CN108130754A - 一种纯棉双层提花家纺织物染整方法 - Google Patents

一种纯棉双层提花家纺织物染整方法 Download PDF

Info

Publication number
CN108130754A
CN108130754A CN201711464136.8A CN201711464136A CN108130754A CN 108130754 A CN108130754 A CN 108130754A CN 201711464136 A CN201711464136 A CN 201711464136A CN 108130754 A CN108130754 A CN 108130754A
Authority
CN
China
Prior art keywords
dyeing
add
anhydrous sodium
sodium sulphate
pure cotton
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201711464136.8A
Other languages
English (en)
Inventor
杜国栋
钟华
于兴建
魏庆刚
韩耀攀
徐峰
亓鹏
张文佳
牛繁琳
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Large Dyehouse Zibo Silk Group Co ltd
Original Assignee
Large Dyehouse Zibo Silk Group Co ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Large Dyehouse Zibo Silk Group Co ltd filed Critical Large Dyehouse Zibo Silk Group Co ltd
Priority to CN201711464136.8A priority Critical patent/CN108130754A/zh
Publication of CN108130754A publication Critical patent/CN108130754A/zh
Pending legal-status Critical Current

Abstract

一种纯棉双层提花家纺织物染整方法,属于纯棉织物染色技术领域。其特征在于,制备步骤为:按照染液配方:母体含有乙烯砜基、羟基乙烯砜硫酸酯基两个活性基团的活性染料;染槽内加入质量分数20%~50%染液,开车运行一道;加入剩余染液,再开车运行一道;加入元明粉运行;加入碱粉运行;加皂洗剂SN‑45,升温运行三道;冷水洗后加入中和酸运行三道;酸洗后下卷。发明人将棉双层提花布染色的工艺改进配合选用的母体含有乙烯砜基、羟基乙烯砜硫酸酯基两个活性基团的活性染料,同时提升了皂洗牢度、染料的提升力、染料的上染速率及曲线、染料的配伍性等因素。

Description

一种纯棉双层提花家纺织物染整方法
技术领域
一种纯棉双层提花家纺织物染整方法,属于纯棉织物染色技术领域。
背景技术
四大天然纤维“棉、丝、毛、麻”中,棉纤维数量最多、应用最广、与人们生活联系最密切。棉纤维是多孔性物质,且其纤维素大分子上存在许多亲水性基团(-OH),所以其吸湿性较好,一般大气条件下,棉纤维的回潮率可达8.5%左右。因此,棉纤维具有吸湿排汗,爽身亲肤的特点,广泛用于服装面料、床品套件的制作。
纯棉双层提花布,组织规格 A层 40s*(12s+10s/2) 173*80 B层 60s*(21s+12s/2)173*90,特殊的双层组织结构设计,织物手感蓬松、柔软,透气性好,舒适保暖,经过烧毛→退浆→漂白→卷染机染色,布面毛羽洁净、光亮,主要用于制作床品套件,销售英国为主的欧洲市场,深受消费者欢迎。
