JPS59127232A - 磁気記録媒体 - Google Patents
磁気記録媒体Info
- Publication number
- JPS59127232A JPS59127232A JP58002454A JP245483A JPS59127232A JP S59127232 A JPS59127232 A JP S59127232A JP 58002454 A JP58002454 A JP 58002454A JP 245483 A JP245483 A JP 245483A JP S59127232 A JPS59127232 A JP S59127232A
- Authority
- JP
- Japan
- Prior art keywords
- thin film
- magnetic recording
- recording medium
- diamond structure
- carbon
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。
め要約のデータは記録されません。
Description
【発明の詳細な説明】
本発明は表面にダイヤモンl、” $造を含んたIyの
薄膜を形成した磁気記録媒体に関する・情報処理様器の
発達に併りい勝気記録装置に対する要望が捷すます厳し
くなってきている。フレキシブルディスク、ハードディ
スク、干−ブと形態はさまざまであるがその要求される
ところは小面積もしくは小体積で高容量の信呆配@を行
りうことである。磁気記録媒体材料として従来のr酸化
鉄に替わってOr OB * CO変性酸化鉄、更には
蒸着CO等高密度記録に適応する材質が見出されている
。更に信頼性についてもフレキシブルディスクの場合t
d 300万バス、ハードティスフの場合は2万回のa
SS後もヘッド及び媒体に損傷が々(、かつ電磁変換特
性の劣化が認められないことが要求されている。これを
遠戚するために5102やSi、Na々どの過膜′(i
−表面に形成することが行りわれている。これらの薄膜
は絶縁体であるために表面が帯電し、やすく、周辺のほ
こりを吸着することがしばしばある、fflわち表面硬
度は硬(かったほこりのために憂勿記録媒体もしくはヘ
ッドヲ損傷することが起きるようになった。
薄膜を形成した磁気記録媒体に関する・情報処理様器の
発達に併りい勝気記録装置に対する要望が捷すます厳し
くなってきている。フレキシブルディスク、ハードディ
スク、干−ブと形態はさまざまであるがその要求される
ところは小面積もしくは小体積で高容量の信呆配@を行
りうことである。磁気記録媒体材料として従来のr酸化
鉄に替わってOr OB * CO変性酸化鉄、更には
蒸着CO等高密度記録に適応する材質が見出されている
。更に信頼性についてもフレキシブルディスクの場合t
d 300万バス、ハードティスフの場合は2万回のa
SS後もヘッド及び媒体に損傷が々(、かつ電磁変換特
性の劣化が認められないことが要求されている。これを
遠戚するために5102やSi、Na々どの過膜′(i
−表面に形成することが行りわれている。これらの薄膜
は絶縁体であるために表面が帯電し、やすく、周辺のほ
こりを吸着することがしばしばある、fflわち表面硬
度は硬(かったほこりのために憂勿記録媒体もしくはヘ
ッドヲ損傷することが起きるようになった。
本発明はこのような欠点がな(、表面硬度が硬く、かつ
帯電し方(てほこりを吸着し7ガい磁気記録媒体を完成
したものである。
帯電し方(てほこりを吸着し7ガい磁気記録媒体を完成
したものである。
本発明の目的は信頼性の高い研偲de録媒体を提供する
ことにある。
ことにある。
カーボンはその同素体としてグラファイトとダイヤモン
ドがあり、いずわも#4.電性を示す。特にダイヤモン
ドは硬度が硬いことは周知のことである7グラフアイト
は潤滑性能にすぐれていることも周知である。
ドがあり、いずわも#4.電性を示す。特にダイヤモン
ドは硬度が硬いことは周知のことである7グラフアイト
は潤滑性能にすぐれていることも周知である。
ダイヤモンド構造を含んだ薄膜げイオンビームスパッタ
