WO2022202131A1 - 水性プライマー塗料組成物及び複層塗膜形成方法 - Google Patents
水性プライマー塗料組成物及び複層塗膜形成方法 Download PDFInfo
- Publication number
- WO2022202131A1 WO2022202131A1 PCT/JP2022/008380 JP2022008380W WO2022202131A1 WO 2022202131 A1 WO2022202131 A1 WO 2022202131A1 JP 2022008380 W JP2022008380 W JP 2022008380W WO 2022202131 A1 WO2022202131 A1 WO 2022202131A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- water
- resin
- film
- coating film
- forming
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B05—SPRAYING OR ATOMISING IN GENERAL; APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D—PROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D1/00—Processes for applying liquids or other fluent materials
- B05D1/36—Successively applying liquids or other fluent materials, e.g. without intermediate treatment
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B05—SPRAYING OR ATOMISING IN GENERAL; APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D—PROCESSES FOR APPLYING FLUENT MATERIALS TO SURFACES, IN GENERAL
- B05D7/00—Processes, other than flocking, specially adapted for applying liquids or other fluent materials to particular surfaces or for applying particular liquids or other fluent materials
- B05D7/02—Processes, other than flocking, specially adapted for applying liquids or other fluent materials to particular surfaces or for applying particular liquids or other fluent materials to macromolecular substances, e.g. rubber
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D123/00—Coating compositions based on homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Coating compositions based on derivatives of such polymers
- C09D123/26—Coating compositions based on homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Coating compositions based on derivatives of such polymers modified by chemical after-treatment
- C09D123/28—Coating compositions based on homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Coating compositions based on derivatives of such polymers modified by chemical after-treatment by reaction with halogens or compounds containing halogen
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D133/00—Coating compositions based on homopolymers or copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and at least one being terminated by only one carboxyl radical, or of salts, anhydrides, esters, amides, imides, or nitriles thereof; Coating compositions based on derivatives of such polymers
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D201/00—Coating compositions based on unspecified macromolecular compounds
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D5/00—Coating compositions, e.g. paints, varnishes or lacquers, characterised by their physical nature or the effects produced; Filling pastes
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D7/00—Features of coating compositions, not provided for in group C09D5/00; Processes for incorporating ingredients in coating compositions
- C09D7/20—Diluents or solvents
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D7/00—Features of coating compositions, not provided for in group C09D5/00; Processes for incorporating ingredients in coating compositions
- C09D7/40—Additives
- C09D7/43—Thickening agents
Definitions
- the present invention relates to a water-based primer coating composition and a method for forming a multilayer coating film.
- a plastic member may be used for a part or the whole of an automobile outer panel.
- plastic members include polyolefin resins such as polypropylene.
- Polyolefin-based resins have low polarity and crystallinity, and thus are difficult to obtain adhesion of a coating film. For this reason, in order to apply a highly polar topcoat, solvent-based primers and colored water-based primers are usually applied, and many of them contain polyolefin resins as an essential component from the viewpoint of improving adhesion.
- organic solvent-based resins have been used for these polyolefin resins for a long time. There are many designs that include substances, and there is a demand for the development of water-based surface treatment agents that include environmentally friendly polyolefin resins.
- Patent Document 2 describes a non-chlorine polyolefin emulsion obtained by converting a non-chlorine polyolefin resin having a melting point of 40 to 100° C. into a water-based solution, and a specific water-based self-emulsifying polyurethane resin.
- Aqueous primer compositions containing certain proportions are disclosed. It is described that this composition has excellent adhesion to polypropylene resin materials, especially during baking at about 80°C.
- the present applicant discloses a repair coating method for a coated body in Patent Document 3.
- an all-water-based coating system or an eco-friendly coating system comprising a water-based primer surfacer, a water-based coloring base, and a water-based clear coating can be obtained.
- the aesthetic appearance of the surface can be maintained for a long period of time.
- the drying temperature is about normal temperature to 60° C., the film-forming property and drying property may not be sufficient.
- JP-A-58-15535 JP 2009-292951 A Japanese Patent Application Laid-Open No. 2020-22948
- the present invention has been made in view of the above circumstances, and is a water-based primer coating capable of forming a primer coating film that is excellent in film-forming properties and coating workability at low temperatures and that is excellent in adhesion to hard-to-adhere members. It is an object of the present invention to provide a composition and a method for forming a multi-layered coating film which can form a multi-layered coating film excellent in appearance and water resistance.
- the present invention provides a water-dispersible and/or water-soluble film-forming resin (A), and a chlorinated or non-chlorinated polyolefin resin (B) having a softening temperature of less than 80°C and a degree of chlorination of 25% or less.
- the content ratio of the film-forming resin (A) and the chlorinated or non-chlorinated polyolefin resin (B) is 1:99 or more and 99:1 or less, and the solid content is 0.5 % or more and 15% or less.
- the minimum film-forming temperature of the film-forming resin (A) is preferably 25°C or lower.
- the film-forming resin (A) preferably contains at least one selected from acrylic resins, urethane resins, polyester resins and polycarbonate resins.
- the film-forming resin (A) is a polymerizable unsaturated monomer (x ) and the hydrophobic polymerizable unsaturated monomer (y) are preferably included in the copolymerization component.
- the aqueous primer coating composition of the present invention further contains a viscosity modifier (C), and the viscosity modifier (C) includes a cellulose-based viscosity modifier, a polyacrylic acid-based viscosity modifier, and a urethane-associated viscosity modifier. It preferably contains at least one selected from regulators.
- the aqueous primer coating composition of the present invention further contains an organic solvent (D), and the organic solvent (D) preferably contains an organic solvent (d1) having a surface tension of 29 dyn/cm 2 or less.
- the water-based primer paint composition of the present invention preferably contains substantially no color pigments.
- the aqueous primer coating composition of the present invention preferably has a structural viscosity index TI value represented by the following formula (1) of 1.1 or more and 5.0 or less.
- TI value Va/Vb (1)
- Va is the apparent viscosity (mPa sec) measured by a rotational viscometer at a temperature of 25 ° C. at a rotation speed of 6 times / minute
- Vb is a rotational viscometer at a temperature of 25 ° C. Viscosity (mPa ⁇ sec) measured at 60 revolutions/minute.
- the method for forming a multilayer coating film of the present invention comprises a step (1) of forming a primer coating film (I) by coating the water-based primer coating composition of the present invention on a resin member; , step (2) of forming a colored base coating film (II) by applying an aqueous colored base coating composition, and on the colored base coating film (II) obtained in step (2), an aqueous two-component clear A step (3) of applying and drying the coating composition to form a clear coating film (III).
- a primer coating other than the water-based primer coating composition of the present invention is applied on the primer coating (I), and the primer coating (I-2 ).
- the drying temperature in step (3) is preferably 50°C or higher and 70°C or lower.
- the dry film thickness of the primer coating film (I) is preferably 1 ⁇ m or more and 8 ⁇ m or less.
- the resin member may include an old coating film or a damaged part of the coated body.
- the water-based primer coating composition of the present invention it is excellent in film-forming properties and coating workability at low temperatures, and has excellent interlaminar adhesion between a member that is difficult to adhere and the upper layer film that is coated on the coating film of the water-based primer coating. It is possible to form a primer coating film excellent in Moreover, according to the multilayer coating film forming method of the present invention, a multilayer coating film having excellent appearance and water resistance can be obtained.
- aqueous means that the solvent is an aqueous solvent
- aqueous solvent means water or a mixed solvent of water and an organic solvent.
- the content of the aqueous solvent in the water-based paint is 30 to 90% by mass, preferably 40 to 80% by mass, more preferably 50 to 70% by mass of the total solvent.
- (meth)acrylate means acrylate and/or methacrylate
- (meth)acrylic acid means acrylic acid and/or methacrylic acid.
- (meth)acryloyl means acryloyl and/or methacryloyl.
- (Meth)acrylamide” means acrylamide and/or methacrylamide.
- the present invention provides a water-based primer coating composition
- a water-based primer coating composition comprising a water-dispersible and/or water-soluble film-forming resin (A), and a chlorinated or non- chlorinated polyolefin-based resin (B), the content ratio of the film-forming resin (A) and the chlorinated or non-chlorinated polyolefin-based resin (B) is 1:99 or more and 99:1 or less, and a solid A water-based primer coating composition having a content of 0.5% by mass or more and 15% by mass or less.
- the details of the constituent components are described below.
- the film-forming resin (A) of the present invention is a component capable of forming a film by drying together with the chlorinated or non-chlorinated polyolefin resin (B) described later, and exhibits at least one of water-dispersible and water-soluble. be.
- the film-forming resin (A) may be simply referred to as resin (A).
- Specific film-forming resins (A) include acrylic resins, polyurethane resins, polyester resins, alkyd resins, and cellulose resins. It preferably contains at least one selected from (a2), polyester resin (a3) and polycarbonate resin (a4).
- the later-described water-soluble acrylic resin (a1-1) or water-dispersed polyurethane resin is particularly preferred.
- the acrylic resin (a1) in the present invention exhibits at least one of water-dispersible and water-soluble.
- One is the water-dispersible acrylic resin (a1-2).
- the water-soluble acrylic resin (a1-1) is preferred from the viewpoint of film-forming properties and compatibility with the chlorinated or non-chlorinated polyolefin resin (B) described below.
- the water-soluble acrylic resin (a1-1) is a resin obtained by polymerizing a hydrophilic group-polymerizable unsaturated monomer and other polymerizable unsaturated monomers with a polymerization initiator in the presence of a hydrophilic organic solvent. and can take a state (transparency) dissolved in a hydrophilic organic solvent or aqueous medium.
- the water-soluble acrylic resin (a1-1) is polymerizable having at least one hydrophilic group selected from a hydroxyl group, a phosphoric acid group, a sulfonic acid group, a carboxyl group, an amino group, an amide group and a polyoxyalkylene chain.
- the copolymer component includes an unsaturated monomer (x) (hereinafter referred to as a hydrophilic group-containing polymerizable unsaturated monomer) and a hydrophobic polymerizable unsaturated monomer (y).
- x unsaturated monomer
- y hydrophobic polymerizable unsaturated monomer
- Hydrophilic group-containing polymerizable unsaturated monomers (x) include hydroxyl group-containing polymerizable unsaturated monomers, amino group-containing polymerizable unsaturated monomers, amide group-containing polymerizable unsaturated monomers, acid group-containing polymerizable unsaturated monomers, polyoxy Examples include alkylene chain-containing polymerizable unsaturated monomers.
- hydroxyl group-containing polymerizable unsaturated monomer examples include hydroxyalkyls such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate.
