WO2024071064A1 - 水分散体、炭素繊維束および一方向材 - Google Patents

水分散体、炭素繊維束および一方向材 Download PDF

Info

Publication number
WO2024071064A1
WO2024071064A1 PCT/JP2023/034807 JP2023034807W WO2024071064A1 WO 2024071064 A1 WO2024071064 A1 WO 2024071064A1 JP 2023034807 W JP2023034807 W JP 2023034807W WO 2024071064 A1 WO2024071064 A1 WO 2024071064A1
Authority
WO
WIPO (PCT)
Prior art keywords
less
resin
mass
ethylene
acid
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2023/034807
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
舜也 水野
祐一 伊東
雅裕 矢野
盛勳 林
政均 周
育昇 李
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Mitsui Chemicals Inc
Formosa Plastics Corp
Original Assignee
Mitsui Chemicals Inc
Formosa Plastics Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Mitsui Chemicals Inc, Formosa Plastics Corp filed Critical Mitsui Chemicals Inc
Priority to CN202380069559.7A priority Critical patent/CN120092116A/zh
Priority to EP23872287.0A priority patent/EP4596785A1/en
Priority to JP2024549386A priority patent/JPWO2024071064A1/ja
Priority to US19/116,146 priority patent/US20260103836A1/en
Publication of WO2024071064A1 publication Critical patent/WO2024071064A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F210/00—Copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond
    • C08F210/16—Copolymers of ethene with alpha-alkenes, e.g. EP rubbers
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F212/00—Copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and at least one being terminated by an aromatic carbocyclic ring
    • C08F212/02—Monomers containing only one unsaturated aliphatic radical
    • C08F212/04—Monomers containing only one unsaturated aliphatic radical containing one ring
    • C08F212/06—Hydrocarbons
    • C08F212/08—Styrene
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F220/00—Copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and only one being terminated by only one carboxyl radical or a salt, anhydride ester, amide, imide or nitrile thereof
    • C08F220/02—Monocarboxylic acids having less than ten carbon atoms; Derivatives thereof
    • C08F220/10—Esters
    • C08F220/12—Esters of monohydric alcohols or phenols
    • C08F220/16—Esters of monohydric alcohols or phenols of phenols or of alcohols containing two or more carbon atoms
    • C08F220/18—Esters of monohydric alcohols or phenols of phenols or of alcohols containing two or more carbon atoms with acrylic or methacrylic acids
    • C08F220/1804—C4-(meth)acrylate, e.g. butyl (meth)acrylate, isobutyl (meth)acrylate or tert-butyl (meth)acrylate
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F4/00—Polymerisation catalysts
    • C08F4/42—Metals; Metal hydrides; Metallo-organic compounds; Use thereof as catalyst precursors
    • C08F4/44—Metals; Metal hydrides; Metallo-organic compounds; Use thereof as catalyst precursors selected from light metals, zinc, cadmium, mercury, copper, silver, gold, boron, gallium, indium, thallium, rare earths or actinides
    • C08F4/60—Metals; Metal hydrides; Metallo-organic compounds; Use thereof as catalyst precursors selected from light metals, zinc, cadmium, mercury, copper, silver, gold, boron, gallium, indium, thallium, rare earths or actinides together with refractory metals, iron group metals, platinum group metals, manganese, rhenium technetium or compounds thereof
    • C08F4/62—Refractory metals or compounds thereof
    • C08F4/64—Titanium, zirconium, hafnium or compounds thereof
    • C08F4/659—Component covered by group C08F4/64 containing a transition metal-carbon bond
    • C08F4/65908—Component covered by group C08F4/64 containing a transition metal-carbon bond in combination with an ionising compound other than alumoxane, e.g. (C6F5)4B-X+
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F8/00—Chemical modification by after-treatment
    • C08F8/46—Reaction with unsaturated dicarboxylic acids or anhydrides thereof, e.g. maleinisation
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J5/00—Manufacture of articles or shaped materials containing macromolecular substances
    • C08J5/04—Reinforcing macromolecular compounds with loose or coherent fibrous material
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J5/00—Manufacture of articles or shaped materials containing macromolecular substances
    • C08J5/04—Reinforcing macromolecular compounds with loose or coherent fibrous material
    • C08J5/0405—Reinforcing macromolecular compounds with loose or coherent fibrous material with inorganic fibres
    • C08J5/042—Reinforcing macromolecular compounds with loose or coherent fibrous material with inorganic fibres with carbon fibres
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J5/00—Manufacture of articles or shaped materials containing macromolecular substances
    • C08J5/04—Reinforcing macromolecular compounds with loose or coherent fibrous material
    • C08J5/06—Reinforcing macromolecular compounds with loose or coherent fibrous material using pretreated fibrous materials
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L33/00—Compositions of homopolymers or copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and only one being terminated by only one carboxyl radical, or of salts, anhydrides, esters, amides, imides or nitriles thereof; Compositions of derivatives of such polymers
    • C08L33/04—Homopolymers or copolymers of esters
    • C08L33/06—Homopolymers or copolymers of esters of esters containing only carbon, hydrogen and oxygen, which oxygen atoms are present only as part of the carboxyl radical
    • C08L33/08—Homopolymers or copolymers of acrylic acid esters
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L75/00—Compositions of polyureas or polyurethanes; Compositions of derivatives of such polymers
    • C08L75/04—Polyurethanes
    • D—TEXTILES; PAPER
    • D01—NATURAL OR MAN-MADE THREADS OR FIBRES; SPINNING
    • D01F—CHEMICAL FEATURES IN THE MANUFACTURE OF ARTIFICIAL FILAMENTS, THREADS, FIBRES, BRISTLES OR RIBBONS; APPARATUS SPECIALLY ADAPTED FOR THE MANUFACTURE OF CARBON FILAMENTS
    • D01F11/00—Chemical after-treatment of artificial filaments or the like during manufacture
    • D01F11/10—Chemical after-treatment of artificial filaments or the like during manufacture of carbon
    • D01F11/14—Chemical after-treatment of artificial filaments or the like during manufacture of carbon with organic compounds, e.g. macromolecular compounds
    • D—TEXTILES; PAPER
    • D06—TREATMENT OF TEXTILES OR THE LIKE; LAUNDERING; FLEXIBLE MATERIALS NOT OTHERWISE PROVIDED FOR
    • D06M—TREATMENT, NOT PROVIDED FOR ELSEWHERE IN CLASS D06, OF FIBRES, THREADS, YARNS, FABRICS, FEATHERS OR FIBROUS GOODS MADE FROM SUCH MATERIALS
    • D06M15/00—Treating fibres, threads, yarns, fabrics, or fibrous goods made from such materials, with macromolecular compounds; Such treatment combined with mechanical treatment
    • D06M15/19—Treating fibres, threads, yarns, fabrics, or fibrous goods made from such materials, with macromolecular compounds; Such treatment combined with mechanical treatment with synthetic macromolecular compounds
    • D06M15/195—Treating fibres, threads, yarns, fabrics, or fibrous goods made from such materials, with macromolecular compounds; Such treatment combined with mechanical treatment with synthetic macromolecular compounds sulfated or sulfonated
    • D—TEXTILES; PAPER
    • D06—TREATMENT OF TEXTILES OR THE LIKE; LAUNDERING; FLEXIBLE MATERIALS NOT OTHERWISE PROVIDED FOR
    • D06M—TREATMENT, NOT PROVIDED FOR ELSEWHERE IN CLASS D06, OF FIBRES, THREADS, YARNS, FABRICS, FEATHERS OR FIBROUS GOODS MADE FROM SUCH MATERIALS
    • D06M15/00—Treating fibres, threads, yarns, fabrics, or fibrous goods made from such materials, with macromolecular compounds; Such treatment combined with mechanical treatment
    • D06M15/19—Treating fibres, threads, yarns, fabrics, or fibrous goods made from such materials, with macromolecular compounds; Such treatment combined with mechanical treatment with synthetic macromolecular compounds
    • D06M15/21—Macromolecular compounds obtained by reactions only involving carbon-to-carbon unsaturated bonds
    • D06M15/227—Macromolecular compounds obtained by reactions only involving carbon-to-carbon unsaturated bonds of hydrocarbons, or reaction products thereof, e.g. afterhalogenated or sulfochlorinated