やプラズマCyD%レーザー蒸着等により形成される。
やプラズマCyD%レーザー蒸着等により形成される。
本発明は磁気記録媒体のt面にこのダイヤモンド構造を
含むカーボンの薄膜を形成することにより信頼性を飛躍
的に向上させたものである^ダイヤモンド構造を含むカ
ーボン薄膜ノ厚み−は1000オングストローム以下で
も充分その効果を示した、又カーボン薄膜中にダイヤモ
ンド構造以外のグラファイト構造を含んでいても効果け
そこ1弥ることはhかった。
含むカーボンの薄膜を形成することにより信頼性を飛躍
的に向上させたものである^ダイヤモンド構造を含むカ
ーボン薄膜ノ厚み−は1000オングストローム以下で
も充分その効果を示した、又カーボン薄膜中にダイヤモ
ンド構造以外のグラファイト構造を含んでいても効果け
そこ1弥ることはhかった。
以下に実施例について本発明を説明すふ、実施例1゜
11+++++厚で125−径のアルミニウム基板上に
反応性スパッタに工りγFe50m の薄膜を形成した
。
反応性スパッタに工りγFe50m の薄膜を形成した
。
更にその上にグラファイトをターゲットとしてイオンビ
ーム照射を行ない1表面にダイヤモンド構造カーボン薄
膜1000オングストロームを形成した。との磁気記録
媒体は表面に特に潤滑剤を徐布せずにヘッドとの接触、
即ちOE3S?2万回以上行斤っても表面に何の損傷も
なく、はこりが付着することもなかった。
ーム照射を行ない1表面にダイヤモンド構造カーボン薄
膜1000オングストロームを形成した。との磁気記録
媒体は表面に特に潤滑剤を徐布せずにヘッドとの接触、
即ちOE3S?2万回以上行斤っても表面に何の損傷も
なく、はこりが付着することもなかった。
実施例2
アルミ基板上にパーマロ405ミクロン、c。
−Ci r O,5ミクロンをスパッタリングで形成し
た。
た。
Oo −Cr薄膜はOrを1Sat係含有している。
このC〇−Cr薄膜の表面に、真空中でダイヤモンド微
粒子にレーザーを照射して昇華して(る成分を付着せし
めた、はとんどダイヤモンド構造のカーボン薄膜で厚み
は500オングストロームあった、この媒体il″12
万回以上のcssに耐えた。
粒子にレーザーを照射して昇華して(る成分を付着せし
めた、はとんどダイヤモンド構造のカーボン薄膜で厚み
は500オングストロームあった、この媒体il″12
万回以上のcssに耐えた。
実施例6゜
硬質ガラス基板上VCO含有γFe1on の薄膜を
形b7シ、更にその上にメタンガスを用いた高周波プラ
ズマにエリダイヤモンド構造とグラファイト構造を含む
カーボン薄膜を1000オングストローム形成L1c、
cpsけ2万個以上行りったが伺ら損傷に認められなか
った。
形b7シ、更にその上にメタンガスを用いた高周波プラ
ズマにエリダイヤモンド構造とグラファイト構造を含む
カーボン薄膜を1000オングストローム形成L1c、
cpsけ2万個以上行りったが伺ら損傷に認められなか
った。
実施例4
アル、ミ基板上に無KMメッキにエリN i −F層を
25μm形威し、更にタングステンを含有するC O−
N i −Pを5μm無電解メッキで形成した。
25μm形威し、更にタングステンを含有するC O−
N i −Pを5μm無電解メッキで形成した。
更にそd上に真空中でイオンガン中にメタンガスを導入
してイオン化上せてダイヤモンド−造含有カーボン膜を
1000オングストローム形成し、た。
してイオン化上せてダイヤモンド−造含有カーボン膜を
1000オングストローム形成し、た。
特に潤滑剤を塗布しh(てもC3EIは2万回をクリア
ーした。 − 以上実施例について詳述した如く表面にダイヤモンド゛
構造含有カーボン薄膜を形成した本発明勝気8e@媒体
は信頼性について抜群の性能を示し。
ーした。 − 以上実施例について詳述した如く表面にダイヤモンド゛
構造含有カーボン薄膜を形成した本発明勝気8e@媒体
は信頼性について抜群の性能を示し。
その工業的ダl来は非常に大きい、
以上
出願人 株式会社 卵訪精工舎
Claims (1)
- 表面にダイヤモンド゛構造を含むカーボンのk Haケ
形戚し/ζこと全特徴とする磁気記録媒体、