WO2022224778A1 - 温度応答性ポリマー及び水系温度応答性組成物 - Google Patents

温度応答性ポリマー及び水系温度応答性組成物 Download PDF

Info

Publication number
WO2022224778A1
WO2022224778A1 PCT/JP2022/016157 JP2022016157W WO2022224778A1 WO 2022224778 A1 WO2022224778 A1 WO 2022224778A1 JP 2022016157 W JP2022016157 W JP 2022016157W WO 2022224778 A1 WO2022224778 A1 WO 2022224778A1
Authority
WO
WIPO (PCT)
Prior art keywords
temperature
group
carbon atoms
formula
bond
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2022/016157
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
敦史 原田
雄己哉 北山
隼也 江本
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
University Public Corporation Osaka
Original Assignee
University Public Corporation Osaka
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by University Public Corporation Osaka filed Critical University Public Corporation Osaka
Priority to JP2023516404A priority Critical patent/JP7873499B2/ja
Publication of WO2022224778A1 publication Critical patent/WO2022224778A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Images

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F8/00—Chemical modification by after-treatment
    • C08F8/46—Reaction with unsaturated dicarboxylic acids or anhydrides thereof, e.g. maleinisation
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L39/00—Compositions of homopolymers or copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and at least one being terminated by a single or double bond to nitrogen or by a heterocyclic ring containing nitrogen; Compositions of derivatives of such polymers