    • D—TEXTILES; PAPER
    • D06—TREATMENT OF TEXTILES OR THE LIKE; LAUNDERING; FLEXIBLE MATERIALS NOT OTHERWISE PROVIDED FOR
    • D06M—TREATMENT, NOT PROVIDED FOR ELSEWHERE IN CLASS D06, OF FIBRES, THREADS, YARNS, FABRICS, FEATHERS OR FIBROUS GOODS MADE FROM SUCH MATERIALS
    • D06M15/00—Treating fibres, threads, yarns, fabrics, or fibrous goods made from such materials, with macromolecular compounds; Such treatment combined with mechanical treatment
    • D06M15/19—Treating fibres, threads, yarns, fabrics, or fibrous goods made from such materials, with macromolecular compounds; Such treatment combined with mechanical treatment with synthetic macromolecular compounds
    • D06M15/21—Macromolecular compounds obtained by reactions only involving carbon-to-carbon unsaturated bonds
    • D06M15/263—Macromolecular compounds obtained by reactions only involving carbon-to-carbon unsaturated bonds of unsaturated carboxylic acids; Salts or esters thereof
    • D—TEXTILES; PAPER
    • D06—TREATMENT OF TEXTILES OR THE LIKE; LAUNDERING; FLEXIBLE MATERIALS NOT OTHERWISE PROVIDED FOR
    • D06M—TREATMENT, NOT PROVIDED FOR ELSEWHERE IN CLASS D06, OF FIBRES, THREADS, YARNS, FABRICS, FEATHERS OR FIBROUS GOODS MADE FROM SUCH MATERIALS
    • D06M15/00—Treating fibres, threads, yarns, fabrics, or fibrous goods made from such materials, with macromolecular compounds; Such treatment combined with mechanical treatment
    • D06M15/19—Treating fibres, threads, yarns, fabrics, or fibrous goods made from such materials, with macromolecular compounds; Such treatment combined with mechanical treatment with synthetic macromolecular compounds
    • D06M15/21—Macromolecular compounds obtained by reactions only involving carbon-to-carbon unsaturated bonds
    • D06M15/263—Macromolecular compounds obtained by reactions only involving carbon-to-carbon unsaturated bonds of unsaturated carboxylic acids; Salts or esters thereof
    • D06M15/27—Macromolecular compounds obtained by reactions only involving carbon-to-carbon unsaturated bonds of unsaturated carboxylic acids; Salts or esters thereof of alkylpolyalkylene glycol esters of unsaturated carboxylic acids
    • D—TEXTILES; PAPER
    • D06—TREATMENT OF TEXTILES OR THE LIKE; LAUNDERING; FLEXIBLE MATERIALS NOT OTHERWISE PROVIDED FOR
    • D06M—TREATMENT, NOT PROVIDED FOR ELSEWHERE IN CLASS D06, OF FIBRES, THREADS, YARNS, FABRICS, FEATHERS OR FIBROUS GOODS MADE FROM SUCH MATERIALS
    • D06M15/00—Treating fibres, threads, yarns, fabrics, or fibrous goods made from such materials, with macromolecular compounds; Such treatment combined with mechanical treatment
    • D06M15/19—Treating fibres, threads, yarns, fabrics, or fibrous goods made from such materials, with macromolecular compounds; Such treatment combined with mechanical treatment with synthetic macromolecular compounds
    • D06M15/37—Macromolecular compounds obtained otherwise than by reactions only involving carbon-to-carbon unsaturated bonds
    • D06M15/53—Polyethers
    • D—TEXTILES; PAPER
    • D06—TREATMENT OF TEXTILES OR THE LIKE; LAUNDERING; FLEXIBLE MATERIALS NOT OTHERWISE PROVIDED FOR
    • D06M—TREATMENT, NOT PROVIDED FOR ELSEWHERE IN CLASS D06, OF FIBRES, THREADS, YARNS, FABRICS, FEATHERS OR FIBROUS GOODS MADE FROM SUCH MATERIALS
    • D06M15/00—Treating fibres, threads, yarns, fabrics, or fibrous goods made from such materials, with macromolecular compounds; Such treatment combined with mechanical treatment
    • D06M15/19—Treating fibres, threads, yarns, fabrics, or fibrous goods made from such materials, with macromolecular compounds; Such treatment combined with mechanical treatment with synthetic macromolecular compounds
    • D06M15/37—Macromolecular compounds obtained otherwise than by reactions only involving carbon-to-carbon unsaturated bonds
    • D06M15/55—Epoxy resins
    • D—TEXTILES; PAPER
    • D06—TREATMENT OF TEXTILES OR THE LIKE; LAUNDERING; FLEXIBLE MATERIALS NOT OTHERWISE PROVIDED FOR
    • D06M—TREATMENT, NOT PROVIDED FOR ELSEWHERE IN CLASS D06, OF FIBRES, THREADS, YARNS, FABRICS, FEATHERS OR FIBROUS GOODS MADE FROM SUCH MATERIALS
    • D06M15/00—Treating fibres, threads, yarns, fabrics, or fibrous goods made from such materials, with macromolecular compounds; Such treatment combined with mechanical treatment
    • D06M15/19—Treating fibres, threads, yarns, fabrics, or fibrous goods made from such materials, with macromolecular compounds; Such treatment combined with mechanical treatment with synthetic macromolecular compounds
    • D06M15/37—Macromolecular compounds obtained otherwise than by reactions only involving carbon-to-carbon unsaturated bonds
    • D06M15/564—Polyureas, polyurethanes or other polymers having ureide or urethane links; Precondensation products forming them
    • D—TEXTILES; PAPER
    • D06—TREATMENT OF TEXTILES OR THE LIKE; LAUNDERING; FLEXIBLE MATERIALS NOT OTHERWISE PROVIDED FOR
    • D06M—TREATMENT, NOT PROVIDED FOR ELSEWHERE IN CLASS D06, OF FIBRES, THREADS, YARNS, FABRICS, FEATHERS OR FIBROUS GOODS MADE FROM SUCH MATERIALS
    • D06M15/00—Treating fibres, threads, yarns, fabrics, or fibrous goods made from such materials, with macromolecular compounds; Such treatment combined with mechanical treatment
    • D06M15/693—Treating fibres, threads, yarns, fabrics, or fibrous goods made from such materials, with macromolecular compounds; Such treatment combined with mechanical treatment with natural or synthetic rubber, or derivatives thereof
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
    • C08F2420/00—Metallocene catalysts
    • C08F2420/06—Cp analog where at least one of the carbon atoms of the non-coordinating part of the condensed ring is replaced by a heteroatom
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J2323/00—Characterised by the use of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Derivatives of such polymers
    • C08J2323/02—Characterised by the use of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Derivatives of such polymers not modified by chemical after treatment
    • C08J2323/04—Homopolymers or copolymers of ethene
    • C08J2323/08—Copolymers of ethene
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J2323/00—Characterised by the use of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Derivatives of such polymers
    • C08J2323/02—Characterised by the use of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Derivatives of such polymers not modified by chemical after treatment
    • C08J2323/16—Ethene-propene or ethene-propene-diene copolymers
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J2423/00—Characterised by the use of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Derivatives of such polymers
    • C08J2423/02—Characterised by the use of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Derivatives of such polymers not modified by chemical after treatment
    • C08J2423/04—Homopolymers or copolymers of ethene
    • C08J2423/08—Copolymers of ethene
    • D—TEXTILES; PAPER
    • D06—TREATMENT OF TEXTILES OR THE LIKE; LAUNDERING; FLEXIBLE MATERIALS NOT OTHERWISE PROVIDED FOR
    • D06M—TREATMENT, NOT PROVIDED FOR ELSEWHERE IN CLASS D06, OF FIBRES, THREADS, YARNS, FABRICS, FEATHERS OR FIBROUS GOODS MADE FROM SUCH MATERIALS
    • D06M2101/00—Chemical constitution of the fibres, threads, yarns, fabrics or fibrous goods made from such materials, to be treated
    • D06M2101/40—Fibres of carbon
    • D—TEXTILES; PAPER
    • D06—TREATMENT OF TEXTILES OR THE LIKE; LAUNDERING; FLEXIBLE MATERIALS NOT OTHERWISE PROVIDED FOR
    • D06M—TREATMENT, NOT PROVIDED FOR ELSEWHERE IN CLASS D06, OF FIBRES, THREADS, YARNS, FABRICS, FEATHERS OR FIBROUS GOODS MADE FROM SUCH MATERIALS
    • D06M2200/00—Functionality of the treatment composition and/or properties imparted to the textile material
    • D06M2200/40—Reduced friction resistance, lubricant properties; Sizing compositions
    • D—TEXTILES; PAPER
    • D10—INDEXING SCHEME ASSOCIATED WITH SUBLASSES OF SECTION D, RELATING TO TEXTILES
    • D10B—INDEXING SCHEME ASSOCIATED WITH SUBLASSES OF SECTION D, RELATING TO TEXTILES
    • D10B2101/00—Inorganic fibres
    • D10B2101/10—Inorganic fibres based on non-oxides other than metals
    • D10B2101/12—Carbon; Pitch