纯棉双层提花布,一般工艺采用S型活性染料卷染机染色,即活性红S-2BF、活性黄S-4RFN、活性兰S-2GLN,通过三元色拼色,卷染机70℃恒温染色,满足客户不同色样标准的需求。S型活性染料含有乙烯砜、一氯均三嗪两个活性基,染料反应性强,固色率高,色泽浓艳,染色水洗牢度、摩擦牢度优良;缺点一是染料的耐光照牢度差,只能达到3~4级,个别色泽,如兰灰色,光照牢度只有2~3级;二是染料配伍性不好,染色上染同步性差,卷染机染色存在首尾色差,缸头缸尾裁头数量较多。这两方面因素影响,制约了产品质量。
发明内容
本发明要解决的技术问题是:克服现有技术的不足,提供一种耐光照牢度强、上染同步性好的纯棉双层提花家纺织物染整方法。
本发明解决其技术问题所采用的技术方案是:该纯棉双层提花家纺织物染整方法,其特征在于,制备步骤为:
1)制备染液,母体含有乙烯砜基、羟基乙烯砜硫酸酯基两个活性基团的活性染料0.8%owf ~2.45%owf、元明粉55 g/L ~65g/L、碱粉8 g/L~12g/L、中和酸2g/L~4g/L预先在副缸内用50℃~60℃的水溶解为染液,搅拌8~12分钟;
2)染槽温度50℃~60℃,染槽内加入质量分数20%~50%染液,开车运行一道;加入剩余染液,再开车运行一道;
3)元明粉加入总量为在染液中的浓度为55g/L~65g/L,运行时先加入元明粉加入总量的20%~50%的元明粉运行一道,再加入剩余元明粉运行一道;再保持50℃~60℃恒温染色二道后;碱粉加入总量为在染液中的浓度为8 g/L ~12g/L,运行时先加入碱粉加入总量的20%~50%的碱粉运行一道,再加入剩余碱粉运行一道;
4)保持50℃~60℃持续恒温染色十道;50℃~60℃水洗两道;加2~4g/L皂洗剂SN-45,升温90℃~95℃,运行三道;
5)冷水洗后加入中和酸2.5~3.5g/L,运行三道;酸洗后下卷。
纯棉双层提花布S型活性染料染色耐光牢度差,主要因为染料母体所含的乙烯砜、一氯均三嗪两个活性基为单侧型结构,与染料母体结合形成的共轭体系较短;S型活性染料三原色的配伍性不好,染色初期阶段,活性兰S-2GLN上染较快,导致卷染机染色两头布卷首尾色光偏兰,红光不足,造成首尾色差,缸头缸尾裁头数量较多,一般裁头6~8米。 发明人选用母体含有乙烯砜基、羟基乙烯砜硫酸酯基两个活性基团的活性染料,染色过程中通过加成反应,与纤维素羟基(-OH)形成醚键,有较好的耐气候牢度和光照牢度;同时,通过工艺控制保证原色配伍性好,染色过程中上染同步性高,卷染机染色首尾色差小,缸头缸尾裁头数量较少,裁头3~5米,经济效益明显。发明人将棉双层提花布染色的工艺改进配合选用的母体含有乙烯砜基、羟基乙烯砜硫酸酯基两个活性基团的活性染料,同时提升了皂洗牢度、染料的提升力、染料的上染速率及曲线、染料的配伍性等因素。
优选的,步骤1)中所述的染液配方为:母体含有乙烯砜基、羟基乙烯砜硫酸酯基两个活性基团的活性染料1.25%owf ~2.05%owf、元明粉58~60g/L、碱粉10~11g/L、中和酸3~3.5g/L。优选的染液配方达到本发明的最佳染色性能。
优选的,步骤1)中所述的母体含有乙烯砜基、羟基乙烯砜硫酸酯基两个活性基团的活性染料为Everzol Lx型活性染料。Everzol Lx型活性染料母体含有乙烯砜基、羟基乙烯砜硫酸酯基两个活性基团,符合本发明的染色要求。
优选的,步骤1)中所述的染槽内加入质量分数30%~35%的染液,开车运行一道;加入剩余染液,再开车运行一道。优选的第一道染色的染液用量能够达到最佳的预染效果,产品的耐气候牢度和光照牢度更好。
优选的,步骤3)中所述的加入元明粉加入总量的25%~30%的元明粉运行一道,加入剩余元明粉运行一道。优选的第一道元明粉的用量能够达到最佳的预处理效果,产品的色牢度更好。
