WO2022145290A1 - Ni電解めっき皮膜を備えるめっき構造体及び該めっき構造体を含むリードフレーム - Google Patents
Ni電解めっき皮膜を備えるめっき構造体及び該めっき構造体を含むリードフレーム Download PDFInfo
- Publication number
- WO2022145290A1 WO2022145290A1 PCT/JP2021/047335 JP2021047335W WO2022145290A1 WO 2022145290 A1 WO2022145290 A1 WO 2022145290A1 JP 2021047335 W JP2021047335 W JP 2021047335W WO 2022145290 A1 WO2022145290 A1 WO 2022145290A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- plating
- plating film
- film
- less
- electrolytic
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C13/00—Alloys based on tin
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C19/00—Alloys based on nickel or cobalt
- C22C19/03—Alloys based on nickel or cobalt based on nickel
-
- C—CHEMISTRY; METALLURGY
- C25—ELECTROLYTIC OR ELECTROPHORETIC PROCESSES; APPARATUS THEREFOR
- C25D—PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR
- C25D3/00—Electroplating: Baths therefor
- C25D3/02—Electroplating: Baths therefor from solutions
- C25D3/12—Electroplating: Baths therefor from solutions of nickel or cobalt
-
- C—CHEMISTRY; METALLURGY
- C25—ELECTROLYTIC OR ELECTROPHORETIC PROCESSES; APPARATUS THEREFOR
- C25D—PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR
- C25D5/00—Electroplating characterised by the process; Pretreatment or after-treatment of workpieces
- C25D5/10—Electroplating with more than one layer of the same or of different metals
- C25D5/12—Electroplating with more than one layer of the same or of different metals at least one layer being of nickel or chromium
-
- C—CHEMISTRY; METALLURGY
- C25—ELECTROLYTIC OR ELECTROPHORETIC PROCESSES; APPARATUS THEREFOR
- C25D—PROCESSES FOR THE ELECTROLYTIC OR ELECTROPHORETIC PRODUCTION OF COATINGS; ELECTROFORMING; APPARATUS THEREFOR
- C25D7/00—Electroplating characterised by the article coated
-
- H—ELECTRICITY
- H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- H10W—GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10
- H10W72/00—Interconnections or connectors in packages
Definitions
- the present invention relates to a Ni electrolytic plating film and a plating structure provided with the plating film, and particularly to a plating structure at a joint portion such as wire bonding in a semiconductor package such as an IC or LSI.
- Patent Documents 1 to 4 disclose that a Ni / Pd / Au electroless plating film is formed on a connection terminal portion of a semiconductor element, and a solder bump is formed on the electroless plating film. ing.
- Patent Document 5 an invention relating to a plating structure consisting of three layers of Ge—Ni / Pd / Au formed by electrolytic plating.
- Patent Document 6 a technique for forming a Ni / Pd-P / Au film by electrolytic plating is also known (Patent Document 6).
- the above plating film can be formed by electrolytic plating or electroless plating, but since electroplating and electroless plating have advantages and disadvantages, they are usually used properly according to the object to be plated. be.
- Japanese Unexamined Patent Publication No. 11-345896 Japanese Unexamined Patent Publication No. 2006-179977 International Publication No. 2006/11215 Japanese Unexamined Patent Publication No. 2016-162770 Japanese Unexamined Patent Publication No. 2009-228021 Japanese Unexamined Patent Publication No. 2012-241260
- Pd-PPF Pre Plated Frame
- thinning of precious metal films such as Au and Pd is being promoted.
- the thinning of the precious metal plating film must not impair the solder wettability. Whether or not this effect can be maintained is determined by evaluating the solder wettability of the plating film after the heat treatment. For example, as described in Patent Document 5, after heat-treating the test piece on which the plating film is formed, the test piece is immersed in a solder bath, and the time until the wet stress value becomes zero (zero cross time: ZCT) is measured. If this time is short enough, it can be considered that the solder wettability is maintained.
