WO2022209775A1 - フィルム及びその調製用材料 - Google Patents
フィルム及びその調製用材料 Download PDFInfo
- Publication number
- WO2022209775A1 WO2022209775A1 PCT/JP2022/011006 JP2022011006W WO2022209775A1 WO 2022209775 A1 WO2022209775 A1 WO 2022209775A1 JP 2022011006 W JP2022011006 W JP 2022011006W WO 2022209775 A1 WO2022209775 A1 WO 2022209775A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- formula
- structural unit
- unit represented
- aliphatic polycarbonate
- group
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
- C08G64/00—Macromolecular compounds obtained by reactions forming a carbonic ester link in the main chain of the macromolecule
- C08G64/02—Aliphatic polycarbonates
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
- C08G64/00—Macromolecular compounds obtained by reactions forming a carbonic ester link in the main chain of the macromolecule
- C08G64/20—General preparatory processes
- C08G64/32—General preparatory processes using carbon dioxide
- C08G64/34—General preparatory processes using carbon dioxide and cyclic ethers
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J5/00—Manufacture of articles or shaped materials containing macromolecular substances
- C08J5/18—Manufacture of films or sheets
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
- C08J2369/00—Characterised by the use of polycarbonates; Derivatives of polycarbonates
Definitions
- the present disclosure relates to film preparation materials and films prepared from the materials. It should be noted that the contents of all documents mentioned herein are hereby incorporated by reference.
- Aliphatic polycarbonates are resins prepared from epoxides and carbon dioxide and can also be used for film formation. However, films prepared with aliphatic polycarbonates were not elastic enough.
- the present inventors conducted studies to provide an aliphatic polycarbonate capable of forming a film exhibiting excellent elasticity.
- the present inventors found the possibility that an aliphatic polycarbonate prepared using cycloalkylene oxide as the alkylene oxide could form a film having excellent elasticity, and conducted further investigations.
- a film preparation material comprising an aliphatic polycarbonate,
- the aliphatic polycarbonate is Formula (1):
- R 1 and R 3 are bonded to each other to form a substituted or unsubstituted saturated or unsaturated aliphatic ring having 3 to 10 ring members together with the carbon atom to which they are bonded, and R 2 and R 4 is the same or different and is a hydrogen atom, an optionally substituted C 1-10 alkyl group, or an optionally substituted C 6-20 aryl group
- R 2 and R 4 is the same or different and is a hydrogen atom, an optionally substituted C 1-10 alkyl group, or an optionally substituted C 6-20 aryl group
- the film has a maximum tensile strength of 20 to 40 MPa and a tensile modulus of 1000 to 4000 MPa measured at 23° C. and a tensile speed of 10 mm/min. material. Section 2.
- the aliphatic polycarbonate is moreover, Formula (2):
- R 5 , R 6 , R 7 and R 8 are the same or different and are a hydrogen atom, an optionally substituted alkyl group having 1 to 10 carbon atoms, or substituted with a substituent is an aryl group having 6 to 20 carbon atoms, which is an aliphatic polycarbonate containing a structural unit represented by Item 1.
- the material according to item 1. Item 3.
- the film is In the dynamic viscoelasticity measurement in tension mode at 10 Hz, the storage modulus E' at 40° C. is 5.0 ⁇ 10 8 to 5.0 ⁇ 10 9 Pa, and the loss tangent is 0.005 to 0.7. 3.
- the aliphatic polycarbonate is A mass average molecular weight (Mw) of 100,000 or more and 500,000 or less, Item 4. The material according to any one of items 1 to 3. Item 5. The aliphatic polycarbonate is The ratio (Mw/Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is 2 or more and 15 or less. Item 5. The material according to any one of items 1 to 4. Item 6.
- the structural unit represented by formula (1) is represented by formula (3):
- Item 6 The material according to any one of Items 2 to 5, which is a structural unit represented by (wherein R9 is hydrogen, a methyl group, or an ethyl group).