优选的,步骤3)中所述的加入碱粉加入总量的30%~35%的碱粉运行一道,加入剩余碱粉运行一道。优选的第一道碱洗时碱粉的用量能够达到最佳的碱洗效果,更好的提高色牢度的同时能更好的保证织物色彩不褪色,不混色。
优选的,步骤5)中所述的水洗为加水升温至85℃~92℃一道一换,水洗二道;重新加水升温至75℃~85℃水洗一道;重新加水升温至50℃~60℃水洗一道。优选的水系工艺能够达到最佳的洗涤效果,更好的提高色牢度的同时能更好的保证织物色彩不褪色,不混色。
优选的,步骤5)中所述的冷水的温度为0℃~5℃。本发明在酸洗前先用冷水洗涤固色,能更好地保护植物的纤维强度,保证织物寿命并保持更好的触感。
原理解释:owf.是“On Weight the fabric”的缩写,是指浓度以织物重量为基准,相对织物重量的百分比。g/L 为浓度单位,表明在每升水中投料克数。元明粉、碱粉均为工业级,市场有售;皂洗剂斯诺夫SN-45,无锡德冠化工有限公司;中和酸,哈根化工有限公司。
与现有技术相比,本发明的一种纯棉双层提花家纺织物染整方法所具有的有益效果是:本发明针对现有技术的上述不足,优化、改进纯棉双层提花布卷染机生产工艺,提高产品的耐光色牢度,降低裁头率。本发明选用母体含有乙烯砜基、羟基乙烯砜硫酸酯基两个活性基团的活性染料,染色过程中通过加成反应,与纤维素羟基(-OH)形成醚键,有较好的耐气候牢度和光照牢度;同时,通过工艺控制保证原色配伍性好,染色过程中上染同步性高,卷染机染色首尾色差小,缸头缸尾裁头数量较少,裁头3~5米,经济效益明显。将棉双层提花布染色的工艺改进配合选用的母体含有乙烯砜基、羟基乙烯砜硫酸酯基两个活性基团的活性染料,同时提升了皂洗牢度、染料的提升力、染料的上染速率及曲线、染料的配伍性等因素。
具体实施方式
下面结合具体实施例对本发明做进一步说明,其中实施例1为最佳实施。其中,实施例和对比例所用纯棉双层提花布组织规格均为A层 40s*(12s+10s/2) 173*80 B层 60s*(21s+12s/2) 173*90,实施例采用优选的永光化学Everzol Lx型活性染料60℃恒温染色,对比例采用常规工艺S型活性染料70℃恒温染色。
实施例1
本实施例中生产纯棉双层提花布粉色,采用Everzol Lx型活性染料60℃恒温染色,其方法按如下步骤:
配方:Everzol Red LX 0.7%owf、Everzol Yellow LX 0.5%owf、Everzol BuleLX0.25% owf、明粉59g/L、碱粉10.5g/L、中和酸3.25g/L;
1)加染料:染槽温度60℃,染料预先在副缸内用50℃~60℃的水溶解,充分搅拌10分钟,加入质量分数32%染料,开车运行一道;加入剩余染料,开车运行一道;
2)加元明粉:60℃恒温染色加入质量分数28%的元明粉运行一道,加入剩余元明粉运行一道;
3)恒温染色:60℃恒温染色二道;
4)加碱粉:加入质量分数32%的碱粉运行一道,加入剩余碱粉运行一道;
5)恒温染色:60℃持续恒温染色十道;
6)温水洗:60℃水洗两道;
7)皂洗:加3g/L皂洗剂SN-45,升温95℃,运行三道,排掉废水;
8)热水洗:加水升温至90℃一道一换,水洗二道,排掉;
9)温水洗:加水升温至80℃水洗一道排掉;加水升温至60℃水洗一道排掉;
10)酸洗: 4℃冷水加入中和酸3g/L,运行三道;
11)酸洗后下卷。
实施例2
本实施例中生产纯棉双层提花布土黄色,采用Everzol Lx型活性染料60℃恒温染色,其方法按如下步骤:
Everzol Red LX 0.35%owf、Everzol Yellow LX 0.75%owf、Everzol Bule LX0.15%owf、元明粉60g/L、碱粉10g/L、中和酸3g/L;
1)加染料:染槽温度60℃,染料预先在副缸内用50℃~60℃的水溶解,充分搅拌10分钟,加入质量分数35%的染液,开车运行一道;加入剩余染料,开车运行一道;
