WO2011153827A1 - Flame-retardant polyester resin composition and molded article thereof - Google Patents

Flame-retardant polyester resin composition and molded article thereof Download PDF

Info

Publication number
WO2011153827A1
WO2011153827A1 PCT/CN2011/000972 CN2011000972W WO2011153827A1 WO 2011153827 A1 WO2011153827 A1 WO 2011153827A1 CN 2011000972 W CN2011000972 W CN 2011000972W WO 2011153827 A1 WO2011153827 A1 WO 2011153827A1
Authority
WO
WIPO (PCT)
Prior art keywords
flame
polyester resin
resin composition
parts
weight
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/CN2011/000972
Other languages
English (en)
French (fr)
Inventor
Takeshi Kamijo
Chungui Zhao
Hongbo Li
Yueting Pan
Syunji Kono
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Toray Fibers and Textiles Research Laboratories China Co Ltd
Original Assignee
Toray Fibers and Textiles Research Laboratories China Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toray Fibers and Textiles Research Laboratories China Co Ltd filed Critical Toray Fibers and Textiles Research Laboratories China Co Ltd
Priority to JP2013513524A priority Critical patent/JP5720778B2/ja
Priority to CN2011800195023A priority patent/CN102844375A/zh
Publication of WO2011153827A1 publication Critical patent/WO2011153827A1/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K5/00—Use of organic ingredients
    • C08K5/16—Nitrogen-containing compounds
    • C08K5/34—Heterocyclic compounds having nitrogen in the ring
    • C08K5/3467—Heterocyclic compounds having nitrogen in the ring having more than two nitrogen atoms in the ring
    • C08K5/3477—Six-membered rings
    • C08K5/3492—Triazines
    • C08K5/34928—Salts
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K2201/00—Specific properties of additives
    • C08K2201/002—Physical properties
    • C08K2201/005—Additives being defined by their particle size in general