- Item 8. A film containing an aliphatic polycarbonate, The aliphatic polycarbonate is Formula (1):
- R 1 and R 3 are bonded to each other to form a substituted or unsubstituted saturated or unsaturated aliphatic ring having 3 to 10 ring members together with the carbon atom to which they are bonded, and R 2 and R 4 is the same or different and is a hydrogen atom, an optionally substituted C 1-10 alkyl group, or an optionally substituted C 6-20 aryl group
- R 2 and R 4 is the same or different and is a hydrogen atom, an optionally substituted C 1-10 alkyl group, or an optionally substituted C 6-20 aryl group
- aliphatic polycarbonate containing a structural unit represented by The maximum tensile strength measured at 23 ° C. and a tensile speed of 10 mm / min is 20 to 40 MPa, and the tensile modulus is 1000 to 4000 MPa. the film.
- Item 9 The aliphatic polycarbonate is moreover, Formula (2):
- R 5 , R 6 , R 7 and R 8 are the same or different and are a hydrogen atom, an optionally substituted alkyl group having 1 to 10 carbon atoms, or substituted with a substituent is an aryl group having 6 to 20 carbon atoms, which is an aliphatic polycarbonate containing a structural unit represented by Item 9.
- Item 9 The film according to Item 8 or 9.
- the aliphatic polycarbonate is A mass average molecular weight (Mw) of 100,000 or more and 500,000 or less, Item 11.
- the aliphatic polycarbonate is The ratio (Mw/Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is 2 or more and 15 or less.
- Item 13 The structural unit represented by formula (1) is represented by formula (3):
- Item 13 The film according to any one of Items 9 to 12, which is a structural unit represented by (wherein R9 is hydrogen, a methyl group, or an ethyl group).
- a film with excellent elasticity and a material for preparing the film are provided.
- the present disclosure preferably includes, but is not limited to, film-preparing materials comprising certain aliphatic polycarbonates, films prepared from such materials, and the like, as disclosed herein. Include everything a trader can perceive.
- Film preparation materials included in the present disclosure include certain aliphatic polycarbonates.
- an aliphatic polycarbonate may be described as APC.
- the film preparation materials included in the present disclosure are sometimes referred to as "materials of the present disclosure”.
- Certain aliphatic polycarbonates included in the materials of this disclosure are also sometimes referred to as aliphatic polycarbonates (APCs) of this disclosure.
- the APC of the present disclosure is represented by formula (1):
- R 1 and R 3 are bonded to each other to form a substituted or unsubstituted saturated or unsaturated aliphatic ring having 3 to 10 ring members together with the carbon atom to which they are bonded, and R 2 and R 4 is the same or different and is a hydrogen atom, an optionally substituted C 1-10 alkyl group, or an optionally substituted C 6-20 aryl group ) contains structural units represented by In addition, the said structural unit may be called structural unit (1).
- APC of the present disclosure further has formula (2):
- R 5 , R 6 , R 7 and R 8 are the same or different and are a hydrogen atom, an optionally substituted alkyl group having 1 to 10 carbon atoms, or substituted with a substituent an aryl group having 6 to 20 carbon atoms, which may contain a structural unit represented by
- the said structural unit may be called structural unit (2).
- the substituted or unsubstituted saturated or unsaturated aliphatic ring having 3 to 10 ring members formed by combining R 1 and R 3 with each other includes, for example, 3 to 8 optionally substituted (3, 4, 5, 6, 7, or 8) membered aliphatic rings. More specifically, the aliphatic ring includes cyclopentane ring, cyclopentene ring, cyclohexane ring, cyclohexene ring, cycloheptane ring and the like.
- the substituent when the aliphatic ring is substituted with a substituent, examples of the substituent include an alkyl group, an aryl group, an alkoxy group, an acyloxy group, a silyl group, a sulfanyl group, a cyano group, a nitro group, a sulfo group, formyl group, halogen atom (eg, fluorine atom, chlorine atom, bromine atom, iodine atom) and the like. Also, the aliphatic ring may be substituted with one or more substituents.
- substituents include an alkyl group, an aryl group, an alkoxy group, an acyloxy group, a silyl group, a sulfanyl group, a cyano group, a nitro group, a sulfo group, formyl group, halogen atom (eg, fluorine atom, chlorine atom, bromine atom, io
- the alkyl group here includes, for example, methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, sec-butyl group, tert-butyl group and the like.