- hydroxyalkyls such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate.
- Examples of the acid group-containing polymerizable unsaturated monomers include carboxyl group-containing polymerizable unsaturated monomers, phosphoric acid group-containing polymerizable unsaturated monomers, and sulfonic acid-containing polymerizable unsaturated monomers.
- Carboxyl group-containing polymerizable unsaturated monomers include (meth)acrylic acid, maleic acid, crotonic acid, and ⁇ -carboxyethyl acrylate, with (meth)acrylic acid and maleic acid being preferred.
- the phosphoric acid group-containing polymerizable unsaturated monomers include 2-acryloyloxyethyl acid phosphate, 2-methacryloyloxyethyl acid phosphate, 2-acryloyloxypropyl acid phosphate, 2-methacryloyloxypropyl acid phosphate, and the like.
- sulfonic acid group-containing polymerizable unsaturated monomers examples include sulfonic acid group-containing polymerized monomers such as 2-acrylamido-2-methylpropanesulfonic acid, allylsulfonic acid, styrenesulfonic acid sodium salt, sulfoethyl methacrylate and its sodium salt or ammonium salt. and polyunsaturated monomers.
- polyoxyalkylene chain-containing polymerizable unsaturated monomers include polyoxyethylene chains, polyoxypropylene chains, and polymerizable unsaturated compounds having block chains of polyoxyethylene and polyoxypropylene. Specific examples include polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, polyethylene (propylene) glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, and the like.
- a polymerizable unsaturated monomer having at least one hydrophilic group selected from a phosphoric acid group, a sulfonic acid group, a carboxyl group, an amino group, an amide group and a polyoxyalkylene chain may be included.
- Carboxyl group-containing polymerizable unsaturated monomers, phosphoric acid group-containing polymerizable unsaturated monomers, and sulfonic acid-containing polymerizable unsaturated monomers are more preferred from the viewpoint of drying property, water resistance and weather resistance.
- a phosphoric acid group-containing water-soluble acrylic resin in which a carboxyl group-containing polymerizable unsaturated monomer and a phosphoric acid group-containing polymerizable unsaturated monomer are used in combination is preferable because it has the effect of improving the film-forming properties and adhesiveness of the coating film.
- the content of the hydrophilic group-containing polymerizable unsaturated monomer (x) based on the total amount of the copolymerizable monomer component is preferably 3% by mass or more and 30% by mass or less, and 5% by mass or more and 25% by mass. The following are more preferable.
- the hydrophilic group-containing polymerizable unsaturated monomer (x) in the case of containing a polyoxyalkylene chain-containing polymerizable unsaturated monomer, from the viewpoint of the water resistance of the multilayer coating film, the total amount of copolymerization components as a reference , preferably 15% by mass or less, more preferably 1% by mass or more and 13% by mass or less.
- a neutralizing agent is not particularly limited as long as it can neutralize the carboxyl group.
- examples include inorganic bases such as sodium hydroxide and potassium hydroxide, trimethylamine, dimethylaminoethanol, 2-methyl -Amino-1-propanol, triethylamine, and organic amines such as ammonia.
- the hydrophobic polymerizable unsaturated monomer (y) to be copolymerized with the hydrophilic group-containing polymerizable unsaturated monomer (x) is a linear, branched or cyclic monomer having 4 or more carbon atoms, preferably 6 to 18 carbon atoms. is a polymerizable unsaturated monomer having a saturated or unsaturated hydrocarbon group, excluding monomers having a hydrophilic group such as a hydroxyl group-containing polymerizable unsaturated monomer.
- Hydrophobic polymerizable unsaturated monomers (y) include, for example, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, tridecyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, cyclohexyl (meth)acrylate, Alkyl or cycloalkyl (meth)acrylates such as methylcyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, cyclododecyl (meth)acrylate, tricyclodecan
- the hydrophobic polymerizable unsaturated monomer (y) may be a methacrylate having a branched alkyl group, such as tert-butyl methacrylate, or a cyclic alkyl structure ( It is particularly preferred to contain at least one polymerizable unsaturated monomer selected from the group consisting of meth)acrylates such as cyclohexyl (meth)acrylate, isobornyl (meth)acrylate and adamantyl (meth)acrylate.
- methacrylates such as cyclohexyl (meth)acrylate, isobornyl (meth)acrylate and adamantyl (meth)acrylate.
- the content of the hydrophobic polymerizable unsaturated monomer (y) based on the total amount of copolymerizable monomer components is preferably 30% by mass or more and 80% by mass or less, and 45% by mass or more and 70% by mass or less. It is more preferable to have
- the hydrophilic organic solvent used for polymerization is not strictly classified, but for example, an organic solvent that dissolves at least 20 g in 100 g of water at 20° C. can be used, such as an alcohol-based organic solvent; an ether-based organic solvent; ethylene glycol ether-based organic solvents; diethylene glycol ether-based organic solvents; propylene glycol ether-based organic solvents; dipropylene glycol ether-based organic solvents; These can be used individually or in combination of 2 or more types.
- the hydroxyl value of the water-soluble acrylic resin (a1-1) is not particularly limited, it is preferably 1 mgKOH/g or more and 200 mgKOH/g or less, and 5 mgKOH/g or more and 100 mgKOH/g or less from the viewpoint of drying property and finishing property. is more preferable.
- the acid value of the water-soluble acrylic resin (a1-1) is preferably 1 mgKOH/g or more and less than 100 mgKOH/g from the viewpoint of compatibility between the storage stability and drying property of the paint and the water resistance of the coating film, and 5 mgKOH/g. more preferably 60 mgKOH/g or less.
- the weight average molecular weight of the water-soluble acrylic resin (a1-1) is preferably 1,000 or more and 500,000 or less, more preferably 1,500 or more and 150,000 or less, and even more preferably 2,000 or more and 70,000 or less.
- the amount of the water-soluble acrylic resin (a1-1) contained in the water-based primer coating composition is 0.5 based on the total resin solid content contained in the water-based primer coating composition, from the viewpoint of weather resistance and drying properties. It is preferably from 1% by mass to 20% by mass, more preferably from 1% by mass to 15% by mass.
- the water-dispersible acrylic resin (a1-2) is a water-dispersed acrylic resin, and the water-dispersible acrylic resin is further divided into an emulsion type and a colloidal dispersion type.
- the emulsion type refers to a form obtained by emulsion polymerization or the like using water as a solvent in the presence of an emulsifier, or a form obtained by mechanically forcibly dispersing a completely water-insoluble resin in water. called a type.
- the above monomer mixture is polymerized in the absence of a solvent or in the presence of an appropriate organic solvent, and is added dropwise to water, mixed, and dispersed by removing the excess organic solvent as necessary.
- a form in which water is added to disperse after removing the excess organic solvent according to the conditions is called a colloidal dispersion type.
- a colloidal dispersion type acrylic resin is preferable because the resulting composite coating film has excellent hardness, water resistance and adhesion.
- the water-dispersible acrylic resin (a1-2) is a copolymer obtained by copolymerizing the hydrophilic group-containing polymerizable unsaturated monomer (x) as an essential component and optionally other polymerizable unsaturated monomers. It is dispersed in Suitable examples include those obtained by one-step or multi-step emulsion polymerization using a polymerizable unsaturated monomer component and a polymerization initiator in the presence of water and a dispersion stabilizer.
- the hydrophilic group-containing polymerizable unsaturated monomer those listed in the section of the water-soluble acrylic resin (a1-1) can be suitably used, but a carboxyl group-containing polymerizable unsaturated monomer is preferable.
- Examples of polymerizable unsaturated monomers that can be copolymerized components of the water-dispersible acrylic resin (a1-2) include methyl (meth) acrylate, ethyl (meth) acrylate, propyl (meth) acrylate, and n-butyl (meth) acrylate.
- the dispersion stabilizer used in the emulsion polymerization of the water-dispersible acrylic resin (a1-2) is not particularly limited, but examples include sodium dialkylsulfosuccinate, sodium dodecylbenzenesulfonate, and sodium lauryl sulfate. , anionic emulsifiers such as sodium polyoxyethylene alkylphenyl ether sulfate and sodium alkyldiphenyl ether disulfonate, nonionic emulsifiers such as polyoxyethylene higher alcohol ethers and polyoxyethylene alkylphenyl ethers, and anionic emulsifiers having a radically polymerizable double bond or cationic reactive emulsifiers.
- anionic emulsifiers such as sodium polyoxyethylene alkylphenyl ether sulfate and sodium alkyldiphenyl ether disulfonate
- nonionic emulsifiers such as polyoxyethylene higher alcohol ethers and poly
- the reactive emulsifier is an emulsifier having both a nonionic group, an anionic group and a cationic group and a polymerizable unsaturated group in the molecule, and the polymerizable unsaturated group is specifically includes a (meth)allyl group, (meth)acryloyl group, propenyl group, butenyl group and the like.
- Commercially available reactive emulsifiers include "Latemul” (registered trademark) (trade name, manufactured by Kao Corporation), "Eleminol” (registered trademark) (trade name, manufactured by Sanyo Kasei Co., Ltd.), and "Aqualon” (registered trademark).
- polymerization initiator conventionally known ones can be used without limitation, and examples include peroxide-based polymerization initiators, azo-based polymerization initiators, and the like.
- the hydroxyl value of the water-dispersible acrylic resin (a1-2) is not particularly limited, it is preferably 1 mgKOH/g or more and 200 mgKOH/g or less, and 5 mgKOH/g or more and 100 mgKOH/g from the viewpoint of drying property and finishing property. It is more preferably 8 mgKOH/g or more and 50 mgKOH/g or less. From the viewpoint of the water resistance of the primer coating film, the water-dispersible acrylic resin (a1-2) preferably has a solid content acid value of 10 mgKOH/g or less, more preferably 8 mgKOH/g or less.
- the anionic groups such as carboxyl groups contained in the acrylic resin may be neutralized with a basic compound and then dispersed in water, or an aqueous dispersion containing a basic compound may be used. It is also possible to add and disperse an acrylic resin in the medium.
- the basic compound that serves as a neutralizing agent for the hydroxyl group-containing acrylic resin is not particularly limited. Specific examples include inorganic bases such as sodium hydroxide and potassium hydroxide, trimethylamine, dimethylaminoethanol, 2-methyl 2- Organic amines such as amino-1-propanol, triethylamine and ammonia can be mentioned. Among them, organic amine compounds are preferred, and tertiary amines such as triethylamine, tributylamine, dimethylethanolamine and diethylenetriamine are particularly preferred.
