JP3184783B2 - 制振材料 - Google Patents

制振材料

Info

Publication number
JP3184783B2
JP3184783B2 JP18077397A JP18077397A JP3184783B2 JP 3184783 B2 JP3184783 B2 JP 3184783B2 JP 18077397 A JP18077397 A JP 18077397A JP 18077397 A JP18077397 A JP 18077397A JP 3184783 B2 JP3184783 B2 JP 3184783B2
Authority
JP
Japan
Prior art keywords
weight
vibration damping
styrene
parts
damping material
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Lifetime
Application number
JP18077397A
Other languages
English (en)
Other versions
JPH1112430A (ja
Inventor
正 長谷川
邦彦 佐藤
元 松田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Aron Kasei Co Ltd
Original Assignee
Aron Kasei Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Family has litigation
First worldwide family litigation filed litigation Critical https://patents.darts-ip.com/?family=16089084&utm_source=google_patent&utm_medium=platform_link&utm_campaign=public_patent_search&patent=JP3184783(B2) "Global patent litigation dataset” by Darts-ip is licensed under a Creative Commons Attribution 4.0 International License.
Application filed by Aron Kasei Co Ltd filed Critical Aron Kasei Co Ltd
Priority to JP18077397A priority Critical patent/JP3184783B2/ja
Publication of JPH1112430A publication Critical patent/JPH1112430A/ja
Application granted granted Critical
Publication of JP3184783B2 publication Critical patent/JP3184783B2/ja
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Description