Definitions

  • the present invention relates to an aqueous dispersion, a carbon fiber bundle, and a unidirectional material.
  • Carbon fiber is lightweight, strong, and rigid, and is therefore used as a reinforcing material in a wide range of fields. Carbon fiber is also sometimes used in combination with thermoplastic resin to form fiber-reinforced resin. This fiber-reinforced resin is similarly used in a wide range of fields, as it has excellent mechanical properties and dimensional stability.
  • Patent Document 1 describes a masterbatch resin composition that contains an ethylene- ⁇ -olefin copolymer that meets certain requirements.
  • Polyolefin resins are sometimes used as matrix resins for fiber-reinforced resins.
  • polypropylene resins are used as the matrix resin.
  • the use of polyolefin resins as treatment agents for carbon fibers has also been considered.
  • Patent Document 2 describes the use of carbon fiber bundles treated with a fiber treatment agent containing a specific propylene resin in a fiber-reinforced resin composition suitable for a tape winding molding method using a laser fusion method. Patent Document 2 describes that the carbon fiber bundles are less likely to produce fuzz when rubbed.
  • Patent Document 2 describes that treating carbon fiber bundles with a fiber treatment agent containing a specific propylene-based resin suppresses the generation of fuzz when rubbed.
  • a fiber treatment agent containing a specific propylene-based resin suppresses the generation of fuzz when rubbed.
  • the carbon fibers may protrude from the cut end surface and generate fuzz.
  • fiber-reinforced resins in which carbon fibers are oriented in one direction are often cut into tape-like shapes for use, and the generation of fuzz from the cut end surface can easily become a problem.
  • the inventors therefore investigated various methods for more efficiently suppressing the generation of fuzz from the cut end surfaces, and found that the use of hydrocarbon-based synthetic oils could suppress the generation of fuzz to the same extent as or even better than that of Patent Document 2.
  • hydrocarbon-based synthetic oils were used, the interlayer shear strength (ILSS) decreased when UD sheets were laminated and fused, and the concentration of carbon fibers decreased, resulting in poor processability.
  • ILSS interlayer shear strength
  • the present invention has been made in consideration of the above problems, and aims to provide an aqueous dispersion containing a resin component that can be used as a bundling agent for carbon fiber bundles used in unidirectional materials, which can suppress the generation of fuzz from the cut end surface when carbon fiber bundles are cut, and can also improve the ILSS and bundling ability of carbon fibers when UD sheets are stacked and fused, as well as carbon fiber bundles for use in unidirectional materials obtained by treating carbon fibers with the aqueous dispersion, and unidirectional materials.
  • the resin component contains an ethylene/ ⁇ -olefin copolymer (A) or an acid-modified product thereof (B) that satisfies all of the following requirements (a1) to (a3):
  • the ratio of the total mass of the resin component to the total mass of the aqueous dispersion is 0.01% by mass or more and 50% by mass or less.
  • Water dispersion. (a1) the kinetic viscosity at 100°C is 10 mm2/s or more and 5,000 mm2 /s or less; (a2) the content of structural units derived from ethylene is 30 mol% or more and 85 mol% or less; (a3) the molecular weight distribution (Mw/Mn) of the molecular weight measured by gel permeation chromatography (GPC) and calculated as polystyrene is 2.5 or less.
  • An aqueous dispersion in which a resin component is dispersed in water and used for bundling carbon fibers used in the production of a unidirectional material in which carbon fibers oriented in one direction are impregnated with a resin
  • the resin component is A first resin component which is an ethylene/ ⁇ -olefin copolymer (A) or an acid-modified product thereof (B) satisfying all of the following requirements (a1) to (a3):
  • a second resin component which is at least one resin selected from the group consisting of an acrylic resin (C), a urethane resin (D) and a diene rubber (E),
  • the ratio of the total mass of the resin component to the total mass of the aqueous dispersion is 0.01% by mass or more and 50% by mass or less.
  • Water dispersion (a1) a kinetic viscosity at 100°C of 10 mm2/s or more and 5,000 mm2 /s or less; (a2) a content of structural units derived from ethylene of 30 mol% or more and 85 mol% or less; and (a3) a molecular weight distribution (Mw/Mn) measured by gel permeation chromatography (GPC) and calculated as polystyrene is 2.5 or less.
  • Mw/Mn molecular weight distribution measured by gel permeation chromatography
  • a first resin component which is an ethylene- ⁇ -olefin copolymer (A) or an acid-modified product (B) thereof which satisfies all of the requirements (a1) to (a3), and a second resin component which is at least one resin selected from the group consisting of an acrylic resin (C), a urethane resin (D), and a diene rubber (E).
  • [5] The aqueous dispersion according to any one of [1] to [4], wherein the copolymer (A) satisfies at least one of the following requirements (a4) to (a7): (a4) The weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) and calculated as polystyrene is 1,000 or more and 50,000 or less. (a5) The B value represented by the following formula [1] is 1.1 or more.
  • P E represents the content (mol %) of structural units derived from ethylene
  • P O represents the content (mol %) of structural units derived from ⁇ -olefins
  • P OE represents the content (mol %) of ethylene- ⁇ -olefin chains in all dyad chains.
  • the sizing agent contains an ethylene/ ⁇ -olefin copolymer (A) or an acid-modified product thereof (B) that satisfies all of the following requirements (a1) to (a3): the storage modulus at 25° C.
  • a resin component of the sizing agent containing the ethylene/ ⁇ -olefin copolymer (A) or the acid-modified copolymer (B) thereof is 100 MPa or more and 100,000 MPa or less; Carbon fiber bundle.
  • the kinetic viscosity at 100°C is 10 mm2/s or more and 5,000 mm2 /s or less;
  • the content of structural units derived from ethylene is 30 mol% or more and 85 mol% or less; and
  • Mw/Mn molecular weight distribution of the molecular weight obtained by measuring by gel permeation chromatography (GPC) and converting it into polystyrene is 2.5 or less.
  • a carbon fiber bundle formed by bundling carbon fibers used for producing a unidirectional material formed by impregnating unidirectionally oriented carbon fibers with a resin The carbon fibers are bundled by a bundling agent attached to the carbon fibers,
  • the sizing agent comprises a first resin component which is an ethylene/ ⁇ -olefin copolymer (A) or an acid-modified product thereof (B) satisfying all of the following requirements (a1) to (a3): and a second resin component which is at least one resin selected from the group consisting of an acrylic resin (C), a urethane resin (D), and a diene rubber (E). Carbon fiber bundle.
  • a first resin component which is an ethylene- ⁇ -olefin copolymer (A) or an acid-modified product (B) thereof which satisfies all of the requirements (a1) to (a3), and a second resin component which is at least one resin selected from the group consisting of an acrylic resin (C), a urethane resin (D), and a diene rubber (E).
  • Another aspect of the present invention for solving the above problems relates to the carbon fiber bundles according to the following [13] to [15].
  • Unidirectional material [14] The unidirectional material according to [13], having a thin film shape.
  • the present invention provides an aqueous dispersion containing a resin component that can be used as a bundling agent for carbon fiber bundles used in unidirectional materials, which can suppress the generation of fuzz from the cut end surface when carbon fiber bundles are cut, and can improve the ILSS and bundling ability of carbon fibers when UD sheets are stacked and fused, as well as carbon fiber bundles used in unidirectional materials obtained by treating carbon fibers with the aqueous dispersion, and unidirectional fibers.
  • Aqueous Dispersion One embodiment of the present invention relates to an aqueous dispersion in which a resin component is dispersed in water, which is used for bundling carbon fibers used in the manufacture of unidirectional materials.
  • the above aqueous dispersion contains a resin component and water as a dispersion medium.
  • Resin Component contains an ethylene/ ⁇ -olefin copolymer (A) or an acid-modified product thereof (B).
  • the ethylene/ ⁇ -olefin copolymer (A) satisfies all of the following requirements (a1) to (a3):
  • (a1) The kinematic viscosity at 100°C is 10 mm2/s or more and 5,000 mm2 /s or less.
  • the content of structural units derived from ethylene is 30 mol% or more and 85 mol% or less.
  • Mw/Mn The molecular weight distribution (Mw/Mn) of the molecular weight obtained by measuring by gel permeation chromatography (GPC) and converting it into polystyrene is 2.5 or less.
  • the kinetic viscosity of the ethylene/ ⁇ -olefin copolymer (A) which satisfies the requirement (a1) is a value measured by the method described in JIS K2283 (2000).
  • the kinetic viscosity of the ethylene/ ⁇ -olefin copolymer (A) is from 10 mm 2 /s to 5,000 mm 2 /s, preferably from 10 mm 2 /s to 2,500 mm 2 /s, more preferably from 15 mm 2 /s to 2,500 mm 2 /s, and even more preferably from 15 mm 2 /s to 500 mm 2 /s.
  • the ethylene/ ⁇ -olefin copolymer (A) has a kinetic viscosity of 10 mm 2 /s or more, the amount of easily volatile components tends to be reduced, the copolymer is less likely to ignite, and storage stability tends to be improved, and further, the weight loss of the aqueous dispersion due to volatilization tends to be reduced.
  • the ethylene/ ⁇ -olefin copolymer (A) has a kinetic viscosity of 5,000 mm2 /s or less, the ethylene/ ⁇ -olefin copolymer (A) becomes soft and viscous oil-like, so that it adheres to the surface of the carbon fiber and easily suppresses the generation of fluff, and also makes it easier for the resin component to disperse more uniformly in water.
  • the content of structural units derived from ethylene in the ethylene/ ⁇ -olefin copolymer (A) which satisfies requirement (a2) is a value obtained by measuring with 13 C-NMR according to the method described in "Polymer Analysis Handbook" (Asakura Publishing, first edition, published in 2008, pp. 184-211). Alternatively, it may be a value obtained by measuring a sample obtained by this method as a known sample using Fourier transform infrared spectroscopy (FT-IR).
  • FT-IR Fourier transform infrared spectroscopy
  • the content of structural units derived from ethylene in the ethylene/ ⁇ -olefin copolymer (A) is 30 mol% or more and 85 mol% or less, preferably 40 mol% or more and 70 mol% or less, and more preferably 45 mol% or more and 65 mol% or less.
  • the content of structural units derived from ethylene in the ethylene/ ⁇ -olefin copolymer (A) is 85 mol% or less, crystallization of the ethylene/ ⁇ -olefin copolymer (A) is unlikely to occur, and as a result, the viscosity of the copolymer is unlikely to increase, and the generation of fluff is easily suppressed.
  • the resin component is less likely to become solid, and is more likely to disperse uniformly in water.
  • the molecular weight distribution (Mw/Mn) of the ethylene- ⁇ -olefin copolymer (A) which is requirement (a3) is the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) measured by the above GPC.