Definitions

  • the present disclosure relates to temperature-responsive polymers and water-based temperature-responsive compositions.
  • a temperature-responsive polymer is a functional polymer whose affinity with solvents changes with changes in temperature. Temperature-responsive polymers are expected to be applied to functional cell sheets, drug transport carriers, and the like. In recent years, it has been reported that a polymer material exhibits temperature-responsive behavior by adding a third component molecule (also referred to as an “effector”) to a two-component system of a polymer and a solvent.
  • a third component molecule also referred to as an “effector”
  • Non-Patent Document 1 Angew. Int. Ed. 2005, 44, 5658-5661
  • Non-Patent Document 2 Angew. Chem. Int. Ed. 2007, 46, 2708-2711
  • Non-Patent Document 3 J. Am. Chem. Soc. 2012, 134, 8344-8347 describes a temperature-responsive polymer using an organic compound having hydrogen bond-forming properties as an effector.
  • Non-Patent Document 4 (Angew. Chem. 2013, 125, 4268-4272) reports and describes a temperature-responsive polymer using an organic compound that forms a charge-transfer complex as an effector.
  • Non-Patent Documents 3 and 4 exhibit stimuli-responsiveness in organic solvents, but do not exhibit temperature-responsiveness in water.
  • An object of the present disclosure is to provide a polymeric material exhibiting temperature responsiveness in water, the temperature responsiveness such as the lower critical solution temperature (LCST) of which can be changed by various factors.
  • LCST lower critical solution temperature
  • the present inventors have found that a polymer having a specific ring structure with a polar bond such as an amide bond and a carboxylate group in the side chain exhibits temperature responsiveness when polyvalent cations such as calcium ions are coexisted in water as an effector. was found to show
  • the present invention includes the following aspects.
  • a temperature-responsive polymer having a polar bond and a carboxylate group in a side chain wherein the temperature-responsive polymer has the formula (1) contains a structural unit represented by In formula (1), each M independently represents a hydrogen atom or a monovalent cation, and each A independently represents a polar bond selected from the group consisting of an amide bond, an ester bond, a carbonate bond, a urethane bond and a urea bond.
  • each Cy surrounded by a circle independently represents a hydrocarbon ring structure having 4 to 30 carbon atoms
  • the hydrocarbon ring structure includes a halogen atom, an alkyl group having 1 to 4 carbon atoms, and a carbon atom It may have one or more substituents selected from the group consisting of alkoxy groups of numbers 1 to 4, and the carbon atom that constitutes the hydrocarbon ring structure and is bonded to A and the carbon atom that constitutes the hydrocarbon ring structure, COOM are vicinal to each other
  • R 1 is each independently a hydrogen atom or an alkyl group having 1 to 4 carbon atoms
  • R 2 is each independently a single bond or a carbon atom of 1 to A temperature-responsive polymer representing 3 alkanediyl groups.
  • the temperature-responsive polymer is a temperature-responsive polymer having an amide bond and a carboxylate group in a side chain, and has the formula (2) contains a structural unit represented by In formula (2), M each independently represents a hydrogen atom or a monovalent cation, A represents an amide bond, Cy surrounded by a hexagon each independently represents a benzene ring, a cyclohexane ring, a cyclohexene ring, and represents a six-membered ring structure selected from the group consisting of cyclohexadiene rings, each R 1 independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and each R 2 independently represents a single bond or a carbon atom represents an alkanediyl group having 1 to 3 numbers, and R 3 , R 4 ,
  • each M independently represents a hydrogen atom or a monovalent cation
  • each R 1 independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
  • R 2 each independently represents a single bond or an alkanediyl group having 1 to 3 carbon atoms
  • R 3 , R 4 , R 5 and R 6 each independently represent a hydrogen atom, a halogen atom, a carbon atom represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms, and two groups out of R 3 , R 4 , R 5 and R 6 are an aliphatic ring, an aromatic ring or a bridge
  • each M independently represents a hydrogen atom or a monovalent cation
  • each R 1 independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
  • R 2 each independently represents a single bond or an alkanediyl group having 1 to 3 carbon atoms
  • R 3 , R 4 , R 5 and R 6 each independently represent a hydrogen atom, a halogen atom, a carbon atom represents an alkyl group having 1 to 4 carbon atoms or an alkoxy group having 1 to 4 carbon atoms, and two groups out of R 3 , R 4 , R 5 and R 6 are an aliphatic ring, an aromatic ring or a bridge
  • a water-based temperature-responsive composition containing a temperature-responsive polymer can be designed according to various uses.
  • FIG. 1 H-NMR chart of PAA-Pht. 1 H-NMR chart of PAA-CHex. 1 is a graph showing the influence of presence and type of cations on transmittance in aqueous compositions containing PAA-Pht.
  • FIG. 10 is a graph showing the reversibility of the temperature responsiveness of PAA-Pht in the presence of Ca 2+ .
  • FIG. 2 is a graph showing the Ca 2+ concentration dependence of the temperature response of PAA-Pht in the presence of Ca 2+ . 2 is a graph showing the polymer concentration dependence of temperature responsiveness of PAA-Pht in the presence of Ca 2+ .
  • FIG. 10 is a graph showing pH dependence of temperature response of PAA-Pht in the presence of Ca 2+ .
  • FIG. 4 is a graph showing the effect of the type of divalent cation in an aqueous temperature-responsive composition containing PAA-Pht. 4 is another graph showing the effect of the type of divalent cation in an aqueous temperature-responsive composition containing PAA-Pht.
  • 2 is a graph showing the Ca 2+ concentration dependence of the temperature response of PAA-CHex in the presence of Ca 2+ .
  • 2 is a graph showing the polymer concentration dependence of temperature responsiveness of PAA-CHex in the presence of Ca 2+ .
  • the temperature-responsive polymer of one embodiment has a polar bond and a carboxylate group in the side chain, and has the formula (1) Including structural units represented by
  • each M independently represents a hydrogen atom or a monovalent cation
  • each A independently represents a polar bond selected from the group consisting of an amide bond, an ester bond, a carbonate bond, a urethane bond and a urea bond.
  • each Cy surrounded by a circle independently represents a hydrocarbon ring structure having 4 to 30 carbon atoms, and the hydrocarbon ring structure is a halogen atom, an alkyl group having 1 to 4 carbon atoms, and the number of carbon atoms It may have one or more substituents selected from the group consisting of 1 to 4 alkoxy groups, and forms a hydrocarbon ring structure with the carbon atom that forms a hydrocarbon ring structure and bonds to A, and binds to COOM.
  • each R 1 independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms
  • each R 2 independently represents a single bond or an alkane having 1 to 3 carbon atoms represents a diyl group.
  • the mechanism by which the temperature-responsive polymer of the present disclosure exhibits temperature-responsiveness in water in the presence of polyvalent cations is thought to be as follows.
  • a hydrocarbon ring structure, such as a six-membered ring structure, pendant to the polymer backbone ensures that the temperature responsive polymer exhibits hydrophobicity above the lower critical solution temperature (LCST).
  • Groups that form polar bonds such as amide groups and ester groups in side chains are sites that hydrate with water molecules in the system, and dissolve the temperature-responsive polymer in water at temperatures lower than the LCST.