【発明の詳細な説明】
【0001】
【発明の属する技術分野】本発明は回転軸の軸受部の騒
音対策等に適用される制振材料に関するものである。
【0002】
【発明が解決しようとする課題】従来、この種の制振材
料としてはスチレン−イソプレン−スチレンブロック共
重合体(SIS)やスチレン−イソプレン−ブタジエン
−スチレンブロック共重合体(SIBS)が使用されて
いた(特開平2−102212号)。これらブロック共
重合体は制振性はあるが、圧縮永久歪が大きいと言う問
題点があった。
【0003】
【課題を解決するための手段】本発明は上記従来の課題
を解決するための手段として、スチレン−ブタジエン−
スチレンブロック共重合体(SBS)および/またはス
チレン−ブタジエン−スチレンブロック共重合体(SB
S)の水素添加物85〜65重量部と、スチレン−イソ
プレン−スチレンブロック共重合体(SIS)の水素添
加物および/またはスチレン−イソプレン−スチレンブ
ロック共重合体(SIS)15〜35重量部との混合物
からなる制振材料を提供するものである。該制振材料に
用いられるSISはイソプレンブロックのビニル結合含
有量が40重量%以上のものが好ましい。本発明におい
ては、上記組成に更にポリフェニレンエーテル樹脂(P
PO)を添加することによって、圧縮永久歪は更に改良
され、また硬度調節のためにポリプロピレン(PP)お
よび/または柔軟剤および/または充填剤を添加しても
よい。
【0004】
【発明の実施の形態】本発明の制振材料においてSBS
および/またはSBS水素添加物は優れたゴム弾性を示
し、ビニル結合含有量が40重量%以上のSIS水素添
加物および/またはSISは上記SBSやSBS水素添
加物の制振性を改良するものであり、更にPPOを添加
混合することによって圧縮永久歪が改良される。
【0005】本発明では制振材料の硬度調節のためにP
Pおよび/または柔軟剤が使用されてもよい。柔軟剤と
してはパラフィン、ミネラルオイル、プロセスオイル、
流動パラフィン等が使用される。本発明の制振材料には
炭酸カルシウム、炭酸マグネシウム、シリカ、タルク、
ポリエチレン等の充填剤が添加されてもよい。
【0006】本発明の制振材料においてSBSおよび/
またはSBS水素添加物とSIS水素添加物および/ま
たはSISとの混合重量比は85:15〜65:35と
する。SIS水素添加物および/またはSISとの混合
重量比が15を下回ると制振性の改良効果が顕著ではな
く、また35を上回ると圧縮永久歪が低下し、更に射出
成形性も悪化する。
【0007】PPOは上記SBSおよび/またはSBS
水素添加物とSIS水素添加物および/またはSISと
の混合物(以下混合エラストマーと言う)100重量部
に対して60重量部以下の添加量、望ましくは50〜2
0重量部の範囲の添加量で使用される。PPOの使用量
が60重量部を上回ると射出成形性に悪影響が及ぼさ
れ、20重量部を下回るとPPOの圧縮永久歪改良効果
が顕著でなくなる。
【0008】PPは上記したように制振材料の硬度の調
節に用いられ、通常上記混合エラストマー100重量部
に対して10〜50重量部程度添加される。柔軟剤も上
記したように制振材料の硬度の調節に用いられ、通常上
記混合エラストマー100重量部に対して50〜300
重量部程度添加される。更に充填剤は通常上記混合エラ
ストマー100重量部に対して25〜100重量部程度
添加される。上記成分の他、例えば老化防止剤、紫外線
吸収剤、顔料が添加されてもよい。
【0009】〔実施例1〕(SBS:SIS混合エラス
トマー) 表1の処方(重量比)のエラストマー試料をバンバリー
ミキサーで混合調製した。
【表1】 上記試料についてtan δ(20℃,60℃)、圧縮永久
歪、流動性を測定し、その結果は表2に示される。
【表2】 tan δ:レオバイブロン使用(振動周波数100Hz) 圧縮永久歪:JIS−K−6301記載の方法により、70℃×22時間後 の圧縮永久歪を測定 流動性:ASTM−D−1238記載の方法により、200℃×5kgf の 条件で測定を行なった。
【0010】本発明の試料No.1−1〜1−5はいずれ
もtan δ(20℃,60℃)が0.1以上であり、優れ
た制振性を有し、また圧縮永久歪も60%以下である。
更に流動性も1.0g/min.以上であり射出成形性も良
好である。
【0011】〔比較例1〕(SBS:SIS混合エラス
トマー) 表3の処方(重量比)のエラストマー試料をバンバリー
ミキサーで混合調製した。
【表3】 上記試料についてtan δ(20℃,60℃)、圧縮永久
歪、流動性を実施例1と同様に測定した。その結果は表
4に示される。
【表4】
【0012】試料No.1C−1はSBSを85重量部以
上含むものであり、tan δ(20℃,60℃)は0.1
以下であり制振性が悪い。更にSISを35重量部以上
含有する1C−2は圧縮永久歪が60%以上であり、流
動性が1.0以下であり、射出成形性が不良である。
【0013】〔実施例2〕(SBS水素添加物:SIS
水素添加物混合エラストマー) 表5の処方(重量比)のエラストマー試料を実施例1と
同様にバンバリーミキサーで混合調製した。
【表5】 上記試料についてtan δ(20℃,60℃)、圧縮永久
歪、流動性を実施例1と同様に測定した。その結果は表
6に示される。
【表6】
【0014】本発明の試料No.2−1〜2−5はいずれ
もtan δ(20℃,60℃)が0.1以上であり、優れ
た制振性を有し、また圧縮永久歪も60%以下である。
更に流動性も1.0g/min.以上であり射出成形性も良
好である。
【0015】〔比較例2〕(SBS水素添加物:SIS
水素添加物混合エラストマー) 表7の処方(重量比)のエラストマー試料を実施例1と
同様にバンバリーミキサーで混合調製した。
【表7】 上記試料について実施例1と同様にtan δ(20℃,6
0℃)、圧縮永久歪、流動性を測定した。その結果は表
8に示される。
【表8】
【0016】試料No.2C−1はSBS水素添加物を8
5重量比以上含むものであり、tanδ(20℃,60
℃)は0.1以下で制振性が悪い。更にSIS水素添加
物を35重量比以上含有する2C−2は圧縮永久歪が6
0%以上であり流動性が1.0以下であり、射出成形性
が不良である。
【0017】〔実施例3〕(SBS水素添加物:SIS
水素添加物:PPO混合エラストマー) 表9の処方(重量比)のエラストマー試料を実施例1と
同様にバンバリーミキサーで混合調製した。
【表9】 上記試料についてtan δ(20℃,60℃)、圧縮永久
歪、流動性を実施例1と同様に測定した。その結果は表
10に示される。
【表10】
【0018】PPOを添加した本実施例の試料は、いず
れもtan δ(20℃,60℃)が0.1以上であり、優
れた制振性を有し、また実施例2試料No.2−2等と比
較すればPPOの添加によって圧縮永久歪は大巾に改良
されている。
【0019】〔比較例3〕(SBS水素添加物:SIS
水素添加物:PPO混合エラストマー) 表11の処方(重量比)のエラストマー試料を実施例1
と同様にバンバリーミキサーで混合調製した。
【表11】 上記試料についてtan δ(20℃,60℃)、圧縮永久
歪、流動性を実施例1と同様に測定した。その結果は表
12に示される。
【表12】
【0020】PPOの添加量が20重量部を下回る試料
No.3C−1は実施例2試料No.2−2等と比較すれば
圧縮永久歪の改良効果に差はなく、また60重量部を上
回る試料No.3C−2は流動性が1.0g/min.以下で
あり、射出成形性が悪化している。
【0021】
【発明の効果】本発明では優れたゴム弾性を有するSB
Sおよび/またはSBS水素添加物にSIS水素添加物
および/またはSISを添加して制振性を改良するか
ら、広い温度範囲で制振性に優れしかも圧縮永久歪が小
さい制振材料が得られる。該圧縮永久歪は更にPPOを
添加することによって大巾に改良される。本発明の制振
材料はしたがって自動車、家庭電化製品等の回転軸の軸
受部。エンジン等の部材のマウント部等に適用され、優
れた制振性を示す。
───────────────────────────────────────────────────── フロントページの続き (56)参考文献 特開 平8−157547(JP,A) 特開 平2−102212(JP,A) (58)調査した分野(Int.Cl.7,DB名) C08L 53/02 C08L 23/12 C08L 71/12

Claims (4)

    (57)【特許請求の範囲】
  1. 【請求項1】スチレン−ブタジエン−スチレンブロック
    共重合体および/またはスチレン−ブタジエン−スチレ
    ンブロック共重合体の水素添加物85〜65重量部と、
    スチレン−イソプレン−スチレンブロック共重合体の水
    素添加物および/またはスチレン−イソプレン−スチレ
    ンブロック共重合体15〜35重量部との混合物からな
    る制振材料
  2. 【請求項2】該スチレン−イソプレン−スチレンブロッ
    ク共重合体のイソプレンブロックのビニル結合含有量は
    40重量%以上である請求項1に記載の制振材料
  3. 【請求項3】請求項1または2に記載の混合物100重
    量部に更にポリフェニレンエーテル樹脂を60重量部以
    下の量で添加混合した制振材料
  4. 【請求項4】請求項1または2または3に記載の混合物
    に更にポリプロピレンおよび/または柔軟剤および/ま
    たは充填剤を添加混合した制振材料
JP18077397A 1997-06-20 1997-06-20 制振材料 Expired - Lifetime JP3184783B2 (ja)