- the average particle size of the water-dispersible acrylic resin (a1) is preferably 0.02 ⁇ m or more and 1.0 ⁇ m or less, more preferably 0.05 ⁇ m or more and 0.3 ⁇ m or less.
- the average particle size of the water-dispersible resin is the value of the volume average particle size measured by the Coulter Counter method at a measurement temperature of 20°C. Measurement by the Coulter counter method can be performed using, for example, "COULTER N4 type" (manufactured by Beckman Coulter, trade name).
- the water-dispersible acrylic resin (a1-2) may be a single-layer type or a multi-layer type such as a core-shell type.
- the glass transition temperature of the water-dispersible acrylic resin (a1) is preferably in the range of -45°C to 20°C from the viewpoint of drying property and film-forming property.
- polyurethane resin (a2)- an aqueous dispersion of polyurethane resin (sometimes referred to as a water-dispersed polyurethane resin) or a water-soluble polyurethane resin can be used.
- polyurethane resin (a2) those known in the art can be used without limitation. Polyurethane resin emulsions or polyurethane resin dispersions can be mentioned.
- a water-dispersed polyurethane resin is preferable from the viewpoint of handling workability.
- the polyurethane resin (a2) is an aqueous dispersion
- its average particle size is preferably 0.01 ⁇ m or more and 1.0 ⁇ m or less, more preferably 0.1 ⁇ m or more and 0.5 ⁇ m or less, and further It is preferably more than 50 ⁇ m and 250 nm or less.
- polyisocyanate compounds as constituent components include aliphatic diisocyanate compounds such as hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, dimer acid diisocyanate, and lysine diisocyanate; buret type adducts and isocyanurate ring adducts of these diisocyanate compounds; isophorone diisocyanate, 4,4′-methylenebis(cyclohexyl isocyanate), methylcyclohexane-2,4-(or -2,6-) diisocyanate, 1,3-(or 1,4-) di(isocyanatomethyl)cyclohexane, 1 Alicyclic diisocyanate compounds such as ,4-cyclohexane diisocyanate, 1,3-cyclopentane diisocyanate, 1,2-cyclohexane diisocyanate; biuret type adducts and isocyanurate ring adduct
- polyol examples include polyether polyols such as polyethylene glycol, polypropylene glycol, polyethylene-propylene (block or random) glycol, polytetramethylene ether glycol, polyhexamethylene ether glycol, polyoctamethylene ether glycol; dicarboxylic acid (adipic acid , succinic acid, sebacic acid, glutaric acid, maleic acid, fumaric acid, phthalic acid, etc.) and glycols (ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, 3-methyl-1,5 - pentanediol, neopentyl glycol, bishydroxymethylcyclohexane, etc.), such as polyethylene adipate, polybutylene adipate, polyhexamethylene adipate, polyneopentyl adipate, poly-3-methylpentyl adipate, polyethylene/ polyester polyol
- carboxyl group-containing diols examples include dimethylolacetic acid, dimethylolpropionic acid, and dimethylolbutyric acid.
- the production of the above urethane prepolymer can be carried out based on a conventionally known method.
- the polyurethane resin (a2) may be neutralized with a neutralizing agent.
- the neutralizing agent is not particularly limited as long as it can neutralize the carboxyl group, and those mentioned in the section of the basic compound of the acrylic resin (a1) can be used.
- the polyurethane resin (a2) preferably has a cyclic structure in its molecule. More preferably, the polyisocyanate constituting the polyurethane resin (a2) contains a compound derived from an alicyclic diisocyanate compound as part of its component. From the viewpoint of film-forming properties and water resistance, the polyurethane resin (a2) preferably has a solid content acid value of 40 mgKOH/g or less, more preferably 5 mgKOH/g or more and 30 mgKOH/g or less. Further, the polyurethane resin (a2) preferably has a minimum film-forming temperature of 5° C. or lower from the viewpoint of film-forming properties and water resistance.
- the concentration of the polyurethane resin (a2) (polyurethane resin solid content concentration) can be appropriately determined according to the purpose of use, but is preferably 20 to 60% by mass. By using a polyurethane resin that satisfies this concentration range, handling becomes easy and the concentration of the polyurethane resin in the obtained primer composition can be easily adjusted.
- a commercially available product can be used as the polyurethane resin (a2). Specifically, Daiichi Kogyo Seiyaku Co., Ltd. "Super Flex” series, Nicca Chemical Co., Ltd. “Neo Sticker”, “Evaphanol” series, Sumika Covestro Urethane Co., Ltd. "Bihydrol” series, etc. are exemplified. be.
- the polyester resin (a3) is a reaction product produced by an ordinary method, for example, by an esterification reaction of a polybasic acid and a polyhydric alcohol, and may contain hydroxyl groups.
- Polybasic acids are compounds having two or more carboxyl groups in one molecule, such as phthalic acid, isophthalic acid, terephthalic acid, succinic acid, adipic acid, azelaic acid, sebacic acid, tetrahydrophthalic acid, hexahydro Phthalic acid, maleic acid, fumaric acid, itaconic acid, trimellitic acid, pyromellitic acid and their anhydrides, etc.
- polyhydric alcohols are compounds having two or more hydroxyl groups in one molecule.
- ⁇ -olefin epoxides such as propylene oxide and butylene oxide
- monoepoxy compounds such as Cardura E10 (manufactured by Japan Epoxy Resin Co., Ltd., trade name, glycidyl ester of synthetic highly branched saturated fatty acid), etc.
- the compound may be introduced into the polyester resin.
- a carboxyl group into a polyester resin for example, it can be introduced by adding an acid anhydride to a hydroxyl-containing polyester and half-esterifying it.
- the polyester resin (a3) is preferably linear in terms of chipping resistance, adhesion, finishing properties, weather resistance and gasohol resistance of the resulting coating film.
- the polybasic acid is preferably adipic acid
- the polyhydric alcohols are ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,5-pentanediol, 6-hexanediol is preferred.
- the hydroxyl value is preferably 85 mgKOH/g or more and 250 mgKOH/g or less, more preferably 100 mgKOH/g or more and 220 mgKOH/g or less.
- the number average molecular weight of the polyester resin (a3) is preferably 500 or more and 2500 or less, more preferably 800 or more and 2000 or less.
- the polycarbonate resin (a4) is a compound containing two or more carbonate groups in the molecule, and may contain a hydroxyl group.
- the polycarbonate resin (a4) is a compound obtained by subjecting a known polyol and a carbonylating agent to a polycondensation reaction by a conventional method.
- Diols and trihydric or higher alcohols can be mentioned as polyols that are raw materials for the polycarbonate resin (a4).
- diols include 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, and 1,7-heptanediol.
- trihydric or higher alcohols include glycerin, trimethylolethane, trimethylolpropane, a dimer of trimethylolpropane, and pentaerythritol. These trihydric or higher alcohols can be used alone or in combination of two or more.
- a known carbonylating agent can be used as the carbonylating agent that is a raw material for the polycarbonate resin (a4).
- alkylene carbonate, dialkyl carbonate, diaryl carbonate, phosgene, etc. can be mentioned, and these can be used alone or in combination of two or more.
- Preferred among these are ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, dibutyl carbonate, diphenyl carbonate and the like.
- the number average molecular weight of the polycarbonate resin (a4) is preferably 500 or more and 2500 or less, more preferably 800 or more and 2000 or less, from the viewpoint of film-forming properties at low temperatures and water resistance.
- polycarbonate resin (a4) examples include UM-90, UH-100, UH-200, and UC-100 (trade name, manufactured by Ube Industries, Ltd.).
- -Other resins As the film-forming resin (A), those listed above can be suitably used, but other resins may also be included.
- Other resins include acrylic resins other than the above water-dispersed acrylic resins and water-soluble acrylic resins, silicone resins, urethane resins other than water-dispersed polyurethane resins, fluorine resins, epoxy resins, alkyd resins, and mixed resins thereof, or Modified resins, for example, acrylic-modified polyester resins, acrylic silicone resins, acrylic-modified epoxy resins, epoxy ester resins and the like. Moreover, these may be used individually or may use 2 or more types together.
- resins may be used as long as they do not affect the storability, coating film performance, and weather resistance of the paint. It is preferably 20% by mass or less, more preferably less than 5% by mass, relative to the resin solid content.
- the minimum film-forming temperature (MFT) of the film-forming resin (A) is preferably 25° C. or lower. When the minimum film-forming temperature of the film-forming resin (A) is 25° C. or lower, film-forming properties at low temperatures are improved.
- the minimum film-forming temperature of the film-forming resin (A) is more preferably 10° C. or lower, more preferably 5° C. or lower, from the viewpoint of improving the film-forming properties at low temperatures, particularly around room temperature. °C or less is particularly preferred. Although the lower limit is not particularly limited, it may be -50°C or higher, further -10°C or higher, and particularly -5°C or higher from the viewpoint of improving the drying property.
- the MFT can be measured, for example, by an MFT tester manufactured by Tester Sangyo Co., Ltd.
- the glass transition temperature Tg of the film-forming resin (A) is preferably ⁇ 50° C. or higher and 60° C. or lower, and preferably ⁇ 30° C. or higher and 45° C. or lower. More preferably, the temperature is -10°C or higher and 20°C or lower.
- the glass transition temperature of the homopolymer of each monomer is the value according to the Polymer Hand Book (4th Edition). 10,000, and the glass transition temperature measured by differential scanning thermal analysis is used.
- the SP value of the film-forming resin (A) is preferably as low as 9.5 or less from the viewpoint of compatibility with the chlorinated or non-chlorinated polyolefin resin (B), film-forming properties, and water adhesion resistance. preferably 9.3 or less, even more preferably 9.1.
- the lower limit is not particularly limited, but may be, for example, 8.0 or more, and may be 8.2 or more.
- the solubility parameter (SP value) of the film-forming resin (A) in the present invention is described in Polymer Engineering and Science, 14, No. 2, p. 147 (1974) and is calculated by the following Fedors formula.
- SP ⁇ ( ⁇ e1)/ ⁇ ( ⁇ v1) ⁇ (In the formula, ⁇ e1 is the cohesive energy per unit functional group, and ⁇ v1 is the molecular volume per unit functional group.)
- the SP value of the copolymer or blend was the sum of the SP values of each component of the monomer unit or blend multiplied by the mass fraction.
- the chlorinated or non-chlorinated polyolefin resin (B) has a softening temperature of less than 80° C. and a degree of chlorination of 25% or less.
- the chlorinated or non-chlorinated polyolefin resin (B) may be simply referred to as resin (B).
- the chlorinated or non-chlorinated polyolefin resin (B) has a softening temperature of less than 80° C., it has good compatibility with the film-forming resin (A) and good low-temperature film-forming properties.