  • the side-chain carboxylate groups interact with coexisting multivalent cations to change the conformation of the temperature-responsive polymer in response to temperature.
  • the pKa of a carboxylate group varies depending on the hydrocarbon ring structure, such as a six-membered ring structure, to which the carboxylate group is attached, such as a benzene ring or an aliphatic ring (cyclohexane ring, cyclohexene ring and cyclohexadiene ring).
  • a benzene ring or an aliphatic ring (cyclohexane ring, cyclohexene ring and cyclohexadiene ring).
  • an aliphatic ring is more hydrophobic than a benzene ring.
  • the LCST of the temperature-responsive polymer changes due to the difference in the pKa of the carboxylate group and the hydrophobicity of the hydrocarbon ring structure such as the six-membered ring structure.
  • temperature-responsive polymers in which carboxylate groups are attached to aliphatic rings tend to exhibit lower LCST than temperature-responsive polymers in which carboxylate groups are attached to benzene rings.
  • a group such as an amide group or an ester group that constitutes a polar bond is bonded to a carbon atom of a hydrocarbon ring structure such as a six-membered ring structure, and a carboxylate group is bonded to a group such as an amide group or an ester group.
  • the orientation of the carboxylate groups with respect to the polymer backbone and groups such as amide groups, ester groups, etc. is restricted by being attached to the carbon atom in the vicinal position of the carbon atom.
  • the carboxylate groups are separated from the main chain of the polymer and are difficult to orient. Therefore, in the temperature-responsive polymer of the present disclosure, it is considered that the conformational change inside the polymer molecule mainly contributes to the expression of temperature-responsiveness rather than the intermolecular interaction of the polymer molecules.
  • each M independently represents a hydrogen atom or a monovalent cation.
  • Monovalent cations include, for example, lithium, sodium, potassium, and ammonium ions.
  • M is preferably a hydrogen atom or a sodium ion.
  • each A independently represents a polar bond selected from the group consisting of an amide bond, an ester bond, a carbonate bond, a urethane bond and a urea bond.
  • A is preferably selected from the group consisting of an amide bond and an ester bond because it effectively restricts the orientation of the carboxylate groups, and more preferably an amide bond because it is more resistant to hydrolysis.
  • each encircled Cy independently represents a hydrocarbon ring structure having 4 to 30 carbon atoms.
  • the carbon atom that forms the hydrocarbon ring structure and is bonded to A and the carbon atom that forms the hydrocarbon ring structure and is bonded to COOM are at vicinal positions to each other.
  • the hydrocarbon ring structure may be a saturated or unsaturated aliphatic or aromatic ring.
  • Hydrocarbon ring structures may be monocyclic, fused, spiro, or bridged.
  • each encircled Cy independently has a six-membered ring structure.
  • a double bond is preferably present between the carbon atom of the six-membered ring structure to which the polar bond A is bonded and the carbon atom of the six-membered ring structure to which the COOM (carboxylate group) is bonded. It is believed that in this embodiment the orientation of the carboxylate groups with respect to the polymer backbone and the polar bond A can be more restricted to obtain precise temperature responsiveness.
  • the six-membered ring structure is a benzene ring or a cyclohexene ring.
  • the hydrocarbon ring structure may have one or more substituents selected from the group consisting of halogen atoms, alkyl groups having 1 to 4 carbon atoms, and alkoxy groups having 1 to 4 carbon atoms.
  • Halogen atoms include fluorine, chlorine, bromine and iodine.
  • alkyl groups having 1 to 4 carbon atoms include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group and t-butyl group.
  • alkoxy groups having 1 to 4 carbon atoms include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, sec-butoxy, and t-butoxy groups.
  • the substituent is a methyl group, an ethyl group, a methoxy group, or an ethoxy group.
  • the hydrocarbon ring structure has no substituents.
  • each R 1 independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
  • alkyl groups having 1 to 4 carbon atoms include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group and t-butyl group.
  • R 1 is preferably a hydrogen atom, a methyl group, or an ethyl group, more preferably a hydrogen atom.
  • each R 2 independently represents a single bond or an alkanediyl group having 1 to 3 carbon atoms.
  • alkanediyl group having 1 to 3 carbon atoms include a methanediyl group (—CH 2 —), an ethane-1,2-diyl group (—CH 2 CH 2 —), an ethane-1,1-diyl group ( —CH(CH 3 )—), propane-1,3-diyl group (—CH 2 CH 2 CH 2 —), propane-1,2-diyl group (—CH 2 CH(CH 3 )—), and propane A -2,2-diyl group (-C(CH 3 ) 2 -) can be mentioned.
  • R2 is preferably a single bond or a methanediyl group, more preferably a methanediyl group.
  • the temperature-responsive polymer has an amide bond and a carboxylate group in the side chain, and has the formula (2) It is preferable to include a structural unit represented by
  • M each independently represents a hydrogen atom or a monovalent cation
  • A represents an amide bond
  • Cy surrounded by a hexagon each independently represents a benzene ring, a cyclohexane ring, a cyclohexene ring, and represents a six-membered ring structure selected from the group consisting of cyclohexadiene rings
  • each R 1 independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms
  • each R 2 independently represents a single bond or a carbon atom represents an alkanediyl group having 1 to 3 numbers
  • R 3 , R 4 , R 5 and R 6 each independently represent a hydrogen atom, a halogen atom, an alkyl group having 1 to 4 carbon atoms, or 1 to 4 carbon atoms
  • 4 alkoxy group, two of R 3 , R 4 , R 5 and R 6 may form an aliphatic ring, an aromatic ring or a bridged structure.
  • each M independently represents a hydrogen atom or a monovalent cation.
  • Monovalent cations include, for example, lithium, sodium, potassium, and ammonium ions.
  • M is preferably a hydrogen atom or a sodium ion.
  • each Cy surrounded by a hexagon independently represents a six-membered ring structure selected from the group consisting of a benzene ring, a cyclohexane ring, a cyclohexene ring, and a cyclohexadiene ring.
  • the position of the double bond in the cyclohexene ring and cyclohexadiene ring is not particularly limited. In one embodiment, there is a double bond between the carbon atom of the six membered ring structure to which the amide group is attached and the carbon atom of the six membered ring structure to which the carboxylate group is attached.
  • Cy surrounded by a hexagon is preferably a benzene ring or a cyclohexene ring.
  • each R 1 independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
  • alkyl groups having 1 to 4 carbon atoms include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group and t-butyl group.
  • R 1 is preferably a hydrogen atom, a methyl group, or an ethyl group, more preferably a hydrogen atom.
  • each R 2 independently represents a single bond or an alkanediyl group having 1 to 3 carbon atoms.
  • alkanediyl group having 1 to 3 carbon atoms include a methanediyl group (—CH 2 —), an ethane-1,2-diyl group (—CH 2 CH 2 —), an ethane-1,1-diyl group ( —CH(CH 3 )—), propane-1,3-diyl group (—CH 2 CH 2 CH 2 —), propane-1,2-diyl group (—CH 2 CH(CH 3 )—), and propane A -2,2-diyl group (-C(CH 3 ) 2 -) can be mentioned.
  • R2 is preferably a single bond or a methanediyl group, more preferably a methanediyl group.
  • R 3 , R 4 , R 5 and R 6 each independently represent a hydrogen atom, a halogen atom, an alkyl group having 1 to 4 carbon atoms, or an alkoxy group having 1 to 4 carbon atoms.
  • Halogen atoms include fluorine, chlorine, bromine and iodine.
  • alkyl groups having 1 to 4 carbon atoms include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group and t-butyl group.