Definitions

  • the present invention relates to a flame-retardant resin composition
  • a flame-retardant resin composition comprising a non-halogen-based flame retardant incorporated into a polyester resin, and also to a molded article thereof.
  • Polyester resins have been used in a wide range of fields, such as machine mechanism parts, electrical/electronic parts, and automobile parts, taking advantage of their excellent characteristics including injection moldability, mechanical properties, and the like.
  • Polyester resins are essentially flammable. Therefore, when they are used as industrial materials for machine mechanism parts, electrical/electronic parts, automobile parts, and the like, safety against fire, i.e., flame retardancy, is required in addition to the balance of general chemical and physical characteristics. In such cases, high-level flame retardancy showing V0 of UL-94 standard is often required.
  • Patent Documents 1 to 8 and the like disclose the addition of red phosphorus. These are useful flame-retardant resin materials without using halogen-based flame retardant. However, there has been a problem in that specific coloring is caused, and, due to the color tone of the product, the application thereof is limited.
  • Patent Documents 9 to 13 disclose the incorporation of a styrene-based resin into a composition containing a resin, such as PBT or polyphenylene ether, and a phosphate ester. These are useful flame-retardant resin materials without using halogen-based flame retardant.
  • Patent Document 14 discloses a composition comprising an organic phosphorus-based flame retardant that contains a polyester and a phosphate ester, glass fibers, and a vinyl-based resin. These are useful
  • Patent Document 15 discloses the incorporation of a flame retardant made of a phosphorus-containing compound containing a phosphate ester, a specific aromatic resin, aromatic nylon, polycarbonate resin, polyarylate resin, polyepoxy resin, and polyphenylene ether resin into a resin component containing a polyester-based resin and a
  • the resin component mentioned above containing a polyester-based resin and a styrene-based resin is a resin component useful in the improvement of moldability, such as warpage, and the flame retardant mentioned above is a useful flame retardant without using halogen-based flame retardant.
  • the flame retardant mentioned above is a useful flame retardant without using halogen-based flame retardant.
  • Patent Documents 16 to 21 disclose the incorporation of an aromatic phosphate ester and melamine cyanurate. These are useful flame-retardant resin materials without using halogen-based flame retardant, but there has been a problem in that it is difficult to balance of mechanical properties and flame retardancy.
  • Patent Document 1 JP-A-51-150553
  • Patent Document 2 JP-A-58-108248
  • Patent Document 3 JP-A-59-81351
  • Patent Document 4 JP-A-5-78560
  • Patent Document 5 JP-A-5-287119
  • Patent Document 6 JP-A-5-295164
  • Patent Document 7 JP-A-5-320486
  • Patent Document 8 JP-A-5-339417
  • Patent Document 9 JP-A-10-77396
  • Patent Document 12 JP-A-10-182956
  • Patent Document 13 JP-A-2000-26710
  • Patent Document 14 JP-A-2000-212412
  • Patent Document 15 JP-A-2001-49096
  • Patent Document 16 JP-A-3-281652
  • Patent Document 18 JP-A-7-233311
  • Patent Document 19 JP-A-8-73713
  • Patent Document 21 WO2004/029154
  • An object of the present invention is to provide a flame-retardant polyester resin composition which is excellent in the balance of flame retardancy and mechanical properties without using a halogen-based flame retardant, and also a molded article .
  • the present invention is a flame-retardant polyester resin composition
  • a flame-retardant polyester resin composition comprising (A) a polyester resin and (B) a salt of a triazine-based compound with cyanuric acid or isocyanuric acid.
  • the composition includes the component (B) in an amount of 1 to 70 parts by weight based on 100 parts by weight of the component (A) , and, in the composition, the number of particles of the component (B) with a maximum size of more than 15 ⁇ is 1 or less per 100 ⁇ x 100 ⁇ cross section.
  • the present invention is also a molded article made of the flame-retardant polyester resin composition.
  • the molded article made of the flame-retardant polyester resin composition of the present invention uses a
  • non-halogen-based flame retardant that is believed to have less impact on the environment, and has safety against electrical fire in the equipment and also has high flame retardancy to fire on the molded article itself.
  • the molded article is thus useful for electrical/electronic parts, machine mechanism parts, and automobile parts.
  • breakers Specifically, breakers, electromagnetic switches, focus cases, flyback transformers, molded articles for fusers for copiers and printers, general household electrical appliances, housings for office-automation equipments, coil bobbins, connectors, relays, disk drive chassis, transformers, switch parts, receptacle parts, motor parts, sockets, plugs, condensers, various cases, resistors, electrical/electronic parts into which metal terminals or conducting wires are incorporated, computer-associated parts, audio parts, laser discs and like sound parts, illumination parts, parts associated with telegraph/telephone devices, air conditioner parts, parts for household electrical appliances such as VTRs and televisions, parts for copiers, parts for fax machines, parts for optical devices, automobile ignition parts , connectors for automobiles, various electrical equipment parts for automobiles, and the like can be mentioned.
  • the polyester resin to serve as the component (A) is a polymer or copolymer having, as a main structural unit, one or more kinds of structural units selected from dicarboxylic acids or ester-forming derivatives thereof, diols or ester-forming derivatives thereof, hydroxycarboxylic acids or ester-forming derivatives thereof , and lactone.
  • the polyester resin may also be a commercial product .
  • aromatic polyester resins are preferable, such as polyethylene terephthalate (PET) , polypropylene terephthalate, polybutylene terephthalate (PBT) , polycyclohexane dimethylene terephthalate, polyethylene naphthalate, polypropylene naphthalate, polybutylene
  • naphthalate polyethylene isophthalate/terephthalate, polypropylene isophthalate/terephthalate, polybutylene isophthalate/terephthalate, polyethylene
  • a polyester resin selected from polyethylene terephthalate, polypropylene terephthalate, polybutylene terephthalate, and polycyclohexane dimethylene terephthalate is preferable, and a polyester resin selected from polyethylene terephthalate and polybutylene terephthalate is particularly preferable. It is also preferable to use two or more kinds of these aromatic polyester resins mixed in arbitrary amounts.
  • PET and PBT are preferable to use PET and PBT together.
  • PET/PBT 0/100 to 80/20% by weight, and more preferably 0/100 to 60/40% by weight.
  • the salt of a triazine-based compound and cyanuric acid or isocyanuric acid to serve as the component (B) is preferably an adduct of cyanuric acid or isocyanuric acid and a triazine-based compound, and it is usually an adduct having composition of 1 : 1 (molar ratio) or, in some cases, 1:2 (molar ratio) .
  • the triazine-based compounds those that do not form a salt with cyanuric acid or isocyanuric acid are excluded.
  • salts of a triazine-based compound and cyanuric acid or isocyanuric acid in particular, salts of melamine, benzoguanamine, acetoguanamine,
  • salts of melamine, benzoguanamine, and acetoguanamine are particularly preferable.
  • These salts are produced by a known method. For example, a mixture of a triazine-based compound and cyanuric acid or isocyanuric acid is formed into an aqueous slurry and thoroughly mixed to produce a salt thereof in particulate form, and then the slurry is filtered and dried, whereby a salt in powder form can be generally obtained.
  • the above salt does not have to be completely pure, and there may be some unreacted triazine-based compound, cyanuric acid, or isocyanuric acid remaining.
  • the average particle size of the salt before incorporating into a resin is preferably 0.01 to 100 ⁇ , and more preferably 1 to 80 ym.
  • a dispersant such as tris ( ⁇ -hydroxyethyl) isocyanurate, a known surface treating agent, or the like may also be used.
  • the amount of the salt of a triazine-based compound and cyanuric acid or isocyanuric acid incorporated is preferably 1 to 70 parts by weight, more preferably 35 to 70 parts by weight, based on 100 parts by weight of the polyester resin.
  • the salt content is more than 70 parts by weight, the flame retardancy and mechanical properties of the resin composition are insufficient. Such a content is thus undesirable.
  • the number of particles of the salt of a triazine-based compound and cyanuric acid or isocyanuric acid with a maximum size of more than 15 ym is 1 or less on average per 100 ym x 100 ym cross section.
  • Average herein means the average of the results of cross-sectional observation of at least 5 points per kind of resin composition.
  • the maximum size of the salt means the greatest length of a particle of the salt observed in a cross-sectional photograph.
  • the particle when the particle is elliptical, it means the major axis, when the particle is quadrangle, it means the long diagonal line.
