboxylic acids, dicarboxylic acids having a double bond, and dicarboxylic acids having a sulfonic acid group.
- aliphatic dicarboxylic acids include aliphatic dicarboxylic acids, dicarboxylic acids having a double bond, and dicarboxylic acids having a sulfonic acid group.
- the alcohol component is not particularly limited, but an aliphatic diol is preferable.
- the polyester resin is not particularly limited, but it is particularly preferable that the alcohol component / acid component has a molar ratio of 45/55 to 55/45 among all components.
- the acid value is preferably 90 mgKOH / g or less, and more preferably 50 mgKOH / g or less.
- the hydroxyl value is preferably 50 mgKOH / g or less, and more preferably 30 mgKOH / g or less.
- it is preferably 3 mgKOH / g or more.
- a crosslinking agent can be used during the synthesis of the binder resin in order to increase the mechanical strength of the toner and control the molecular weight of the toner molecules.
- the crosslinking agent used in the toner of the present invention is not particularly limited, but specifically, a bifunctional crosslinking agent or a polyfunctional crosslinking agent can be used.
- Difunctional linking agents such as divinylbenzene, bis (4-acryloxypolyethoxyphenyl) propane, ethylene glycol diacrylate, 1,3-butylene glycol diacrylate, 1,4-butanediol diacrylate, 1,5-pentane Diol diacrylate, 1,6-hexanediol diacrylate, neopentyl glycol diacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, polyethylene glycol # 200, # 400, # 600 diacrylate, Dipropylene glycol diacrylate, polypropylene glycol diacrylate, polyester-type diacrylate, and dimethacrylate above can be substituted for dimethacrylate Ones, and the like.
- the polyfunctional crosslinking agent is not particularly limited, but pentaerythritol triacrylate, trimethylol ethane triacrylate, trimethylol propane triacrylate, tetramethylol methane tetraacrylate, oligoester acrylate and its methacrylate, 2, 2 -Bis (4-methacryloxyphenyl) propane, diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, triallyl trimellitate and the like.
- crosslinking agents are preferably used in an amount of 0.05 to 10 parts by weight, more preferably 0.1 to 5 parts by weight, based on 100 parts by weight of the polymerizable monomer used to obtain the binder resin. It is more preferable.
- the glass transition temperature of the binder resin is preferably 45 to 80 ° C., more preferably 55 to 70 ° C.
- the number average molecular weight (Mn) of the binder resin is preferably 2,500 to 50,000.
- the weight average molecular weight (Mw) of the binder resin is preferably 10,000 to 1,000,000.
- the wax used as the constituent material of the toner in the present invention is not particularly limited, but petroleum wax such as paraffin wax, microcrystalline wax, petrolatum and derivatives thereof, montan wax and derivatives thereof, Fischer-Tropsch method Hydrocarbon waxes and derivatives thereof, polyolefin waxes and their derivatives represented by polyethylene, natural waxes such as carnauba wax and candelilla wax, and derivatives thereof.
- the derivatives include oxides, block copolymers with vinyl monomers, and graft modified products.
- Examples thereof include alcohols such as higher aliphatic alcohols, aliphatics such as stearic acid and palmitic acid or compounds thereof, acid amides, esters, ketones, hydrogenated castor oil and derivatives thereof, plant waxes, and animal waxes. These can be used alone or in combination.
- alcohols such as higher aliphatic alcohols, aliphatics such as stearic acid and palmitic acid or compounds thereof, acid amides, esters, ketones, hydrogenated castor oil and derivatives thereof, plant waxes, and animal waxes. These can be used alone or in combination.
- the addition amount of the wax is preferably in the range of 2.5 to 15.0 parts by mass, more preferably in the range of 3.0 to 10.0 parts by mass with respect to 100 parts by mass of the binder resin.
- the wax used in the present invention preferably has a melting point of 50 to 200 ° C., more preferably 55 to 150 ° C.
- the melting point of the wax is 50 ° C. or higher and 200 ° C. or lower, the toner's blocking resistance is further improved, and the wax seepage at the time of fixing can be improved, and the releasability in oilless fixing can be improved. it can.
- the melting point in the present invention refers to the peak temperature of the maximum endothermic peak in the differential scanning calorimetry (DSC) curve measured according to ASTM D3418-82. Specifically, the melting point of the wax was measured using a differential scanning calorimeter (manufactured by METTLER TRADE Co., Ltd .: DSC822) with a measurement temperature range of 30 to 200 ° C., a heating rate of 5 ° C./min, The DSC curve in the temperature range of 30 to 200 ° C. is obtained by the second temperature raising process, and is the peak temperature of the maximum endothermic peak in the obtained DSC curve.
- DSC differential scanning calorimetry
- the toner of the present invention may contain a charge control agent as necessary. This makes it possible to easily control the optimum triboelectric charge amount according to the development system.
- the charge control agent As the charge control agent, a known one can be used, and a charge control agent that has a high charging speed and can stably maintain a constant charge amount is particularly preferable. Further, when the toner is produced by a direct polymerization method, a charge control agent having a low polymerization inhibitory property and substantially free from a solubilized product in an aqueous dispersion medium is particularly preferable.
- the charge control agent is a polymer or copolymer having a sulfonic acid group, a sulfonic acid group or an alkoxysulfonyl group, a salicylic acid derivative and a metal complex thereof, a monoazo metal compound, an acetylacetone metal compound, and is used for controlling the toner to be negatively charged.