  • alkoxy groups having 1 to 4 carbon atoms include methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, sec-butoxy, and t-butoxy groups.
  • R 3 , R 4 , R 5 and R 6 are preferably a hydrogen atom, a methyl group, an ethyl group, a methoxy group or an ethoxy group, more preferably a hydrogen atom.
  • two groups among R 3 , R 4 , R 5 and R 6 may form an aliphatic ring, an aromatic ring or a bridged structure. In one embodiment, adjacent two groups of R 3 , R 4 , R 5 and R 6 form an aliphatic or aromatic ring.
  • Cy is a benzene ring and R 4 and R 5 form a benzene ring as an aromatic ring
  • Cy is a cyclohexene ring and R 4 and R 5 form a cyclohexane ring as an aliphatic ring
  • the cyclohexene ring to which the amide group and the carboxylate group are bonded together with the octahydro forms a naphthalene ring.
  • two groups of R 3 , R 4 , R 5 and R 6 form a bridge structure.
  • Cy is a cyclohexane ring and R 3 and R 6 form a bridged structure with a methanediyl group (--CH 2 --), they form a norbornane ring (bicyclo[2.2.1]heptane ring).
  • the aliphatic ring, aromatic ring or bridged structure formed by two groups are halogen atoms, alkyl groups having 1 to 4 carbon atoms, and carbon atoms. It may have one or more substituents selected from the group consisting of 1 to 4 alkoxy groups.
  • a plurality of substituents may be the same or different. Exemplary and suitable substituents are the same as those described for R 3 , R 4 , R 5 and R 6 .
  • the total number of carbon atoms in the formed ring structure is preferably 8-18.
  • a in formula (2) is an amide bond, specifically a group represented by the formula: -NRCO- (R is a hydrogen atom or a monovalent group).
  • R is a hydrogen atom or a monovalent group.
  • each R 7 independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
  • alkyl groups having 1 to 4 carbon atoms include methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group and t-butyl group.
  • R7 is preferably a hydrogen atom, a methyl group, or an ethyl group, more preferably a hydrogen atom.
  • the carbonyl carbon of the amide bond is bonded to the carbon atom of the six-membered ring structure.
  • the nitrogen atom of the amide bond is bonded to the carbon atom of the six-membered ring structure.
  • Such a difference in bonding mode of the amide bond changes the lower critical solution temperature of the temperature-responsive polymer.
  • the temperature-responsive polymer containing the structural unit represented by formula (2a) is higher than the temperature-responsive polymer containing the structural unit represented by formula (2b), which has an equivalent structure other than the bonding mode of the amide bond. It often exhibits a high lower critical solution temperature.
  • the temperature responsiveness of the temperature responsive polymer can also be changed by selecting the form of the amide bond.
  • the structural unit of formula (2) comprises or consists of a structural unit of formula (3a).
  • M, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 and R 7 are the same as in formula (2a).
  • the structural unit of formula (2) comprises or consists of a structural unit of formula (4a).
  • M, R 1 , R 2 , R 3 , R 4 , R 5 , R 6 and R 7 are the same as in formula (2a).
  • the temperature-responsive polymer may be a homopolymer or a copolymer.
  • the structural unit represented by formula (1) or formula (2) contained in the temperature-responsive polymer is preferably 5 mol% or more, more preferably 20 mol % or more, more preferably 50 mol % or more. When the temperature-responsive polymer contains 5 mol % or more of the above structural units in total, temperature-responsiveness can be imparted to the temperature-responsive polymer.
  • the structural unit represented by formula (1) or formula (2) contained in the temperature-responsive polymer is 100 mol% or less, 90 mol% or less, or 80 mol% when expressed as a molar ratio based on all structural units. It can be mol % or less.
  • the weight average molecular weight of the temperature-responsive polymer is preferably 5,000 to 1,000,000, more preferably 7,500 to 500,000, still more preferably 10,000 to 100,000.
  • weight average molecular weight means molecular weight converted to standard polystyrene by gel permeation chromatography (GPC).
  • the temperature-responsive polymer has the same polymer main chain as the temperature-responsive polymer, and has functional groups A 1 such as hydroxyl groups, amino groups, carboxy groups, alkoxycarbonyl groups, and isocyanato groups.
  • a precursor polymer having can be done.
  • a compound A3 having a site that reacts with both functional group A1 and functional group A2 may be used.
  • the pendant reagent may be an acid anhydride in which A2 and COOM are intramolecularly condensed.
  • a catalyst or a dehydration condensation agent may be used to advance the above reaction.
  • n is the degree of polymerization of the precursor polymer, preferably 20-5,000, more preferably 30-2,500, still more preferably 40-500.
  • Formula (1A) represents a temperature-responsive polymer.
  • a temperature-responsive polymer in which A is an amide bond can be obtained by reacting a precursor polymer having an amino group with an acid anhydride or acid halide, or by reacting a precursor polymer having a carboxy group or an alkoxycarbonyl group. It can be obtained by reacting a polymer with an amine.
  • the temperature-responsive polymer in which A is an ester bond reacts a precursor polymer having a hydroxyl group with an acid anhydride or an acid halide, or reacts with a precursor polymer having a carboxy group or an alkoxycarbonyl group. It can be obtained by reacting with a hydroxyl group-containing compound.
  • the temperature-responsive polymer in which A is a carbonate bond is obtained by reacting a precursor polymer having a hydroxyl group, a hydroxyl group-containing compound, and a carbonate compound such as dimethyl carbonate, diethyl carbonate, or diphenyl carbonate. be able to.
  • the temperature-responsive polymer in which A is a urethane bond reacts a precursor polymer having a hydroxyl group with an isocyanato group-containing compound, or reacts a precursor polymer having an isocyanato group with a hydroxyl group-containing compound.
  • the temperature-responsive polymer in which A is a urea bond is obtained by reacting a precursor polymer having an amino group with an isocyanato group-containing compound, or reacting a precursor polymer having an isocyanato group with an amine.
  • the temperature-responsive polymer in which A is a urea bond is obtained by reacting a precursor polymer having an amino group with an isocyanato group-containing compound, or reacting a precursor polymer having an isocyanato group with an amine.
  • the temperature-responsive polymer can also be obtained by radically polymerizing polymerizable monomers corresponding to structural units of the temperature-responsive polymer, as schematically shown in the reaction formula below.
  • a radical polymerization initiator may be used to initiate the radical polymerization.
  • COOM may be protected once with a protective agent prior to radical polymerization and deprotected and regenerated after radical polymerization is complete.
  • n is the degree of polymerization of the precursor polymer, preferably 20-5,000, more preferably 30-2,500, still more preferably 40-500.
  • Formula (1A) represents a temperature-responsive polymer.
  • a method for producing a temperature-responsive polymer containing a structural unit represented by formula (2) will be described in detail below for illustrative purposes.
  • a person skilled in the art of organic synthesis and polymer synthesis can appropriately produce a temperature-responsive polymer containing structural units other than those represented by formula (2) by referring to the following description.
  • a precursor polymer having an amino group represented by formula (5) such as polyvinylamine or polyallylamine
  • a phthalic anhydride compound represented by formula (6a) or 3 represented by formula (7a) is combined with a phthalic anhydride compound represented by formula (6a) or 3 represented by formula (7a).