  • the molecular weight distribution (Mw/Mn) of the ethylene- ⁇ -olefin copolymer (A) is 2.5 or less, preferably 2.3 or less, and more preferably 2.0 or less.
  • the larger the molecular weight distribution (Mw/Mn) of the polymer the more low molecular weight components and high molecular weight components the polymer contains.
  • the molecular weight distribution (Mw/Mn) of the ethylene- ⁇ -olefin copolymer (A) is 2.5 or less, the amount of low molecular weight components is reduced, so that the amount of easily volatile components is reduced, the copolymer is less likely to ignite, and the shelf life tends to improve, and further the weight loss of the aqueous dispersion due to volatilization tends to be reduced.
  • the molecular weight distribution (Mw/Mn) of the ethylene- ⁇ -olefin copolymer (A) is 2.5 or less, the amount of high molecular weight components is reduced, so that the resin components tend to be more uniformly dispersed in water.
  • the lower limit of the molecular weight distribution (Mw/Mn) is not particularly limited, but is usually 1.0 or more.
  • the ethylene/ ⁇ -olefin copolymer (A) preferably satisfies at least one of the following requirements (a4) to (a7) in addition to the above requirements (a1) to (a3).
  • the weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) and calculated as polystyrene is 1,000 or more and 50,000 or less.
  • the B value represented by the following formula [1] is 1.1 or more.
  • P E represents the content (mol %) of structural units derived from ethylene
  • P O represents the content (mol %) of structural units derived from ⁇ -olefins
  • P OE represents the content (mol %) of ethylene- ⁇ -olefin chains in all dyad chains.
  • the ethylene/ ⁇ -olefin copolymer (A) satisfies at least two of the above requirements (a4) to (a7), even more preferable that it satisfies any three requirements, and particularly preferable that it satisfies all requirements.
  • the weight average molecular weight (Mw) of the ethylene- ⁇ -olefin copolymer (A) which is requirement (a4) is the weight average molecular weight (Mw) measured by the above GPC.
  • the weight average molecular weight (Mw) of the ethylene- ⁇ -olefin copolymer (A) is preferably 1,000 to 50,000, more preferably 1,500 to 30,000, even more preferably 1,500 to 20,000, and particularly preferably 1,500 to 7,000.
  • the weight average molecular weight (Mw) of the ethylene- ⁇ -olefin copolymer (A) is 1,000 or more, the amount of easily volatile components tends to be reduced, the copolymer is less likely to ignite, and the shelf life tends to be improved, and the weight loss of the aqueous dispersion due to volatilization tends to be reduced.
  • the weight average molecular weight (Mw) of the ethylene- ⁇ -olefin copolymer (A) is 50,000 or less, the resin component tends to be more uniformly dispersed in water.
  • the B value of the ethylene/ ⁇ -olefin copolymer (A) satisfying requirement (a5) is an index showing the randomness of the distribution of copolymerized monomer sequences in the molecular chain of the ethylene/ ⁇ -olefin copolymer (A).
  • P E , P O and P OE in formula [1] can be determined by measuring a 13 C-NMR spectrum based on known documents such as reports by J. C. Randall [Macromolecules, 15, 353 (1982)] and J. Ray [Macromolecules, 10, 773 (1977)], "Polymer Analysis Handbook" (Asakura Publishing, first edition, published in 2008, pp. 184-211).
  • the B value of the ethylene/ ⁇ -olefin copolymer (A) is preferably 1.1 or more, and more preferably 1.2 or more.
  • the upper limit of the B value of the ethylene/ ⁇ -olefin copolymer (A) is not particularly limited, but is usually 2.0 or less.
  • the larger the B value the fewer the chain structures of each constituent unit (constituent units derived from ethylene or constituent units derived from other ⁇ -olefins), the more uniform the distribution of these constituent units, and the narrower the composition distribution of the copolymer.
  • the B value of the ethylene/ ⁇ -olefin copolymer (A) is 1.1 or more, crystallization of the ethylene/ ⁇ -olefin copolymer (A) is less likely to occur, and as a result, the viscosity of the copolymer is less likely to increase, making it easier to suppress the generation of fluff.
  • the copolymer is less likely to become solid, and the resin components are more likely to disperse uniformly in water.
  • the amount of unsaturated bonds in the ethylene/ ⁇ -olefin copolymer (A) which is requirement (a6) is the number of unsaturated bonds per 1000 carbon atoms measured by 1 H-NMR.
  • unsaturated bonds include double bonds derived from vinyl compounds, vinylidene compounds, di-substituted olefin compounds, tri-substituted olefin compounds, etc.
  • the amount of unsaturated bonds in the ethylene/ ⁇ -olefin copolymer (A) is preferably less than 0.5, more preferably less than 0.3, even more preferably less than 0.2, and particularly preferably less than 0.1.
  • the amount of unsaturated bonds in the ethylene/ ⁇ -olefin copolymer (A) is less than 0.5, the oxidative stability and heat resistance of the ethylene/ ⁇ -olefin copolymer (A) are improved, and the heat resistance of the sizing agent also tends to be improved.
  • Requirement (a7) that the melting point of the ethylene- ⁇ -olefin copolymer (A) is not observed means that the heat of fusion ( ⁇ H) (unit: J/g) measured by differential scanning calorimetry (DSC) is not substantially measured, that is, in differential scanning calorimetry (DSC), no peak is observed within the measurement range below, or the observed heat of fusion is 1 J/g or less.
  • ⁇ H heat of fusion
  • DSC differential scanning calorimetry
  • the melting point (Tm) and heat of fusion ( ⁇ H) are determined by analyzing the DSC curve obtained by differential scanning calorimetry (DSC) when the ethylene- ⁇ -olefin copolymer (A) cooled to -100°C is heated to 150°C at a heating rate of 10°C/min, based on JIS K7121 (2012). If the ethylene- ⁇ -olefin copolymer (A) is a polymer for which a melting point (Tm) is not observed, crystallization of the ethylene- ⁇ -olefin copolymer (A) is unlikely to occur, and as a result, the viscosity of the copolymer is unlikely to increase, making it easier to suppress the generation of fluff. It also makes it less likely to become solid, making it easier for the resin components to disperse more evenly in water.
  • DSC differential scanning calorimetry
  • the above requirements (a1) to (a7) can be adjusted by methods known to those skilled in the art.
  • the kinetic viscosity of the ethylene- ⁇ -olefin copolymer (A) at 100°C can be adjusted by the molecular weight. If the ethylene- ⁇ -olefin copolymer (A) has a high molecular weight, the viscosity can be high, and if the ethylene- ⁇ -olefin copolymer (A) has a low molecular weight, the viscosity can be low.
  • the molecular weight distribution (Mw/Mn) (requirement (a3)) of the ethylene- ⁇ -olefin copolymer (A) can be adjusted by removing low molecular weight components by a known method such as reduced pressure distillation. Furthermore, the amount of unsaturated bonds (requirement (a6)) can be reduced by hydrogenation by a known method.
  • Ethylene- ⁇ -olefin copolymer (A) is a copolymer of ethylene and an ⁇ -olefin other than ethylene.
  • the ⁇ -olefin include linear or branched ⁇ -olefins having 3 to 20 carbon atoms, such as propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene.
  • linear or branched ⁇ -olefins having 3 to 10 carbon atoms are preferred, with propylene, 1-butene, 1-hexene, and 1-octene being more preferred.
  • propylene is preferred from the viewpoint of further increasing the fluidity of the aqueous dispersion.
  • the ethylene/ ⁇ -olefin copolymer (A) may also contain structural units derived from monomers other than ⁇ -olefins, such as polar group-containing monomers, aromatic vinyl compounds, alicyclic vinyl compounds, and cyclic olefins.
  • the content of the structural units derived from monomers other than the ⁇ -olefins is preferably 20 parts by mass or less, and more preferably 10 parts by mass or less, per 100 parts by mass of the total amount of structural units derived from ethylene and ⁇ -olefins.
  • the ethylene/ ⁇ -olefin copolymer (A) may be used alone or in combination of two or more.
  • two or more ethylene/ ⁇ -olefin copolymers (A) each having a different type of ⁇ -olefin may be used in combination.
  • the above requirements (a1) to (a7) are values obtained from the total of the multiple types of ethylene/ ⁇ -olefin copolymers (A).
  • the acid-modified product (B) is an acid-modified product obtained by acid-modifying the above-mentioned ethylene- ⁇ -olefin copolymer (A). It is known that the acid-modified product (B) tends to improve the stability of the aqueous dispersion when it is made into an aqueous dispersion, compared with the above-mentioned ethylene- ⁇ -olefin copolymer (A). This is disclosed, for example, in JP 2016-102157 A.
  • the acid-modified product (B) can be, for example, a polymer in which the ethylene- ⁇ -olefin copolymer (A) has been graft-modified with a graft component.
  • a polymer in which the ethylene- ⁇ -olefin copolymer (A) has been graft-modified with a graft component When the amount of unsaturated bonds in the ethylene- ⁇ -olefin copolymer (A) is small (for example, when the requirement (a6) described above is satisfied), it is presumed that the graft component is randomly graft-bonded to the main chain skeleton of the ethylene- ⁇ -olefin copolymer (A).
  • Examples of the graft component include unsaturated carboxylic acids having 3 to 10 carbon atoms (preferably 3 to 8 carbon atoms) and derivatives of the unsaturated carboxylic acids.
  • Examples of derivatives of the unsaturated carboxylic acids include anhydrides, esters, amides, and imides of unsaturated carboxylic acids.
  • Examples of the unsaturated carboxylic acids include monobasic acids such as acrylic acid and methacrylic acid, and dibasic acids such as maleic acid, fumaric acid, itaconic acid, citraconic acid, and 5-norbornene-2,3-dicarboxylic acid.
  • Examples of the anhydrides of the unsaturated carboxylic acids include anhydrides of dibasic acids such as maleic acid, itaconic acid, citraconic acid, and 5-norbornene-2,3-dicarboxylic acid.
  • Examples of the esters of the unsaturated carboxylic acids include esters or half esters such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, glycidyl acrylate, monoethyl maleate, diethyl maleate, monomethyl fumarate, dimethyl fumarate, monomethyl itaconic acid, and diethyl itaconic acid.
  • Examples of the amidations of the unsaturated carboxylic acids include acrylamide, methacrylamide, monoamide maleate, diamide maleate, N-monoethyl maleate, N,N-diethyl maleate, N-monobutyl maleate, N,N-dibutyl maleate, monoamide fumarate, diamide fumarate, N-monobutyl fumarate, and N,N-dibutyl fumarate.
  • Examples of the imides of the unsaturated carboxylic acids include maleimide, N-butylmaleimide, and N-phenylmaleimide.
  • maleic acid and maleic anhydride are preferred because they have high polarity as a single monomer and are less likely to produce by-products such as homopolymers in a modification reaction using peroxide.
  • These graft components can be used alone or in combination of two or more.
  • the acid-modified product (B) preferably satisfies at least one of the following requirements (b1) to (b4).
  • the acid value is 1 mgKOH/g or more and 300 mgKOH/g or less.
  • the apparent viscosity at 150°C is 1 cPs or more and 1,000 cPs or less.
  • the weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) and calculated as polystyrene is 1,000 or more and 50,000 or less.
  • the molecular weight distribution (Mw/Mn) measured by gel permeation chromatography (GPC) and calculated as polystyrene is 2.5 or less.