  • the cross section is observed under an optical microscope or transmission electron microscope.
  • the optical microscope or transmission electron microscope apparatus used for observation is not particularly limited, and may be an apparatus usually used .
  • the pretreatment on a sample for the cross-sectional photograph is not particularly limited, and staining or the like may be performed for facilitating the observation.
  • Optical microscope or transmission electron microscope observation requires the preparation of an ultrathin section. However, depending on the conditions of the sample, embedding in a resin is also possible.
  • observation magnification of the optical microscope or transmission electron microscope when the magnification is too small, it is difficult to observe particles, when it is too large, the observation is localized. Therefore, observation is performed at a magnification of 200 to 1,000 times. Further, in order to increase the accuracy of observation results, it is also preferable to combine the observation results at low magnification and at high magnification from the same observation site.
  • the present inventors have found that this diffraction line greatly affects the dispersion of the salt of a triazine-based compound and cyanuric acid or isocyanuric acid in a resin.
  • the full width at half maximum of the peak is preferably 0.5° or less, more preferably 0.4° or less, and still more preferably 0.35° or less. When the full width at half maximum of the peak of the diffraction line is small, this indicates that the crystal structure of the salt is uniform.
  • the present inventors have found that although the reason for this is unclear, when the full width at half maximum of the peak is 0.4° or less, the salt is particularly unlikely to aggregate and is easily dispersible in a resin. A full width at half maximum of more than 0.4° causes uneven distribution of the salt in a resin due to aggregation, resulting in insufficient mechanical properties, and thus is undesirable.
  • the amount of such extract is small.
  • the amount of the extract which is extracted from the component (B) by a 80% by volume methanol/20% by volume benzene mixed solvent is preferably 0.1% by weight or less, more preferably 0.06% by weight or less, and still more preferably 0.05% by weight or less.
  • non-halogen flame retardants other than the component (B) can be further added as a component ( C ) , and this may be expected to shorten the burning time during burning or reduce gas generation during burning.
  • non-halogen flame retardants include, but are not limited to, phosphate esters, phosphinate salts, aluminum hydroxide, hydrotalcite, boric acid, calcium borate, calcium borate hydrate, zinc borate, zinc borate hydrate, zinc hydroxide, zinc hydroxide hydrate, zinc tin hydroxide, zinc tin hydroxide hydrate, red phosphorus, heat-expandable graphite, and dawsonite.
  • thermosetting resin such as a thermosetting melamine resin, a thermosetting phenolic resin, or a thermosetting epoxy resin
  • a coupling agent, an epoxy compound, or fats and oils such as stearic acid may also be mixed or applied to cover the surface.
  • a compound selected from phosphate esters and phosphinate salts is favorable in the balance of mechanical properties and flame retardancy, and thus is preferably used. Further, it is preferable to use a phosphate ester and a phosphinate salt together, because this further enhances the effectiveness.
  • the content of the component (C) is preferably 1 to 100 parts by weight, more preferably 10 to 40 parts by weight, based on 100 parts by weight of the polyester. A content of more than 100 parts by weight causes mold deposit, and thus is undesirable.
  • the phosphate ester is not particularly limited, and generally commercially available phosphate esters and synthesized phosphate esters are usable. Specific examples thereof include tricresyl phosphate, trixylenyl phosphate, cresyl diphenyl phosphate, triphenyl phosphate,
  • tris-isopropylbiphenyl phosphate trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, tributoxyethyl phosphate, octyl diphenyl phosphate,
  • neopentyl-glycol-based phosphate esters substituted neopentyl-glycol phosphonates , nitrogen-containing phosphate esters, and aromatic phosphate esters of the following formula (1).
  • aromatic phosphate esters are preferable, and an aromatic phosphate ester of the following formula (1) is particularly preferable:
  • Ar 1 , Ar 2 , Ar 3 , and Ar 4 represent the same or different non-halogen-containing aromatic groups.
  • X represents a structure selected from the formulae (2) to (4) below.
  • R 1 to R 8 represent the same or different hydrogen atoms or C1-5 alkyl groups
  • Y represents a direct bond, or a group selected from 0, S, SO2, C(CH 3 )2, CH 2 , and CHPh
  • Ph represents a phenyl group.
  • n in the formula (1) is an integer of 0 or more.
  • k and m in the formula (1) are each an integer of 0 or more and 2 or less, and (k + m) is an integer of 0 or more and 2 or less.
  • the aromatic phosphate ester may be a mixture of aromatic phosphate esters having different ns or different structures.
  • n in the above formula (1) is an integer of 0 or more, and the upper limit is preferably 40 or less in terms of flame retardancy.
  • n is preferably 0 to 10, and particularly preferably 0 to 5.
  • k and m are each an integer of 0 or more and 2 or less, and k + m is an integer of 0 or more and 2 or less. It is preferable that k and m are each an integer of 0 or more and 1 or less, and it is particularly preferable that k and m are each 1.
  • R 1 to R 8 represent the same or different hydrogen or Ci_ 5 alkyl groups.
  • Specific examples of the Ci_ 5 alkyl groups herein include a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, a sec-butyl group, a tert-butyl group, n-isopropyl, neopentyl, a tert-pentyl group, 2-isopropyl, neopentyl, a tert-pentyl group, 3-isopropyl, neopentyl, a tert-pentyl group, neoisopropyl , neopentyl, and a tert-pentyl group.
  • a group selected from hydrogen, a methyl group, and an ethyl group is preferable, and hydrogen is
  • Ar 1 , Ar 2 , Ar 3 , and Ar 4 represent the same or different non-halogen-containing aromatic groups.
  • aromatic groups include aromatic groups having a skeleton selected from a benzene skeleton, a naphthalene skeleton, an indene skeleton, and an anthracene skeleton. Among them, those having a benzene skeleton or a naphthalene skeleton are preferable. They may be substituted with a non-halogen-containing organic residue, and preferably with a Ci-8 organic residue. When they have a substituent, the number of substituents is not limited either, but is preferably 1 to 3.
  • Ar 1 , Ar 2 , Ar 3 , and Ar include aromatic groups such as a phenyl group, a tolyl group, a xylyl group, a cumenyl group, a mesityl group, a naphthyl group, an indenyl group, and an anthryl group.
  • aromatic groups such as a phenyl group, a tolyl group, a xylyl group, a cumenyl group, a mesityl group, a naphthyl group, an indenyl group, and an anthryl group.
  • a group selected from a phenyl group, a tolyl group, a xylyl group, a cumenyl group, and a naphthyl group is preferable
  • a group selected from a phenyl group, a tolyl group, and a xylyl group is particularly preferable .
  • an aromatic phosphate ester As a specific example of an aromatic phosphate ester, the following compound (6) or (7) is preferable, and (6) is particularly preferable.
  • PX-200 As commercially available phosphate esters, one kind or two or more kinds selected from PX-200 , PX-201, PX-130, CR-733S, TPP, CR-741, CR747, TCP, TXP, and CDP manufactured by Daihachi Chemical Industry Co., Ltd. are usable. It is preferable to use one kind or two or more kinds selected from PX-200, TPP, CR-733S, CR-741, and CR747, and it is particularly preferable to use one selected from PX-200, CR-733S, and CR-741. Among them, PX-200 is particularly effective in improving hydrolysis resistance and contact contamination resistance when used together with a vinyl-based resin and an alkaline earth metal compound, and thus is most preferable.
  • a flame retardant including at least one kind selected from phosphinate salts, diphosphinate salts, and polymers thereof is preferable .
  • the phosphinate salt is preferably a salt of a metal selected from calcium, aluminum, and zinc.
  • a flame retardant including one or more kinds of phosphinate salts of the following formula (8), diphosphinate salts of the following formula (9), and polymers thereof is particularly preferable:
  • R and R in the formula may be the same or different and are Ci_6 alkyl groups or aryl groups.
  • R 9 and R 10 may be straight or branched, examples thereof including a methyl group, an ethyl group, a propyl group, an isopropyl group, a n-butyl group, a tert-butyl group, a pentyl group, and a phenyl group.
  • R 11 is a straight or branched Ci_io alkylene group or Ce-io arylene group, alkylarylene group, or arylalkylene group.
  • Examples thereof include a methylene group, an ethylene group, a propylene group, an isopropylene group, a n-butylene group, a tert-butylene group, a pentylene group, an octylene group, a dodecylene group, a phenyl group, a naphthylene group, a methylphenylene group, an ethylphenylene group, a
  • M is calcium, aluminum, or zinc. M is preferably aluminum. Further, p is 1 to 4, q is 1 to 4, and r is 1 to 4.