- Quaternary ammonium salts such as borate, and onium salts such as phosphonium salts and analogs thereof, and lake pigments thereof, triphenylmethane dyes and lake lake pigments
- the rake agents include phosphotungstic acid, phosphomolybdic acid Phosphotungstomolybdic acid, tannic acid, lauric acid, gallic acid, ferricyanide, ferrocyanide), higher fatty acid metal salts, dibutyltin oxide, dioctyltin oxide, dicyclohexyltin oxide
- diorganotin oxide, dibutyltin tin borate, dioctyl tin borate, diorgano tin borate such as dicyclohexyl tin borate, resin charge control agent and the like. These can be used alone or in combination of two or more.
- inorganic fine particles and resin particles may be externally added to the toner particles.
- the inorganic fine particles include silica, titanium oxide, alumina or their double oxides, and fine particles obtained by surface treatment thereof.
- the resin particles include resin particles such as vinyl resins, polyester resins, and silicone resins. It is done. These inorganic fine particles and resin particles are external additives having the functions of a flow aid and a cleaning aid.
- Examples of the method for producing toner particles include a pulverization method, a suspension polymerization method, a suspension granulation method, an emulsion polymerization method, an emulsion aggregation method, a dissolution suspension method, and an ester extension polymerization method.
- the suspension polymerization method is a production method including the following steps.
- the polymerization initiator may be contained in the polymerizable monomer composition, or may be added before or during granulation.
- a dispersion liquid (pigment dispersion) in which the colorant is dispersed in the first polymerizable monomer is used as the second polymerizable monomer. It is preferably prepared by mixing. That is, after the colorant is sufficiently dispersed in the first polymerizable monomer, it is mixed with the second polymerizable monomer together with the other toner materials, so that the colorant is in a better dispersion state. Can be present in the toner particles.
- the first polymerizable monomer and the second polymerizable monomer may be the same polymerizable monomer or different polymerizable monomers.
- polymerization initiator used in the suspension polymerization method a known polymerization initiator can be used. Specific examples include azo compounds, organic peroxides, inorganic peroxides, organometallic compounds, and photopolymerization initiators.
- 2,2′-azobis isobutyronitrile
- 2,2′-azobis (4-methoxy-2,4-dimethyl) Azo polymerization initiators such as valeronitrile), 2,2′-azobis (2,4-dimethylvaleronitrile), dimethyl 2,2′-azobis (isobutyrate), benzoyl peroxide, ditert-butyl peroxide, tert Organic peroxide polymerization initiators such as butyl peroxyisopropyl monocarbonate, tert-hexyl peroxybenzoate, tert-butyl peroxybenzoate, inorganic peroxide polymerization initiators such as potassium persulfate and ammonium persulfate, Hydrogen peroxide-ferrous, BPO-dimethylaniline, cerium (IV) salt-alcohol Redox initiators and the like.
- the photopolymerization initiator include acetopheny
- the addition amount of the polymerization initiator is preferably 0.1 to 20 parts by mass, more preferably 0.1 to 10 parts by mass with respect to 100 parts by mass of the polymerizable monomer.
- the kind of the polymerizable initiator is slightly different depending on the polymerization method, but is used alone or in combination with reference to the 10-hour half-life temperature.
- the aqueous medium used in the suspension polymerization method preferably contains a dispersion stabilizer.
- a dispersion stabilizer known inorganic and organic dispersion stabilizers can be used.
- Inorganic dispersion stabilizers include calcium phosphate, magnesium phosphate, aluminum phosphate, zinc phosphate, magnesium carbonate, calcium carbonate, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, calcium metasilicate, calcium sulfate, sulfuric acid Examples include barium, bentonite, silica, and alumina.
- organic dispersion stabilizer examples include polyvinyl alcohol, gelatin, methyl cellulose, methyl hydroxypropyl cellulose, ethyl cellulose, sodium salt of carboxymethyl cellulose, starch and the like.
- Nonionic, anionic and cationic surfactants can also be used. Specific examples include sodium dodecyl sulfate, sodium tetradecyl sulfate, sodium pentadecyl sulfate, sodium octyl sulfate, sodium oleate, sodium laurate, potassium stearate, calcium oleate and the like.
- the dispersion stabilizers in the present invention, it is preferable to use a poorly water-soluble inorganic dispersion stabilizer that is soluble in acid.
- the dispersion stabilizer when preparing an aqueous dispersion medium using a hardly water-soluble inorganic dispersion stabilizer, the dispersion stabilizer is added in an amount of 0.2 to 2 to 100 parts by mass of the polymerizable monomer. From the viewpoint of droplet stability in the aqueous medium of the polymerizable monomer composition, it is preferable to use the monomer in a ratio of 0.0 part by mass.
- the aqueous medium is preferably prepared using water in the range of 300 to 3000 parts by mass with respect to 100 parts by mass of the polymerizable monomer composition.
- a commercially available dispersion stabilizer when preparing an aqueous medium in which the poorly water-soluble inorganic dispersion stabilizer is dispersed, a commercially available dispersion stabilizer may be used as it is.
- a dispersion stabilizer in order to obtain dispersion stabilizer particles having a fine and uniform particle size, it is preferable to produce and prepare the poorly water-soluble inorganic dispersion stabilizer while stirring at high speed in water.