- ZCT zero cross time
- the present invention has been made in view of such a problem, and an object of the present invention is to provide a Ni plating film having excellent solder wettability and a plating structure provided with the Ni plating film. do.
- Ni (nickel) electrolytic plating film containing a predetermined amount of P (phosphorus) to provide a Ni electrolytic plating film having excellent solder wettability. It was found that the present invention can be formed, and the present invention has been completed. The problem is solved by the means shown below.
- the film thickness of the Ni electrolytic plating film is 0.1 ⁇ m or more and 10 ⁇ m or less and the P content is 0.05 wt% or more and less than 0.2 wt%
- the film thickness of the Ni electrolytic plating film is 0.06 ⁇ m or more.
- the Ni electrolytic plating film contains P of 0.01 wt% or more and 1.0 wt% or less and the content of P is 0.01 wt% or more and less than 0.05 wt%, the film thickness of the Ni electrolytic plating film is 0.
- the thickness of the Ni electrolytic plating film is 0.06 ⁇ m or more and 10 ⁇ m or less, and the P content is 0.
- the film thickness of the Ni electrolytic plating film is 0.
- the P content is 0.05 wt% or more and less than 0.2 wt%
- the thickness of the Ni electrolytic plating film is 0.06 ⁇ m or more and 10 ⁇ m or less
- the P content is 0.01 ⁇ m or more and 10 ⁇ m or less.
- the present invention has an excellent effect that a Ni electrolytic plating film having excellent solder wettability can be obtained. Further, it has an excellent effect that the thinning of the Ni-plated electrolytic film can be achieved while maintaining good solder wettability.
- the Ni plating film In the process of forming a plating film, it is the Ni plating film that takes a particularly long time to form, so thinning the Ni plating film can lead to a significant reduction in tact time.
- electroless plating does not use electricity, it can be plated uniformly without being affected by the flow of electricity, but because it forms a film using a chemical reaction, the rate of forming the film is slow and it is also possible. , It is necessary to chemically stabilize the plating bath, and maintenance of the chemical solution and the plating tank may be costly. Under these circumstances, when a plating film is formed on the entire surface of the lead frame, the plating film is usually formed by electrolytic plating.
- the present inventor has earnestly studied the improvement of solder wettability in such an electrolytic plating film, and found that the solder wettability of the plating film is improved by containing a predetermined amount of P (phosphorus) in the Ni electrolytic plating film. I found that I could do it. In particular, it has been found that sufficient solder wettability can be maintained even when the Ni plating film is thinned. As a result, the tact time due to the thinning of the Ni plating film can be shortened, and the cost is expected to be reduced.
- the Ni electrolytic plating film according to the embodiment of the present invention is characterized by containing 0.01 wt% or more and 1.0 wt% or less of P (phosphorus).
- P phosphorus
- the lower limit of the P content is preferably 0.08 wt% or more, more preferably 0.18 wt% or more, and the upper limit of the P content is preferably 0.8 wt% or less, more preferably 0. It is 61 wt% or less.
- the film thickness of the Ni electrolytic plating film can be determined in relation to the P content, and when the P content is 0.01 wt% or more and less than 0.05 wt%, the film thickness of the Ni electrolytic plating film is When it is 0.1 ⁇ m or more and 10 ⁇ m or less and the P content is 0.05 wt% or more and less than 0.2 wt%, the film thickness of the Ni electrolytic plating film is 0.06 ⁇ m or more and 10 ⁇ m or less, and the P content is When it is 0.2 wt% or more and 1.0 wt% or less (or 0.8 wt% or less, 0.61 wt% or less), the thickness of the Ni electrolytic plating film is 0.01 ⁇ m or more and 10 ⁇ m or less. It can be said that the Ni electrolytic plating film of the present embodiment is particularly excellent in that good solder wettability can be ensured even when the film thickness of the Ni electrolytic plating film is reduced to 1 ⁇ m or less. ...