  • a flame retardant including at least one kind selected from phosphinate salts, diphosphinate salts, and polymers thereof with a
  • nitrogen-containing compound and/or a boron-containing compound are also commercially available from Clariant Japan.
  • OP1312 can be mentioned.
  • OP1240 is preferably used.
  • An epoxy compound may be further incorporated into the polyester resin composition of the present invention.
  • epoxy compounds examples include glycidyl ester compounds, glycidyl ether compounds, and glycidyl ester ether compounds.
  • One or more kinds thereof can be used.
  • an epoxy compound having an epoxy equivalent of less than 500 is preferable.
  • an epoxy compound having an epoxy equivalent of less than 400 is particularly preferable.
  • the epoxy equivalent herein means the number of grams of an epoxy compound containing one gram equivalent of an epoxy group.
  • the epoxy equivalent can be determined by a method in which an epoxy compound is dissolved in pyridine, then 0.05 N hydrochloric acid is added thereto, followed by heating at 45°C, and back titration is performed with 0.05 N caustic soda using a mixture of thymol blue and cresol red as an indicator.
  • an epoxy compound using a monofunctional glycidyl ester compound together with a glycidyl ether compound, or alternatively a monofunctional glycidyl ester compound is preferably used.
  • a monofunctional glycidyl ester compound is more preferable.
  • glycidyl ester compounds include, but are not limited to, glycidyl benzoate, glycidyl t-butylbenzoate, glycidyl p-toluate, glycidyl
  • cyclohexanecarboxylate glycidyl pelargonate, glycidyl stearate, glycidyl laurate, glycidyl palmitate, glycidyl behenate, glycidyl versatate, glycidyl oleate, glycidyl linoleate, glycidyl linolenate, glycidyl behenolate, glycidyl stearolate, diglycidyl terephthalate, diglycidyl isophthalate, diglycidyl phthalate, diglycidyl naphthalenedicarboxylate, diglycidyl bibenzoate, diglycidyl methyl terephthalate, diglycidyl hexahydrophthalate, diglycidyl tetrahydrophtalate, diglycidyl cyclohexanedicarboxylate, diglycidyl
  • glycidyl ether compounds include, but are not limited to, diglycidyl ethers obtained by allowing a bisphenol to react with epichlorohydrin, such as phenyl glycidyl ether, o-phenyl phenyl glycidyl ether,
  • the amount of the epoxy compound incorporated is preferably 0.1 to 5 parts by weight, particularly preferably 0.3 to 4 parts by weight, based on 100 parts by weight of the polyester.
  • fiber-reinforced material may be incorporated into the polyester resin composition of the present invention.
  • Such fiber-reinforced materials include glass fibers, aramid fibers, and carbon fibers.
  • glass fibers it is preferable to use chopped-strand-type or roving-type glass fibers used as an ordinary reinforcement material for polyester resins, which are glass fibers treated with a silane coupling agent, such as an amino silane compound or an epoxy silane compound, and/or a sizing agent including urethane, vinyl acetate, bisphenol A diglycidyl ether, one or more kinds of epoxy compounds such as novolac-type epoxy compounds, etc.
  • a silane coupling agent such as an amino silane compound or an epoxy silane compound
  • a sizing agent including urethane, vinyl acetate, bisphenol A diglycidyl ether, one or more kinds of epoxy compounds such as novolac-type epoxy compounds, etc.
  • the silane coupling agent and/or sizing agent may be used in an emulsion liquid.
  • the amount incorporated is preferably 0 to 100 parts by weight, more preferably 25 to 90 parts by weight, based on 100 parts by weight of the polyester.
  • inorganic fillers other than the fiber-reinforced material may be further incorporated into the polyester resin composition of the present invention.
  • examples of such inorganic fillers other than the fiber-reinforced material include, but are not limited to, acicular, granular, powdery, and laminated inorganic fillers.
  • the inorganic fillers other than the fiber-reinforced material may have been subjected to a surface treatment, such as coupling agent treatment, an epoxy compound, or ionization treatment.
  • the granular, powdery, and laminated inorganic fillers preferably have an average particle size of 0.1 to 20 m, and particularly preferably 0.2 to 10 ⁇ .
  • the amount of the inorganic filler incorporated other than the fiber-reinforced material is, as a total with the amount of the fiber-reinforced agent incorporated, preferably 0 to 100 parts by weight based on 100 parts by weight of the polyester.
  • a fluorine-based resin can be further incorporated into the polyester resin composition of the present invention to suppress the meltdown of the flame-retardant resin composition during burning and also to improve flame retardancy.
  • the luorine-based resin is a resin containing fluorine in the molecule. Specific examples thereof include
  • the fluorine-based resin in terms of flame retardancy and mechanical properties, the amount incorporated is preferably 0.02 to 5 parts by weight, more preferably 0.2 to 2 parts by weight, based on 100 parts by weight of the polyester.
  • a polycarbonate resin can be further incorporated into the polyester resin composition of the present invention to further improve flame retardancy. Examples of the
  • polycarbonate resins include aromatic homo- or
  • copolycarbonates obtained by allowing an aromatic dihydric phenol-based compound to react with phosgene or a carbonic acid diester.
  • Such an aromatic homo- or copolycarbonate resin preferably has a weight-average molecular weight within a range of 10,000 to 1,100,000, and more preferably has a
  • glass-transition temperature of about 150°C and a weight-average molecular weight within a range of 10,000 to 1, 000, 000. It is also possible to use polycarbonate resins with different weight-average molecular weights together. A polycarbonate resin having a weight-average molecular weight within a range 60,000 to 1,100,000 is particularly preferable . Weight-average molecular weight is obtained from measurement in terms of polystyrene by gel permeation chromatography using tetrahydrofuran as the solvent. A weight-average molecular weight of less than 10,000 causes a decrease in the mechanical properties of the polyester resin composition, and thus is undesirable. A weight-average molecular weight of more than 110, 000 causes a loss of the fluidity of the composition during molding, and thus is undesirable.
  • melt flow index a polycarbonate resin having a melt viscosity index (melt flow index) within a range of 1 to 100 g/10 minutes as measured by a melt-indexer under conditions where the temperature is 300°C and the load is 1.2 kg according to ASTM D1238 is preferable, and
  • aromatic dihydric phenol-based compounds examples include 2, 2-bis (4-hydroxyphenyl) propane,
  • the polycarbonate resin When the polycarbonate resin is incorporated in an amount of more than 20 parts by weight based on 100 parts by weight of the polyester, hydrolysis resistance may be greatly reduced, and therefore caution is necessary. In terms of hydrolysis resistance and flame retardancy, the amount of the polycarbonate resin incorporated is preferably 0.1 to 10 parts by weight based on 100 parts by weight of the polyester. Further, it is also possible to incorporate a polycarbonate resin oligomer in an amount within a range where the characteristics of the present invention are not impaired.
  • the incorporation of a small amount of an acid phosphate ester is useful as an ester interchange inhibitor for the polyester and the polycarbonate resin.
  • a decrease in the heat distortion temperature, for example, is inhibited.
  • the acid phosphate ester is preferably an alkyl acid phosphate compound of a partial ester of an alcohol and phosphoric acid.
  • a low-molecular-weight one is a colorless liquid, while a high-molecular-weight one is a solid in the form of white wax or flakes.
  • acid phosphate esters include, but are not limited to, monomethyl acid phosphate, monoethyl acid phosphate, monoisopropyl acid phosphate, monobutyl acid phosphate, monolauryl acid phosphate, monostearyl acid phosphate, monododecyl acid phosphate, monobehenyl acid phosphate, dimethyl acid phosphate, diethyl acid phosphate, diisopropyl acid phosphate, dibutyl acid phosphate, lauryl acid phosphate, distearyl acid phosphate, didodecyl acid phosphate, dibehenyl acid phosphate, trimethyl acid phosphate, triethyl acid phosphate, a mixture of the above mono- and di- acid phosphate esters, a mixture of mono-, di-, and tri- acid phosphate esters, and a mixture of one or more kinds of the above compounds.
  • the acid phosphate esters include long-chain alkyl acid phosphate compounds, such as a mixture of mono- and distearyl acid phosphates .
  • a compound is commercially available from Asahi Denka Kogyo Co. , Ltd. under the name of "ADEKASTAB (registered trademark)" AX-71, and is a flaky solid having a melting point.
  • ADEKASTAB registered trademark
  • the amount of the acid phosphate ester incorporated is preferably 0.01 to 0.5 parts by weight, more preferably 0.02 to 0.3 parts by weight, based on 100 parts by weight of the polyester.