  • a temperature-responsive polymer represented by Formula (3A) or Formula (4A) can be obtained.
  • R 1 and R 2 are as described for formula (2)
  • R 7 is as described for formula (2a).
  • n is the degree of polymerization of the precursor polymer, preferably 20-5,000, more preferably 30-2,500, still more preferably 40-500.
  • R 3 , R 4 , R 5 and R 6 in formulas (6a) and (7a) are as described for formula (2).
  • the precursor polymer having amino groups may be in the form of having free amino groups or in the form of salts such as hydrochlorides, hydrobromides, sulfates, phosphates and acetates.
  • the precursor polymer having amino groups is preferably selected from the group consisting of polyvinylamine and polyallylamine, more preferably polyallylamine.
  • polyvinylamine and its salt is publicly known.
  • polyvinylamine is obtained by polymerizing N-vinylformamide using an azo initiator or the like as a polymerization initiator and hydrolyzing the resulting polyvinylformamide. can be obtained.
  • a method for producing polyallylamine and its salt is publicly known.
  • an inorganic acid salt of monoallylamine is dissolved in a polar solvent with an azo group and a cationic nitrogen in the molecule.
  • An inorganic acid salt of polyallylamine can be obtained by polymerizing in the presence of a radical initiator containing a group having an atom, or a specific azo initiator.
  • Polyallylamine may be obtained by dialyzing the resulting inorganic acid salt of polyallylamine.
  • polyvinylamine includes PVAM (manufactured by Mitsubishi Chemical Corporation).
  • polyallylamine and salts thereof include the PAA (registered trademark) series (manufactured by Nittobo Medical Co., Ltd.).
  • the reaction between the precursor polymer and the acid anhydride compound is carried out by dissolving the precursor polymer in a buffer solution such as carbonate buffer solution, and adjusting the pH of the buffer solution to 9 to 10 using an alkaline compound such as sodium hydroxide or potassium hydroxide. It can be carried out by adding the acid anhydride compound at 10° C. to 50° C. with adjustment.
  • the reaction time can be appropriately determined depending on the reactivity of the acid anhydride compound and the amount used, and can be, for example, 10 minutes to 48 hours. Thereafter, salt exchange is performed using sodium chloride or the like as necessary, and post-treatments such as dialysis and freeze-drying are performed to obtain a temperature-responsive polymer.
  • n is the degree of polymerization of the temperature-responsive polymer, preferably 20-5,000, more preferably 30-2,500, still more preferably 40-500.
  • the ethylenically unsaturated monomer represented by formula (6b) is, for example, methacrylic acid (where R 1 is a methyl group and R 2 is a single bond) or acrylic acid (where R 1 is a hydrogen atom and R 2 is a single bond). case) and the amino group of an anthranilic acid ester compound corresponding to the structure shown in formula (6b), such as anthranilic acid methyl ester, to form an amide bond to hydrolyze the ester of the anthranilic acid moiety.
  • the ethylenically unsaturated monomers represented by formula (6b) can, for example, replace the carboxyl group of methacrylic acid or acrylic acid with 1-hydroxybenzotriazole (HOBt), 1-hydroxy-7-azabenzotriazole (HOAt ), an alcohol such as ethyl(hydroxyimino)cyanoacetate, and a dehydrating reagent such as water-soluble carbodiimide, and then condensed with the amino group of the anthranilic acid compound corresponding to the structure shown in formula (6b). It can also be obtained by performing a reaction.
  • HABt 1-hydroxybenzotriazole
  • HOAt 1-hydroxy-7-azabenzotriazole
  • an alcohol such as ethyl(hydroxyimino)cyanoacetate
  • a dehydrating reagent such as water-soluble carbodiimide
  • the monomer composition may further contain a monomer other than the ethylenically unsaturated monomer corresponding to the structural unit represented by formula (2).
  • monomers include vinyl compounds such as styrene, vinyl toluene, vinyl acetate, vinyl chloride and N-vinylpyrrolidone; ) acrylate compounds; and (meth)acrylamide compounds such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, and N-isopropyl(meth)acrylamide.
  • (meth)acrylic means acrylic or methacrylic
  • “(meth)acrylate” means acrylate or methacrylate.
  • the copolymerization ratio of these monomers can be appropriately determined within a range that does not impair the temperature responsiveness of the temperature responsive polymer.
  • Radical polymerization can be carried out in an organic solvent using a known radical polymerization initiator.
  • radical polymerization initiators include organic peroxides such as benzoyl peroxide, cumene peroxide, and di-t-butyl peroxide; 2,2′-azobisisobutyronitrile, 2,2′-azobis ( 2,4-dimethylvaleronitrile), 2,2′-azobis(4-methoxy-2,4-dimethylvaleronitrile) and other azo compounds; and redox initiators.
  • a radical polymerization initiator may be used alone or in combination of two or more.
  • the amount of the radical polymerization initiator used is preferably 0.1-20 mol %, more preferably 0.5-10 mol %, relative to the total monomers in the monomer composition.
  • organic solvents examples include ketones such as acetone and methyl ethyl ketone (MEK); alcohols such as ethanol, methanol and isopropyl alcohol (IPA); ethers such as ethylene glycol dimethyl ether and propylene glycol monomethyl ether; ethyl acetate and propylene glycol monomethyl ether acetate. , 2-ethoxyethyl acetate; aromatic hydrocarbons such as toluene and xylene; sulfoxides such as dimethylsulfoxide; and amides such as dimethylformamide and dimethylacetamide.
  • An organic solvent may be used independently and may use 2 or more types together.
  • the polymerization temperature is preferably 20-100°C, more preferably 30-80°C.
  • the polymerization time can be appropriately determined according to the desired molecular weight, and can be, for example, 10 minutes to 120 hours.
  • Water-based temperature-responsive composition An embodiment of the water-based temperature-responsive composition contains the above temperature-responsive polymer and polyvalent cations. Water-based temperature-responsive compositions generally have reversible temperature responsiveness.
  • the water-based temperature-responsive composition contains water as a solvent.
  • the water-based temperature-responsive composition may further contain an organic solvent as a solvent.
  • organic solvents include alcohols such as methanol, ethanol, n-propanol and isopropanol, ethers such as diethyl ether and tetrahydrofuran, esters such as ethyl acetate and butyl acetate, sulfoxides such as dimethylsulfoxide, dimethylformamide, and dimethylacetamide. and amides of In embodiments in which the solvent contains an organic solvent, the content of the organic solvent is preferably 0.1% by mass to 50% by mass, more preferably 0.2% by mass to 100% by mass. 30 mass %, more preferably 0.5 mass % to 20 mass %.
  • Polyvalent cations determine the conformation of the temperature-responsive polymer by interacting with two or more carboxylate groups on the side chains of the temperature-responsive polymer, especially two or more carboxylate groups within the polymer molecule. , the conformation of temperature-responsive polymers is thought to change with temperature. Since each polyvalent cation has its own hydration Gibbs energy, changing the type of polyvalent cation changes the hydration state of the temperature-responsive polymer. Therefore, the LCST of the temperature-responsive polymer can be adjusted by properly using polyvalent cations. Polyvalent cations may be used alone or in combination of two or more. By using two or more polyvalent cations together and appropriately determining the ratio thereof, the LCST of the temperature-responsive polymer can be adjusted more precisely.