2)加元明粉:60℃恒温染色加入质量分数25%的元明粉运行一道,加入剩余元明粉运行一道;
3)恒温染色:60℃恒温染色二道;
4)加碱粉:加入质量分数35%的碱粉运行一道,加入剩余碱粉运行一道;
5)恒温染色:60℃持续恒温染色十道;
6)温水洗:60℃水洗两道;
7)皂洗:加3.5g/L皂洗剂SN-45,升温93℃,运行三道,排掉废水;
8)热水洗:加水升温至91℃一道一换,水洗二道,排掉;
9)温水洗:加水升温至82℃水洗一道排掉;加水升温至60℃水洗一道排掉;
10)酸洗:冷水加入中和酸3.2g/L,运行三道;
11)酸洗后下卷。
实施例3
本实施例中生产纯棉双层提花布兰灰色,采用Everzol Lx型活性染料55℃恒温染色,其方法按如下步骤:
Everzol Red LX 0.35%owf、Everzol Yellow LX 0.575%owf、Everzol Bule LX0.325%owf、元明粉58g/L、碱粉11g/L、中和酸3.5g/L;
1)加染料:染槽温度55℃,染料预先在副缸内用55℃的水溶解,充分搅拌10分钟,加入质量分数30%的染液,开车运行一道;加入剩余染料,开车运行一道;
2)加元明粉:55℃恒温染色加入质量分数30%的元明粉运行一道,加入剩余元明粉运行一道;
3)恒温染色:55℃恒温染色二道;
4)加碱粉:加入质量分数30%的碱粉运行一道,加入剩余碱粉运行一道;
5)恒温染色:55℃持续恒温染色十道;
6)温水洗:55℃水洗两道;
7)皂洗:加2.5g/L皂洗剂SN-45,升温92℃,运行三道,排掉废水;
8)热水洗:加水升温至87℃一道一换,水洗二道,排掉;
9)温水洗:加水升温至78℃水洗一道排掉;加水升温至55℃水洗一道排掉;
10)酸洗:冷水加入中和酸2.8g/L,运行三道;
11)酸洗后下卷。
实施例4
本实施例中生产纯棉双层提花布兰灰色,采用Everzol Lx型活性染料50℃恒温染色,其方法按如下步骤:
配方:Everzol Red LX 0.5%owf、Everzol Yellow LX 0.25%owf、Everzol BuleLX0.05% owf、元明粉65g/L、碱粉12g/L、中和酸2g/L;
1)加染料:染槽温度50℃,染料预先在副缸内用50℃的水溶解,充分搅拌10分钟,加入1/2,开车运行一道;加入剩余1/2染料,开车运行一道;
2)加元明粉:50℃恒温染色加入1/2元明粉运行一道,加入剩余1/2元明粉运行一道;
3)恒温染色:50℃恒温染色二道;
4)加碱粉:加入1/2碱粉运行一道,加入剩余1/2碱粉运行一道;
5)恒温染色:50℃持续恒温染色十道;
6)温水洗:50℃水洗两道;
7)皂洗:加4g/L皂洗剂SN-45,升温95℃,运行三道,排掉废水;
8)热水洗:加水升温至85℃一道一换,水洗二道,排掉;
9)温水洗:加水升温至75℃水洗一道排掉;加水升温至50℃水洗一道排掉;
10)酸洗:冷水加入中和酸3.5g/L,运行三道;
11)酸洗后下卷。
实施例5
本实施例中生产纯棉双层提花布兰灰色,采用Everzol Lx型活性染料60℃恒温染色,其方法按如下步骤:
Everzol Red LX 0.85%owf、Everzol Yellow LX 0.775%owf、Everzol Bule LX0.825%owf、元明粉55g/L、碱粉8g/L、中和酸4g/L;
1)加染料:染槽温度60℃,染料预先在副缸内用50℃~60℃的水溶解,充分搅拌10分钟,加入质量分数20%的染料,开车运行一道;加入剩余染料,开车运行一道;
2)加元明粉:60℃恒温染色加入质量分数20%的元明粉运行一道,加入剩余元明粉运行一道;
3)恒温染色:60℃恒温染色二道;
4)加碱粉:加入质量分数20%的碱粉运行一道,加入剩余碱粉运行一道;