  • a flame-retardant synergist that supports flame retardancy such as a silicone compound, a phenol resin, a phosphonitrile compound, ammonium polyphosphate, or melamine phosphate, can be further incorporated into the polyester resin composition of the present invention, and one or more kinds are used. Further, when such a flame-retardant synergist is incorporated, in terms of flame retardancy and mechanical properties, the amount incorporated is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 7.5 parts by weight, based on 100 parts by weight of the polyester.
  • silicone compounds include silicone resins, silicone oils, and silicone powders.
  • silicone resins include polyorganosiloxanes having a group and siloxane chemically bonded together, the group being selected from a saturated or unsaturated monovalent hydrocarbon group, a hydrogen atom, a hydroxyl group, an alkoxyl group, an aryl group, a vinyl group, or an allyl group.
  • One having a viscosity of about 200 to 300,000,000 cP at room temperature is preferable, but the silicone resin is not limited thereto, and, with respect to the product form, it may be in the form of oil, powder, or gum.
  • silicone oils include polyorganosiloxanes having a group and siloxane chemically bonded together, the group being selected from a saturated or unsaturated monovalent hydrocarbon group, a hydrogen atom, a hydroxyl group, an alkoxyl group, an aryl group, a vinyl group, or an allyl group.
  • One having a viscosity of about 0,65 to 100,000 cSt at room temperature is preferable, but the silicone oil is not limited thereto, and, with respect to the product form, it may be in the form of oil, powder, or gum.
  • silicone powders include those obtained by incorporating an inorganic filler into the silicone resin and/or silicone oil mentioned above.
  • silica or the like is preferably used as the inorganic filler.
  • the phenol resin may be any phenol resin as long as it is a polymer having a plurality of phenolic hydroxy groups .
  • examples thereof include novolac-type, resol-type, and heat-reactive resins, as well as resins obtained by
  • novolac-type phenol resin that has no curing agent added and is not heat-reactive or a melamine-modified, novolac-type phenol resin is preferable.
  • the form is not particularly limited, any of those in pulverized form, granular form, flaky form, powdery form, acicular form, liquid form, and the like are usable, and one kind or two or more kinds thereof can be used as required.
  • phenolic resins are also usable
  • a reaction vessel is prepared in such a manner that the molar ratio between phenols and aldehydes is 1:0.7 to 1:0.9, then a catalyst such as oxalic acid, hydrochloric acid, sulfuric acid, or toluenesulfonic acid is further added thereto followed by heating, and a reflux reaction is performed for a predetermined period of time. Vacuum dehydration or standing dehydration is then performed to remove produced water, and still remaining water and unreacted phenols are removed. By such a method, a novolac-type phenol resin can be obtained.
  • Co-condensed phenol resins obtained by using these resins or a plurality of raw material components can be used alone, or it is also possible to use two or more kinds thereof.
  • a reaction vessel is prepared in such a manner that the molar ratio between phenols and aldehydes is 1:1 to 1:2, and a catalyst such as sodium hydroxide, aqueous ammonia, or other basic substances is added thereto, followed by the same reaction and treatment as in the case of the novolac-type phenol resin; a resol-type phenol resin can thus be obtained.
  • examples of the phenols include phenol, o-cresol, m-cresol, p-cresol, thymol, p-tert-butylphenol , tert-butylcatechol, catechol, isoeugenol, o-methoxyphenol , 4 , 4 ' -dihydroxyphenyl-2 , 2-propane, isoamyl salicylate, benzyl salicylate, methyl salicylate, and 2 , 6-di-tert-butyl-p-cresol
  • phenol phenol, o-cresol, m-cresol, p-cresol, thymol, p-tert-butylphenol , tert-butylcatechol, catechol, isoeugenol, o-methoxyphenol , 4 , 4 ' -dihydroxyphenyl-2 , 2-propane, isoamyl salicylate, benzyl salicylate, methyl salicy
  • examples of the aldehydes include formaldehyde, paraformaldehyde, polyoxymethylene, andtrioxane.
  • One kind or two or more kinds of these aldehydes can be used as required.
  • the molecular weight of the phenolic resin is not particularly limited, but is preferably 200 to 2,000 in number-average molecular weight. It is particularly preferably within a range of 400 to 1,500, because this leads to excellent mechanical properties, fluidity, and economical efficiency .
  • the molecular weight of a phenolic resin can be measured, as a tetrahydrofuran solution, using a polystyrene standard sample by gel permeation chromatography.
  • examples of the phosphonitrile compounds include phosphonitrile compounds having as a main component a phosphonitrile linear polymer and/or cyclic polymer, which may be linear, cyclic, or a mixture thereof.
  • the phosphonitrile linear polymer and/or cyclic polymer can be synthesized by a known method described in "Hosfazen-kagobutsu no Gosei to Oyo (Synthesis and Application of Phosphazene Compound)" written by Kajiwara, etc.
  • phosphorus pentachloride or phosphorus trichloride as a phosphorus source is allowed to react with ammonium chloride or ammonia gas as a nitrogen source (it is also possible to purify a cyclic product ) by a known method, and the obtained substance is substituted with alcohols, phenols, or amines, whereby synthesis can be achieved.
  • ammonium polyphosphates examples include ammonium polyphosphates, melamine-modified ammonium
  • the ammonium polyphosphate may be coated with a thermosetting resin, such as a phenol resin, urethane resin, melamine resin, urea resin, epoxy resin, or urea resin having thermosetting properties, and one kind or two or more kinds may be used.
  • a thermosetting resin such as a phenol resin, urethane resin, melamine resin, urea resin, epoxy resin, or urea resin having thermosetting properties
  • examples of the melamine polyphosphates include melamine polyphosphates such as melamine phosphates and melamine pyrophosphates, and one kind or two or more kinds may be used.
  • an ethylene (co) polymer may be further incorporated for the purpose of improving the toughness of the composition, such as impact strength.
  • ethylene (co) polymers include ethylene polymers and ethylene copolymers, such as high-density polyethylene, low-density polyethylene, and ultra-low-density polyethylene.
  • An ethylene copolymer can be obtained by copolymerizing ethylene and a monomer copolymerizable therewith.
  • Examples of the copolymerizable monomers include propylene, butene-1, vinyl acetate, isoprene, butadiene, monocarboxylic acids such as acrylic acid and methacrylic acid, ester acids thereof, and dicarboxylic acids such as maleic acid, fumaric acid, and itaconic acid.
  • An ethylene copolymer can be produced by a known method. Specific examples of the ethylene copolymers include ethylene/propylene, ethylene/butene-1 , ethylene/vinyl acetate, ethylene/ethyl acrylate, ethylene/methyl acrylate, and ethylene/ethyl methacrylate acrylate.
  • a copolymer obtained by grafting or copolymerization of an anhydride or glycidyl methacrylate with the ethylene (co) polymer is also preferable to use.
  • a copolymer obtained by grafting or copolymerization of an anhydride or glycidyl methacrylate with polyethylene has excellent compatibility with a polyester component and thus is preferably used.
  • the amount incorporated is preferably 1 to 10 parts by weight, more preferably 2 to 7.5 parts by weight, based on 100 parts by weight of the polyester.
  • Phenoxy resins, oxazoline compounds, carbodiimide compounds, and the like which are materials for improving hydrolysis resistance, can be further incorporated into the polyester resin composition of the present invention.
  • a phenoxy resin is preferably used.
  • the amount incorporated is preferably 0.1 to 7.5 parts by weight, more preferably 0.2 to 5 parts by weight, based on 100 parts by weight of the polyester.
  • phenoxy resins examples include phenoxy resins obtained by allowing an aromatic dihydric phenol-based compound to react with epichlorohydrin in various proportions.
  • the molecular weight of the phenoxy resin is not particularly limited, but those having a viscosity-average molecular weight within a range of 1,000 to 100,000 are preferable.
  • the aromatic dihydric phenol-based compounds 2 , 2-bis ( 4-hydroxyphenyl ) propane,
  • 2.2-bis (4-hydroxyphenyl) methane, and the like are usable. They may be used alone or as a mixture. Further, the form of the phenoxy resin is not particularly limited, and any of those in pulverized form, granular form, flaky form, powdery form, liquid form, and the like are usable. One kind or two or more kinds of these phenoxy resins can be used as required.
  • a hindered-phenol-based antioxidant and/or a phosphite-based antioxidant can be further incorporated as a stabilizer into the polyester resin composition of the present invention.
  • the amount incorporated is preferably 0.1 to 1 part by weight, more preferably 0.2 to 0.5 parts by weight, based on 100 parts by weight of the polyester .
  • the amount incorporated is less than 0.1 parts by weight, heat aging resistance is not sufficient, while when it is more than 1 part by weight, mechanical properties and flame retardancy are impaired. Such an amount is thus undesirable.
  • antioxidants include triethylene