  • polyvalent cations include, but are not limited to, divalent cations such as magnesium ions, calcium ions, strontium ions, and barium ions. More preferably, the polyvalent cation contains at least one selected from the group consisting of magnesium ions, calcium ions, and strontium ions.
  • the polyvalent cation is a calcium ion.
  • the LCST of the temperature-responsive polymer can also be adjusted by changing the concentration of polyvalent cations. In one embodiment, when the concentration of polyvalent cations reaches a certain value (saturation concentration) or higher, the LCST of the temperature-responsive polymer hardly changes.
  • concentration of polyvalent cations can be appropriately determined according to the types of temperature-responsive polymer and polyvalent cations used, and the desired LCST.
  • the concentration of polyvalent cations can be, for example, but not limited to, 0.01 mM to 1000 mM, 0.1 mM to 500 mM, or 0.5 mM to 250 mM.
  • the concentration of the temperature-responsive polymer has little effect on the LCST of the temperature-responsive polymer. This suggests that conformational changes of molecular chains are more dominant in temperature responsiveness than intermolecular interactions of temperature responsive polymers.
  • the concentration of the temperature responsive polymer can be, for example, 0.1 mg/mL to 20 mg/mL, 0.2 mg/mL to 10 mg/mL, or 0.4 mg/mL to 5 mg/mL, but is limited to these. not.
  • the LCST of the temperature-responsive polymer can also be adjusted by changing the pH of the water-based temperature-responsive composition.
  • pH regions eg, pH 6 and above
  • interactions between the carboxylate groups of the temperature responsive polymer and multivalent cations affect the conformation of the temperature responsive polymer.
  • a lower pH region for example pH 5 or less
  • the carboxylate groups of the temperature-responsive polymer are protonated to carboxy groups, and the hydrogen bonding between the carboxy groups rather than the interaction between the carboxylate groups and polyvalent cations is responsible for the temperature response. affect sexuality.
  • the pH of the water-based temperature-responsive composition is preferably 4-9, more preferably 4.5-8, still more preferably 5-7.5.
  • the water-based temperature-responsive composition may contain monovalent cations within a range that does not impair the LCST of the temperature-responsive polymer.
  • Monovalent cations include, for example, lithium, sodium, potassium, and ammonium ions.
  • the concentration of monovalent cations is preferably 1000 mM or less, more preferably 500 mM or less, and even more preferably 150 mM or less.
  • the LCST of the water-based temperature-responsive composition is adjusted by one or more of the side chain structure of the temperature-responsive polymer, the type and concentration of polyvalent cations, and the pH of the water-based temperature-responsive composition. can be done.
  • the water-based temperature-responsive composition has an LCST of 25°C to 80°C.
  • the LCST of the aqueous temperature-responsive composition is preferably 30°C to 42°C, more preferably 35°C to 40°C.
  • LCST measures the transmittance of a water-based temperature-responsive composition under the conditions of a measurement wavelength of 500 nm and a heating rate of 1 ° C./min to create a graph, in which the vertical axis is transmittance (%) and the horizontal axis is is defined as the temperature at which the transmittance becomes 90% from the graph where is the temperature (°C).
  • the water-based temperature-responsive composition can be prepared by dissolving the temperature-responsive polymer and the polyvalent cation source in a solvent containing water and, if necessary, an organic solvent.
  • polyvalent cation sources include salts containing polyvalent cation elements.
  • salts include chlorides such as calcium chloride, magnesium chloride and strontium chloride; sulfates such as calcium sulfate, magnesium sulfate and strontium sulfate; and phosphates such as calcium phosphate, magnesium phosphate and strontium phosphate. is mentioned.
  • the temperature-responsive polymer and water-based temperature-responsive composition of the present disclosure are suitable for use in water-based functional materials such as functional cell sheets, drug transport carriers, mechanochemical materials, temperature sensors, separation membranes, and water retention agents. can be used.
  • Synthesis of PAA-Pht Polyallylamine hydrochloride (PAA-HCl, polyallylamine weight average molecular weight Mw 15,000, manufactured by Nittobo Medical Co., Ltd.) was dissolved in a carbonate buffer solution to a concentration of 2.5 mg/mL. The pH of the solution was adjusted to 9.5 using aqueous sodium hydroxide. Three equivalents of phthalic anhydride relative to the side chain amino groups of the polyallylamine were added in increments of one equivalent every hour. The pH of the solution was adjusted to 9.5 after each addition of phthalic anhydride.
  • PAA-HCl polyallylamine weight average molecular weight Mw 15,000, manufactured by Nittobo Medical Co., Ltd.
  • PAA-Pht has the following structural units.
  • M is Na.
  • Synthesis Example 2 Synthesis of PAA-CHex PAA-HCl used in Synthesis Example 1 was dissolved in a carbonate buffer solution to a concentration of 2.5 mg/mL, and the pH of the solution was adjusted to 9.5 using an aqueous sodium hydroxide solution. adjusted to 3 equivalents of 1-cyclohexene-1,2-dicarboxylic anhydride relative to the side chain amino groups of polyallylamine were added in increments of 1 equivalent every hour. The pH of the solution was adjusted to 9.5 each time 1-cyclohexene-1,2-dicarboxylic anhydride was added. After stirring for 24 hours, sodium chloride was added in an amount of 100 molar equivalents to the side chain amino groups of the polyallylamine, and the mixture was stirred overnight.
  • PAA-CHex has the following structural units.
  • M is Na.
  • the transmittance was measured using an ultraviolet-visible-near-infrared spectrophotometer V-550 (manufactured by JASCO Corporation).
  • Sodium chloride, magnesium chloride, calcium chloride and strontium chloride were used as cation sources.
  • PAA-Pht does not exhibit temperature responsiveness in aqueous compositions that do not contain polyvalent cations or contain monovalent sodium ions.
  • PAA-Pht in aqueous compositions containing divalent calcium ions, PAA-Pht exhibits temperature responsiveness in which the transmittance sharply decreases at high temperatures from around 38.6°C.
  • Temperature-responsive behavior of PAA - Pht Effect of type of divalent cation .2, polymer concentration 4 mg/mL), and the change in transmittance was measured under the conditions of a measurement wavelength of 500 nm and a heating rate of 1° C./min.
  • the measurement results are shown in FIG. 8A as a graph with transmittance (%) on the vertical axis and temperature (° C.) on the horizontal axis.
  • LCST the temperature at which the transmittance becomes 90% was determined from the graph shown in FIG. 8A.
  • FIG. 8B shows a graph in which the vertical axis is the LCST (° C.) and the horizontal axis is the absolute value (kJ/mol) of hydration Gibbs energies ( ⁇ hyd G) of Mg 2+ , Ca 2+ , and Sr 2+ .
  • PAA-CHex also exhibits temperature responsiveness in water in the presence of polyvalent cations, and the LCST is slightly low. Also, it can be seen that the LCST sharply decreases as the calcium ion concentration increases from 0 mM, but changes in the LCST are small when the calcium ion concentration exceeds 60 mM.
  • the temperature-responsive polymer and water-based temperature-responsive composition of the present disclosure are suitable for use in water-based functional materials such as functional cell sheets, drug transport carriers, mechanochemical materials, temperature sensors, separation membranes, and water retention agents. can be used.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Organic Chemistry (AREA)
  • General Chemical & Material Sciences (AREA)
  • Addition Polymer Or Copolymer, Post-Treatments, Or Chemical Modifications (AREA)
PCT/JP2022/016157 2021-04-23 2022-03-30 温度応答性ポリマー及び水系温度応答性組成物 Ceased WO2022224778A1 (ja)