- the P content is 0.01 wt% or more and less than 0.05 wt%, if the thickness of the Ni plating film is thinner than 0.1 ⁇ m, the diffusion prevention effect of the base metal (Cu or Cu alloy) is weakened, and the surface surface is weakened. Cu oxide is formed on the surface, and the solder wettability is lowered. Further, when the P content is 0.05 wt% or more and less than 0.2 wt%, if the thickness of the Ni plating film is thinner than 0.06 ⁇ m, the diffusion prevention effect of the base metal (Cu or Cu alloy) becomes weak. , Cu oxide is formed on the surface, and the solder wettability is lowered.
- the film thickness is preferably 0.06 ⁇ m or more, more preferably 0.1 ⁇ m or more, and further preferably 0.2 ⁇ m or more.
- the thicker the film thickness of the Ni electrolytic plating film the higher the solder wettability.
- the film thickness is 10 ⁇ m or less, more preferably 5 ⁇ m or less, further preferably 1 ⁇ m or less, and most preferably 0.5 ⁇ m or less.
- the following structure can be adopted as the plating structure according to the embodiment of the present invention.
- the Ni plating film is the P-containing Ni electrolytic plating film according to the present embodiment. Any of the above plating films can be formed by an electrolytic plating film.
- the Pd plating film may be a Pd alloy as well as a pure Pd.
- This embodiment is particularly effective when Cu or a Cu alloy is used as the substrate (base metal), but does not prevent the use of other materials such as Fe or Fe alloy.
- the plating structure can be selected according to the application and required characteristics.
- the Au plating film and Pd plating film formed on the outermost surface have the main purpose of preventing oxidation of the Ni plating film and preventing diffusion of Ni onto the surface.
- a metal strike plating film can be formed as a base in each of the Ni plating film, the Pd plating film, and the Au plating film. Generally, strike plating may be performed as a pretreatment for the purpose of improving the adhesion of the electrolytic plating film.
- metal strike plating composed of any one of Au, Ag, Pd and Cu.
- Pd plating film and / or an Au plating film it is preferable to carry out metal strike plating composed of any one of Au, Ag and Pd.
- the film thickness of the metal strike plating film is not particularly limited, but can be, for example, 0.001 to 0.5 ⁇ m. It is preferably 0.01 to 0.1 ⁇ m.
- Another embodiment of the present invention is a lead frame provided with the above-mentioned plating structure.
- Lead frames are often composed of copper or copper alloys.
- the plating structure according to the present embodiment can be formed not only on the lead frame but also on the solder pad portion used in flip chip mounting, and it can be inferred that similarly excellent bonding can be obtained.
- a Ni / Pd / Au plating film may be formed by electroless plating.
- a phosphorus compound may be used as a reducing agent in the plating solution, and in that case, P (phosphorus) is inevitably contained in the Ni film. It is possible to form a Ni film with a P content of 0 wt% by using a reducing agent other than a phosphorus compound, but since it is derived from a reducing agent, the P content in the Ni film is controlled to 2 wt% or less. It's very difficult to do.
- the Ni plating film according to this embodiment can be formed by electrolytic plating using a nickel plating bath containing a phosphorus compound.
- a nickel plating bath containing a phosphorus compound As the phosphorus compound, hypophosphoric acid, phosphoric acid, phosphoric acid and the like can be used. Further, other phosphorus-containing compounds can be substituted.
- As the nickel plating bath a watt bath, a sulfamic acid bath, a citric acid bath and the like can be used. Further, a plating bath containing other nickel can be used as an alternative.
- the phosphorus compounds and nickel plating baths shown above are exemplary and not limited.
- the amount of nickel salt in the Ni plating bath can be 40 to 125 g / L in terms of metal.