  • octadecyl-3- (3, 5-di-t-butyl-4-hydroxyphenyl ) propionate, 3, 5-di-t-butyl-4-hydroxybenzyl phosphonate diethyl ester, 1, 3, 5-trimethyl-2 , 4, 6-tris (3, 5-di-t-butyl-4-hydroxybenzyl ) b enzene, bis- or
  • N, N' -trimethylenebis (3, 5-di-t-butyl-4-hydroxy-hydrocinnamam ide) .
  • examples of the phosphite-based stabilizers include tris (2 , 4-di-t-butylphenyl) phosphite,
  • lubricants can be further added to the polyester resin composition of the present invention to improve fluidity and mold release properties during molding.
  • lubricants include, but are not limited to, metallic soaps such as calcium stearate and barium stearate; fatty acid esters; salts of fatty acid esters (including those partially converted into a salt) ; fatty acid amides such as ethylene bis stearamide; fatty acid amides made of a polycondensate of ethylenediamine, stearic acid, and sebacic acid or a polycondensate of phenylenediamine, stearic acid, and sebacic acid; polyalkylene wax; anhydride-modified
  • the amount added is preferably 0.05 to 2 parts by weight, more preferably 0.1 to 1 part by weight, based on 100 parts by weight of the polyester.
  • one or more kinds of carbon black, titanium oxide, and pigments and dyes of various colors can be incorporated into the polyester resin composition of the present invention to prepare the resin in various colors and also to improve weather (light) resistance and electrical conductivity.
  • the pigment or the dye is incorporated, in terms of the mechanical properties of the resulting composition, the amount
  • incorporated is preferably 0.1 to 10 parts by weight, more preferably 0.1 to 5 parts by weight, based on 100 parts by weight of the polyester.
  • carbon black examples include, but are not limited to, channel black, furnace black, acetylene black, anthracene black, soot, turpentine soot, and graphite.
  • Carbon black having an average particle size of 500 nm or less and a dibutyl phthalate oil absorption of 50 to 400 cm 3 /100 g is preferably used. It may have been treated with, as a treatment agent, aluminum oxide, silicon oxide, zinc oxide, zirconium oxide, polyol, a silane coupling agent, or the like.
  • titanium oxide titanium oxide that is in a crystal form such as rutile form or anatase form and has an average particle size of 5 ⁇ or less is preferably used.
  • the carbon black, titanium oxide, and pigments and dyes of various colors may be melt-blended or simply blended with various thermoplastic resins and used as a mixed material.
  • a thermoplastic resin polyalkylene
  • terephthalate is preferably used.
  • a material including one or more kinds of known additives such as sulfur-based antioxidants, ultraviolet absorbers, plasticizers, and antistatic agents, can also be used to the extent that they do not interfere with an object of the present invention .
  • a polyphenylene ether resin or polyphenylene sulfide resin further improves flame retardancy, it may reduce tracking resistance, hydrolysis resistance, and metal contamination properties. Therefore, such a resin is not preferably incorporated. When it is incorporated, the amount is preferably not more than 5% by weight.
  • the flame-retardant polyester resin composition of the present invention and a molded article are produced by a known method.
  • a polyester resin, a vinyl-based resin, a phosphate ester, a salt of a triazine-based compound with cyanuric acid or isocyanuric acid, and an alkaline earth metal compound if necessary as well as an epoxy compound and a fiber-reinforced material such as glass fibers, further if necessary as well as an inorganic filler other than the fiber-reinforced material, a fluorine-based compound, a polycarbonate resin, various flame-retardant synergists, an ethylene (co) polymer, a material for improving hydrolysis resistance, a hindered-phenol-based antioxidant, and a phosphite-based antioxidant, together with other necessary additives and coloring agents such as pigments and dyes, are fed to a kneading machine after premixing or without premixing, and thoroughly melt-kneaded
  • the premixing include dry blending and mixing using a mechanical mixing apparatus, such as a tumbler, a ribbon mixer, or a Henschel mixer.
  • a mechanical mixing apparatus such as a tumbler, a ribbon mixer, or a Henschel mixer.
  • the method may also be such that the fiber-reinforced material is added from a side feeder installed between a main loading part and a vent part of a multi-screw extruder such as a twin-screw extruder.
  • the method may be such that a liquid addition nozzle is installed between a main loading part and a vent part of a multi-screw extruder such as a twin-screw extruder, and the additive is added using a plunger pump, or that the additive is supplied from the main loading part or the like using a metering pump.
  • the kneading machine may be, but is not limited to, for example, a single-screw extruder, twin-screw extruder, or triple-screw extruder equipped with a "uni-melt" or
  • the flame-retardant polyester resin composition thus obtained can be molded by a known method. It can be formed into a molded article of any shape by, for example, injection molding, extrusion molding, compression molding, sheet forming, film forming, etc. In particular, inj ection molding is preferable, and it is also possible to perform insert molding where a part of a metal component is directly integrated with the molded article .
  • PET (hereinafter abbreviated as PET)
  • Mitsui PET j005 manufactured by Mitsui PET Resin
  • PET having an intrinsic viscosity of 0.65 25°C, 1:1 mixed solvent of phenol/tetrachloroethane was used.
  • the X-ray diffraction spectra of these salts were measured using an X-ray diffraction apparatus (manufactured by Rigaku Corporation, Multiflex) .
  • the full width at half maximum of the diffraction line with the highest peak intensity was measured.
  • PC polycarbonate resin
  • Iupilon S3000 manufactured by Mitsubishi Engineering-Plastics Corporation
  • Reference Example 7 A polyphenylene sulfide "Torelina” M2588 (manufactured by Toray Industries Inc.) (hereinafter abbreviated as PPS) was used.
  • Teflon registered trademark 6-J
  • Teflon manufactured by Dupont-Mitsui Fluorochemicals Co. , Ltd.
  • Teflon Polytetrafluoroethylene
  • 0.2 parts by weight of the polytetrafluoroethylene was added.
  • a silicone powder "DC4-7105" (manufactured by Dow Corning Toray Silicone Co., Ltd.) was used. To the resin materials of all the examples, 0.2 parts by weight of the silicon powder was added .
  • pentaerythrityl-tetrakis [3- (3, 5-di-t-butyl-4-hydroxyphenyl ) propionate] was used.
  • 0.2 parts by weight of the hindered-phenol-based antioxidant was added.
  • twin-screw extruder having a screw diameter of 30 mm and L/D of 35 equipped with a co-rotating vent
  • the raw materials were mixed according to the incorporation composition shown in Tables 2 to 4, and added from the main loading part. Further, in the examples where GF was incorporated, a side feeder was installed between the main loading part and the vent part to add GF , and the raw materials other than G F were added from the main loading part. Melt-mixing was performed under extrusion conditions where the kneading temperature was 270°C and the screw rotation was at 150 rpm. The melt-mixture was discharged in strand form, passed through a cooling bus, and pelletized using a strand cutter.
  • the obtained pellets were used, or, alternatively, the obtained pellets were dried and then molded to prepare each specimen, and the following physical properties were measured.
  • the results are shown in Tables 2 to 4.
  • the measurement method for each characteristic is as follows.
  • a specimen for the evaluation of flame retardancy was formed by injection molding under the conditions where the molding temperature was 270°C and the die temperature was 70°C. Flame retardancy was evaluated in accordance with the evaluation criteria defined in the UL94 vertical test. Flame retardancy decreases in the following order: V-0 > V-l > V-2. Further, the thickness of the specimens was 1/32 inch, 1/16 inch, and 1/8 inch. Generally, even in the specimens of the same V-0 rank, a specimen that is thinner but satisfies the evaluation criteria has higher flame retardancy of the raw material.
  • an IS0527 dumbbell specimen having a thickness of 4 mm was formed by injection molding under the conditions where the molding temperature was 270°C and the die temperature was 70°C.
  • the tensile strength and tensile elongation were measured according to IS0527-1, 2.
  • an IS0527 dumbbell specimen having a thickness of 4 mm was formed by injection molding under the conditions where the molding temperature was 270°C and the die temperature was 70°C.
  • the flexural strength was measured according to IS0527-1, 2.
  • the molded article made of the flame-retardant polyester resin composition of the present invention uses a
  • non-halogen-based flame retardant that is believed to have less impact on the environment, and has safety against electrical fire in the equipment and also has high flame retardancy to fire on the molded article itself.
  • the molded article is thus useful for electrical/electronic parts, machine mechanism parts, and automobile parts.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Organic Chemistry (AREA)
  • Compositions Of Macromolecular Compounds (AREA)
PCT/CN2011/000972 2010-06-11 2011-06-10 Flame-retardant polyester resin composition and molded article thereof Ceased WO2011153827A1 (en)