Priority Applications (1)

Application Number Priority Date Filing Date Title
JP2023516404A JP7873499B2 (ja) 2021-04-23 2022-03-30 温度応答性ポリマー及び水系温度応答性組成物

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2021-073565 2021-04-23
JP2021073565 2021-04-23

Publications (1)

Publication Number Publication Date
WO2022224778A1 true WO2022224778A1 (ja) 2022-10-27

Family

ID=83722215

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2022/016157 Ceased WO2022224778A1 (ja) 2021-04-23 2022-03-30 温度応答性ポリマー及び水系温度応答性組成物

Country Status (2)

Country Link
JP (1) JP7873499B2 (cg-RX-API-DMAC7.html)
WO (1) WO2022224778A1 (cg-RX-API-DMAC7.html)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2026076489A1 (en) * 2024-10-09 2026-04-16 The Regents Of The University Of California Electrochemical temperature measurement using redox-active polymers

Citations (11)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH06279549A (ja) * 1992-11-23 1994-10-04 Elf Atochem Sa 硬化可能な粉末状フッ素化共重合体と、その製造方法と、粉末塗装へのその利用
JPH0912817A (ja) * 1995-06-23 1997-01-14 Elf Atochem Sa 自己架橋性ワニス及び塗料用結合剤
JPH09157235A (ja) * 1995-12-13 1997-06-17 Mitsui Toatsu Chem Inc 新規n−アリル置換フタル酸ハーフアミド化合物
JPH09202755A (ja) * 1996-01-26 1997-08-05 Mitsui Toatsu Chem Inc N−アリル置換メチルエンドメチレンテトラヒドロフタル酸ハーフアミド化合物
JPH09202756A (ja) * 1996-01-26 1997-08-05 Mitsui Toatsu Chem Inc N−アリル置換メチルテトラヒドロフタル酸ハーフアミド化合物
JP2003262957A (ja) * 2002-03-07 2003-09-19 Fuji Photo Film Co Ltd 感光性着色組成物、カラーフィルタ及びその製造方法
JP2003270784A (ja) * 2002-03-14 2003-09-25 Fuji Photo Film Co Ltd 着色感光性組成物、カラーフィルタ及びその製造方法
JP2004163853A (ja) * 2002-09-25 2004-06-10 Fuji Photo Film Co Ltd 画像記録材料
JP2005208366A (ja) * 2004-01-23 2005-08-04 Fuji Photo Film Co Ltd ポジ型レジスト組成物及びそれを用いたパターン形成方法
JP2012073598A (ja) * 2010-08-31 2012-04-12 Fujifilm Corp 感光性組成物、感光性フィルム、感光性積層体、永久パターン形成方法、及びプリント基板
JP2021175792A (ja) * 2020-04-28 2021-11-04 信越化学工業株式会社 ヨウ素化芳香族カルボン酸型ペンダント基含有ポリマー、レジスト材料及びパターン形成方法