- the softening temperature can be measured by visual evaluation using a melting point measuring instrument. For example, using a melting point measuring instrument "ATM-01" manufactured by AS ONE Co., Ltd., about 0.1 g of a pre-formed polyolefin resin (B) sample is placed on a hot plate, and the temperature is gradually raised from room temperature. , the temperature at which the sample melts is defined as the softening temperature.
- the degree of chlorination of the chlorinated or non-chlorinated polyolefin resin (B) is 25% or less from the viewpoint of compatibility between substrate wettability, adhesion to resin members, and adhesion to the base paint to be coated thereon. more preferably 1% or more and 20% or less. When it is 25% or less, it becomes possible to achieve both adhesion to the resin member and adhesion to the base paint.
- the degree of chlorination of the chlorinated polyolefin resin is measured according to JIS-K7229.
- the chlorinated polyolefin resin (b1) and the non-chlorinated polyolefin resin (b2) are described below.
- Chlorinated polyolefin resin (b1) is preferably obtained by chlorinating a polyolefin or a modified product obtained by modifying it with an (anhydrous) unsaturated carboxylic acid or the like.
- polyolefins examples include homopolymers or copolymers of olefins selected from ethylene, propylene, butene, 3-methyl-1-butene, 3-methyl-1-heptene and the like, and the olefins and vinyl acetate. , butadiene, acrylic acid ester, methacrylic acid ester and the like. Specifically, chlorinated polyethylene, chlorinated polypropylene, chlorinated ethylene-propylene copolymer, chlorinated ethylene-vinyl acetate copolymer and the like are suitable.
- Modified products of these polyolefins include modified products obtained by adding an (anhydrous) unsaturated carboxylic acid to the above polyolefins, and modified products obtained by reacting the above polyolefins with an (anhydrous) unsaturated carboxylic acid and an active hydrogen compound.
- a body etc. can be used suitably.
- Examples of the (anhydrous) unsaturated carboxylic acid include (anhydrous) maleic acid, fumaric acid, (anhydrous) itaconic acid, and (meth)acrylic acid.
- Modified products are usually obtained by reacting polyolefins and (anhydrous) unsaturated carboxylic acids in the presence of organic peroxides and the like.
- chlorinated polyolefin-based resin (b1) an acrylic obtained by grafting an acrylic resin to the above-mentioned polyolefin or a modified product obtained by modifying it with an (anhydrous) unsaturated carboxylic acid or the like is chlorinated. Modified chlorinated polyolefins may also be used.
- Acrylic-modified chlorinated polyolefin is usually obtained by dropping a polymerizable unsaturated monomer mixture that forms an acrylic resin in the presence of a chlorinated product of polyolefin or a modified product thereof and causing a grafting reaction.
- a reaction can be carried out in an organic solvent at a polymerization temperature of usually about 60 to 100° C. in the presence of a radical polymerization initiator such as benzoyl peroxide or azoisobutyronitrile by a known polymerization method such as It is carried out by solution polymerization or the like.
- Examples of polymerizable unsaturated monomers to be dropped during graft polymerization include methyl (meth) acrylate, ethyl (meth) acrylate, n-, i-propyl (meth) acrylate, n-, i-, t-butyl (meth) acrylate.
- the weight average molecular weight of the chlorinated polyolefin-based resin (b1) is generally preferably from about 2,000 to 300,000, more preferably from about 5,000 to 100,000.
- the chlorinated polyolefin resin (b1) can be water-dispersed by dispersing the above-mentioned unsaturated carboxylic acid- or acid anhydride-modified polyolefin in an aqueous medium. Some or all of the carboxyl groups in the anhydride-modified polyolefin can be neutralized with an amine compound and/or water-dispersed with an emulsifier. From the viewpoint of improving water dispersibility, it is desirable to use both neutralization and water dispersing with an emulsifier.
- Non-chlorinated polyolefin resin (b2) preferably has a polyolefin molecule as a main skeleton and a hydrophilic group such as a carboxyl group introduced into the molecule.
- unsaturated carboxylic acid- or acid anhydride-modified polyolefin is suitable.
- Unsaturated carboxylic acid- or acid anhydride-modified polyolefins can usually be obtained by graft copolymerizing unsaturated carboxylic acids or acid anhydrides onto polyolefins by a method known per se.
- the unsaturated carboxylic acid or acid anhydride that can be used for modification contains at least one, preferably one polymerizable double bond in one molecule and has 3 to 10 carbon atoms and does not contain chlorine.
- Aliphatic carboxylic acids or anhydrides thereof are included, and specific examples include (meth)acrylic acid, maleic acid, fumaric acid, itaconic acid, maleic anhydride, and the like. Maleic acid is preferred.
- the amount of graft copolymerization with the unsaturated carboxylic acid or its acid anhydride with respect to the polyolefin can be varied according to the physical properties desired for the modified polyolefin, but generally it is 0.00 based on the solid weight of the polyolefin. It is preferably 5% by mass or more and 4% by mass or less, more preferably 1% by mass or more and 3% by mass or less, and even more preferably 1.2% by mass or more and 2.8% by mass or less.
- the polyolefin to be modified includes, for example, one or more olefins having 2 to 10 carbon atoms such as ethylene, propylene, butylene, and hexene. Polyolefins are included, and those containing propylene as polymerized units are particularly preferred.
- the mass fraction of propylene units in the modified polyolefin is generally preferably from 0.5 to 1, more preferably from 0.7 to 0.7, from the viewpoint of compatibility with other components, adhesion of the formed coating film, and the like. It is more preferably 99 or less, and still more preferably 0.8 or more and 0.99 or less.
- the obtained polyolefin has a narrow molecular weight distribution and is excellent in random copolymerization.
- those produced by (co)polymerizing olefins using a single-site catalyst as the polymerization catalyst are preferred.
- the single-site catalyst is a polymerization catalyst having a uniform (single-site) active site structure, and among the single-site catalysts, metallocene catalysts are particularly preferred.
- the metallocene-based catalyst is a metallocene (bis(cyclopentadienyl ) a metal complex and its derivative), a co-catalyst such as an aluminoxane or a boron-based catalyst for activating this, and an organoaluminum compound such as trimethylaluminum.
- Olefin (co)polymerization can be carried out according to a per se known method, for example, by continuously adding an alkylaluminum and a metallocene catalyst while supplying an olefin such as propylene or ethylene and hydrogen to a reaction vessel. .
- the above unsaturated carboxylic acid- or acid anhydride-modified polyolefin may be further acrylic-modified.
- Acrylic unsaturated monomers that can be used for acrylic modification include chlorine-free monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, C1-C20 alkyl esters of (meth)acrylic acid such as hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, and stearyl (meth)acrylate; C1-C21 hydroxyalkyl esters of (meth)acrylic acid such as 2-hydroxyethyl (meth)acrylate and 3-hydroxypropyl (meth)acrylate; (meth)acrylic acid, glycidyl (meth)acrylate, (meth)acrylate Other
- a chlorine-free acrylic unsaturated monomer having reactivity with the carboxyl group in the unsaturated carboxylic acid or acid anhydride-modified polyolefin produced as described above for example, by reacting glycidyl (meth)acrylate or the like to introduce a polymerizable unsaturated group into a polyolefin, and then the polyolefin into which the polymerizable unsaturated group has been introduced is added with the above acrylic unsaturated monomer alone or in combination of two types. It can be carried out by (co)polymerizing a combination of the above.
- the amount of the acrylic unsaturated monomer used in the acrylic modification of polyolefin can be varied according to the physical properties desired for the modified polyolefin. In general, it is preferably 30% by mass or less, more preferably 0.1% by mass or more and 20% by mass or less, based on the solid content mass of the unsaturated carboxylic acid or acid anhydride-modified polyolefin to be obtained. , more preferably 0.15% by mass or more and 15% by mass or less.
- the unsaturated carboxylic acid- or acid anhydride-modified polyolefin may be further modified with a compound having a polyoxyalkylene chain.
- a compound having a polyoxyalkylene chain examples include a polyoxyethylene chain, a polyoxypropylene chain, and a block chain of polyoxyethylene and polyoxypropylene.
- the number average molecular weight of the compound having the polyoxyalkylene chain is generally preferably 400 or more and 3000 or less, more preferably 500 or more and 2000 or less. If the number-average molecular weight is less than 400, the effect as a hydrophilic group cannot be sufficiently exhibited, and water resistance may be adversely affected. , which can be difficult to handle.
- the unsaturated carboxylic acid- or acid anhydride-modified polyolefin has a melting point of 120° C. or less from the viewpoint of compatibility with other components, adhesion of the formed coating film to plastic members, and interlayer adhesion to the top coat layer. , more preferably 60° C. or higher and 110° C. or lower, and even more preferably 70° C. or higher and 100° C. or lower.
- the weight average molecular weight (Mw) of the unsaturated carboxylic acid- or acid anhydride-modified polyolefin is preferably 10,000 or more and 230,000 or less, more preferably 30,000 or more and 200,000 or less, and 60,000 or more and 150,000 or less. More preferred.
- the weight-average molecular weight (Mw) of the unsaturated carboxylic acid- or acid anhydride-modified polyolefin is a value obtained by converting the weight-average molecular weight measured by gel permeation chromatography based on the weight-average molecular weight of polystyrene.
- "HLC/GPC150C” manufactured by Waters Co., Ltd., 60 cm x 1
- o-dichlorobenzene was used as a solvent
- the column temperature was 135°C
- the flow rate was 1.0 ml/min.
- Injection samples were prepared by dissolving a solution concentration of 5 mg of polyolefin in 3.4 ml of o-dichlorobenzene at 140° C. for 1-3 hours.
- a column for gel permeation chromatography "GMHHR-H(S)HT" (manufactured by Tosoh Corporation, trade name) can be used.
- unsaturated carboxylic acid- or acid anhydride-modified polyolefins generally have a weight-average molecular weight to number-average molecular weight ratio (Mw/Mn) from the viewpoint of compatibility with other components and adhesion of formed coating films. is preferably 1.5 or more and 7.0 or less, more preferably 1.8 or more and 6.0 or less, and even more preferably 2.0 or more and 4.0 or less.
- the unsaturated carboxylic acid- or acid anhydride-modified polyolefin generally has a heat of fusion of 1 mJ/mg or more and 50 mJ/mg from the viewpoint of the adhesion of the formed coating film to plastic members and the interlayer adhesion with the topcoat film layer. It is preferably 2 mJ/mg or more and 50 mJ/mg or less.