  • the acid-modified product (B) satisfies at least two of the above requirements (b1) to (b4), even more preferable that it satisfies any three of the requirements, and particularly preferable that it satisfies all of the requirements.
  • the acid value of the acid-modified product (B), which is requirement (b1), is a value indicating the number of milligrams of potassium hydroxide required to neutralize the acid contained in 1 g of the acid-modified product (B), and is an index of the graft amount of the graft component.
  • This acid value is a value measured by a method conforming to JIS K0070 (1992).
  • the acid value of the acid-modified product (B) is preferably 1 mgKOH/g or more and 300 mgKOH/g or less, more preferably 5 mgKOH/g or more and 200 mgKOH/g or less, and even more preferably 10 mgKOH/g or more and 150 mgKOH/g or less.
  • the oxidation of the acid-modified product (B) is 1 mgKOH/g or more, the polarity of the acid-modified product (B) becomes high, and the stability of the aqueous dispersion tends to improve.
  • the acid-modified product (B) has an oxidation level of 300 mg KOH/g or less, hydrogen bonding between the graft components is suppressed, the increase in viscosity of the acid-modified product (B) is suppressed, and the resin component tends to disperse more uniformly in water.
  • the acid value of the acid-modified product (B) can be adjusted by the graft amount of the graft component to the ethylene- ⁇ -olefin copolymer (A). For example, the acid value of the acid-modified product (B) can be increased by increasing the graft amount.
  • the apparent viscosity (Brookfield viscosity) of the acid-modified product (B) at 150°C, which is requirement (b2), is the Brookfield viscosity measured by the method described in JIS K7117-1 (1999).
  • the apparent viscosity of the acid-modified product (B) at 150°C is preferably 1 cPs or more and 1,000 cPs or less, more preferably 5 cPs or more and 800 cPs or less, and even more preferably 5 cPs or more and 50 cPs or less.
  • the acid-modified product (B) tends to have an excellent balance between low volatility and handleability and dispersibility in water.
  • the weight average molecular weight (Mw) of the acid-modified product (B), which satisfies requirement (b3), is preferably 1,000 to 50,000, more preferably 1,000 to 30,000, even more preferably 1,500 to 30,000, and particularly preferably 2,000 to 10,000.
  • the weight average molecular weight (Mw) of the acid-modified product (B) is 1,000 or more, the amount of easily volatile components tends to be reduced, the product tends to be less flammable, the product tends to have improved storage stability, and the weight loss of the aqueous dispersion due to volatilization tends to be reduced.
  • the weight average molecular weight (Mw) of the acid-modified product (B) is 50,000 or less, the resin component tends to be uniformly dispersed in water.
  • the molecular weight distribution (Mw/Mn) of the acid-modified product (B), which is requirement (b4), is preferably 2.5 or less, more preferably 2.3 or less, and even more preferably 2.0 or less.
  • Mw/Mn molecular weight distribution of the acid-modified product (B)
  • the amount of low molecular weight components is reduced, which reduces the amount of easily volatile components, making the product less flammable and tending to improve storage stability, and also tends to reduce the amount of weight loss of the aqueous dispersion due to volatilization.
  • the molecular weight distribution (Mw/Mn) of the ethylene- ⁇ -olefin copolymer (A) is 2.5 or less, the amount of high molecular weight components is reduced, which makes it easier for the resin components to be dispersed more uniformly in water.
  • the lower limit of the molecular weight distribution (Mw/Mn) is not particularly limited, but is usually 1.0 or more.
  • the acid-modified product (B) preferably further satisfies the following requirement (b5): (b5) No melting point observed
  • the acid-modified substance (B) is preferably a polymer with no observable melting point (Tm).
  • Tm melting point
  • Tm no observable melting point
  • the method for measuring the melting point (Tm) of the acid-modified substance (B) and the definition of no observable melting point (Tm) are as explained in requirement (a7) for the ethylene- ⁇ -olefin copolymer (A). If the acid-modified substance (B) is a polymer with no observable melting point (Tm), crystallization of the acid-modified substance (B) is unlikely to occur, and as a result, the viscosity of the copolymer is unlikely to increase, it is unlikely to become solid, and the resin component is likely to disperse more uniformly in water.
  • the acid-modified substance (B) may be used alone or in combination of two or more.
  • two or more types of acid-modified substances (B) having different types of ⁇ -olefins may be used in combination.
  • the above requirements (b1) to (b5) are values obtained from the total of the multiple types of acid-modified substances (B).
  • the use of the ethylene- ⁇ -olefin copolymer (A) or its acid-modified product (B) can more efficiently suppress the generation of fluff from the cut end surface of bundled carbon fibers. Further, according to further findings of the present inventors, when the resin component containing the ethylene- ⁇ -olefin copolymer (A) or its acid-modified product (B) further satisfies the following requirement (I) or (II), the ILSS of the laminate formed by fusing and laminating UD sheets produced using bundled carbon fibers can be increased, and the bundling property of the carbon fibers can also be improved.
  • the storage modulus at 25° C. is 100 MPa or more and 100,000 MPa or less.
  • the composition further contains an acrylic resin (C), a urethane resin (D), and a diene rubber (E).
  • the resin component needs to satisfy at least one of the above requirements (I) and (II), but it is preferable for it to satisfy both.
  • the ethylene- ⁇ -olefin copolymer (A) or its acid-modified form (B) is also referred to simply as the "first resin component”
  • the acrylic resin (C), urethane resin (D), and diene rubber (E) are also referred to simply as the "second resin component.”
  • the ethylene- ⁇ -olefin copolymer (A) or its acid-modified form (B) is used as a bundling material, the generation of fuzz is suppressed more than ever before, but it is difficult to improve both the ILSS and the bundling ability at the same time.
  • the amount of these resin components attached to the carbon fibers is small, it is difficult to improve the bundling ability of the carbon fibers, and on the other hand, if the amount of these resin components attached is large, it is difficult to increase the ILSS of the laminate formed by fusing and laminating UD sheets using carbon fibers.
  • the bundling property of the carbon fibers can be improved regardless of the amount of the resin component attached to the carbon fibers. It is believed that improving the bundling property also makes it possible to more efficiently suppress the generation of fuzz from the cut end surface.
  • the ethylene- ⁇ -olefin copolymer (A) or its acid-modified form (B) as a bundling material and setting the storage modulus of the resin component at 25°C to 100 MPa or more, the cohesive force when made into a laminate is improved, and the ILSS of the laminate made by fusing and stacking UD sheets using carbon fibers can be increased.
  • the ethylene- ⁇ -olefin copolymer (A) or its acid-modified form (B) as a bundling material and setting the storage modulus of the resin component at 25°C to 100,000 MPa or less, the fuzzing suppression effect of the ethylene- ⁇ -olefin copolymer (A) or its acid-modified form (B) is fully exerted, and fuzzing from the cut end surface can be sufficiently suppressed.
  • a shear stress occurs in the direction of peeling between layers in a laminate formed by fusing and stacking UD sheets using carbon fiber, cracks that occur in the resin part and the propagation of the cracks can be suppressed, and the ILSS of the laminate can be increased.
  • the storage modulus of the resin component at 25°C is preferably 1,000 MPa or more and 100,000 MPa or less, and more preferably 10,000 MPa or more and 100,000 MPa or less.
  • the storage modulus of the resin component at 25°C can be adjusted to the above range by using the above-mentioned ethylene- ⁇ -olefin copolymer (A) or its acid-modified form (B) in combination with another resin having a higher storage modulus.
  • the other resin may be the second resin component described in requirement (II), or may be another resin component such as an epoxy resin or an olefin resin (excluding the ethylene- ⁇ -olefin copolymer (A) and its acid-modified form (B)).
  • the ILSS of the laminate obtained by fusing and laminating UD sheets produced using bundled carbon fibers can be increased, and the bundling property of the carbon fibers can also be improved.
  • the urethane resin (D) is preferred from the viewpoints of increasing the ILSS and the convergence property, and also enhancing the effect of suppressing fuzz.
  • These second resin components may be used alone or in combination of two or more types.
  • the acrylic resin (C) is a polymeric compound containing 40 mass% or more of structural units derived from monomers having a (meth)acryloyl group based on the total amount of all structural units, however, in this specification, polymeric compounds corresponding to the diene rubber (E) are not included in the acrylic resin (C).
  • (meth)acryloyl means acryloyl and methacryloyl
  • (meth)acrylic means acrylic and methacrylic
  • (meth)acrylate means acrylate and methacrylate
  • (meth)acrylo means acrylo and methacrylo.
  • the acrylic resin (C) contains a structural unit derived from a monomer having one unsaturated vinyl group in the molecule. From the viewpoint of obtaining a desired storage modulus, the acrylic resin (C) may contain a structural unit derived from a monomer having two or more unsaturated vinyl groups in the molecule.
  • Examples of monomers having one unsaturated vinyl group in the molecule include (meth)acrylic acid ester monomers, aromatic vinyl monomers, vinyl ester monomers, vinyl cyan compound monomers, halogenated monomers, olefin monomers, diene monomers, other vinyl monomers, unsaturated carboxylic acids, and acrylamides. Of these, acrylic acid ester monomers, methacrylic acid ester monomers, aromatic vinyl monomers, vinyl ester monomers, vinyl cyan compound monomers, unsaturated carboxylic acids, acrylamides, and hydroxyl group-containing monomers are preferred.
  • Examples of (meth)acrylic acid ester monomers include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-amyl (meth)acrylate, isoamyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, octadecyl (meth)acrylate, cyclohexyl (meth)acrylate, phenyl (meth)acrylate, benzyl (meth)acrylate, and glycidyl (meth)acrylate.
  • the (meth)acrylic acid ester monomer may be a monomer having a hydroxyl group.
  • monomers having a hydroxyl group include 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate.
  • aromatic vinyl monomers examples include styrene, p-methylstyrene, ⁇ -methylstyrene, 2-methylstyrene, vinyltoluene, t-butylstyrene, chlorostyrene, vinylxylene, vinylnaphthalene, vinylanthracene, vinylanisole, and divinylbenzene.
  • Examples of vinyl ester monomers include vinyl acetate.
  • Examples of vinyl cyanide compounds include (meth)acrylonitrile.
  • Examples of halogenated monomers include vinylidene chloride and vinyl chloride.
  • Examples of olefin monomers include ethylene and propylene.
  • Examples of diene monomers include butadiene and chloroprene.
  • Examples of other vinyl monomers include vinyl ether, vinyl ketone, and vinyl pyrrolidone.
