WO2013054593A1 - Procédé de fabrication d'électrode en forme de feuille, électrode en forme de feuille et accumulateur au lithium-ion - Google Patents

Procédé de fabrication d'électrode en forme de feuille, électrode en forme de feuille et accumulateur au lithium-ion Download PDF

Info

Publication number
WO2013054593A1
WO2013054593A1 PCT/JP2012/071036 JP2012071036W WO2013054593A1 WO 2013054593 A1 WO2013054593 A1 WO 2013054593A1 JP 2012071036 W JP2012071036 W JP 2012071036W WO 2013054593 A1 WO2013054593 A1 WO 2013054593A1
Authority
WO
WIPO (PCT)
Prior art keywords
electrode
sheet
cutting blade
cutting
width
Prior art date
Application number
PCT/JP2012/071036
Other languages
English (en)
Japanese (ja)
Inventor
鞍懸淳
山道裕司
阿部敏浩
黒石知樹
有吉英朗
Original Assignee
日立マクセルエナジー株式会社
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 日立マクセルエナジー株式会社 filed Critical 日立マクセルエナジー株式会社
Priority to JP2013538467A priority Critical patent/JP5768137B2/ja
Publication of WO2013054593A1 publication Critical patent/WO2013054593A1/fr

Abstract

L'invention concerne la fabrication d'une électrode en forme de feuille (1) par découpe d'un substrat d'électrode allongé (30) comportant une couche de mélange d'électrode (35) formée de manière intermittente sur au moins une surface d'un collecteur, l'électrode en forme de feuille comprenant une partie d'électrode sensiblement rectangulaire (20) sur laquelle la couche de mélange d'électrode est formée et une partie patte (27) comprenant une région dans laquelle la couche de mélange d'électrode n'est pas formée. Un procédé de fabrication de l'électrode en forme de feuille comprend : une étape consistant à former la partie patte de l'électrode en forme de feuille et un premier côté (21) à partir duquel la partie patte fait saillie en utilisant une première lame de découpe (41) ayant une largeur de coupe (W41) plus large que la largeur du substrat de l'électrode ; et une étape consistant à former un second côté (22), faisant face au premier côté de l'électrode en forme de feuille, en utilisant une seconde lame de coupe (42) ayant une largeur de coupe (W42) plus large que la largeur du substrat de l'électrode. Cela permet de fabriquer efficacement et à bas coût des électrodes en forme de feuille ayant des tailles différentes en utilisant les mêmes lames de coupe.
PCT/JP2012/071036 2011-10-14 2012-08-21 Procédé de fabrication d'électrode en forme de feuille, électrode en forme de feuille et accumulateur au lithium-ion WO2013054593A1 (fr)

Priority Applications (1)

Application Number Priority Date Filing Date Title
JP2013538467A JP5768137B2 (ja) 2011-10-14 2012-08-21 シート状電極の製造方法

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2011226881 2011-10-14
JP2011-226881 2011-10-14

Publications (1)

Publication Number Publication Date
WO2013054593A1 true WO2013054593A1 (fr) 2013-04-18

Family

ID=48081653

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2012/071036 WO2013054593A1 (fr) 2011-10-14 2012-08-21 Procédé de fabrication d'électrode en forme de feuille, électrode en forme de feuille et accumulateur au lithium-ion

Country Status (2)

Country Link
JP (1) JP5768137B2 (fr)
WO (1) WO2013054593A1 (fr)