- the melting point and the heat of fusion of the unsaturated carboxylic acid- or acid anhydride-modified polyolefin were determined by a differential scanning calorimeter "DSC-5200" (trade name, manufactured by Seiko Electronics Industries, Ltd.) using 20 mg of the modified polyolefin. It was obtained by measuring the calorie from 100°C to 150°C at a heating rate of 10°C/min.
- the melting point of the unsaturated carboxylic acid- or acid anhydride-modified polyolefin can be adjusted by changing the monomer composition of the polyolefin, particularly the amount of the ⁇ -olefin monomer.
- the sample to be measured is first heated to 120°C, cooled to room temperature at a rate of 10°C/min, allowed to stand for 2 days or more, and the calorie is measured by the method described above. be able to.
- the non-chlorinated polyolefin resin (b2) can be water-dispersed by dispersing the unsaturated carboxylic acid- or acid anhydride-modified polyolefin described above in an aqueous medium.
- the non-chlorinated polyolefin resin (b2) is usually obtained by neutralizing some or all of the carboxyl groups in the unsaturated carboxylic acid- or acid anhydride-modified polyolefin with an amine compound and/or dispersing it in water with an emulsifier. can be done. From the viewpoint of improving water dispersibility, it is desirable to use both neutralization and water dispersing with an emulsifier.
- amine compounds used for neutralization include tertiary amines such as triethylamine, tributylamine, dimethylethanolamine and triethanolamine; secondary amines such as diethylamine, dibutylamine, diethanolamine and morpholine; A primary amine etc. are mentioned.
- the amount used is preferably from 0.1 molar equivalents to 1.0 molar equivalents relative to the carboxyl groups in the unsaturated carboxylic acid- or acid anhydride-modified polyolefin.
- the emulsifier examples include polyoxyethylene monooleyl ether, polyoxyethylene monostearyl ether, polyoxyethylene monolauryl ether, polyoxyethylene tridecyl ether, polyoxyethylene phenyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene Nonions such as ethylene octylphenyl ether, polyoxyethylene monolaurate, polyoxyethylene monostearate, polyoxyethylene monooleate, sorbitan monolaurate, sorbitan monostearate, sorbitan trioleate, polyoxyethylene sorbitan monolaurate emulsifiers; anionic emulsifiers such as sodium salts or ammonium salts of alkylsulfonic acids, alkylbenzenesulfonic acids, alkylphosphoric acids, etc.; or a reactive anionic emulsifier having both the anionic group and the polymerizable unsaturated group in one molecule. These emulsifiers can be used alone
- the above-mentioned emulsifier can usually be used in an amount of 1 part by mass or more and 20 parts by mass or less per 100 parts by mass of the solid content of the unsaturated carboxylic acid- or acid anhydride-modified polyolefin.
- the method for emulsifying the unsaturated carboxylic acid- or acid anhydride-modified polyolefin is not particularly limited, and known methods such as phase inversion emulsification, D-phase emulsification, forced emulsification, gel emulsification, self-emulsification, inversion emulsification, and high-pressure emulsification can be employed. .
- the self-emulsification method is preferable from the viewpoint of the appearance and water resistance of the resulting coating film.
- aqueous dispersion of the unsaturated carboxylic acid- or acid anhydride-modified polyolefin obtained as described above is prepared in the presence of the water-dispersed unsaturated carboxylic acid- or acid anhydride-modified polyolefin as described in the description of acrylic modification.
- a non-chlorinated polyolefin resin (b2) containing an acrylic-modified unsaturated carboxylic acid- or acid anhydride-modified polyolefin can also be obtained by emulsion polymerization of such acrylic unsaturated monomers.
- the minimum film-forming temperature of the chlorinated or non-chlorinated polyolefin resin (B) is more preferably 20° C. or lower, more preferably 15° C. or lower, from the viewpoint of improving film-forming properties at low temperatures, particularly around room temperature. is more preferable, and 13° C. or less is particularly preferable.
- the lower limit is not particularly limited, it may be -10°C or higher, further -5°C or higher, and particularly 5°C or higher from the viewpoint of improving the drying property.
- a commercially available product can also be used as the chlorinated or non-chlorinated polyolefin resin (B).
- Commercially available products are exemplified below: Auroren AE-301, Superchron E-415, E-480T manufactured by Nippon Paper Chemicals; Arrowbase DA-1010 manufactured by Unitika; Hardren EW-5515, Hardren EW-5303 manufactured by Toyobo Co., Ltd. , Hardren EW-5250 and the like, but are not limited to these.
- the content ratio of the resin (A) and the resin (B) is 1:99 or more and 99:1 or less, preferably 10:90 or more and 90:10 or less, More preferably, it is 40:60 or more and 80:20 or less.
- the content ratio of the resin (A) and the resin (B) is within the above range, the recoating compatibility when recoating the water-based base coating composition is good, and the coating film hardness is excellent and high. This is particularly preferred because a multilayer coating film with a finished appearance may be obtained.
- the solid content of the aqueous primer coating composition of the present invention is preferably 0.5% by mass or more and 15% by mass or less from the viewpoint of the balance between film-forming properties, water resistance and coating workability, and 0.8. It is more preferably 5% by mass or more and 10% by mass or less, and even more preferably 5% by mass or more and 8% by mass or less.
- the solid content is 0.5% by mass or more, the coating film hardness can be sufficiently maintained.
- the solid content is 15% by mass or less, good film-forming properties and water resistance can be achieved.
- solid content means that about 2.0 g of a sample is collected in an aluminum foil cup with a diameter of about 5 cm, and the residue (g) after heating at 110 ° C. for 1 hour is measured as a non-volatile content. This is the value calculated by
- the surface tension ( ⁇ com) of the aqueous primer coating composition of the present invention is preferably 33 dyne/cm 2 or less, more preferably 31 dyne/cm 2 or less.
- the lower limit of the surface tension ( ⁇ com) of the water-based primer coating composition is 15 dyne/s from the viewpoint of improving the wettability of the base coating applied thereon without excessively lowering the surface tension of the water-based primer coating composition.
- the aqueous primer coating composition of the present invention may contain a viscosity modifier (C).
- a viscosity modifier C
- Specific examples of viscosity modifiers (C) include silica-based fine powders, mineral-based viscosity modifiers, micronized barium sulfate powders, fatty acid amides, polyamides, acrylamides, long-chain polyaminoamides, aminoamides, and their Polyamide viscosity modifiers such as salts (e.g.
- aminoplast viscosity modifiers such as hydrophobically modified ethoxylate aminoplasts, organic resin fine particle viscosity modifiers, diurea viscosity modifiers, urethane association viscosity modifiers Modifiers, polyacrylic acid-based viscosity modifiers (also referred to as alkali-swelling viscosity modifiers), cellulose-based viscosity modifiers, and the like can be mentioned.
- viscosity modifier (C) mineral-based viscosity modifiers, polyacrylic acid-based viscosity modifiers, cellulose-based viscosity modifiers, and urethane-associated viscosity modifiers are preferred from the standpoint of sagging resistance of the formed coating film.
- at least one selected from cellulose-based viscosity modifiers, polyacrylic acid-based viscosity modifiers and urethane-associated viscosity modifiers may be included. More preferred are urethane associative viscosity modifiers. These viscosity modifiers can be used alone or in appropriate combination of two or more.
- mineral-based viscosity modifiers include inorganic layered compound-based viscosity modifiers such as swelling layered silicates whose crystal structure has a 2:1 type structure.
- inorganic layered compound-based viscosity modifiers such as swelling layered silicates whose crystal structure has a 2:1 type structure.
- smectite group clay minerals such as natural or synthetic montmorillonite, saponite, hectorite, stevensite, beidellite, nontronite, bentonite, laponite Na type tetrasilicic fluoromica, Li type tetrasilicic fluoromica, Na Swellable mica group clay minerals such as salt-type fluorine teniolite and Li-type fluorine teniolite; vermiculite; substituted products or derivatives thereof; and mixtures thereof.
- urethane-associated viscosity modifier examples include polyether polyol-based urethane prepolymers and urethane-modified polyether viscosity modifiers.
- Commercially available urethane-associated viscosity modifiers include ADEKA NOL series such as “ADEKA NOL UH-814N”, “UH-752”, “UH-756VF", “UH-420", and “UH-462” , manufactured by ADEKA), "SN Thickener 621N”, “SN Thickener 623N” (all trade names, manufactured by San Nopco), "Leoleate 244", "Leoleate 278" (all trade names, manufactured by Elementis Japan), etc. is mentioned.
- polyacrylic acid-based viscosity modifiers examples include sodium polyacrylate and polyacrylic acid-(meth)acrylic acid ester copolymers.
- polyacrylic acid-based viscosity modifiers examples include “Primal ASE-60”, “Primal TT615", and “Primal RM5" (trade names) manufactured by Dow Chemical Company, and “SN Thickener 613" manufactured by San Nopco. ", "SN Thickener 618”, “SN Thickener 630”, “SN Thickener 634", and “SN Thickener 636” (these are trade names).
- the solid content acid value of the polyacrylic acid viscosity modifier is preferably 30 mgKOH/g or more and 300 mgKOH/g or less, more preferably 80 mgKOH/g or more and 280 mgKOH/g or less.
- Cellulose-based viscosity modifiers include, for example, carboxymethyl cellulose, methyl cellulose, hydroxyethyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, cellulose nanofibers, and the like.
- Cellulose nanofibers are preferable from the viewpoint of obtaining a multilayer coating film having a pearly luster feeling with little change in grain feeling due to the use of cellulose nanofibers.
- the cellulose nanofibers are also called cellulose nanofibrils, fibrillated cellulose, and nanocellulose crystals.
- the cellulose nanofibers should have a number average fiber diameter of 2 nm or more and 500 nm or less from the viewpoint of obtaining a multi-layered coating film having a pearly luster that is bright in highlights and has a small change in graininess depending on the viewing direction. is preferably 2 nm or more and 250 nm or less, more preferably 2 nm or more and 150 nm or less, and the number average fiber length is preferably 0.1 ⁇ m or more and 20 ⁇ m or less, and 0.1 ⁇ m or more and 15 ⁇ m or less. more preferably 0.1 ⁇ m or more and 10 ⁇ m or less.
- the above number average fiber diameter and number average fiber length can be obtained, for example, by dispersing a sample of cellulose nanofibers diluted with water, casting it on a hydrophilized carbon film-coated grid, and examining it with a transmission electron microscope ( It is measured and calculated from an image observed with a TEM.
- the above cellulose nanofiber can be obtained by defibrating a cellulose raw material and stabilizing it in water.
