WO2016186203A1 - Feuille mécano-luminescente - Google Patents

Feuille mécano-luminescente Download PDF

Info

Publication number
WO2016186203A1
WO2016186203A1 PCT/JP2016/065044 JP2016065044W WO2016186203A1 WO 2016186203 A1 WO2016186203 A1 WO 2016186203A1 JP 2016065044 W JP2016065044 W JP 2016065044W WO 2016186203 A1 WO2016186203 A1 WO 2016186203A1
Authority
WO
WIPO (PCT)
Prior art keywords
layer
stress
stimulated luminescent
sheet
retroreflective
Prior art date
Application number
PCT/JP2016/065044
Other languages
English (en)
Japanese (ja)
Inventor
祐子 青山
博孝 増山
Original Assignee
大日本印刷株式会社
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 大日本印刷株式会社 filed Critical 大日本印刷株式会社
Priority to JP2017519416A priority Critical patent/JP6705448B2/ja
Publication of WO2016186203A1 publication Critical patent/WO2016186203A1/fr

Abstract

La présente invention concerne une feuille mécano-luminescente qui est excellente en termes d'effet de prévention de falsification et d'attractivité de conception. La présente invention concerne une feuille mécano-luminescente, caractérisée par le fait que cette dernière comprend : une base ; une couche de rétroréflexion formée sur une surface de la base et comprenant des particules de rétroréflexion et un matériau résineux ; et une couche mécano-luminescente formée sur la surface de la base qui est sur le côté inverse par rapport à la couche de rétroréflexion et comprenant des particules mécano-luminescentes et une résine liante.
PCT/JP2016/065044 2015-05-21 2016-05-20 Feuille mécano-luminescente WO2016186203A1 (fr)

Priority Applications (1)

Application Number Priority Date Filing Date Title
JP2017519416A JP6705448B2 (ja) 2015-05-21 2016-05-20 応力発光シート

Applications Claiming Priority (6)

Application Number Priority Date Filing Date Title
JP2015103985 2015-05-21
JP2015103975 2015-05-21
JP2015-103985 2015-05-21
JP2015-103978 2015-05-21
JP2015-103975 2015-05-21
JP2015103978 2015-05-21

Publications (1)

Publication Number Publication Date
WO2016186203A1 true WO2016186203A1 (fr) 2016-11-24

Family

ID=57320475

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2016/065044 WO2016186203A1 (fr) 2015-05-21 2016-05-20 Feuille mécano-luminescente

Country Status (2)

Country Link
JP (1) JP6705448B2 (fr)
WO (1) WO2016186203A1 (fr)

Cited By (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN107354419A (zh) * 2017-06-28 2017-11-17 中国航发北京航空材料研究院 一种石墨烯改性可视耐磨涂层的制备方法
CN107354420A (zh) * 2017-06-28 2017-11-17 中国航发北京航空材料研究院 制备残余应力涂层用石墨烯改性热喷涂粉末的制备方法
JP2021000744A (ja) * 2019-06-20 2021-01-07 大日本印刷株式会社 スレッド状印刷物および偽造防止用紙、並びにロールフィルム印刷物および偽造防止用紙の製造方法

Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2000511479A (ja) * 1996-05-20 2000-09-05 ミネソタ マイニング アンド マニュファクチャリング カンパニー タンパー指示多層シート
WO2007023869A1 (fr) * 2005-08-25 2007-03-01 National Institute Of Advanced Industrial Science And Technology Structure luminescente de contrainte

Patent Citations (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2000511479A (ja) * 1996-05-20 2000-09-05 ミネソタ マイニング アンド マニュファクチャリング カンパニー タンパー指示多層シート
WO2007023869A1 (fr) * 2005-08-25 2007-03-01 National Institute Of Advanced Industrial Science And Technology Structure luminescente de contrainte

Cited By (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN107354419A (zh) * 2017-06-28 2017-11-17 中国航发北京航空材料研究院 一种石墨烯改性可视耐磨涂层的制备方法
CN107354420A (zh) * 2017-06-28 2017-11-17 中国航发北京航空材料研究院 制备残余应力涂层用石墨烯改性热喷涂粉末的制备方法
CN107354419B (zh) * 2017-06-28 2020-03-17 中国航发北京航空材料研究院 一种石墨烯改性可视耐磨涂层的制备方法
CN107354420B (zh) * 2017-06-28 2020-05-19 中国航发北京航空材料研究院 制备残余应力涂层用石墨烯改性热喷涂粉末的制备方法
JP2021000744A (ja) * 2019-06-20 2021-01-07 大日本印刷株式会社 スレッド状印刷物および偽造防止用紙、並びにロールフィルム印刷物および偽造防止用紙の製造方法
JP7314643B2 (ja) 2019-06-20 2023-07-26 大日本印刷株式会社 スレッド状印刷物および偽造防止用紙、並びにロールフィルム印刷物および偽造防止用紙の製造方法

Also Published As

Publication number Publication date
JPWO2016186203A1 (ja) 2018-03-08
JP6705448B2 (ja) 2020-06-03

Similar Documents

Publication Publication Date Title
JP5608891B2 (ja) 光学的に変化する磁性顔料を含む転写箔、転写箔の製造方法、転写箔の使用、および転写箔を備える物品または書類
CN104349904B (zh) 用于印刷能触知的安全特征的方法
JP5686495B2 (ja) 光学的可変接着剤を組み込んだセキュリティ・デバイス
US9223235B2 (en) Fine particles, particle group, anti-counterfeiting ink, anti-counterfeiting toner, anti-counterfeiting sheet, and anti-counterfeiting medium
CN107000463B (zh) 安全元件、用于制造安全元件的方法和配有安全元件的数据载体
TWI509374B (zh) 由全息圖及變色墨水所形成之安全裝置
JP6981404B2 (ja) 偽造防止構造体
JP4273754B2 (ja) 偽造防止転写箔、偽造防止シール、及び、偽造防止媒体ならびにその製造方法
JP6705448B2 (ja) 応力発光シート
CN102083633B (zh) 成角度发光的安全元件及其制造方法
KR102345076B1 (ko) 정보 기록체, 및 개인 증명체
JP5880653B2 (ja) 微粒子含有シートの製造方法
JP2005506228A5 (fr)
JP4592964B2 (ja) 真正性識別体、真正性の識別可能な情報記録媒体および物品、並びに真正性識別性ラベルおよび転写シート
JP2004223975A (ja) 偽造防止媒体、情報表示媒体、偽造防止転写箔、偽造防止シール、及び、それらの製造方法
JP4138082B2 (ja) 中間転写記録媒体および印画物
CN115135511A (zh) 可uv固化且可热封的墨
JP2000318290A (ja) 偽造防止シート
JP6699656B2 (ja) ホログラムシート、応力発光シートおよび偽造防止用紙
JP2011104942A (ja) 積層表示体
CN108602339B (zh) 层叠体、层叠体的制造方法以及个人认证介质
JP6455076B2 (ja) ホログラム積層体および情報記録媒体
JP5771961B2 (ja) 微粒子含有シートの製造方法
JP2016215517A (ja) スクラッチシート
JP6024794B2 (ja) 微粒子含有シートの製造方法

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 16796596

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2017519416

Country of ref document: JP

Kind code of ref document: A

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 16796596

Country of ref document: EP

Kind code of ref document: A1