Priority Applications (2)

Application Number Priority Date Filing Date Title
JP2013513524A JP5720778B2 (ja) 2010-06-11 2011-06-10 難燃性ポリエステル樹脂組成物およびその成形品
CN2011800195023A CN102844375A (zh) 2010-06-11 2011-06-10 阻燃性聚酯树脂组合物及成型品

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
CN201010204523.X 2010-06-11
CN 201010204523 CN102276963A (zh) 2010-06-11 2010-06-11 一种阻燃性聚酯树脂组合物及成型品

Publications (1)

Publication Number Publication Date
WO2011153827A1 true WO2011153827A1 (en) 2011-12-15

Family

ID=45097501

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/CN2011/000972 Ceased WO2011153827A1 (en) 2010-06-11 2011-06-10 Flame-retardant polyester resin composition and molded article thereof

Country Status (3)

Country Link
JP (1) JP5720778B2 (cg-RX-API-DMAC7.html)
CN (2) CN102276963A (cg-RX-API-DMAC7.html)
WO (1) WO2011153827A1 (cg-RX-API-DMAC7.html)

Families Citing this family (8)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN102276963A (zh) * 2010-06-11 2011-12-14 东丽纤维研究所(中国)有限公司 一种阻燃性聚酯树脂组合物及成型品
CN103660306A (zh) * 2012-09-24 2014-03-26 东丽先端材料研究开发(中国)有限公司 一种无卤阻燃热塑性聚酯组合物的成型方法
CN102911486B (zh) * 2012-11-07 2015-01-07 新疆蓝山屯河聚酯有限公司 利用再生pet树脂制备pet/pbt合金的方法
CN103013062A (zh) * 2012-12-10 2013-04-03 彩虹集团公司 一种复合型阻燃聚酯及其制备方法
CN106479297A (zh) * 2016-11-21 2017-03-08 青岛爱尔家佳新材料股份有限公司 一种气凝胶水性膨胀型防火涂料及其制备方法
JP7412352B2 (ja) * 2019-03-25 2024-01-12 ポリプラスチックス株式会社 熱可塑性樹脂の耐トラッキング性向上方法
CN116731483B (zh) * 2023-06-06 2026-07-21 上海金山锦湖日丽塑料有限公司 一种具有高耐水解性的无卤阻燃增强聚酯复合材料
US20260159671A1 (en) * 2023-10-05 2026-06-11 Lg Chem, Ltd. Polybutylene terephthalate resin composition, method of preparing the same, and molded article including the same