- the cellulose raw material means materials in various forms mainly composed of cellulose, and specifically, for example, pulp (wood pulp, jute, manila hemp, pulp derived from herbs such as kenaf, etc.); produced by microorganisms Natural cellulose such as cellulose; regenerated cellulose spun after dissolving cellulose in some solvent such as cuprammonium solution or morpholine derivative; and fine cellulose obtained by depolymerizing cellulose by mechanical treatment or the like.
- Anion-modified cellulose nanofibers can also be used as the cellulose nanofibers.
- anion-modified cellulose nanofibers include carboxylated cellulose nanofibers, carboxylmethylated cellulose nanofibers, sulfonic acid group-containing cellulose nanofibers, and phosphate group-containing cellulose nanofibers.
- a functional group such as a carboxyl group or a carboxylmethyl group is introduced into a cellulose raw material by a known method, and the obtained modified cellulose is washed to prepare a modified cellulose dispersion, It can be obtained by defibrating this dispersion.
- the carboxylated cellulose is also called oxidized cellulose.
- the oxidized cellulose is obtained, for example, by oxidizing the cellulose raw material in water using an oxidizing agent in the presence of a compound selected from the group consisting of N-oxyl compounds, bromides, iodides, or mixtures thereof. be able to.
- cellulose nanofibers include, for example, Rheocrysta (registered trademark) manufactured by Daiichi Kogyo Seiyaku Co., Ltd. and Auro Visco (registered trademark) manufactured by Oji Holdings Co., Ltd.
- the aqueous primer coating composition of the present invention may contain an organic solvent (D).
- the organic solvent (D) preferably contains an organic solvent (d1) having a surface tension of 29 dyn/cm 2 or less from the viewpoint of improving wettability to the resin member.
- Organic solvent (d1)- examples include the following.
- the solubility in water (20° C.) of the organic solvent (d1) is preferably 0.5 g/100 g or more and 100 g/100 g or less of water, more preferably 60 g/100 g or more and 100 g/100 g or less of water. preferable.
- the numbers in [ ] in the specific examples below indicate the solubility in 100 g of water (20° C.).
- organic solvent (d1) examples include isoamyl acetate (boiling point 142° C., [1.7 g/100 g], no hydroxyl group), ethylene glycol monoethyl ether (also known as Cellosolve, boiling point 135° C., [100 g/100 g/ 100 g], with hydroxyl group), isopropyl glycol (alias: ethylene glycol monoisopropyl ether, boiling point 142 ° C., 100 g or more / 100 g], with hydroxyl group), methoxypropyl acetate (alias: propylene glycol monomethyl ether acetate, boiling point 146 ° C., [19 .8 g/100 g], no hydroxyl group), ethylene glycol monomethyl ether propionate (boiling point 160° C., [18.5 g/100 g], no hydroxyl group), ethoxypropyl acetate (boiling point 154° C.,
- the water-based primer coating composition contains the organic solvent (d1), its content is 0.1% by mass or more and 20% by mass or less in the total solvent in the water-based primer coating composition from the viewpoint of improving substrate wettability. is preferred, and more preferably 3% by mass or more and 15% by mass or less.
- the aqueous primer coating composition of the present invention preferably has a structural viscosity index TI value represented by the following formula (1) of 1.1 or more and 5.0 or less.
- the structural viscosity index TI value is defined by the following formula (1).
- TI value Va/Vb (1)
- Va is the apparent viscosity (mPa sec) measured by a rotational viscometer at a temperature of 25° C. at a rotation speed of 6 times/minute
- Vb is a rotation speed of 60 rotations/minute. It is the measured viscosity (mPa ⁇ sec).
- the aqueous primer coating composition of the present invention is substantially free of colored pigments. "Substantially” means 1% by mass or less relative to the total solid content in the aqueous primer coating composition.
- the water-based primer coating composition of the present invention comprises a pigment component (extending pigment) other than a coloring pigment, a film-forming aid, a neutralizer, a viscosity modifier (rheology control agent) other than the viscosity modifier (C), and an antifoaming agent.
- a pigment component extending pigment
- a viscosity modifier rheology control agent
- an ultraviolet absorber a light stabilizer
- a surface conditioner a cross-linking agent
- a cross-linking agent for example, cross-linking agents such as polyisocyanate cross-linking agents, oxazoline cross-linking agents, polycarbodiimide cross-linking agents, blocked polyisocyanate cross-linking agents, and melamine cross-linking agents can be used.
- one-pack paint, multi-pack paint such as two-pack paint, etc. can be appropriately selected.
- a cross-linking agent is contained, for example, 1 to 20 parts, preferably 3 to 10 parts, per 100 parts by mass of the resin solid content of the film-forming resin (A) contained in the water-based primer coating composition. Can be adjusted as appropriate.
- the water-based primer coating composition of the present invention can be used as a primer coating in a multi-layer coating including a primer coating, a colored base coating and a clear coating, and has excellent film-forming properties and coating workability at low temperatures. Excellent adhesion to hard-to-adhere materials.
- the paints forming the primer coating film, the colored base coating film and the clear coating film are all water-based paints, even in a so-called "all-water-based coating system", the obtained multi-layer coating film has water resistance and adhesion properties. Excellent for
- the method for forming a multilayer coating film of the present invention comprises a step (1) of forming a primer coating film (I) by coating the water-based primer coating composition of the present invention on a resin member; In step (2) of forming a colored base coating film (II) by applying an aqueous colored base coating composition, and on the colored base coating film (II) obtained in step (2), an aqueous two-pack type A step (3) of applying and drying a clear coating composition to form a clear coating film (III).
- Step (1) -Resin member-
- Materials for the resin member include resins such as polyethylene resin, cycloolefin resin, polypropylene resin, acrylonitrile-butadiene-styrene (ABS) resin, polyamide resin, acrylic resin, vinylidene chloride resin, polycarbonate resin, polyurethane resin, epoxy resin, etc.
- Plastic materials, such as various FRP, are mentioned.
- the water-based primer coating composition of the present invention is particularly preferable because it has excellent adhesion even to a difficult-to-adhere member such as a cycloolefin resin or a polypropylene resin.
- the resin member includes an old coating film or a damaged part of the coated body. That is, the aqueous primer coating composition of the present invention is suitable for repairing automobiles, repairing automobile parts, and the like.
- the coating method of the aqueous primer coating composition of the present invention is not particularly limited, and examples thereof include brush coating, roller coating, air spray coating, airless spray coating, rotary atomization coating, curtain coating and the like.
- a wet coating film can be formed by these coating methods.
- dry-to-the-touch state for example, a “dry-to-the-touch state” defined in JIS K 5600-1-1 (1999) (a state in which the center of the coated surface is lightly touched with a fingertip and the fingertip is not stained) or " It may be in a “semi-cured dry state” (a state in which the center of the coated surface is gently and lightly rubbed with a fingertip to leave no scratches on the coated surface).
- a water-based colored base coating composition, a water-based two-component clear coating composition, and an undercoat coating, which will be described later, can also be applied in the same manner.
- the dry film thickness of the primer coating film (I) is preferably 1 ⁇ m or more and 8 ⁇ m or less from the viewpoint of the balance between adhesion and coating workability.
- the dry film thickness is 1 ⁇ m or more, the resin member can be satisfactorily coated, and when the dry film thickness is 8 ⁇ m or less, the adhesion of the upper layer film of the primer coating film can be improved. can.
- the number of times of coating is not particularly limited, and the above dry film thickness may be obtained by coating once or multiple times.
- the water-based colored base coating composition is preferably a one-component water-based colored base coating composition.
- the water-based colored base coating composition a known one can be used, and examples thereof include a composition containing a water-dispersed urethane resin and/or a water-soluble acrylic resin.
- Step (3) Aqueous two-liquid type clear paint composition -
- the first component contains a water-soluble resin such as a dispersion type acrylic resin
- the second component contains a polyisocyanate compound (curing agent).
- the drying temperature in step (3) is preferably 50°C or higher and 70°C or lower.
- the drying temperature is 50° C. or higher, film-forming properties and workability are improved at low temperatures.
- the drying temperature is 70° C. or less, deformation of the resin member of the object to be coated can be prevented.
- the undercoat film (I-2) includes, for example, undercoat paints called primer surfacers, and known primer surfacers can be used without particular limitations.
- primer surfacers can be used without particular limitations.
- it can be formed by drying a primer surfacer containing a film-forming resin selected from acrylic resins, polyester resins, alkyd resins, urethane resins, fluorine resins, epoxy resins, silicone resins, and polyether resins.
- the primer surfacer can be appropriately selected from multi-component coating forms such as one-component coating and two-component coating.
- the primer surfacer may contain the cross-linking agent described above.
- the undercoat paint is preferably water-based from the viewpoint of an environmentally friendly coating system and from the viewpoint of improving water-resistant adhesion in a multi-layer coating film.
- the solids content of the undercoat is more than 15% by mass, preferably 25 to 80% by mass, and can be appropriately adjusted.
- the method for forming a multilayer coating film of the present invention can be an all-water-based coating system or an environmentally friendly coating system. can maintain its aesthetic appearance for a long period of time.
- the resulting water-soluble acrylic resin (A-1) had a glass transition temperature of 37°C, an acid value of 31 mgKOH/g, a hydroxyl value of 43 mgKOH/g, a weight average molecular weight of 45000, and a minimum film-forming temperature of 5°C or less. rice field.
- a water-soluble acrylic resin (A-2) having a solid content of 50% and containing a carboxyl group and a phosphoric acid group as a film-forming resin. got The resulting water-soluble acrylic resin (A-2) had a glass transition temperature of 34° C., an acid value of 50.6 mgKOH/g, a hydroxyl value of 5.8 mgKOH/g, a weight average molecular weight of 4000, and a minimum film-forming temperature of 5. °C or less.
- the resulting water-soluble acrylic resin (A-3) had a glass transition temperature of 37°C, an acid value of 35 mgKOH/g, a hydroxyl value of 26 mgKOH/g, a weight average molecular weight of 45000, and a minimum film-forming temperature of 5°C or less. rice field.
- the resulting water-dispersed acrylic resin (A-6) had a solid content acid value of 3 mgKOH/g, a glass transition temperature of ⁇ 44° C., an average particle size of 0.1 ⁇ m, a hydroxyl value of 21 mgKOH/g, and a weight average molecular weight of 500,000 or more, and the minimum film-forming temperature was 0° C. or less.
- Example 1 80 parts of the water-soluble acrylic resin (A-1) solution (resin solid content: 40 parts) and 200 parts of the polyolefin resin (B-1) solution (resin solid content: 60 parts), which is the film-forming resin obtained in Production Example 1 ), 2 parts of “BYK-347” and 14 parts of “Viscarex HV30” were added, then stirring was continued for 1 hour, and the pH was adjusted to 8.5 with dimethylethanolamine, followed by propylene glycol. Monopropyl ether and deionized water were added in the amounts (parts) shown in Table 1 and stirred to give a water-based primer coating composition No. 6.5% solids content. got 1.