- a preferable dispersion stabilizer can be obtained by mixing sodium phosphate aqueous solution and calcium chloride aqueous solution under high speed stirring to form calcium phosphate fine particles.
- the toner particles contained in the toner of the present invention may be particles produced by a suspension granulation method.
- the suspension granulation method does not have a heating step, so it suppresses the resin-wax compatibilization that occurs when a low-melting wax is used, and suppresses the decrease in the glass transition temperature of the toner caused by the compatibilization. can do.
- the suspension granulation method has a wide range of options for the toner material used as the binder resin, and it is easy to use a polyester resin, which is generally advantageous for fixability, as a main component. Therefore, this is an advantageous production method for producing a toner having a resin composition to which the suspension polymerization method is difficult to apply.
- toner particles can be produced as follows.
- a colorant, a binder resin and a wax are mixed in a solvent to prepare a solvent composition (pigment dispersion).
- the solvent composition is dispersed in a liquid medium, and particles of the solvent composition are granulated to obtain a toner particle suspension.
- toner particles can be obtained by heating the obtained suspension or reducing the pressure in the reaction vessel to remove the solvent.
- the solvent composition is preferably prepared by mixing a dispersion obtained by dispersing a colorant in a first solvent together with a second solvent together with other toner materials. This allows the pigment to be present in the toner particles in a better dispersed state.
- Solvents that can be used in the suspension granulation method include hydrocarbons such as toluene, xylene, and hexane, halogen-containing hydrocarbons such as methylene chloride, chloroform, dichloroethane, trichloroethane, and carbon tetrachloride, methanol, ethanol, Alcohols such as butanol and isopropyl alcohol, polyhydric alcohols such as ethylene glycol, propylene glycol, diethylene glycol and triethylene glycol, cellosolves such as methyl cellosolve and ethyl cellosolve, ketones such as acetone, methyl ethyl ketone and methyl isobutyl ketone, benzyl Examples include ethers such as alcohol ethyl ether, benzyl alcohol isopropyl ether and tetrahydrofuran, and esters such as methyl acetate, ethyl acetate and butyl
- the amount of the solvent used is preferably in the range of 50 to 5000 parts by mass, more preferably in the range of 120 to 1000 parts by mass with respect to 100 parts by mass of the binder resin.
- the liquid medium such as an aqueous medium used in the suspension granulation method preferably contains a dispersion stabilizer.
- a dispersion stabilizer those used in the suspension polymerization method can be used.
- the amount of the dispersion stabilizer used is in the range of 0.01 to 20 parts by mass with respect to 100 parts by mass of the binder resin.
- the liquid composition in a liquid medium such as an aqueous medium is used. It is preferable in terms of droplet stability.
- toner particles are produced by a pulverization method, a charge control agent and other additives are used as necessary for the colorant, binder resin, and wax.
- the pulverized toner particles can be produced using a known production apparatus such as a mixer, a thermal kneader, or a classifier.
- the binder resin, colorant, and wax, and other materials such as a charge control agent as necessary, are sufficiently mixed by a mixer such as a Henschel mixer or a ball mill.
- a mixer such as a Henschel mixer or a ball mill.
- it is melted using a heat kneader such as a roll, a kneader or an extruder.
- the wax is dispersed while the resins are mixed with each other by kneading and kneading.
- toner particles can be obtained by pulverization and classification.
- the binder resin may be used alone or in combination of two or more.
- the binder resin may be used alone or in combination of two or more.
- the emulsion aggregation method is a production method including the following steps. Preparing a wax dispersion in which wax is dispersed in an aqueous medium; Preparing a resin particle dispersion in which resin particles are dispersed in an aqueous medium; A step of preparing a colorant dispersion in which a colorant is dispersed in an aqueous medium, Aggregation step of mixing the wax dispersion, the resin particle dispersion, and the colorant dispersion and aggregating the wax, the resin particles, and the colorant contained in each dispersion to form aggregate particles And heating and aggregating the aggregate particles.
- the aqueous medium means a medium containing water as a main component. Specific examples of the aqueous medium include water itself, water added with a pH adjusting agent, water added with an organic solvent, and the like.
- a dispersant such as a surfactant can be added to each component dispersion (wax dispersion, resin particle dispersion, colorant dispersion).
- the colorant is dispersed by a known method, and a media type dispersing machine such as a rotary shearing type homogenizer, a ball mill, a sand mill, and an attritor, and a high pressure opposed collision type dispersing machine are preferably used.
- Surfactants include water-soluble polymers, inorganic compounds, and ionic or nonionic surfactants.
- ionicity with high dispersibility is preferable from the viewpoint of dispersibility, and an anionic surfactant is particularly preferably used.
- the molecular weight of the surfactant is preferably 100 to 10,000, and more preferably 200 to 5,000.
- the surfactant include water-soluble polymers such as polyvinyl alcohol, methyl cellulose, carboxymethyl cellulose, and sodium polyacrylate; sodium dodecylbenzenesulfonate, sodium octadecyl sulfate, sodium oleate, sodium laurate, and potassium stearate.
- Anionic surfactants such as; cationic surfactants such as laurylamine acetate and lauryltrimethylammonium chloride; zwitterionic surfactants such as lauryldimethylamine oxide; polyoxyethylene alkyl ether, polyoxyethylene alkylphenyl ether, Surfactants such as nonionic surfactants such as polyoxyethylene alkylamine; tricalcium phosphate, aluminum hydroxide, calcium sulfate, carbonic acid Calcium, inorganic compounds such as barium carbonate.