Citations (10)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH06157880A (ja) * 1992-11-17 1994-06-07 Mitsubishi Petrochem Co Ltd ポリアルキレンテレフタレート系難燃性樹脂組成物
WO1999067326A1 (de) * 1998-06-23 1999-12-29 Basf Aktiengesellschaft Flammgeschützte polyesterformmassen
JP2005325216A (ja) * 2004-05-13 2005-11-24 Toray Ind Inc ネジまたは端子挿入部位を有する成形品
CN1894319A (zh) * 2003-12-17 2007-01-10 通用电气公司 阻燃性聚酯组合物
JP2007039853A (ja) * 2005-08-05 2007-02-15 Mitsubishi Engineering Plastics Corp 難燃性ポリブチレンテレフタレート不織布
CN101346429A (zh) * 2005-12-26 2009-01-14 胜技高分子株式会社 形成可透射激光的构件的阻燃性树脂组合物
US20090036578A1 (en) * 2003-12-17 2009-02-05 Sabic Innovative Plastics Ip Bv Polyester Compositions, Method Of Manufacture, And Uses Thereof
JP2009227750A (ja) * 2008-03-19 2009-10-08 Toray Ind Inc 難燃性ポリブチレンテレフタレート樹脂組成物
JP2010024272A (ja) * 2008-07-15 2010-02-04 Mitsubishi Engineering Plastics Corp 難燃性熱可塑性樹脂組成物
CN101684192A (zh) * 2008-09-23 2010-03-31 东丽纤维研究所(中国)有限公司 无卤阻燃热塑性聚酯树脂组合物

Family Cites Families (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS5693754A (en) * 1979-12-28 1981-07-29 Toray Ind Inc Flame-retardant polyamide composition
JPH10316843A (ja) * 1997-05-16 1998-12-02 Kanegafuchi Chem Ind Co Ltd 難燃性ポリエステル樹脂組成物
ATE551331T1 (de) * 2004-10-15 2012-04-15 Basf Se Verfahren zur herstellung von melamincyanurat in kristalliner form
JP2007077356A (ja) * 2005-09-16 2007-03-29 Mitsubishi Engineering Plastics Corp 難燃性ポリエステルフィルム
JP2010006965A (ja) * 2008-06-27 2010-01-14 Toray Ind Inc 難燃性熱可塑性ポリエステル樹脂組成物
CN102276963A (zh) * 2010-06-11 2011-12-14 东丽纤维研究所(中国)有限公司 一种阻燃性聚酯树脂组合物及成型品

Patent Citations (10)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH06157880A (ja) * 1992-11-17 1994-06-07 Mitsubishi Petrochem Co Ltd ポリアルキレンテレフタレート系難燃性樹脂組成物
WO1999067326A1 (de) * 1998-06-23 1999-12-29 Basf Aktiengesellschaft Flammgeschützte polyesterformmassen
CN1894319A (zh) * 2003-12-17 2007-01-10 通用电气公司 阻燃性聚酯组合物
US20090036578A1 (en) * 2003-12-17 2009-02-05 Sabic Innovative Plastics Ip Bv Polyester Compositions, Method Of Manufacture, And Uses Thereof
JP2005325216A (ja) * 2004-05-13 2005-11-24 Toray Ind Inc ネジまたは端子挿入部位を有する成形品
JP2007039853A (ja) * 2005-08-05 2007-02-15 Mitsubishi Engineering Plastics Corp 難燃性ポリブチレンテレフタレート不織布
CN101346429A (zh) * 2005-12-26 2009-01-14 胜技高分子株式会社 形成可透射激光的构件的阻燃性树脂组合物
JP2009227750A (ja) * 2008-03-19 2009-10-08 Toray Ind Inc 難燃性ポリブチレンテレフタレート樹脂組成物
JP2010024272A (ja) * 2008-07-15 2010-02-04 Mitsubishi Engineering Plastics Corp 難燃性熱可塑性樹脂組成物
CN101684192A (zh) * 2008-09-23 2010-03-31 东丽纤维研究所(中国)有限公司 无卤阻燃热塑性聚酯树脂组合物

Also Published As

Publication number Publication date
JP5720778B2 (ja) 2015-05-20
CN102844375A (zh) 2012-12-26
JP2013532205A (ja) 2013-08-15
CN102276963A (zh) 2011-12-14

Similar Documents

Publication Publication Date Title
US7135509B2 (en) Flame-retardant polybutylene terephthalate resin composition and formed article
US9505926B2 (en) Flame-retardant thermoplastic polyester resin composition and molded article
CN102307947B (zh) 阻燃性热塑性树脂组合物和成型品
JP5720778B2 (ja) 難燃性ポリエステル樹脂組成物およびその成形品
CN105793354B (zh) 热塑性聚酯树脂组合物及成型品
JP4911547B2 (ja) 難燃性ポリブチレンテレフタレート樹脂組成物および成形品
US8034870B2 (en) Flame-retardant polyester composition
JP2013001772A (ja) 難燃性熱可塑性ポリエステル樹脂組成物および成形品
JP4281313B2 (ja) 難燃性ポリブチレンテレフタレート樹脂組成物および成形品
JP2009227750A (ja) 難燃性ポリブチレンテレフタレート樹脂組成物
JP2010037375A (ja) 難燃性熱可塑性ポリエステル樹脂組成物および成形品
JP4810743B2 (ja) 難燃性樹脂組成物
JP2019044037A (ja) 熱可塑性ポリエステル樹脂組成物および成形品
JP2009227749A (ja) 難燃性ポリブチレンテレフタレート樹脂組成物
KR20130132004A (ko) 기계적 특성이 우수한 비할로겐 난연화 폴리에스테르 수지 조성물 및 이의 성형품
JP4810744B2 (ja) 難燃性樹脂組成物および成形品
KR100869891B1 (ko) 난연성 폴리부틸렌테레프탈레이트 수지 조성물 및 성형품
JP4665433B2 (ja) 難燃性ポリエチレンテレフタレート樹脂組成物
JP5248724B2 (ja) 難燃性ポリブチレンテレフタレート樹脂組成物および成形品
JP4830206B2 (ja) 難燃性ポリブチレンテレフタレート樹脂組成物および成形品
JP2005325216A (ja) ネジまたは端子挿入部位を有する成形品
JP2005325215A (ja) ウェルド部位を有する成形品
JP2002060597A (ja) 難燃性ポリブチレンテレフタレート樹脂組成物および成形品
JP5194357B2 (ja) 難燃性ポリエチレンテレフタレート樹脂組成物
JP2004075868A (ja) 難燃性ポリブチレンテレフタレート樹脂組成物および成形品

Legal Events

Date Code Title Description
WWE Wipo information: entry into national phase

Ref document number: 201180019502.3

Country of ref document: CN

121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 11791819

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2013513524

Country of ref document: JP

Kind code of ref document: A

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 11791819

Country of ref document: EP

Kind code of ref document: A1