  • Examples of unsaturated carboxylic acids include (meth)acrylic acid, itaconic acid, fumaric acid, and maleic acid.
  • Examples of acrylamides include (meth)acrylamide and N,N'-dimethyl(meth)acrylamide.
  • Examples of monomers having two or more unsaturated vinyl groups in the molecule include di(meth)acrylate, tri(meth)acrylate, tetra(meth)acrylate, hexadi(meth)acrylate, divinylbenzene, and methylenebis(meth)acrylamide.
  • monomers having two or more unsaturated vinyl groups in the molecule include polyethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate, 1,6-butylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, polypropylene glycol di(meth)acrylate, 2,2'-bis(4-(meth)acryloxypropyloxyphenyl)propane, and 2,2'-bis(4-(meth)acryloxydiethoxyphenyl)propane.
  • di(meth)acrylates including trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, and tetramethylolmethane tri(meth)acrylate; tetra(meth)acrylates including ditrimethyloltetra(meth)acrylate, tetramethylolmethane tetra(meth)acrylate, and pentaerythritol tetra(meth)acrylate; hexa(meth)acrylates including dipentaerythritol hexa(meth)acrylate; methylenebis(meth)acrylamide; and divinylbenzene.
  • These monomers may be used alone or in combination of two or more.
  • the acrylic resin (C) is blended in the form of a water dispersion, such as a water dispersion polymerized by emulsion polymerization or a self-emulsifying water dispersion having hydrophilic groups in the molecular skeleton including the terminals.
  • a water dispersion such as a water dispersion polymerized by emulsion polymerization or a self-emulsifying water dispersion having hydrophilic groups in the molecular skeleton including the terminals.
  • the urethane resin (D) is a polymeric compound having a urethane bond in the main chain, and is typically a polymeric compound obtained by bonding a polyisocyanate, a polyol, and an optionally used chain extender.
  • polyisocyanates include aromatic isocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, polymeric diphenylmethane diisocyanate, tolidine diisocyanate, naphthalene diisocyanate, xylylene diisocyanate, and tetramethylxylylene diisocyanate, aliphatic isocyanates such as hexamethylene diisocyanate, trimethylhexamethylene diisocyanate, and isophorone diisocyanate, and alicyclic isocyanates.
  • aromatic isocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, polymeric diphenylmethane diisocyanate, tolidine diisocyanate, naphthalene diisocyanate, xylylene diisocyanate, and tetramethylxylylene diisocyanate
  • polyols examples include polyether-based polyols, including polyethylene glycol, polypropylene glycol, and polytetramethylene glycol, as well as polycarbonate-based polyols, including polyhexamethylene carbonate, etc.
  • chain extenders include low molecular weight glycols such as ethylene glycol, as well as compounds with active hydrogen atoms such as low molecular weight diamines and low molecular weight amino alcohols.
  • the urethane-based resin (D) is blended in the form of an aqueous dispersion, such as a self-emulsifying aqueous dispersion having hydrophilic groups in the molecular skeleton including the terminals. From the same viewpoint, it is also preferable that the urethane-based resin (D) is self-crosslinking, which can form a crosslinked structure by evaporating water.
  • the diene rubber (E) is a polymeric rubber compound having a structural unit derived from a diene monomer in the main chain.
  • the diene rubber (E) preferably contains 10 mass% or more of the structural unit derived from the diene monomer based on the total amount of all structural units.
  • the diene rubber (E) is a polymeric compound obtained by polymerizing a diene monomer and a monomer having an unsaturated vinyl group that can be copolymerized with the diene monomer.
  • diene monomers examples include butadiene, isoprene, and chloroprene.
  • Examples of monomers having an unsaturated vinyl group that can be copolymerized with diene monomers include monofunctional monomers such as styrene, ethylene, acrylonitrile, and alkyl (meth)acrylates, as well as polyfunctional monomers such as divinylbenzene, ethylene glycol dimethacrylate, butylene glycol diacrylate, triallyl cyanurate, triallyl isocyanurate, trimethylolpropane triacrylate, and pentaerythritol tetraacrylate.
  • monofunctional monomers such as styrene, ethylene, acrylonitrile, and alkyl (meth)acrylates
  • polyfunctional monomers such as divinylbenzene, ethylene glycol dimethacrylate, butylene glycol diacrylate, triallyl cyanurate, triallyl isocyanurate, trimethylolpropane triacrylate, and pentaerythritol tetraacrylate.
  • the diene rubber (E) is compounded in the form of a water dispersion.
  • the diene rubber (E) can be dispersed in water using an emulsifier component such as a surfactant.
  • the second resin component is preferably compatible with the first resin component.
  • the term “multiple types of resin components are compatible” means that when these resin components are heated to a temperature 10°C higher than the melting points of all the resins (or the glass transition temperature when no melting point is observed), mixed, and then cooled to 25°C, a single phase is formed as seen with the naked eye. Note that when the resin components include one with a melting point (or glass transition temperature) of 0°C or lower, this means that a single phase is formed as seen with the naked eye when these resin components are mixed at 10°C.
  • the ratio of the first resin component to the second resin component, by mass, is preferably 10/90 or more and 90/10 or less, more preferably 20/80 or more and 85/15 or less, and even more preferably 30/70 or more and 80/20 or less.
  • first resin component/second resin component By increasing the amount of the first resin component, it is possible to more efficiently suppress the generation of fuzz from the cut end surface.
  • second resin component By increasing the amount of the second resin component, it is possible to further improve the bundling property and to further increase the ILSS of the laminate formed by fusing and laminating UD sheets made using bundled carbon fibers.
  • the water dispersion is prepared by dispersing the above-mentioned resin component in water.
  • the ratio of the total mass of the resin components to the total mass of the aqueous dispersion is 0.01% by mass or more and 50% by mass or less.
  • the ratio of the resin components is preferably 10% by mass or more and 50% by mass or less, more preferably 15% by mass or more and 45% by mass or more, and even more preferably 20% by mass or more and 40% by mass or less.
  • the resin components are diluted with water, and the ratio of the resin components is preferably 0.01% by mass or more and 20% by mass or less, more preferably 0.05% by mass or more and 10% by mass or less, and even more preferably 0.1% by mass or more and 5% by mass or less.
  • the proportion of the total mass of water to the total mass of the water dispersion is 50% by mass or more and 99.99% by mass or less.
  • the proportion of water is preferably 50% by mass or more and 90% by mass or less, more preferably 55% by mass or more and 85% by mass or less, and even more preferably 60% by mass or more and 80% by mass or less.
  • the proportion of water is preferably 80% by mass or more and 99.99% by mass or less, more preferably 90% by mass or more and 99.95% by mass or less, and even more preferably 95% by mass or more and 99.9% by mass or less.
  • the total content of the water and resin components in the aqueous dispersion is preferably 60% by mass or more and 99% by mass or less, more preferably 70% by mass or less and 95% by mass or less, and even more preferably 80% by mass or more and 95% by mass or less, based on the total mass of the aqueous dispersion.
  • the aqueous dispersion may contain other components such as surfactants, pH adjusters, and organic solvents.
  • the content of the above-mentioned other components in the aqueous dispersion is preferably 1% by mass or more and 40% by mass or less, more preferably 5% by mass or more and 30% by mass or less, and even more preferably 5% by mass or more and 20% by mass or less, based on the total mass of the aqueous dispersion.
  • the aqueous dispersion can be prepared by mixing the above components.
  • Another embodiment of the present invention relates to a carbon fiber bundle bundled using the above-mentioned resin component as a bundling agent.
  • This carbon fiber bundle is used to produce a fiber-reinforced resin (unidirectional material) in which the carbon fibers are oriented in one direction.
  • the carbon fiber bundle has a plurality of carbon fibers bundled by a bundling agent that is a resin component adhered to the carbon fibers, and the resin component contains the above-mentioned ethylene- ⁇ -olefin copolymer (A) or its acid-modified product (B).
  • the resin component further satisfies the above-described requirement (I) or (II).
  • the storage modulus at 25° C. is 100 MPa or more and 100,000 MPa or less.
  • the composition further contains an acrylic resin (C), a urethane resin (D), and a diene rubber (E).
  • the amount of resin component attached to the carbon fibers is preferably 0.1% by mass or more and 5.0% by mass or less, more preferably 0.2% by mass or more and 3.0% by mass or less, even more preferably 0.2% by mass or more and 2.0% by mass or less, and particularly preferably 0.5% by mass or more and 1.5% by mass or less, based on the total mass of the carbon fibers.
  • the amount of attachment is 0.1% by mass or more, the bundling property tends to be further improved.
  • the amount of attachment is 5.0% by mass or less, the ILSS of the laminate formed by fusing and laminating UD sheets made using bundled carbon fibers can be further increased.
  • the average fiber diameter of the carbon fibers is not particularly limited, but from the viewpoint of improving both the mechanical properties and the surface appearance of the resulting molded article, it is preferably 1 ⁇ m or more and 20 ⁇ m or less, and more preferably 3 ⁇ m or more and 15 ⁇ m or less.
  • the number of single fibers in the carbon fiber bundle is not particularly limited, but is usually 100 to 350,000, preferably 1,000 to 250,000, and more preferably 5,000 to 220,000.
  • the above-mentioned aqueous dispersion also shows excellent effects when used for fiber bundles (large tow) with 40,000 or more fibers.
  • the carbon fiber bundle can be produced by applying the above-mentioned aqueous dispersion to carbon fibers and drying them. From the viewpoint of uniformly attaching the resin component between the individual fibers, it is preferable that the aqueous dispersion is applied by a roller dipping method, a roller transfer method, a spray method, or the like.
  • Unidirectional Material Another embodiment of the present invention relates to a unidirectional material obtained by impregnating the above-mentioned carbon fiber bundle with a resin.
  • the unidirectional material may be in the form of a thin film (UD sheet) or pellets.
  • the resin may be a thermoplastic resin or a thermosetting resin.
  • the resin may be a crystalline resin or a non-crystalline resin.
  • thermoplastic resins examples include polyolefin resins such as polyethylene, polypropylene, polybutene, and poly4-methyl-1-pentene, polyamide resins, polyester resins, polystyrene resins, thermoplastic polyimide resins, polyamideimide resins, polycarbonate resins, polyphenylene ether resins, polyphenylene sulfide resins, polyacetal resins, acrylic resins, polyetherimide resins, polysulfone resins, polyether ketone resins, polyether ether ketone resins, polyarylate resins, polyether nitrile resins, polyvinyl chloride resins, ABS resins, and fluororesins.