- Aqueous Primer Coating Composition No. 1 had a surface tension of 30 dyn/cm 2 or less.
- Example 2 water-based primer coating composition No. 1 having a solid content shown in Tables 1 and 2 was prepared in the same manner as in Example 1, except that each component was formulated as shown in Tables 1 and 2. 2-24 were obtained.
- the blending amounts in Tables 1 and 2 indicate the solid content blending amounts.
- Aqueous Primer Coating Composition No. The surface tensions of 2-6, 9-16, 17 and 22 were 30 dyn/cm 2 or less.
- Aqueous Primer Coating Composition No. The surface tension of 7 was 34 dyn/cm 2 .
- Aqueous Primer Coating Composition No. The surface tension of 8 was 32 dyn/cm 2 .
- Film-forming resin A-1 Water-soluble acrylic resin (A-1) obtained in Production Example 1, glass transition temperature 37° C., minimum film-forming temperature 5° C. or lower
- Film-forming resin A-2 Obtained in Production Example 2
- Water-soluble acrylic resin (A-2) Glass transition temperature 37 ° C., minimum film-forming temperature 5 ° C. or less
- Film-forming resin A-3 Water-soluble acrylic resin (A-3) obtained in Production Example 3, glass transition Temperature 37 ° C., minimum film-forming temperature 5 ° C.
- Film-forming resin A-4 product name “Bihydrol UH-2648”, manufactured by Sumika Covestro Urethane Co., Ltd., water-dispersed polyurethane resin (A-4) emulsion, solid content 35 mass%, minimum film-forming temperature of 5 ° C. or less
- Film-forming resin A-5 product name "Bihydrol UH-2606", manufactured by Sumika Covestro Urethane Co., Ltd., water-dispersed polyurethane resin, minimum film-forming temperature of 45 ° C.
- Film-forming resin A-6 Water-dispersed acrylic resin (A-6) obtained in Production Example 4, glass transition temperature -42 ° C., minimum film-forming temperature 0 ° C.
- Film-forming resin A-7 Product name "Evaphanol HA-107C”, manufactured by Nicca Chemical Co., Ltd., water-dispersed polyurethane resin (A-7), solid content 40% by mass, minimum film-forming temperature 0 ° C. or less
- Polyolefin resin B-1 product name "Superchron E-480T”, manufactured by Nippon Paper Industries Co., Ltd., water-dispersed chlorinated polyolefin resin, degree of chlorination 20%, softening temperature 60 to 70 ° C., resin solid content 30%, weight average molecular weight 80000
- Polyolefin resin B-2 Product name “AUROLEN AE-301”, manufactured by Nippon Paper Industries Co., Ltd., water-dispersible non-chlorinated polyolefin resin, degree of chlorination 0%, softening temperature 65 to 75 ° C., resin solid content 30%
- Polyolefin resin B-3 product name "Hardren NZ-1015", manufactured by Toyobo Co., Ltd., water-dispersible non-chlorinated polyolefin resin, degree of chlorination 0%, softening temperature 80 ° C., resin solid content 30%
- Polyolefin resin B-4 Water-disper
- polyolefin resin B-4- The air in a 1 L flask equipped with a stirrer, thermometer, condenser, and nitrogen gas inlet is replaced with nitrogen, and chlorinated polyolefin resin (product name “Superchron 803MW”, manufactured by Nippon Paper Industries Co., Ltd., solid content 30 % by mass, toluene solution), 190.0 g of THF, and 40.0 g of n-butanol were added, heated to 60° C., and stirred until fully dissolved. After confirming dissolution, 3.0 g of dimethylethanolamine was added and stirred for 15 minutes. After 300 g of deionized water was added dropwise over 2 hours, THF was distilled off under reduced pressure to obtain an aqueous dispersion of polyolefin resin B-4 having a solid content of 32%.
- chlorinated polyolefin resin product name “Superchron 803MW”, manufactured by Nippon Paper Industries Co., Ltd., solid content 30 % by mass,
- Viscarex HV30 trade name, manufactured by Rohm and Haas Co., Ltd., polyacrylic acid-based thickener, acid value 270 mg KOH/, active ingredient 28%
- Adekanol UH-756VF trade name, manufactured by ADEKA, urethane associative viscosity modifier, active ingredient 32%
- Propylene glycol monopropyl ether propylene glycol monopropyl ether, boiling point 150° C., solubility in water 100 g/100 g, hydroxyl group present, surface tension 25.9 dyn/cm 2
- Propylene glycol monomethyl ether Also known as 1-methoxy-2-propanol, boiling point 121°C, hydroxyl group present, surface tension 27.7 dyn/cm 2
- aqueous primer coating compositions obtained in Examples 1 to 16 and Comparative Examples 1 to 8 were evaluated for viscosity, film-forming properties and coating workability as test items 1, 2 and 3.
- the following substrates were used, and a coating film was formed on the substrates to prepare test panels.
- a polypropylene (PP) plate cut into a size of 150 mm ⁇ 450 mm ⁇ 0.8 mm thickness was used as an object to be coated.
- the surface tension of this polypropylene plate was 25.7 dyn/cm 2 .
- a test plate was prepared for each test item and used for various tests. Test results are shown in Tables 1 and 2.
- ⁇ Test item 1 Viscosity> Regarding the water-based primer coating composition, in accordance with JIS-K-5600-2-2 (1999), with a digital display rotational viscometer (manufactured by Brook Field, B-type viscometer) of the Stormer viscometer type, The viscosity ( ⁇ ) at 6 rpm (rotations/minute) and the viscosity ( ⁇ ) at 60 rpm (rotations/minute) at 25° C. were measured. In addition, ( ⁇ )/( ⁇ ) was calculated as a thixotropy index value (TI value).
- TI value thixotropy index value
- Each water-based primer coating composition was applied to the above-mentioned object to be coated with an applicator to a dry film thickness of 2 ⁇ m, which was used as a test plate. The coating film after drying was observed, and the film-forming properties of the water-based primer coating composition were evaluated based on the presence or absence of coating film defects such as cracks in the coating film. Evaluation criteria are shown below. As for the evaluation, AA, A, and A- are acceptable, and C and D are unacceptable.
- the aqueous primer coating composition of the present invention is excellent in film-forming properties and coating workability at low temperatures.
- Example 17 (Primer coating film (I)) The water-based primer coating composition obtained in Example 1 was applied to the above-mentioned object to be coated at a dry film thickness shown in Tables 3 and 4, and an air blow was performed until the coating film was dry to the touch, followed by primer coating. A film was formed.
- Test panels were prepared in the same manner as in Example 17, except that the dry film thicknesses of the water-based primer coating composition and its dry film thickness, the undercoat film, the base coating film and the clear coating film were as shown in Tables 3 and 4. made.
- test plates obtained in Examples 17-35 and Comparative Examples 9-16 were evaluated for adhesion (initial) and water resistance. Test results are shown in Tables 3 and 4.
- Remaining number / total number 100 / 100, no small edge chipping of the coating film at the edge of the square
- A: Remaining number / total number 100 / 100, small edge of the coating film at the edge of the square
- C: Remaining number/Total number 90/100 to 99/100
- D: Remaining number/Total number 89 or less/100
- Remaining number / total number 100 / 100, no small edge chipping of the coating film at the edge of the square
- A: Remaining number / total number 100 / 100, small edge of the coating film at the edge of the square Chipped
- C: Remaining number/Total number 99 to 90/100
- D: Remaining number/Total number 89 or less/100
- a multi-layer coating film was produced by the following procedure.
- test panel was prepared in the same manner as in Example 17, except that the water-based primer coating composition and its dry film thickness, the dry film thickness of the primer coating film, base coating film and clear coating film were as shown in Table 5.
- Example 39 The water-based top clear coating composition in Example 17 was combined with a solvent-based top clear coating composition ("Retan PG Eco HS (High Solid) Clear (Q)" and its curing agent (manufactured by Kansai Paint Co., Ltd., urethane curing type, environmentally friendly Mold high-finish, high-solid clear coating composition, not applicable to organic regulations, not applicable to PRTR law, volatile organic compound (VOC) emission amount Rethane PG ECO CLEAR HX (M): Base 100/Hardener 50/Thinner 20 A test plate having a multi-layer coating film was prepared in the same manner as in Example 17, except that it was changed to 63% reduction).
- Retan PG Eco HS (High Solid) Clear (Q) and its curing agent (manufactured by Kansai Paint Co., Ltd., urethane curing type, environmentally friendly Mold high-finish, high-solid clear coating composition, not applicable to organic regulations, not applicable to PRTR law, volatile organic compound (VOC) emission amount Re
- Example 40 The water-based top clear coating composition in Example 30 was replaced with a solvent-based top clear coating composition ("Retan PG Eco HS (High Solid) Clear (Q)" and its curing agent (manufactured by Kansai Paint Co., Ltd., urethane curing type, environmentally friendly Mold high-finish, high-solid clear coating composition, not applicable to organic regulations, not applicable to PRTR law, volatile organic compound (VOC) emission amount Rethane PG ECO CLEAR HX (M): Base 100/Hardener 50/Thinner 20 A test plate having a multi-layer coating film was produced in the same manner as in Example 30, except that it was changed to 63% reduction).
- Retan PG Eco HS (High Solid) Clear (Q) and its curing agent (manufactured by Kansai Paint Co., Ltd., urethane curing type, environmentally friendly Mold high-finish, high-solid clear coating composition, not applicable to organic regulations, not applicable to PRTR law, volatile organic compound (VOC) emission amount Re
- a multi-layer coating film was prepared in the same manner as in Example 17, except that the water-based primer coating composition was set to Note 1.
- Note 1 "KAR Plastic Primer (NE)” (manufactured by Kansai Paint Co., Ltd., solvent-based primer coating composition, adhesion to polypropylene material, solid content 1.5% by mass, organic regulations applicable, PRTR law applicable, volatile organic compounds (VOC) emissions 800g/L or more)
- Remaining number / total number 100 / 100, no small edge chipping of the coating film at the edge of the square
- A: Remaining number / total number 100 / 100, small edge of the coating film at the edge of the square Chipped
- C: Remaining number/Total number 99 to 90/100
- D: Remaining number/Total number 89 or less/100
- the aqueous primer coating composition of the present invention has good adhesion to resin members, and the multilayer coating film formed on resin members has excellent appearance and water resistance.