5)恒温染色:60℃持续恒温染色十道;
6)温水洗:60℃水洗两道;
7)皂洗:加2g/L皂洗剂SN-45,升温95℃,运行三道,排掉废水;
8)热水洗:加水升温至92℃一道一换,水洗二道,排掉;
9)温水洗:加水升温至85℃水洗一道排掉;加水升温至60℃水洗一道排掉;
10)酸洗:冷水加入中和酸2.5g/L,运行三道;
11)酸洗后下卷。
对比例1
本对比例中生产纯棉双层提花布粉色,采用S型活性染料70℃恒温染色,其方法按如下步骤:
配方:活性红S-2BF 0.45%owf、活性黄S-4RFN 0.225%owf、活性兰S-2GLN0.05% owf、元明粉60g/L、碱粉10g/L、中和酸3g/L;
1)加染料:染槽温度70℃,染料预先在副缸内用50℃~60℃的水溶解,充分搅拌10分钟,加入质量分数70%的,开车运行一道;加入剩余染料,开车运行一道;
2)加元明粉:70℃恒温染色加入质量分数70%的元明粉运行一道,加入剩余元明粉运行一道;
3)恒温染色:70℃恒温染色二道;
4)加碱粉:加入质量分数70%的碱粉运行一道,加入剩余碱粉运行一道;
5)恒温染色:70℃持续恒温染色十道;
6)温水洗:70℃水洗两道;
7)皂洗:加3g/L皂洗剂SN-45,升温95℃,运行三道,排掉废水;
8)热水洗:加水升温至90℃一道一换,水洗二道,排掉;
9)温水洗:加水升温至80℃水洗一道排掉;加水升温至60℃水洗一道排掉;
10)酸洗:冷水加入中和酸3g/L,运行三道;
11)酸洗后下卷。
对比例2
本对比例中生产纯棉双层提花布土黄色,采用S型活性染料70℃恒温染色,其方法按如下步骤:
Everzol Red LX 0.85%owf、Everzol Yellow LX 0.775%owf、Everzol Bule LX0.825%owf、元明粉55g/L、碱粉8g/L、中和酸4g/L;
1)加染料:染槽温度60℃,染料预先在副缸内用50℃~60℃的水溶解,充分搅拌10分钟,加入75,开车运行一道;加入剩余1/2染料,开车运行一道;
2)加元明粉:60℃恒温染色加入1/2元明粉运行一道,加入剩余1/2元明粉运行一道;
3)恒温染色:60℃恒温染色二道;
4)加碱粉:加入1/2碱粉运行一道,加入剩余1/2碱粉运行一道;
5)恒温染色:60℃持续恒温染色十道;
6)温水洗:60℃水洗两道;
7)皂洗:加3g/L皂洗剂SN-45,升温95℃,运行三道,排掉废水;
8)热水洗:加水升温至90℃一道一换,水洗二道,排掉;
9)温水洗:加水升温至80℃水洗一道排掉;加水升温至60℃水洗一道排掉;
10)酸洗:冷水加入中和酸3g/L,运行三道;
11)酸洗后下卷。
对比例3
本对比例中生产纯棉双层提花布兰灰色,采用S型活性染料70℃恒温染色,其方法按如下步骤:
Everzol Red LX 0.85%owf、Everzol Yellow LX 0.775%owf、Everzol Bule LX0.825%owf、元明粉55g/L、碱粉8g/L、中和酸4g/L;
1)加染料:染槽温度70℃,染料预先在副缸内用50℃~60℃的水溶解,充分搅拌10分钟,加入1/2,开车运行一道;加入剩余1/2染料,开车运行一道;
2)加元明粉:70℃恒温染色加入1/2元明粉运行一道,加入剩余1/2元明粉运行一道;
3)恒温染色:70℃恒温染色二道;
4)加碱粉:加入1/2碱粉运行一道,加入剩余1/2碱粉运行一道;
5)恒温染色:70℃持续恒温染色十道;
6)温水洗:70℃水洗两道;
7)皂洗:加3g/L皂洗剂SN-45,升温95℃,运行三道,排掉废水;
8)热水洗:加水升温至90℃一道一换,水洗二道,排掉;
9)温水洗:加水升温至80℃水洗一道排掉;加水升温至60℃水洗一道排掉;
10)酸洗:冷水加入中和酸3g/L,运行三道;
11)酸洗后下卷。
性能测试实验