  • polyolefin resins such as polyethylene, polypropylene, polybutene, and poly4-methyl-1-pentene
  • polyamide resins such as polyethylene, polypropylene, polybutene, and poly4-methyl-1-pentene
  • polyester resins such as polyethylene, polyprop
  • thermosetting resins examples include epoxy resins, phenolic resins, melamine resins, urea resins, diallyl phthalate resins, silicone resins, urethane resins, furan resins, ketone resins, xylene resins, thermosetting polyimide resins, unsaturated polyester resins, and diallyl terephthalate resins.
  • thermoplastic resins are preferred from the viewpoint of improving the moldability of the unidirectional material.
  • thermoplastic resins polyamide resins and polyolefin resins are preferred, with polyolefin resins being more preferred from the viewpoint of enabling molding at lower temperatures and improving production efficiency, and polypropylene being even more preferred from the viewpoints of light weight, high rigidity, low water absorption, and improved chemical resistance and chemical stability.
  • the resin may be a resin composition containing additives.
  • additives include known fillers (inorganic fillers, organic fillers), pigments, dyes, weathering stabilizers, heat stabilizers, antistatic agents, antislip agents, antioxidants, antifungal agents, antibacterial agents, flame retardants, and softeners.
  • the resin when unidirectional materials are fused to each other or to other members by laser irradiation, the resin is preferably a resin composition containing a dye that absorbs the laser of the irradiated wavelength.
  • the dye may be any dye that absorbs light of any wavelength between 300 nm and 3000 nm, and is preferably carbon black.
  • the content of the carbon fiber bundles is preferably 1 part by mass or more and 80 parts by mass or less, more preferably 30 parts by mass or more and 75 parts by mass or less, even more preferably 30 parts by mass or more and 60 parts by mass or less, and particularly preferably 35 parts by mass or more and 60 parts by mass or less.
  • the content of the matrix resin is preferably 20 parts by mass or more and 99 parts by mass or less, more preferably 25 parts by mass or more and 70 parts by mass or less, even more preferably 35 parts by mass or more and 70 parts by mass or less, and particularly preferably 40 parts by mass or more and 65 parts by mass or less.
  • the thickness of the unidirectional material is usually 1 to 500 ⁇ m.
  • the unidirectional material can be produced by aligning the spread carbon fiber bundles and bringing them into contact with the above-mentioned resin that has been made flowable by melting or other means.
  • the unidirectional material can be used as it is, or multiple layers can be laminated together to form an integrated laminate.
  • the thickness of the unidirectional material is preferably 1 to 500 ⁇ m, more preferably 5 to 400 ⁇ m, particularly preferably 10 to 300 ⁇ m, and most preferably 10 to 250 ⁇ m.
  • the thickness of the unidirectional material can be adjusted by laminating sheet- or tape-shaped unidirectional material using methods such as press molding, stamp molding, and tape winding molding.
  • the unidirectional material of this embodiment can effectively prevent fuzz from forming on the cut end surface when it is cut into a tape shape. For this reason, it is preferable to use it in the form of a tape.
  • Tape-shaped unidirectional material is useful, for example, as a material for tape winding molding.
  • the tape-shaped unidirectional material is brought into contact with a mandrel and fused by laser irradiation (using thermoplastic resin as the resin). Note that fusion can also be achieved by heating instead of using a laser.
  • the unidirectional material of this embodiment is suitable for use in automobile parts, electrical and electronic parts, and household and office electrical appliance parts.
  • the tape-shaped unidirectional material can also be used favorably for external reinforcement of various containers such as pipes and pressure vessels.
  • the physical properties of the ethylene- ⁇ -olefin copolymer (A) and the acid-modified product (B) were measured using the following methods.
  • Viscosity Characteristics The kinetic viscosity at 100° C. was measured and calculated in accordance with JIS K2283 (2000). The apparent viscosity (Brookfield viscosity) at 150° C. was measured and calculated in accordance with JIS K7117-1 (1999).
  • HLC-8320GPC manufactured by Tosoh Corporation.
  • TSKgel SuperMultipore HZ-M 4 columns was used, the column temperature was 40°C, tetrahydrofuran (manufactured by Wako Pure Chemical Industries, Ltd.) was used as the mobile phase, the development speed was 0.35 ml/min, the sample concentration was 5.5 g/L, the sample injection amount was 20 microliters, and a differential refractometer was used as a detector.
  • PStQuick MP-M As a standard polystyrene, PStQuick MP-M manufactured by Tosoh Corporation was used. According to the procedure of general-purpose calibration, the weight average molecular weight (Mw) and number average molecular weight (Mn) were calculated as polystyrene molecular weight equivalents, and the molecular weight distribution (Mw/Mn) was calculated from these values.
  • PE represents the content (mol %) of structural units derived from ethylene
  • PO represents the content (mol %) of ⁇ -olefin units
  • POE represents the content (mol %) of ethylene- ⁇ -olefin chains in all dyad chains.
  • Amount of unsaturated bonds 1H -NMR spectrum 400 MHz, ECX400P manufactured by JEOL Ltd. was measured using o-dichlorobenzene-d4 as the measurement solvent under the following measurement conditions: measurement temperature 120°C, spectrum width 20 ppm, pulse repetition time 7.0 seconds, and pulse width 6.15 ⁇ sec (45° pulse).
  • the solvent peak ortho-dichlorobenzene 7.1 ppm was used as the chemical shift standard, and the amount of unsaturated bonds per 1000 carbon atoms (units/1000C) was calculated from the ratio of the integral value of the main peak observed at 0-3 ppm to the peak derived from unsaturated bonds observed at 4-6 ppm.
  • the temperature at which the enthalpy curve obtained during the heating process showed a maximum value was taken as the melting point (Tm), and the sum of the endothermic heats associated with melting was taken as the heat of fusion ( ⁇ H). If no peak was observed within the above range, or if the value of the heat of fusion ( ⁇ H) was 1 J/g or less, it was considered that the melting point (Tm) was not observed.
  • the melting point (Tm) and heat of fusion ( ⁇ H) were determined in accordance with JIS K7121 (2012).
  • the ethylene-propylene copolymer (A) had a content of structural units derived from ethylene of 48.5 mol%, a weight average molecular weight (Mw) of 5,165, a molecular weight distribution (Mw/Mn) of 1.7, a B value of 1.2, a kinetic viscosity at 100°C of 152 mm2 /s, an unsaturated bond amount of less than 0.1 bonds/1000°C, a chlorine content of less than 0.1 ppm, and no melting point (melting peak) was observed.
  • This acid-modified material (B) had a weight average molecular weight (Mw) of 7,170, a molecular weight distribution (Mw/Mn) of 1.8, an apparent viscosity (Brookfield viscosity) at 150°C of 71 cPs, an acid value of 60 mgKOH/g, and no melting point (melting peak) was observed.
  • the extruded resin mixture was cooled to 110°C using a jacketed static mixer installed at the extruder port, and then poured into warm water at 80°C to obtain an aqueous dispersion (emulsion) of polypropylene resin.
  • the solid content concentration of the resulting aqueous dispersion was 45% by mass.
  • the obtained aqueous emulsion was cooled to room temperature, and then ion-exchanged water and an aqueous ammonium solution were added to adjust the solid content to 50% by weight and the pH to 7.5, to obtain an aqueous dispersion of acrylic resin (C1).
  • Acrylic resins (C2) to (C5) were obtained in the same manner as for the synthesis of acrylic resin (C1), except that the ratios of each monomer and t-dodecyl mercaptan as a chain transfer agent added when preparing the emulsion were changed to the ratios shown in Table 1.
  • the ratios of each monomer shown in Table 1 indicate the mass ratio (mass%) to the total amount of monomers.
  • E Water Dispersion of Diene Rubber
  • Diene Rubber (each of them is a water dispersion having a solid content concentration of 50% by mass) were prepared.
  • E1 NALSTAR SR-116, manufactured by Nippon A&L Co., Ltd.
  • E2 NALSTAR MR-171, manufactured by Nippon A&L Co., Ltd.
  • E3 Cyatex NA-106, manufactured by Nippon A&L Co., Ltd.
  • This resin liquid was cooled to 60°C, 11.5 g of 29% ammonia water was added, and the mixture was stirred for 30 minutes while maintaining the temperature at 60°C. Then, 175.6 g of ion-exchanged water was added dropwise over 30 minutes. Next, 6.3 parts by mass of an anionic surfactant (Pelex (registered trademark) OT-P, sodium dialkyl sulfosuccinate, manufactured by Kao Corporation) was added and mixed to obtain an aqueous dispersion (emulsion) of an epoxy resin. The solid content concentration of the obtained aqueous dispersion was 25% by mass.
  • an anionic surfactant Pelex (registered trademark) OT-P, sodium dialkyl sulfosuccinate, manufactured by Kao Corporation
  • this resin was extruded and supplied to the peripheral surface of the rotating impregnated roller from the T-die.
  • the temperatures of the extruder and the T-die were adjusted to 260° C., and the temperature of the impregnation roller was also adjusted to 260° C.
  • the amount of resin supplied was adjusted so that the mass ratio of the carbon fiber bundles to the resin was 67/33.
  • the viscoelasticity of the liquid dried body or the dried sheet was measured using a viscoelasticity measuring device (TA Instruments, ARES-G2) at a measurement frequency of 1 Hz, a measurement temperature of 0°C to 150°C (measured from the high temperature side), a temperature rise rate of 3°C/min, and under nitrogen to obtain the storage modulus G' at 25°C.
  • a viscoelasticity measuring device T Instruments, ARES-G2
  • ILSS Interlaminar shear stress
  • the obtained UD sheet laminate was cut out to prepare five test pieces (20 mm x 10 mm), and the interlaminar shear stress (ILSS) was measured in accordance with ASTM D2344 using a short span bending tester (Shimadzu Autograph AG-5KNX, manufactured by Shimadzu Corporation), and the average value was calculated. Evaluation was performed according to the following evaluation criteria. -Evaluation criteria- ⁇ : ILSS was 25 MPa or more. ⁇ : ILSS was 20 MPa or more and less than 25 MPa. ⁇ : ILSS was less than 20 MPa.
  • the aqueous dispersion of the present invention can suppress fuzzing of unidirectional materials while improving ILSS and convergence. Therefore, the present invention is expected to open up possibilities for using unidirectional materials in more diverse applications and contribute to the development of various fields related to unidirectional materials.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Engineering & Computer Science (AREA)
  • Textile Engineering (AREA)
  • Polymers & Plastics (AREA)
  • Organic Chemistry (AREA)
  • Health & Medical Sciences (AREA)
  • Medicinal Chemistry (AREA)
  • Materials Engineering (AREA)
  • Manufacturing & Machinery (AREA)
  • General Chemical & Material Sciences (AREA)
  • Crystallography & Structural Chemistry (AREA)
  • Inorganic Chemistry (AREA)
  • Compositions Of Macromolecular Compounds (AREA)
  • Treatments For Attaching Organic Compounds To Fibrous Goods (AREA)
  • Addition Polymer Or Copolymer, Post-Treatments, Or Chemical Modifications (AREA)
PCT/JP2023/034807 2022-09-28 2023-09-26 水分散体、炭素繊維束および一方向材 Ceased WO2024071064A1 (ja)