Cited By (17)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2015146232A (ja) * 2014-01-31 2015-08-13 株式会社豊田自動織機 電極の製造方法及び電極
WO2016006420A1 (fr) * 2014-07-10 2016-01-14 株式会社村田製作所 Procédé de fabrication d'un dispositif de stockage d'énergie et procédé de fabrication d'électrode
JP2016502742A (ja) * 2013-03-08 2016-01-28 エルジー・ケム・リミテッド ラウンドコーナーを含む電極組立体
KR20160023072A (ko) * 2014-08-21 2016-03-03 주식회사 엘지화학 전극 조립체의 제조방법 및 이를 이용하여 제조된 전극 조립체
US9478773B2 (en) 2012-03-16 2016-10-25 Lg Chem, Ltd. Battery cell of asymmetric structure and battery pack employed with the same
US9484560B2 (en) 2013-02-13 2016-11-01 Lg Chem, Ltd. Electric device having a round corner and including a secondary battery
US9548517B2 (en) 2012-04-05 2017-01-17 Lg Chem, Ltd. Battery cell of stair-like structure
US9620789B2 (en) 2012-03-08 2017-04-11 Lg Chem, Ltd. Battery pack of the stair-like structure
US9685679B2 (en) 2012-05-29 2017-06-20 Lg Chem, Ltd. Stepwise electrode assembly having variously-shaped corner and secondary battery, battery pack and device comprising the same
US9786874B2 (en) 2013-03-08 2017-10-10 Lg Chem, Ltd. Electrode having round corner
US9954203B2 (en) 2013-03-08 2018-04-24 Lg Chem, Ltd. Stepped electrode group stack
US10026994B2 (en) 2012-11-13 2018-07-17 Lg Chem, Ltd. Stepped electrode assembly
CN108565387A (zh) * 2018-03-21 2018-09-21 中航锂电技术研究院有限公司 一种锂离子电池电芯极耳激光成型工艺
JP2020149921A (ja) * 2019-03-15 2020-09-17 Tdk株式会社 非水電解質二次電池用負極及びこれを用いた非水電解質二次電池
US11114652B2 (en) 2017-03-13 2021-09-07 Lg Chem, Ltd. Method for manufacturing secondary battery electrode, and secondary battery electrode manufactured thereby
US11271212B1 (en) * 2021-04-02 2022-03-08 Ses Holdings Pte. Ltd. Anode fabrication by pattern lamination, anodes made thereby, and electrochemical devices incorporating such anodes
JP7411161B2 (ja) 2020-03-31 2024-01-11 株式会社Gsユアサ 蓄電素子

Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH10270014A (ja) * 1997-03-27 1998-10-09 Fuji Film Selltec Kk シート状電極とこれを用いた電池
JP2009181876A (ja) * 2008-01-31 2009-08-13 Ohara Inc リチウムイオン二次電池用積層体の製造方法
JP2011034918A (ja) * 2009-08-05 2011-02-17 Murata Mfg Co Ltd 積層型二次電池用極板の製造方法と積層型二次電池用極板材料
JP2011086505A (ja) * 2009-10-15 2011-04-28 Komatsu Ntc Ltd 積層型電池用電極材および積層型電池

Family Cites Families (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2783811B2 (ja) * 1988-08-20 1998-08-06 三洋電機株式会社 電池及びその極板の製造方法
JP2001160397A (ja) * 1999-12-02 2001-06-12 Sony Corp カード形固体電池用集電体の成形方法及び成形装置

Patent Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH10270014A (ja) * 1997-03-27 1998-10-09 Fuji Film Selltec Kk シート状電極とこれを用いた電池
JP2009181876A (ja) * 2008-01-31 2009-08-13 Ohara Inc リチウムイオン二次電池用積層体の製造方法
JP2011034918A (ja) * 2009-08-05 2011-02-17 Murata Mfg Co Ltd 積層型二次電池用極板の製造方法と積層型二次電池用極板材料
JP2011086505A (ja) * 2009-10-15 2011-04-28 Komatsu Ntc Ltd 積層型電池用電極材および積層型電池