- the amount of the phosphorus compound can be 5 to 300 mg / L in terms of phosphorus. It should be understood that the amounts of nickel salts and phosphorus compounds shown above are exemplary and are not intended to be limited to the
- the Ni electrolytic plating conditions can be as follows. However, this electrolytic plating condition is an example, and there are many processing systems and processing devices for carrying out Ni electrolytic plating, and the electrolytic plating conditions can be changed according to the processing system and processing device. It is clear that you can go. Therefore, it should be noted that there is no intention to limit to the disclosed electroplating conditions.
- Cathode current density 1-10A / dm 2
- Electrolysis time 5 to 30 min pH: 3-6
- Bath temperature 30-60 ° C
- Cathode Copper or copper alloy
- Anode Nickel
- the Pd plating film and the Au plating film can be formed by using a known plating bath and known electrolytic plating conditions (for example, Patent Document 5). Further, the metal strike plating film can also be formed by using a known plating bath and known electrolytic plating conditions.
- ⁇ Preparation of evaluation sample> The lead frame made of Cu alloy is subjected to electrolytic degreasing (liquid temperature: 68 ° C., current density: 10 A / dm 2 , immersion time: 60 seconds) as a pretreatment, and then pickled (5 vol.% Sulfuric acid, 30 seconds). ), And then washed with pure water.
- the pretreated lead frames were sequentially subjected to Ni plating, Pd plating, and Au plating under the following plating conditions. At this time, the evaluation sample was adjusted by changing the P concentration in the Ni plating solution.
- Plating bath Palladium plating solution (manufactured by Matsuda Sangyo Co., Ltd .: Parasigma UF) Pd concentration: 3 g / L Current density: 0.5A / dm 2 Bath temperature: 40 ° C pH: 6.5 Target film thickness: 0.025 ⁇ m
- Anode Iridium oxide
- Plating bath Gold plating solution (manufactured by Matsuda Sangyo Co., Ltd .: Aurora Sigma F) Au concentration: 2 g / L Current density: 2A / dm 2 Bath temperature: 45 ° C pH: 4 Target film thickness: 0.005 ⁇ m
- Anode Iridium oxide
- the phosphorus content in the Ni plating film of each evaluation sample was measured using a radio frequency inductively coupled plasma (ICP) emission spectrophotometer.
- ICP radio frequency inductively coupled plasma
- solder wettability After adding a high-temperature thermal history by holding each evaluation sample under a predetermined temperature condition (400 ° C ⁇ 2 ° C) for a long time, a solder bath (63% -Sn, 37% -Pb, liquid temperature: 230 ° C ⁇ The time required from immersion in 5 ° C. to zero the force received from the solder bath (zero cross time) was measured, and the solder wettability was evaluated. Zero cross time means that the shorter the time, the better the solder wettability.
- the dipping conditions in the solder bath were a dipping depth of 1 mm, a dipping speed of 2 mm / sec, and a dipping time of 5 seconds, and R-type flux (inactive type) was used as the soldering accelerator.
- Table 1 shows the relationship between the P content contained in the Ni film and the zero cross time. As shown in Table 1, it was confirmed that the solder wettability was improved by adding phosphorus. In particular, when the phosphorus content was 0.1 wt% or more and 0.8 wt% or less, the solder wettability was significantly improved. In general, Pb-free solder has poorer solder wettability than Pb-Sn solder, but even when Pb-free solder (Sn-3.0Ag-0.5Cu) is used, the solder wettability is improved. I have confirmed that there are no problems.
- the lead frame made of Cu alloy is subjected to electrolytic degreasing (liquid temperature: 68 ° C., current density: 10 A / dm 2 , immersion time: 60 seconds) as a pretreatment, and then pickled (5 vol.% Sulfuric acid, 30 seconds). ), And then washed with pure water.
- the pretreated lead frame was sequentially subjected to Cu strike plating, Ni plating, Pd plating, and Au plating. At this time, the evaluation sample was adjusted by changing the P concentration in the Ni plating solution. Ni plating, Pd plating, and Au plating were performed under the same conditions as above, and strike plating was as follows.