Priority Applications (4)

Application Number Priority Date Filing Date Title
CN202380069559.7A CN120092116A (zh) 2022-09-28 2023-09-26 水分散体、碳纤维束及单向材料
EP23872287.0A EP4596785A1 (en) 2022-09-28 2023-09-26 Water dispersion, carbon fiber bundle, and unidirectional material
JP2024549386A JPWO2024071064A1 (cg-RX-API-DMAC7.html) 2022-09-28 2023-09-26
US19/116,146 US20260103836A1 (en) 2022-09-28 2023-09-26 Water dispersion, carbon fiber bundle, and unidirectional material

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2022155348 2022-09-28
JP2022-155348 2022-09-28

Publications (1)

Publication Number Publication Date
WO2024071064A1 true WO2024071064A1 (ja) 2024-04-04

Family

ID=90477925

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2023/034807 Ceased WO2024071064A1 (ja) 2022-09-28 2023-09-26 水分散体、炭素繊維束および一方向材

Country Status (6)

Country Link
US (1) US20260103836A1 (cg-RX-API-DMAC7.html)
EP (1) EP4596785A1 (cg-RX-API-DMAC7.html)
JP (1) JPWO2024071064A1 (cg-RX-API-DMAC7.html)
CN (1) CN120092116A (cg-RX-API-DMAC7.html)
TW (1) TW202432332A (cg-RX-API-DMAC7.html)
WO (1) WO2024071064A1 (cg-RX-API-DMAC7.html)

Citations (9)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2005048343A (ja) * 2003-07-31 2005-02-24 Mitsubishi Rayon Co Ltd 炭素繊維束及びその製造方法、並びに熱可塑性樹脂組成物及びその成形品
WO2010074118A1 (ja) * 2008-12-25 2010-07-01 三井化学株式会社 繊維処理用水分散体
JP2016006245A (ja) * 2014-05-22 2016-01-14 ユニチカ株式会社 繊維収束剤、繊維状強化材および繊維強化樹脂組成物
JP2016102157A (ja) 2014-11-28 2016-06-02 三井化学株式会社 水分散体組成物
WO2021177158A1 (ja) 2020-03-02 2021-09-10 三井化学株式会社 一方向性繊維強化熱可塑性樹脂シート及びその製造方法
WO2022009796A1 (ja) * 2020-07-07 2022-01-13 帝人株式会社 サイジング剤付着炭素繊維束
JP2022088914A (ja) * 2020-12-03 2022-06-15 三井化学株式会社 コーティング剤
JP2022155348A (ja) 2021-03-30 2022-10-13 株式会社デンソー エンジン制御装置
WO2022244879A1 (ja) * 2021-05-20 2022-11-24 三井化学株式会社 樹脂組成物及びその用途ならびに製造方法

Family Cites Families (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP6145977B2 (ja) * 2012-09-06 2017-06-14 三菱ケミカル株式会社 炭素繊維束、その製造方法、炭素繊維チョップ、炭素繊維強化熱可塑性樹脂および成形品
JP2021025033A (ja) * 2019-08-06 2021-02-22 三洋化成工業株式会社 水性分散体

Patent Citations (9)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2005048343A (ja) * 2003-07-31 2005-02-24 Mitsubishi Rayon Co Ltd 炭素繊維束及びその製造方法、並びに熱可塑性樹脂組成物及びその成形品
WO2010074118A1 (ja) * 2008-12-25 2010-07-01 三井化学株式会社 繊維処理用水分散体
JP2016006245A (ja) * 2014-05-22 2016-01-14 ユニチカ株式会社 繊維収束剤、繊維状強化材および繊維強化樹脂組成物
JP2016102157A (ja) 2014-11-28 2016-06-02 三井化学株式会社 水分散体組成物
WO2021177158A1 (ja) 2020-03-02 2021-09-10 三井化学株式会社 一方向性繊維強化熱可塑性樹脂シート及びその製造方法
WO2022009796A1 (ja) * 2020-07-07 2022-01-13 帝人株式会社 サイジング剤付着炭素繊維束
JP2022088914A (ja) * 2020-12-03 2022-06-15 三井化学株式会社 コーティング剤
JP2022155348A (ja) 2021-03-30 2022-10-13 株式会社デンソー エンジン制御装置
WO2022244879A1 (ja) * 2021-05-20 2022-11-24 三井化学株式会社 樹脂組成物及びその用途ならびに製造方法

Non-Patent Citations (3)

* Cited by examiner, † Cited by third party
Title
"Koubunshi Bunseki Handbook (Polymer Analysis Handbook", 2008, ASAKURA PUBLISHING CO., LTD., pages: 184 - 211
J. RAY, MACROMOLECULES, vol. 10, 1977, pages 773
J.C. RANDALL, MACROMOLECULES, vol. 15, 1982, pages 353

Also Published As

Publication number Publication date
US20260103836A1 (en) 2026-04-16
JPWO2024071064A1 (cg-RX-API-DMAC7.html) 2024-04-04
EP4596785A1 (en) 2025-08-06
TW202432332A (zh) 2024-08-16
CN120092116A (zh) 2025-06-03

Similar Documents

Publication Publication Date Title
TWI512162B (zh) A carbon fiber bundle and a method for producing the same, and a molded product thereof
KR101354871B1 (ko) 수지 분산체, 도료, 적층체 및 그 제조 방법
KR101669377B1 (ko) 수지 강화용 탄소 섬유속 및 그의 제조 방법, 및 탄소 섬유 강화 열가소성 수지 조성물 및 그의 성형품
TWI635100B (zh) 改質丙烯.α-烯烴共聚合體與其製造方法、含有其之塗佈材、成形用樹脂組成物及熱熔性組成物
KR100802976B1 (ko) 변성 폴리올레핀 수지, 및 이를 함유하는 접착제, 프라미어, 결합제, 조성물 및 폴리올레핀 성형체
KR101864909B1 (ko) 접착제 조성물 및 그것을 이용한 열융착성 부재
JP7224184B2 (ja) グラフトコポリマー含有固形物およびその用途
JP6643475B2 (ja) ルーフィング組成物用のプロピレンに基いたエラストマーおよび同を調製する方法
US10920009B2 (en) Thermosetting resin composition, sheet-molding compound and production method therefor, and fiber-reinforced composite material
JP2007270122A (ja) 樹脂分散体、塗料、積層体及びその製造方法
EP1153949B1 (en) Resin composition
JP6145977B2 (ja) 炭素繊維束、その製造方法、炭素繊維チョップ、炭素繊維強化熱可塑性樹脂および成形品
US20240263051A1 (en) Resin composition, use thereof, and method for producing same
KR102788037B1 (ko) 수지 미립자 및 그 제조 방법
US20260103836A1 (en) Water dispersion, carbon fiber bundle, and unidirectional material
US12415916B2 (en) Dispersion resin composition
WO2023053852A1 (ja) 炭素繊維含有ポリプロピレン組成物
JP7599360B2 (ja) 離型フィルム
CN117255828A (zh) 树脂组合物及其用途以及制造方法
CN121443652A (zh) 改性聚烯烃树脂组合物及该树脂组合物的用途
JP2025026127A (ja) 積層体
JP2023063838A (ja) 積層体および離型紙

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 23872287

Country of ref document: EP

Kind code of ref document: A1

WWE Wipo information: entry into national phase

Ref document number: 2024549386

Country of ref document: JP

WWE Wipo information: entry into national phase

Ref document number: 202380069559.7

Country of ref document: CN

WWE Wipo information: entry into national phase

Ref document number: 2023872287

Country of ref document: EP

NENP Non-entry into the national phase

Ref country code: DE

ENP Entry into the national phase

Ref document number: 2023872287

Country of ref document: EP

Effective date: 20250428

WWP Wipo information: published in national office

Ref document number: 202380069559.7

Country of ref document: CN

WWP Wipo information: published in national office

Ref document number: 2023872287