Cited By (24)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US9620789B2 (en) 2012-03-08 2017-04-11 Lg Chem, Ltd. Battery pack of the stair-like structure
US9478773B2 (en) 2012-03-16 2016-10-25 Lg Chem, Ltd. Battery cell of asymmetric structure and battery pack employed with the same
US9548517B2 (en) 2012-04-05 2017-01-17 Lg Chem, Ltd. Battery cell of stair-like structure
US9685679B2 (en) 2012-05-29 2017-06-20 Lg Chem, Ltd. Stepwise electrode assembly having variously-shaped corner and secondary battery, battery pack and device comprising the same
US10026994B2 (en) 2012-11-13 2018-07-17 Lg Chem, Ltd. Stepped electrode assembly
US9484560B2 (en) 2013-02-13 2016-11-01 Lg Chem, Ltd. Electric device having a round corner and including a secondary battery
US9786874B2 (en) 2013-03-08 2017-10-10 Lg Chem, Ltd. Electrode having round corner
JP2016502742A (ja) * 2013-03-08 2016-01-28 エルジー・ケム・リミテッド ラウンドコーナーを含む電極組立体
US9954203B2 (en) 2013-03-08 2018-04-24 Lg Chem, Ltd. Stepped electrode group stack
JP2015146232A (ja) * 2014-01-31 2015-08-13 株式会社豊田自動織機 電極の製造方法及び電極
JPWO2016006420A1 (ja) * 2014-07-10 2017-05-25 株式会社村田製作所 蓄電デバイスの製造方法及び電極の製造方法
JP2017152395A (ja) * 2014-07-10 2017-08-31 株式会社村田製作所 蓄電デバイスの製造方法及び電極の製造方法
WO2016006420A1 (fr) * 2014-07-10 2016-01-14 株式会社村田製作所 Procédé de fabrication d'un dispositif de stockage d'énergie et procédé de fabrication d'électrode
KR20160023072A (ko) * 2014-08-21 2016-03-03 주식회사 엘지화학 전극 조립체의 제조방법 및 이를 이용하여 제조된 전극 조립체
KR101664945B1 (ko) 2014-08-21 2016-10-11 주식회사 엘지화학 전극 조립체의 제조방법 및 이를 이용하여 제조된 전극 조립체
US11114652B2 (en) 2017-03-13 2021-09-07 Lg Chem, Ltd. Method for manufacturing secondary battery electrode, and secondary battery electrode manufactured thereby
CN108565387A (zh) * 2018-03-21 2018-09-21 中航锂电技术研究院有限公司 一种锂离子电池电芯极耳激光成型工艺
CN111697196A (zh) * 2019-03-15 2020-09-22 Tdk株式会社 非水电解质二次电池用负极及使用其的非水电解质二次电池
JP2020149921A (ja) * 2019-03-15 2020-09-17 Tdk株式会社 非水電解質二次電池用負極及びこれを用いた非水電解質二次電池
JP7411161B2 (ja) 2020-03-31 2024-01-11 株式会社Gsユアサ 蓄電素子
US11271212B1 (en) * 2021-04-02 2022-03-08 Ses Holdings Pte. Ltd. Anode fabrication by pattern lamination, anodes made thereby, and electrochemical devices incorporating such anodes
SE2130311A1 (en) * 2021-04-02 2022-10-03 Ses Holdings Pte Ltd Anode fabrication by pattern lamination, anodes made thereby, and electrochemical devices incorporating such anodes
JP2022158857A (ja) * 2021-04-02 2022-10-17 エスイーエス ホールディングス ピーティーイー リミテッド パターン積層によるアノードの製造方法、その方法によって製造されるアノード、および、そのようなアノードを組み込んだ電気化学装置
SE545847C2 (en) * 2021-04-02 2024-02-20 Ses Holdings Pte Ltd Anode fabrication by pattern lamination

Also Published As

Publication number Publication date
JPWO2013054593A1 (ja) 2015-03-30
JP5768137B2 (ja) 2015-08-26

Similar Documents

Publication Publication Date Title
JP5768137B2 (ja) シート状電極の製造方法
JP6504158B2 (ja) 積層型電池及びその製造方法
US20110244304A1 (en) Stack type battery
EP2772978A1 (fr) Ensemble d'électrodes et dispositif électrochimique comportant un tel ensemble
WO2018154989A1 (fr) Pile rechargeable et son procédé de fabrication
US20140170451A1 (en) Electrode
JP5552398B2 (ja) リチウムイオン電池
JP2012221804A (ja) 組電池
WO2011002064A1 (fr) Batterie stratifiée
US11522227B2 (en) Secondary battery and comb-type electrode
JP2019053862A (ja) 積層電極体及び蓄電素子
KR102085637B1 (ko) 레이저를 이용한 절단 장치
US10431846B2 (en) Energy storage device
WO2014141640A1 (fr) Cellule extérieure de stratifié
JP2011258439A (ja) 二次電池
JP2011048967A (ja) 積層型二次電池および製造方法
JP2012151036A (ja) ラミネート形電池
WO2013105362A1 (fr) Procédé permettant de produire une batterie
JP2008140551A (ja) 非水電解質二次電池
JP2002157997A (ja) 折り畳み型リチウム電池の製造方法
JP2012195123A (ja) 組電池
JP2012164476A (ja) ラミネート形電池およびそれを備えた積層型電池
JP2011048991A (ja) リチウムイオン二次電池
JP5704251B2 (ja) 組電池及び組電池の製造方法
JP2009110812A (ja) 電池及びその製造方法

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 12839848

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2013538467

Country of ref document: JP

Kind code of ref document: A

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 12839848

Country of ref document: EP

Kind code of ref document: A1