- these may be used individually by 1 type and may be used in combination of 2 or more type as needed.
- the wax dispersion used in the emulsion aggregation method is prepared by dispersing wax in an aqueous medium.
- the wax dispersion is prepared by a known method.
- the wax the above-described wax can be used.
- the resin particle dispersion is prepared by dispersing resin particles in an aqueous medium.
- the aqueous medium means a medium containing water as a main component.
- Specific examples of the aqueous medium include water itself, water added with a pH adjusting agent, and water added with an organic solvent.
- the resin particle dispersion used in the present invention is obtained by dispersing resin particles in an aqueous medium.
- the resin particle dispersion is prepared by a known method. For example, in the case of a resin particle dispersion containing resin particles containing a vinyl monomer, particularly a styrene monomer, the monomer is subjected to emulsion polymerization using a surfactant or the like. Thus, a resin particle dispersion can be prepared.
- a resin for example, a polyester resin
- a disperser such as a homogenizer
- the resin particle dispersion can be prepared by evaporating the solvent.
- a resin particle dispersion may be prepared by adding a surfactant to the resin and emulsifying and dispersing in water with a disperser such as a homogenizer or by a phase inversion emulsification method.
- the volume-based median diameter (D50) of the resin particles in the resin particle dispersion is preferably 0.005 to 1.0 ⁇ m, more preferably 0.01 to 0.4 ⁇ m.
- D50 volume-based median diameter
- the average particle diameter of the resin particles can be measured by a measuring method such as a dynamic light scattering method (DLS), a laser scattering method, a centrifugal sedimentation method, a field-flow fractionation method, or an electrical detector method.
- the average particle size of the resin particles is measured by a dynamic light scattering method (DLS) / laser Doppler method at 20 ° C. and 0.01% by mass solid content unless otherwise specified. It means 50% cumulative particle size value (D50) based on volume.
- the colorant dispersion used in the emulsion aggregation method is prepared by dispersing a colorant together with a surfactant in an aqueous medium. Specific examples of the preparation method will be described below.
- the compound represented by the general formula (1) of the present invention is prepared as a dispersion (dye dispersion). It is also possible to prepare a dispersion in which a plurality of compounds represented by the general formula (1) are mixed.
- the colorant is dispersed by a known method, and a media type dispersing machine such as a rotary shearing type homogenizer, a ball mill, a sand mill, and an attritor, and a high pressure opposed collision type dispersing machine are preferably used.
- the amount of the surfactant used is preferably from 0.01 to 10 parts by weight, more preferably from 100 parts by weight of the colorant, from the viewpoint of easy removal of the surfactant in the toner. Is 0.1 to 5.0 parts by mass, and more preferably 0.5 to 3.0 parts by mass. As a result, the amount of the surfactant remaining in the obtained toner is reduced, the image density of the toner is high, and the effect that fog is hardly generated is obtained.
- the method for forming the aggregate particles is not particularly limited, but a pH adjuster, a flocculant, and a stabilizer are added and mixed in the above mixed solution, and temperature and mechanical power (stirring) are appropriately added. A method can be illustrated suitably.
- the pH adjuster is not particularly limited, and examples thereof include alkalis such as ammonia and sodium hydroxide, and acids such as nitric acid and citric acid.
- the flocculant is not particularly limited, and examples thereof include inorganic metal salts such as sodium chloride, magnesium carbonate, magnesium chloride, magnesium nitrate, magnesium sulfate, calcium chloride, aluminum sulfate, and divalent metal complexes. It is done.
- the stabilizer is mainly a surfactant.
- the surfactant is not particularly limited, but is a water-soluble polymer such as polyvinyl alcohol, methyl cellulose, carboxymethyl cellulose, sodium polyacrylate; sodium dodecylbenzenesulfonate, sodium octadecyl sulfate, sodium oleate, lauric acid
- Anionic surfactants such as sodium and potassium stearate; Cationic surfactants such as laurylamine acetate and lauryltrimethylammonium chloride; Zwitterionic surfactants such as lauryldimethylamine oxide; Polyoxyethylene alkyl ether and polyoxy Surfactants such as nonionic surfactants such as ethylene alkylphenyl ether and polyoxyethylene alkylamine; tricalcium phosphate, aluminum hydroxide, sulfuric acid Calcium, calcium carbonate, inorganic compounds such as barium carbonate. In addition, these may be used individually by 1 type and surfactant may be used in combination of 2 or more type as needed.
- the average particle diameter of the aggregated particles formed here is not particularly limited, but it is usually preferable to control the average particle diameter to be approximately the same as the average particle diameter of the toner particles to be obtained.
- the control can be easily performed by appropriately setting and changing the temperature at the time of addition / mixing of the flocculant and the like and the conditions of the stirring and mixing.
- the pH adjusting agent and the surfactant can be appropriately added.
- toner particles are formed by fusing the aggregate particles with heating.
- the heating temperature may be between the glass transition temperature (Tg) of the resin contained in the aggregate particles and the decomposition temperature of the resin. Under the same agitation as in the agglomeration step, the progress of agglomeration is stopped by adding a surfactant or adjusting the pH, and the aggregated particles are fused and united by heating to a temperature higher than the glass transition temperature of the resin particles.