- Table 3 shows the relationship between the P content contained in the Ni film and the zero cross time. As shown in Table 3, it was confirmed that the solder wettability was improved by adding phosphorus. In particular, when the phosphorus content was 0.1 wt% or more and 0.8 wt% or less, the solder wettability was significantly improved. In general, Pb-free solder has poorer solder wettability than Pb-Sn solder, but even when Pb-free solder (Sn-3.0Ag-0.5Cu) is used, the solder wettability is improved. I have confirmed that there are no problems.
- the lead frame made of Cu alloy is subjected to electrolytic degreasing (liquid temperature: 68 ° C., current density: 10 A / dm 2 , immersion time: 60 seconds) as a pretreatment, and then pickled (5 vol.% Sulfuric acid, 30 seconds). ), And then washed with pure water.
- the pretreated lead frame was sequentially subjected to Ni plating, Pd strike plating, Pd plating, and Au plating. At this time, the evaluation sample was adjusted by changing the P concentration in the Ni plating solution. Ni plating, Pd plating, and Au plating were performed under the same conditions as above, and strike plating was as follows.
- Table 5 shows the relationship between the P content contained in the Ni film and the zero cross time. As shown in Table 5, it was confirmed that the solder wettability was improved by adding phosphorus. In particular, when the phosphorus content was 0.1 wt% or more and 0.8 wt% or less, the solder wettability was significantly improved. In general, Pb-free solder has poorer solder wettability than Pb-Sn solder, but even when Pb-free solder (Sn-3.0Ag-0.5Cu) is used, the solder wettability is improved. I have confirmed that there are no problems.
- the lead frame made of Cu alloy is subjected to electrolytic degreasing (liquid temperature: 68 ° C., current density: 10 A / dm 2 , immersion time: 60 seconds) as a pretreatment, and then pickled (5 vol.% Sulfuric acid, 30 seconds). ), And then washed with pure water.
- the pretreated lead frame was sequentially subjected to Ni plating, Pd plating, Au strike plating, and Au plating. At this time, the evaluation sample was adjusted by changing the P concentration in the Ni plating solution. Ni plating, Pd plating, and Au plating were performed under the same conditions as above, and strike plating was as follows.
- Plating bath Au strike plating solution
- Au concentration 1.0 g / L
- Current density 5A / dm 2
- Bath temperature 50 ° C pH: 4
- Target film thickness 0.001 ⁇ m
- Anode Iridium oxide
- Table 7 shows the relationship between the P content contained in the Ni film and the zero cross time. As shown in Table 7, it was confirmed that the solder wettability was improved by adding phosphorus. In particular, when the phosphorus content was 0.1 wt% or more and 0.8 wt% or less, the solder wettability was significantly improved. In general, Pb-free solder has poorer solder wettability than Pb-Sn solder, but even when Pb-free solder (Sn-3.0Ag-0.5Cu) is used, the solder wettability is improved. I have confirmed that there are no problems.
- the present invention has an excellent effect that a Ni electrolytic plating film having excellent solder wettability can be obtained. Further, it has an excellent effect that the thinning of the Ni-plated electrolytic film can be achieved while maintaining good solder wettability.
- the electrolytic plating film and the plating film structure according to the present invention are useful for lead frames, printed wiring boards, rigid boards, flexible boards, tape carriers, connectors, power devices, wires, pins and the like.