Patent Citations (11)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH06279549A (ja) * 1992-11-23 1994-10-04 Elf Atochem Sa 硬化可能な粉末状フッ素化共重合体と、その製造方法と、粉末塗装へのその利用
JPH0912817A (ja) * 1995-06-23 1997-01-14 Elf Atochem Sa 自己架橋性ワニス及び塗料用結合剤
JPH09157235A (ja) * 1995-12-13 1997-06-17 Mitsui Toatsu Chem Inc 新規n−アリル置換フタル酸ハーフアミド化合物
JPH09202755A (ja) * 1996-01-26 1997-08-05 Mitsui Toatsu Chem Inc N−アリル置換メチルエンドメチレンテトラヒドロフタル酸ハーフアミド化合物
JPH09202756A (ja) * 1996-01-26 1997-08-05 Mitsui Toatsu Chem Inc N−アリル置換メチルテトラヒドロフタル酸ハーフアミド化合物
JP2003262957A (ja) * 2002-03-07 2003-09-19 Fuji Photo Film Co Ltd 感光性着色組成物、カラーフィルタ及びその製造方法
JP2003270784A (ja) * 2002-03-14 2003-09-25 Fuji Photo Film Co Ltd 着色感光性組成物、カラーフィルタ及びその製造方法
JP2004163853A (ja) * 2002-09-25 2004-06-10 Fuji Photo Film Co Ltd 画像記録材料
JP2005208366A (ja) * 2004-01-23 2005-08-04 Fuji Photo Film Co Ltd ポジ型レジスト組成物及びそれを用いたパターン形成方法
JP2012073598A (ja) * 2010-08-31 2012-04-12 Fujifilm Corp 感光性組成物、感光性フィルム、感光性積層体、永久パターン形成方法、及びプリント基板
JP2021175792A (ja) * 2020-04-28 2021-11-04 信越化学工業株式会社 ヨウ素化芳香族カルボン酸型ペンダント基含有ポリマー、レジスト材料及びパターン形成方法

Non-Patent Citations (1)

* Cited by examiner, † Cited by third party
Title
PONCE-VARGAS SANDRA M., CORTEZ-LEMUS NORMA A., LICEA-CLAVERÍE ANGEL: "Preparation of Poly( N -Vinylcaprolactam) (NVCL) and Statistical Copolymers of NVCL with Variable Cloud Point Temperature by Using A Trithiocarbonate RAFT Agent", MACROMOLECULAR SYMPOSIA, WILEY VCH VERLAG WEINHEIM, DE, vol. 325-326, no. 1, 1 March 2013 (2013-03-01), DE , pages 56 - 70, XP055978954, ISSN: 1022-1360, DOI: 10.1002/masy.201200045 *

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2026076489A1 (en) * 2024-10-09 2026-04-16 The Regents Of The University Of California Electrochemical temperature measurement using redox-active polymers

Also Published As

Publication number Publication date
JP7873499B2 (ja) 2026-06-12
JPWO2022224778A1 (cg-RX-API-DMAC7.html) 2022-10-27

Similar Documents

Publication Publication Date Title
JP6239043B2 (ja) 包接錯体、自己修復性及び形状記憶性を有するゲル
Wang et al. Synthesis and evaluation of new dicarboxylic acid functional trithiocarbonates: RAFT synthesis of telechelic poly (n-butyl acrylate) s
ES2382574T3 (es) Aductos de adición de Michael como aditivos para papel y fabricación de papel
US11472903B2 (en) Composition for polymerization, polymer of same and method for producing polymer
WO2020179908A1 (ja) 高分子材料及びその製造方法
US20080234391A1 (en) Synthesis of Reversible Shell Crosslinked Nanostructures
CN105164169A (zh) 通过转酰胺化制备高分子量、官能化的聚(甲基)丙烯酰胺聚合物
JP2006249130A5 (cg-RX-API-DMAC7.html)
Suchao-In et al. pH-and thermo-multi-responsive fluorescent micelles from block copolymers via reversible addition fragmentation chain transfer (RAFT) polymerization
Koromilas et al. Synthesis of antimicrobial block copolymers bearing immobilized bacteriostatic groups
JPS59189113A (ja) ポリビニルアルコ−ル系重合体を一成分とするブロツク共重合体の製法
JPS6312485B2 (cg-RX-API-DMAC7.html)
WO2022005775A1 (en) Hydrate inhibitors
CN114502603A (zh) 可降解聚合物材料
WO2023099310A1 (en) Preparation of high solid content, surfactant-free latex using functional amphiphilic waterborne macro-raft agent
JP7161657B2 (ja) 新規の高分子化合物
JP6522388B2 (ja) N−ビニルラクタム系共重合体および樹脂組成物
CN102858818B (zh) 用于生产二烯丙基胺乙酸盐聚合物的方法
JP7206612B2 (ja) ブロック共重合体
CN1261469C (zh) 疏水缔合水溶性共聚物及其制备方法
JPS60212410A (ja) マレイン酸塩共重合体の製造法
JPS59189114A (ja) ポリビニルエステル系重合体を一成分とするブロツク共重合体の製法
WO1994004725A1 (fr) Fibre a fort pouvoir d'absorption d'eau
CN111989310A (zh) 低聚烷氧基胺
JPWO1990008788A1 (ja) 保存性が改善されたn,n―ジアルキルアミノアルキル(メタ)アクリルアミド組成物

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 22791553

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2023516404

Country of ref document: JP

Kind code of ref document: A

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 22791553

Country of ref document: EP

Kind code of ref document: A1