- the heating time may be such that the fusion is sufficiently performed. Specifically, it may be performed for about 10 minutes to 10 hours.
- the fusion step may further include a step (attachment step) in which a fine particle dispersion in which fine particles are dispersed is added and mixed to attach the fine particles to the aggregate particles to form a core / shell structure. is there.
- a step (attachment step) in which a fine particle dispersion in which fine particles are dispersed is added and mixed to attach the fine particles to the aggregate particles to form a core / shell structure. is there.
- Toner particles are obtained by washing, filtering and drying the toner particles obtained after the fusing step under appropriate conditions. In this case, in order to ensure sufficient charging characteristics and reliability as a toner, it is preferable to sufficiently wash the toner particles.
- the washing method is not limited, but can be carried out by filtering the suspension containing toner particles, stirring and washing the obtained filtrate with distilled water, and further filtering this. From the viewpoint of the chargeability of the toner, washing is repeated until the electric conductivity of the filtrate is 150 ⁇ S / cm or less.
- the electric conductivity of the filtrate is 150 ⁇ S / cm or less, it is possible to suppress a decrease in charging characteristics of the toner, and as a result, it is possible to further suppress the occurrence of fogging and improve the image density.
- drying process For the drying, a known method such as a normal vibration type fluidized drying method, a spray drying method, a freeze drying method, or a flash jet method can be used.
- the moisture content of the toner particles after drying is preferably 1.5% by mass or less, and more preferably 1.0% by mass or less.
- the yellow toner of the present invention preferably has a weight average particle diameter (D4) of 4.0 to 9.0 ⁇ m, more preferably 4.9 to 7.5 ⁇ m.
- D4 weight average particle diameter
- the yellow toner of the present invention has a ratio of the weight average particle diameter (D4) to the number average particle diameter (D1) (hereinafter also referred to as weight average particle diameter (D4) / number average particle diameter (D1) or D4 / D1). It is preferably 1.35 or less, and more preferably 1.30 or less.
- the weight average particle diameter (D4) and the number average particle diameter (D1) of the yellow toner of the present invention are adjusted differently depending on the toner particle manufacturing method.
- it can be adjusted by controlling the concentration of the dispersing agent used at the time of preparing the aqueous medium, the reaction stirring speed, or the reaction stirring time.
- the yellow toner of the present invention preferably has an average circularity of 0.930 or more and 0.995 or less as measured by a flow type particle image analyzer, and the toner transferability is greatly improved. From 0.960 to 0.990 is more preferable.
- the toner of the present invention can also be used as a developer used in a liquid development method (hereinafter referred to as a liquid developer).
- a colorant in order to obtain a liquid developer, a colorant, a binder resin, a wax containing a compound represented by the general formula (1), a charge control agent, if necessary, are added to the electrically insulating carrier liquid. It is produced by dispersing or dissolving the agent. Alternatively, it may be prepared by a two-stage method in which a concentrated toner is first prepared and further diluted with an electrically insulating carrier solution to prepare a developer.
- the disperser is not particularly limited, but a media-type disperser such as a rotary shearing homogenizer, a ball mill, a sand mill, and an attritor, and a high-pressure opposed collision disperser are preferably used.
- a media-type disperser such as a rotary shearing homogenizer, a ball mill, a sand mill, and an attritor, and a high-pressure opposed collision disperser are preferably used.
- a known colorant such as a pigment or a dye may be used alone or in combination of two or more kinds in addition to the compound represented by the general formula (1).
- Wax and binder resin are the same as described above.
- the charge control agent is not particularly limited as long as it is used in a liquid developer for electrostatic charge development, but cobalt naphthenate, copper naphthenate, copper oleate, cobalt oleate, octylic acid Zirconium, cobalt octylate, sodium dodecylbenzenesulfonate, calcium dodecylbenzenesulfonate, soybean lecithin, aluminum octoate and the like.
- the electrically insulating carrier liquid used in the present invention is not particularly limited, but it is preferable to use an organic solvent having a high electric resistance of 10 9 ⁇ ⁇ cm or more and a low dielectric constant of 3 or less.
- aliphatic hydrocarbon solvents such as hexane, pentane, octane, nonane, decane, undecane, dodecane, etc., Isopar H, G, K, L, M (manufactured by Exxon Chemical Co., Ltd.), linearlen dimer A- 20, A-20H (made by Idemitsu Kosan Co., Ltd.) and those having a boiling point of 68 to 250 ° C. are preferred. These may be used alone or in combination of two or more in the range where the viscosity of the system does not increase.
- reaction product was identified by a plurality of analysis methods using the following apparatuses. That is, the analysis apparatus used was a 1 H-nuclear magnetic resonance spectrometer (ECA-400, manufactured by JEOL Ltd.) or MALDI MS (autoflex apparatus, manufactured by Bruker Daltonics). In MALDI MS, the detection ion adopted a negative mode.
- ECA-400 1 H-nuclear magnetic resonance spectrometer
- MALDI MS autoflex apparatus, manufactured by Bruker Daltonics
- the yellow toner of the present invention and the comparative yellow toner were produced by the method described below.
- Example 1 5 parts by mass of the compound (1) and 120 parts by mass of styrene were mixed for 3 hours using an attritor (manufactured by Mitsui Mining Co., Ltd.) to obtain a pigment dispersion (1).