Landscapes
- Chemical & Material Sciences (AREA)
- Engineering & Computer Science (AREA)
- Materials Engineering (AREA)
- Metallurgy (AREA)
- Organic Chemistry (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Electrochemistry (AREA)
- Mechanical Engineering (AREA)
- Electroplating Methods And Accessories (AREA)
- Lead Frames For Integrated Circuits (AREA)
- Electroplating And Plating Baths Therefor (AREA)
Priority Applications (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2022506652A JP7096955B1 (ja) | 2020-12-28 | 2021-12-21 | Ni電解めっき皮膜を備えるめっき構造体及び該めっき構造体を含むリードフレーム |
| CN202180065149.6A CN116324002B (zh) | 2020-12-28 | 2021-12-21 | 具有Ni电镀膜的镀敷结构体和包含该镀敷结构体的引线框架 |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2020218234A JP7061247B1 (ja) | 2020-12-28 | 2020-12-28 | ニッケル電解めっき皮膜及びめっき構造体 |
| JP2020-218234 | 2020-12-28 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2022145290A1 true WO2022145290A1 (ja) | 2022-07-07 |
Family
ID=81448161
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2021/047335 Ceased WO2022145290A1 (ja) | 2020-12-28 | 2021-12-21 | Ni電解めっき皮膜を備えるめっき構造体及び該めっき構造体を含むリードフレーム |
Country Status (4)
| Country | Link |
|---|---|
| JP (2) | JP7061247B1 (cg-RX-API-DMAC7.html) |
| CN (1) | CN116324002B (cg-RX-API-DMAC7.html) |
| TW (2) | TWI787896B (cg-RX-API-DMAC7.html) |
| WO (1) | WO2022145290A1 (cg-RX-API-DMAC7.html) |
Families Citing this family (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN116449063B (zh) * | 2023-05-03 | 2024-07-16 | 苏州迪克微电子有限公司 | 一种具有镍金钯镀膜层的钯合金探针结构及其电镀方法 |
Citations (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPS57145351A (en) * | 1981-03-04 | 1982-09-08 | Hitachi Cable Ltd | Lead frame for semiconductor |
| JPH10242372A (ja) * | 1997-02-28 | 1998-09-11 | Nippon Denkai Kk | リードフレーム材とその製法 |
| JPH10284667A (ja) * | 1997-04-04 | 1998-10-23 | Furukawa Electric Co Ltd:The | 耐食性、耐酸化性に優れる電気電子機器用部品材料、及びその製造方法 |
| JP2020017692A (ja) * | 2018-07-27 | 2020-01-30 | Tdk株式会社 | 電子部品パッケージ |
Family Cites Families (9)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US4994329A (en) * | 1988-11-15 | 1991-02-19 | Aisin Seiki Kabushiki Kaisha | Article having nickel plated film comprising a varying content of phosphorus |
| US6117566A (en) * | 1997-02-03 | 2000-09-12 | Nippon Denkai, Ltd. | Lead frame material |
| US6037653A (en) * | 1997-03-25 | 2000-03-14 | Samsung Aerospace Industries, Ltd. | Semiconductor lead frame having multi-layered plating layer including copper-nickel plating layer |
| JP2000077593A (ja) * | 1998-08-27 | 2000-03-14 | Hitachi Cable Ltd | 半導体用リードフレーム |
| TWI263704B (en) * | 2003-03-18 | 2006-10-11 | Ngk Spark Plug Co | Wiring board |
| TW200530433A (en) * | 2004-01-21 | 2005-09-16 | Enthone | Preserving solderability and inhibiting whisker growth in tin surfaces of electronic components |
| US7256481B2 (en) * | 2005-11-30 | 2007-08-14 | Texas Instruments Incorporated | Leadframes for improved moisture reliability and enhanced solderability of semiconductor devices |
| CN100392850C (zh) * | 2006-05-29 | 2008-06-04 | 朱冬生 | 一种引线框架以及具有所述引线框架的半导体器件 |
| CN103667775B (zh) * | 2013-11-27 | 2016-04-13 | 余姚市士森铜材厂 | 一种铜合金半导体引线框架 |
-
2020
- 2020-12-28 JP JP2020218234A patent/JP7061247B1/ja active Active