- the water-based primer coating composition of the present invention does not correspond to the Organic Law, does not correspond to the PRTR Law, can greatly reduce volatile organic compound (VOC) emissions, and can be used as an all-water-based coating system or an environmentally friendly coating system. It can be seen that the multi-layer coating film formed while taking odor, the human body and the environment into consideration is excellent in appearance and water resistance.
Landscapes
- Chemical & Material Sciences (AREA)
- Life Sciences & Earth Sciences (AREA)
- Engineering & Computer Science (AREA)
- Wood Science & Technology (AREA)
- Materials Engineering (AREA)
- Organic Chemistry (AREA)
- Chemical Kinetics & Catalysis (AREA)
- General Chemical & Material Sciences (AREA)
- Paints Or Removers (AREA)
- Application Of Or Painting With Fluid Materials (AREA)
- Laminated Bodies (AREA)
Priority Applications (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| CN202280011202.9A CN116783256B (zh) | 2021-03-24 | 2022-02-28 | 水性底漆涂料组合物以及多层涂膜的形成方法 |
| JP2022544429A JP7134389B1 (ja) | 2021-03-24 | 2022-02-28 | 水性プライマー塗料組成物及び複層塗膜形成方法 |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2021-049684 | 2021-03-24 | ||
| JP2021049684 | 2021-03-24 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2022202131A1 true WO2022202131A1 (ja) | 2022-09-29 |
Family
ID=83395586
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2022/008380 Ceased WO2022202131A1 (ja) | 2021-03-24 | 2022-02-28 | 水性プライマー塗料組成物及び複層塗膜形成方法 |
Country Status (3)
| Country | Link |
|---|---|
| JP (1) | JP7134389B1 (cg-RX-API-DMAC7.html) |
| CN (1) | CN116783256B (cg-RX-API-DMAC7.html) |
| WO (1) | WO2022202131A1 (cg-RX-API-DMAC7.html) |
Families Citing this family (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO2025120726A1 (ja) * | 2023-12-05 | 2025-06-12 | 日本ペイント株式会社 | 複層塗膜の形成方法、複層塗膜および水性プライマー塗料組成物 |
| JP7521676B1 (ja) * | 2023-12-27 | 2024-07-24 | artience株式会社 | 水性プライマー組成物、包装材用積層体及び包装材用積層体の製造方法 |
| CN118772765B (zh) * | 2024-07-04 | 2026-06-12 | 河北钰林新材料科技发展有限公司 | 一种水性实色底色漆及其制备方法和应用 |
| CN119505171B (zh) * | 2024-11-18 | 2026-06-19 | 中国科学院长春应用化学研究所 | 一种改性氯化聚丙烯树脂及其制备方法和在制备保险杠水性底涂中的应用 |
Citations (9)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH06509383A (ja) * | 1991-08-05 | 1994-10-20 | イーストマン ケミカル カンパニー | 水性塗布組成物 |
| JPH07258596A (ja) * | 1994-02-18 | 1995-10-09 | Herberts Gmbh | 水性一液性コーティング組成物およびプラスチック基質の補修ラッカーコーティングのための方法におけるその使用 |
| JP2011012218A (ja) * | 2009-07-06 | 2011-01-20 | Nippon Paper Chemicals Co Ltd | 水性分散液および水性分散体組成物 |
| JP2015223837A (ja) * | 2014-05-30 | 2015-12-14 | 理想科学工業株式会社 | 非水系インク用インクジェット記録媒体及びインクジェット印刷方法 |
| JP2016192666A (ja) * | 2015-03-31 | 2016-11-10 | コニカミノルタ株式会社 | 超音波振動子およびその製造方法ならびに超音波探触子 |
| JP2017088646A (ja) * | 2015-11-02 | 2017-05-25 | サカタインクス株式会社 | インクジェット記録用プライマーインクおよびインクジェット記録用インクセット |
| JP2018527423A (ja) * | 2015-06-29 | 2018-09-20 | ピーピージー・インダストリーズ・オハイオ・インコーポレイテッドPPG Industries Ohio,Inc. | プラスチック基材のためのコーティング |
| WO2019142749A1 (ja) * | 2018-01-16 | 2019-07-25 | 日本製紙株式会社 | 塩素化ポリオレフィン樹脂及びその用途 |
| JP2020022948A (ja) * | 2018-07-27 | 2020-02-13 | 関西ペイント株式会社 | 塗装体の補修塗装方法 |
Family Cites Families (7)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2006160942A (ja) * | 2004-12-09 | 2006-06-22 | Hitachi Chem Co Ltd | 塗料用水性樹脂組成物及び塗装仕上げ方法 |
| CN101421366B (zh) * | 2006-04-11 | 2012-09-05 | 关西涂料株式会社 | 水性底漆组合物 |
| JP4986756B2 (ja) * | 2006-07-31 | 2012-07-25 | トヨタ自動車株式会社 | 自動車内装材用水性塗料組成物 |
| JP5576164B2 (ja) * | 2010-03-30 | 2014-08-20 | 関西ペイント株式会社 | 水性塗料組成物及びプラスチック成型品の塗装方法 |
| CN104822519A (zh) * | 2012-12-04 | 2015-08-05 | 尤尼吉可株式会社 | 鞋构成部件用底漆、其制造方法、鞋构成部件以及鞋 |
| JP6993269B2 (ja) * | 2018-03-21 | 2022-02-04 | 関西ペイント株式会社 | プライマー塗料組成物 |
| GB202212686D0 (en) * | 2022-08-31 | 2022-10-12 | Smart Photonics Holding B V | Method of providing a wafer |
-
2022
- 2022-02-28 WO PCT/JP2022/008380 patent/WO2022202131A1/ja not_active Ceased
- 2022-02-28 JP JP2022544429A patent/JP7134389B1/ja active Active
- 2022-02-28 CN CN202280011202.9A patent/CN116783256B/zh active Active
Patent Citations (9)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH06509383A (ja) * | 1991-08-05 | 1994-10-20 | イーストマン ケミカル カンパニー | 水性塗布組成物 |
| JPH07258596A (ja) * | 1994-02-18 | 1995-10-09 | Herberts Gmbh | 水性一液性コーティング組成物およびプラスチック基質の補修ラッカーコーティングのための方法におけるその使用 |
| JP2011012218A (ja) * | 2009-07-06 | 2011-01-20 | Nippon Paper Chemicals Co Ltd | 水性分散液および水性分散体組成物 |
| JP2015223837A (ja) * | 2014-05-30 | 2015-12-14 | 理想科学工業株式会社 | 非水系インク用インクジェット記録媒体及びインクジェット印刷方法 |
| JP2016192666A (ja) * | 2015-03-31 | 2016-11-10 | コニカミノルタ株式会社 | 超音波振動子およびその製造方法ならびに超音波探触子 |
| JP2018527423A (ja) * | 2015-06-29 | 2018-09-20 | ピーピージー・インダストリーズ・オハイオ・インコーポレイテッドPPG Industries Ohio,Inc. | プラスチック基材のためのコーティング |
| JP2017088646A (ja) * | 2015-11-02 | 2017-05-25 | サカタインクス株式会社 | インクジェット記録用プライマーインクおよびインクジェット記録用インクセット |
| WO2019142749A1 (ja) * | 2018-01-16 | 2019-07-25 | 日本製紙株式会社 | 塩素化ポリオレフィン樹脂及びその用途 |
| JP2020022948A (ja) * | 2018-07-27 | 2020-02-13 | 関西ペイント株式会社 | 塗装体の補修塗装方法 |
Also Published As
| Publication number | Publication date |
|---|---|
| CN116783256B (zh) | 2024-07-12 |
| CN116783256A (zh) | 2023-09-19 |
| JPWO2022202131A1 (cg-RX-API-DMAC7.html) | 2022-09-29 |
| JP7134389B1 (ja) | 2022-09-09 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP7134389B1 (ja) | 水性プライマー塗料組成物及び複層塗膜形成方法 | |
| JP5060202B2 (ja) | 光輝性塗膜形成方法 | |
| JP6770812B2 (ja) | 複層塗膜形成方法 | |
| JP5532712B2 (ja) | 樹脂分散体組成物、及びそれを含有してなるプライマー、塗料、及びその積層体 | |
| JP5148474B2 (ja) | 水性プライマー組成物及び該組成物を使用するプラスチック成型品の塗装方法 | |
| JP2008115385A (ja) | 下塗剤としての結合剤混合物含有水性被覆組成物 | |
| JP2018171614A (ja) | 複層塗膜形成方法 | |
| JP5865372B2 (ja) | 多成分系の水性着色ベースコート塗料組成物 | |
| WO2017131104A1 (ja) | プライマー塗料組成物および塗膜形成方法 | |
| EP1693429B1 (en) | Aqueous intermediate coating composition and method for forming multilayer coating film | |
| JP2016087569A (ja) | 複層塗膜の形成方法 | |
| JP6399548B2 (ja) | 水性着色ベース塗料組成物及びそれを用いた補修塗装方法 | |
| WO2022075269A1 (ja) | ベース塗料組成物および塗装物品 | |
| JP3242595B2 (ja) | 水性プライマー塗料組成物 | |
| CN117500891A (zh) | 水性涂料组合物 | |
| JP7441769B2 (ja) | 自動車部品用成型品上への複層塗膜の塗装方法 | |
| JP5323361B2 (ja) | 複層塗膜形成方法 | |
| JP2961804B2 (ja) | 塗料用樹脂組成物 | |
| JP3927141B2 (ja) | プラスチック素材の塗膜形成方法および塗装物品 | |
| JPWO2006054611A1 (ja) | 水性着色塗料、疎水性メラミン樹脂水分散体及びその製造方法、水性塗料組成物、並びに、複層塗膜形成方法 | |
| JP3436552B2 (ja) | 水をベースとしたアクリルシラン及びポリウレタンを含有するコーティング組成物 | |
| JP6640578B2 (ja) | プライマー塗料組成物および塗膜形成方法 | |
| JP5084151B2 (ja) | 水性中塗り塗料組成物及びこれを用いる複層塗膜形成方法 | |
| JP2013139512A (ja) | 多成分系の水性着色ベースコート塗料組成物 | |
| JP2003105258A (ja) | 水性塗料用樹脂組成物 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| ENP | Entry into the national phase |
Ref document number: 2022544429 Country of ref document: JP Kind code of ref document: A |
|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 22774929 Country of ref document: EP Kind code of ref document: A1 |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 202280011202.9 Country of ref document: CN |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| 122 | Ep: pct application non-entry in european phase |
Ref document number: 22774929 Country of ref document: EP Kind code of ref document: A1 |