- High-speed stirring device T. K 710 parts of ion-exchanged water and 450 parts of a 0.1 mol / L trisodium phosphate aqueous solution were added to a 2 L four-necked flask equipped with a homomixer (manufactured by PRIMIX Corporation). While stirring at a rotational speed of 12000 rpm, the mixture was heated to 60 ° C. To this, 68 parts by mass of a 1.0 mol / L-calcium chloride aqueous solution was gradually added to prepare an aqueous medium containing a small amount of poorly water-soluble dispersion stabilizer calcium phosphate.
- the polymer fine particle dispersion was transferred to a washing container, and while stirring, diluted hydrochloric acid was added to adjust the pH to 1.5, and the mixture was stirred for 2 hours.
- Solid-liquid separation was performed with a filter to obtain polymer fine particles. Redispersion of polymer fine particles in water and solid-liquid separation were repeated until the phosphoric acid-calcium compound containing calcium phosphate was sufficiently removed. Thereafter, the polymer fine particles finally solid-liquid separated were sufficiently dried with a dryer to obtain yellow toner particles (1).
- Example 2 ⁇ Examples 2 and 3>
- 5 parts by mass of the compound (1) was changed to 6 parts by mass (Example 2) of the compound (2) and 7 parts by mass (Example 3) of the compound (14), respectively.
- yellow toners (2) and (3) were obtained.
- the volume-based median diameter of the colorant particles in the compound (1) dispersion was 0.2 ⁇ m, and the concentration of the compound (1) dispersion was 10% by mass.
- Example 11 and 12 Yellow toner in the same manner as in Example 10, except that 100 parts by mass of compound (1) was changed to 60 parts by mass of compound (5) (Example 11) and 55 parts by mass of compound (21) (Example 12). (11) and (12) were obtained.
- Compound (19) 5 parts by mass Aluminum 1,4-di-t-butylsalicylate compound 0.5 part by mass Paraffin wax (peak temperature (melting point) 78 ° C.
- the material was mixed well with a Henschel mixer (FM-75J type, manufactured by Mitsui Mining Co., Ltd.) and then 60 kg in a twin-screw kneader (PCM-45 type, manufactured by Ikekai Steel Co., Ltd.) set at a temperature of 130 ° C.
- the mixture was kneaded with a feed amount of / hr (the kneaded material temperature at the time of discharge was about 150 ° C.).
- the obtained kneaded product was cooled, coarsely crushed with a hammer mill, and then finely pulverized with a mechanical pulverizer (T-250: manufactured by Turbo Kogyo Co., Ltd.) at a Feed amount of 20 kg / hr.
- a mechanical pulverizer T-250: manufactured by Turbo Kogyo Co., Ltd.
- the obtained toner finely pulverized product was classified by a multi-division classifier using the Coanda effect to obtain yellow toner particles (13).
- Example 14 and 15 Yellow toner in the same manner as in Example 13, except that 5 parts by mass of compound (19) were changed to 5 parts by mass of compound (22) (Example 14) and 5 parts by mass of compound (28) (Example 15), respectively. (14) and (15) were obtained.
- Example 16 5 parts by mass of compound (1) I.
- Pigment Yellow 185 manufactured by BASF, trade name “PALIOTOL Yellow D1155” was changed to 4 parts by mass, and the compound (1) was changed to 3 parts by mass.
- a yellow toner (16) was obtained in the same manner as in Example 1 except for this.
- Example 17 C. I. 100 parts by weight of Pigment Yellow 180 (manufactured by DIC Corporation, trade name “SYMULER Fast Yellow BY2000GT”), 15 parts by weight of Neogen RK, 885 parts by weight of ion-exchanged water, and a wet jet mill JN100 (manufactured by Toko) For about 1 hour and C.I. I. Pigment Yellow 180 dispersion was obtained.
- Pigment Yellow 180 manufactured by DIC Corporation, trade name “SYMULER Fast Yellow BY2000GT”
- Neogen RK 15 parts by weight of Neogen RK
- 885 parts by weight of ion-exchanged water 885 parts by weight of ion-exchanged water
- a wet jet mill JN100 manufactured by Toko
- the volume-based median diameter of the colorant particles in Pigment Yellow 180 dispersion is 0.2 ⁇ m.
- the concentration of Pigment Yellow 180 dispersion was 10% by mass.
- Example 10 -160 parts by mass of the resin particle dispersion used in Example 10-10 parts by mass of the wax dispersion used in Example 10-C.I. I. Pigment Yellow 180 Dispersion 3 parts by weight Compound used in Example 10 (1) Dispersion 4 parts by weight Magnesium sulfate 0.2 part Disperse the above material using a homogenizer (manufactured by IKA: Ultra Tarrax T50) Then, the mixture was heated to 65 ° C. with stirring. After stirring at 65 ° C. for 1 hour, observation with an optical microscope confirmed that aggregate particles having an average particle diameter of about 6.0 ⁇ m were formed.