耐摩擦牢度参照国家标准GB/T3920~2008进行试验,耐水洗色牢度参照国家标准GB/T5713~1997进行试验,耐汗渍牢度参照国家标准GB/T3922~1995进行试验,耐皂洗牢度参照国家标准GB/T3921~2008进行试验,耐光照色牢度采用自有设备光照48小时,用GB/T250-2008《评定变色用灰卡》评定色差级别。
附表1 实施例1~5的测试结果
附表2对比例1~3的测试结果
通过表1、2可看出,实施例1~5的耐摩擦牢度、耐水洗色牢度、耐汗渍牢度和耐皂洗牢度耐光照牢度等指标,与对比例1~3比较,要高出0.5~1级,具有较好的色牢度;实施例1~3的裁头数量与对比例1~3比较,平均每缸产品要少裁头2.7米。
以上所述,仅是本发明的较佳实施例而已,并非是对本发明作其它形式的限制,任何熟悉本专业的技术人员可能利用上述揭示的技术内容加以变更或改型为等同变化的等效实施例。但是凡是未脱离本发明技术方案内容,依据本发明的技术实质对以上实施例所作的任何简单修改、等同变化与改型,仍属于本发明技术方案的保护范围。

Claims (8)

1.一种纯棉双层提花家纺织物染整方法,其特征在于,制备步骤为:
1)制备染液,母体含有乙烯砜基、羟基乙烯砜硫酸酯基两个活性基团的活性染料0.8%owf ~2.45%owf预先在副缸内用50℃~60℃的水溶解为染液,搅拌8~12分钟;
2)染槽温度50℃~60℃,染槽内加入质量分数20%~50%染液,开车运行一道;加入剩余染液,再开车运行一道;
3)元明粉加入总量按使元明粉在染液中的浓度达到55 g/L ~65g/L计量,运行时先加入元明粉加入总量的20%~50%的元明粉运行一道,再加入剩余元明粉运行一道;再保持50℃~60℃恒温染色二道后;碱粉加入总量按使碱粉在染液中的浓度达到8 g/L ~12g/L计量,运行时先加入碱粉加入总量的20%~50%的碱粉运行一道,再加入剩余碱粉运行一道;
4)保持50℃~60℃持续恒温染色十道;50℃~60℃水洗两道;加2~4g/L皂洗剂SN-45,升温90℃~95℃,运行三道;
5)冷水洗后加入中和酸至中和酸浓度为2.5~3.5g/L,运行三道;酸洗后下卷。
2.根据权利要求1所述的一种纯棉双层提花家纺织物染整方法,其特征在于:步骤1)中所述的染液配方为:母体含有乙烯砜基、羟基乙烯砜硫酸酯基两个活性基团的活性染料1.25%owf ~2.05%owf、元明粉58~60g/L、碱粉10~11g/L、中和酸3~3.5g/L。
3.根据权利要求1所述的一种纯棉双层提花家纺织物染整方法,其特征在于:步骤1)中所述的母体含有乙烯砜基、羟基乙烯砜硫酸酯基两个活性基团的活性染料为Everzol Lx型活性染料。
4.根据权利要求1所述的一种纯棉双层提花家纺织物染整方法,其特征在于:步骤2)中所述的染槽内加入质量分数30%~35%的染液,开车运行一道;加入剩余染液,再开车运行一道。
5.根据权利要求1所述的一种纯棉双层提花家纺织物染整方法,其特征在于:步骤3)中所述的加入元明粉加入总量的25%~30%的元明粉运行一道,加入剩余元明粉运行一道。
6.根据权利要求1所述的一种纯棉双层提花家纺织物染整方法,其特征在于:步骤3)中所述的加入碱粉加入总量的30%~35%的碱粉运行一道,加入剩余碱粉运行一道。
7.根据权利要求1所述的一种纯棉双层提花家纺织物染整方法,其特征在于:步骤5)中所述的水洗为加水升温至85℃~92℃一道一换,水洗二道;重新加水升温至75℃~85℃水洗一道;重新加水升温至50℃~60℃水洗一道。
8.根据权利要求1所述的一种纯棉双层提花家纺织物染整方法,其特征在于:步骤5)中所述的冷水的温度为0℃~5℃。
CN201711464136.8A 2017-12-28 2017-12-28 一种纯棉双层提花家纺织物染整方法 Pending CN108130754A (zh)