-
2021
- 2021-07-02 TW TW110124466A patent/TWI787896B/zh active
- 2021-12-21 WO PCT/JP2021/047335 patent/WO2022145290A1/ja not_active Ceased
- 2021-12-21 JP JP2022506652A patent/JP7096955B1/ja active Active
- 2021-12-21 CN CN202180065149.6A patent/CN116324002B/zh active Active
- 2021-12-27 TW TW110148835A patent/TWI790062B/zh active
Patent Citations (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPS57145351A (en) * | 1981-03-04 | 1982-09-08 | Hitachi Cable Ltd | Lead frame for semiconductor |
| JPH10242372A (ja) * | 1997-02-28 | 1998-09-11 | Nippon Denkai Kk | リードフレーム材とその製法 |
| JPH10284667A (ja) * | 1997-04-04 | 1998-10-23 | Furukawa Electric Co Ltd:The | 耐食性、耐酸化性に優れる電気電子機器用部品材料、及びその製造方法 |
| JP2020017692A (ja) * | 2018-07-27 | 2020-01-30 | Tdk株式会社 | 電子部品パッケージ |
Also Published As
| Publication number | Publication date |
|---|---|
| CN116324002A (zh) | 2023-06-23 |
| JP7096955B1 (ja) | 2022-07-06 |
| TWI787896B (zh) | 2022-12-21 |
| TW202233899A (zh) | 2022-09-01 |
| JP2022103538A (ja) | 2022-07-08 |
| TW202225489A (zh) | 2022-07-01 |
| JPWO2022145290A1 (cg-RX-API-DMAC7.html) | 2022-07-07 |
| CN116324002B (zh) | 2025-02-21 |
| TWI790062B (zh) | 2023-01-11 |
| JP7061247B1 (ja) | 2022-04-28 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| CN101029408B (zh) | 无晶须的电镀结构及电镀方法 | |
| US3147547A (en) | Coating refractory metals | |
| CN110325665B (zh) | 无电解镀敷工艺 | |
| TW201000686A (en) | Electronic component and method for manufacturing the same | |
| KR20070026832A (ko) | 주석계 도금 피막 및 그 형성 방법 | |
| KR101270770B1 (ko) | 인쇄회로기판의 도금방법 | |
| JP3916586B2 (ja) | リードフレームのめっき方法 | |
| JP5766318B2 (ja) | リードフレーム | |
| JP7096955B1 (ja) | Ni電解めっき皮膜を備えるめっき構造体及び該めっき構造体を含むリードフレーム | |
| KR20190020831A (ko) | 무전해 팔라듐/금도금 프로세스 | |
| JP2009235579A (ja) | リードフレーム | |
| JP2003013249A (ja) | 置換金メッキ液 | |
| JP2014123760A5 (cg-RX-API-DMAC7.html) | ||
| JPH10284667A (ja) | 耐食性、耐酸化性に優れる電気電子機器用部品材料、及びその製造方法 | |
| JP2005105307A (ja) | リフローSnめっき部材、前記部材の製造方法、および前記部材が用いられた電気電子機器用部品 | |
| HK40087590A (en) | Plating structure comprising ni electrolytic plating film, and lead frame including said plating structure | |
| HK40087590B (en) | Plating structure comprising ni electrolytic plating film, and lead frame including said plating structure | |
| JP6521553B1 (ja) | 置換金めっき液および置換金めっき方法 | |
| JP2000012762A (ja) | 耐食性に優れる電気電子機器用部品材料、及びその製造方法 | |
| WO2021166641A1 (ja) | めっき積層体 | |
| JP4704313B2 (ja) | リードフレームのめっき方法 | |
| CN100481422C (zh) | 电子元器件 | |
| KR102966027B1 (ko) | 도금 적층체 | |
| JP5508329B2 (ja) | リードフレーム | |
| JP2001185836A (ja) | 配線基板及び配線基板の製造方法及び製造装置 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| ENP | Entry into the national phase |
Ref document number: 2022506652 Country of ref document: JP Kind code of ref document: A |
|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 21915150 Country of ref document: EP Kind code of ref document: A1 |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| 122 | Ep: pct application non-entry in european phase |
Ref document number: 21915150 Country of ref document: EP Kind code of ref document: A1 |
|
| WWG | Wipo information: grant in national office |
Ref document number: 202180065149.6 Country of ref document: CN |