- a homogenizer manufactured by IKA: Ultra Tarrax T50
- Pigment Yellow 155 manufactured by Clariant, trade name “Toner Yellow 3GP”
- Toner Yellow 3GP Cosmetic Yellow 3GP
- Compound (22) 3 parts by weight-1,4-di-t-butylsalicylic acid aluminum compound 0.5 part by weight-Paraffin wax (peak temperature (melting point) 78 ° C of maximum endothermic peak in DSC measurement) 5 parts by weight
- the materials were mixed well with a Henschel mixer (FM-75J type, manufactured by Mitsui Mining Co., Ltd.), and then mixed with a twin-screw kneader (PCM-45 type, manufactured by Ikekai Steel Co., Ltd.) set at a temperature of 130 ° C.
- the mixture was kneaded with a feed amount of hr (kneaded material temperature at the time of discharge was about 150 ° C.).
- the obtained kneaded product was cooled, coarsely crushed with a hammer mill, and then finely pulverized with a mechanical pulverizer (T-250: manufactured by Turbo Kogyo Co., Ltd.) at a Feed amount of 20 kg / hr.
- toner particles were obtained by classifying the obtained finely pulverized toner with a multi-division classifier using the Coanda effect.
- To 100 parts by mass of the toner particles 1.8 parts by mass of hydrophobized silica fine powder having a specific surface area measured by the BET method of 200 m 2 / g is dry-mixed with a Henschel mixer (manufactured by Mitsui Mining Co., Ltd.). Toner (18) was obtained.
- a surfactant preferably alkylbenzenesulfonate
- a measurement sample toner
- the electrolytic solution in which the sample is suspended is subjected to a dispersion treatment with an ultrasonic disperser for about 1 to 3 minutes.
- the toner volume distribution and number distribution are obtained.
- the number average particle diameter (D1) is calculated from the number distribution
- the weight average particle diameter (D4) is calculated from the volume distribution
- D4 / D1 is obtained from them (the median value of each channel is the representative value for each channel).
- D1 the median value of each channel is the representative value for each channel.
- the above channels include 2.00 to 2.52 ⁇ m, 2.52 to 3.17 ⁇ m, 3.17 to 4.00 ⁇ m, 4.00 to 5.04 ⁇ m, 5.04 to 6.35 ⁇ m, 6.35 to 8 0.000, 8.00 to 10.08 ⁇ m, 10.08 to 12.70 ⁇ m, 12.70 to 16.00 ⁇ m, 16.00 to 20.20 ⁇ m, 20.20 to 25.40 ⁇ m, 25.40 to 32.00 ⁇ m 13 channels of 32.00 to 40.30 ⁇ m are used.
- Table 1 shows the particle size distribution of the obtained toner.
- PY185, PY180, and PY155 are C.I. I. Pigment yellow 185, C.I. I. Pigment yellow 180, C.I. I. Pigment Yellow 155 is shown.
- a CRG filled with each yellow toner was prepared for each evaluation item.
- Each CRG filled with each toner was set in the image forming apparatus and evaluated for each evaluation item described below.
- OD (Y) is 1.6 or more (optical density is very high)
- the toner produced using the dye compound (colorant) of the general formula (1) has a higher coloring power and light resistance than the toner produced using the comparative compound. It turns out that is excellent. It was also found that there was no effect on the coloring power with respect to the amount of wax.
- the toner can be used as a toner having high coloring power and high light resistance.
Landscapes
- Physics & Mathematics (AREA)
- General Physics & Mathematics (AREA)
- Developing Agents For Electrophotography (AREA)
Priority Applications (1)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| US14/850,003 US9811014B2 (en) | 2014-03-24 | 2015-09-10 | Yellow toner and production method therefor |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2014-060338 | 2014-03-24 | ||
| JP2014060338A JP6355378B2 (ja) | 2014-03-24 | 2014-03-24 | イエロートナーおよびその製造方法 |
Related Child Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| US14/850,003 Continuation US9811014B2 (en) | 2014-03-24 | 2015-09-10 | Yellow toner and production method therefor |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2015146099A1 true WO2015146099A1 (ja) | 2015-10-01 |
Family
ID=54194649
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2015/001563 Ceased WO2015146099A1 (ja) | 2014-03-24 | 2015-03-20 | イエロートナーおよびその製造方法 |
Country Status (3)
| Country | Link |
|---|---|
| US (1) | US9811014B2 (https=) |
| JP (1) | JP6355378B2 (https=) |
| WO (1) | WO2015146099A1 (https=) |
Families Citing this family (9)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| DE112013001217T5 (de) * | 2012-02-29 | 2015-01-08 | Canon Kabushiki Kaisha | Pigmentdispersion und gelbe Resist-Zusammensetzung für Farbfilter und Tintenzusammensetzung, die die Pigmentdispersion enthält |
| JP6478810B2 (ja) * | 2015-05-27 | 2019-03-06 | キヤノン株式会社 | イエロートナー |
| JP6738183B2 (ja) | 2015-05-27 | 2020-08-12 | キヤノン株式会社 | トナー |
| JP6543116B2 (ja) * | 2015-07-02 | 2019-07-10 | キヤノン株式会社 | 色素化合物、トナー及び該トナーの製造方法 |
| JP6727819B2 (ja) * | 2016-01-28 | 2020-07-22 | キヤノン株式会社 | トナー |
| JP6824643B2 (ja) * | 2016-06-17 | 2021-02-03 | キヤノン株式会社 | トナー |
| US10310396B2 (en) * | 2017-05-15 | 2019-06-04 | Canon Kabushiki Kaisha | Method of producing toner |
| EP3582013B1 (en) * | 2018-06-13 | 2023-08-09 | Canon Kabushiki Kaisha | Toner and method for producing toner |
| JP6921902B2 (ja) | 2018-07-30 | 2021-08-18 | キヤノン株式会社 | 化合物、インク、カラーフィルター用レジスト組成物、カラーフィルター、感熱転写記録用シート、及びトナー |
Citations (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2011257707A (ja) * | 2010-06-11 | 2011-12-22 | Nippon Zeon Co Ltd | イエロートナー |
| JP2011257706A (ja) * | 2010-06-11 | 2011-12-22 | Nippon Zeon Co Ltd | イエロートナー |
| WO2012039361A1 (ja) * | 2010-09-24 | 2012-03-29 | 株式会社日本触媒 | アゾ化合物およびこれを含むカラーフィルタ用色素 |
| JP2014029520A (ja) * | 2012-06-27 | 2014-02-13 | Canon Inc | イエロートナー |
Family Cites Families (11)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US5853929A (en) * | 1993-06-28 | 1998-12-29 | Zeneca Limited | Trichromatic set of colored toners |
| JPH07140716A (ja) | 1993-06-29 | 1995-06-02 | Toyobo Co Ltd | 電子写真用トナ− |
| JP4111358B2 (ja) | 1998-03-31 | 2008-07-02 | コニカミノルタホールディングス株式会社 | カラートナーとその製造方法 |
| WO2008069045A1 (ja) * | 2006-11-30 | 2008-06-12 | Canon Kabushiki Kaisha | 色素化合物及び該色素化合物を含有するイエロートナー |
| WO2008114886A1 (ja) | 2007-03-19 | 2008-09-25 | Canon Kabushiki Kaisha | 色素化合物、イエロートナー、感熱転写記録用シート、及びインク |
| WO2013002294A1 (en) | 2011-06-28 | 2013-01-03 | Canon Kabushiki Kaisha | Yellow toner |
| CN104160339A (zh) | 2012-03-07 | 2014-11-19 | 佳能株式会社 | 黄色调色剂及黄色调色剂的生产方法 |
| US9244373B2 (en) | 2012-08-22 | 2016-01-26 | Canon Kabushiki Kaisha | Toner and method of producing toner |
| US8927185B2 (en) | 2012-08-22 | 2015-01-06 | Canon Kabushiki Kaisha | Toner and toner production method |
| CN104583876A (zh) | 2012-08-24 | 2015-04-29 | 佳能株式会社 | 黄色调色剂和黄色调色剂的制造方法 |
| WO2014034098A1 (ja) | 2012-08-30 | 2014-03-06 | キヤノン株式会社 | イエロートナー |
-
2014
- 2014-03-24 JP JP2014060338A patent/JP6355378B2/ja not_active Expired - Fee Related
-
2015
- 2015-03-20 WO PCT/JP2015/001563 patent/WO2015146099A1/ja not_active Ceased
- 2015-09-10 US US14/850,003 patent/US9811014B2/en not_active Expired - Fee Related
Patent Citations (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2011257707A (ja) * | 2010-06-11 | 2011-12-22 | Nippon Zeon Co Ltd | イエロートナー |
| JP2011257706A (ja) * | 2010-06-11 | 2011-12-22 | Nippon Zeon Co Ltd | イエロートナー |
| WO2012039361A1 (ja) * | 2010-09-24 | 2012-03-29 | 株式会社日本触媒 | アゾ化合物およびこれを含むカラーフィルタ用色素 |
| JP2014029520A (ja) * | 2012-06-27 | 2014-02-13 | Canon Inc | イエロートナー |
Also Published As
| Publication number | Publication date |
|---|---|
| JP6355378B2 (ja) | 2018-07-11 |
| US20150378273A1 (en) | 2015-12-31 |
| US9811014B2 (en) | 2017-11-07 |
| JP2015184454A (ja) | 2015-10-22 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP6355378B2 (ja) | イエロートナーおよびその製造方法 | |
| JP6016502B2 (ja) | マゼンタトナー及びその製造方法 | |
| JP6182022B2 (ja) | イエロートナー | |
| JP6053578B2 (ja) | イエロートナー及び該イエロートナーの製造方法 | |
| JP6129026B2 (ja) | トナー | |
| JP6129027B2 (ja) | トナー | |
| US9069273B2 (en) | Yellow toner and method for producing the yellow toner | |
| JP2017003818A (ja) | トナー | |
| JP2014059555A (ja) | トナー及びトナーの製造方法 | |
| JP2014029520A (ja) | イエロートナー | |
| JP2013117022A (ja) | 着色樹脂粉体及び該着色樹脂粉体を用いたトナー | |
| JP2013047795A (ja) | マゼンタトナー | |
| EP2701007B1 (en) | Toner and method of producing toner | |
| JP6418869B2 (ja) | トナー | |
| JP6478810B2 (ja) | イエロートナー | |
| JP6543116B2 (ja) | 色素化合物、トナー及び該トナーの製造方法 | |
| JP2017014414A (ja) | 色素化合物、トナー及び該トナーの製造方法 | |
| JP2017003992A (ja) | トナー |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 15768585 Country of ref document: EP Kind code of ref document: A1 |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| 122 | Ep: pct application non-entry in european phase |
Ref document number: 15768585 Country of ref document: EP Kind code of ref document: A1 |