- the aryl group include phenyl group, o-tolyl group, m-tolyl group, p-tolyl group, naphthyl group and indenyl group.
- alkoxy groups include methoxy, ethoxy, isopropoxy, and tert-butoxy groups.
- Examples of acyloxy groups include acetoxy, propionyloxy, butyryloxy, isobutyryloxy, pivaloyloxy, and benzoyloxy groups.
- the alkoxycarbonyl group includes a methoxycarbonyl group, an ethoxycarbonyl group, a tert-butoxycarbonyl group and the like.
- the aliphatic ring is not particularly limited, but an unsubstituted saturated 3- to 8-membered aliphatic ring is preferable, and cyclopentane ring and cyclohexane ring are particularly preferable.
- the alkyl groups represented by R 2 and R 4 , R 5 , R 6 , R 7 and R 8 have 1, 2, 3, 4, 5, 6, 7, 8, 9 or 10 carbon atoms, A linear or branched alkyl group.
- the number of carbon atoms is preferably 1 to 9, more preferably 1 to 8, even more preferably 1 to 6, still more preferably 1 to 4.
- the alkyl groups represented by R 2 and R 4 , R 5 , R 6 , R 7 and R 8 may be substituted with one or more substituents.
- substituents include alkoxy groups, acyloxy groups, alkoxycarbonyl groups, aryl groups, and halogen atoms (eg, fluorine, chlorine, bromine, and iodine atoms).
- the alkoxy group here includes, for example, a methoxy group, an ethoxy group, an isopropoxy group, a tert-butoxy group and the like.
- Examples of acyloxy groups include acetoxy, propionyloxy, butyryloxy, isobutyryloxy, pivaloyloxy, and benzoyloxy groups.
- the alkoxycarbonyl group includes a methoxycarbonyl group, an ethoxycarbonyl group, a tert-butoxycarbonyl group and the like.
- the aryl group include phenyl group, o-tolyl group, m-tolyl group, p-tolyl group, naphthyl group and indenyl group.
- the aryl groups represented by R 2 and R 4 , R 5 , R 6 , R 7 and R 8 have 6, 7, 8, 9, 10, 11, 12, 13, 14, 15 carbon atoms, 16, 17, 18, 19 or 20 aryl groups, preferably 6-14.
- Examples include phenyl group, indenyl group, naphthyl group, tetrahydronaphthyl group and the like.
- the aryl groups represented by R 2 and R 4 as well as R 5 , R 6 , R 7 and R 8 may be substituted with one or more substituents.
- substituents on the aryl group include alkyl groups, aryl groups, alkoxy groups, acyloxy groups, alkoxycarbonyl groups, halogen atoms (eg, fluorine atom, chlorine atom, bromine atom, iodine atom) and the like.
- the alkyl group here includes, for example, methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, sec-butyl group, tert-butyl group and the like.
- Examples of the aryl group include phenyl group, o-tolyl group, m-tolyl group, p-tolyl group, naphthyl group and indenyl group.
- Examples of alkoxy groups include methoxy, ethoxy, isopropoxy, and tert-butoxy groups.
- Examples of acyloxy groups include acetoxy, propionyloxy, butyryloxy, isobutyryloxy, pivaloyloxy, and benzoyloxy groups.
- the alkoxycarbonyl group includes a methoxycarbonyl group, an ethoxycarbonyl group, a tert-butoxycarbonyl group and the like.
- R 2 and R 4 are preferably the same or different and each represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. Among them, R 2 and R 4 are more preferably hydrogen atoms.
- R 5 , R 6 , R 7 and R 8 are preferably the same or different and each preferably represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. Among them, R 2 and R 4 are preferably hydrogen atoms.
- R 5 , R 6 and R 7 are more preferably hydrogen atoms
- R 8 is more preferably an alkyl group having 1 to 4 carbon atoms.
- R9 is hydrogen, a methyl group, or an ethyl group.
- the content of the structural unit (1) is, for example, 1 to 100 mol% with respect to the total amount of the molar amount of the structural unit (1) and the molar amount of the structural unit (2). It can be.
- the upper or lower limit of the range is 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, 50, 51, 52, 53, 54, 55, 56, 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, It may be 98 or 99 mol %.
- the content (ratio) of the structural units (1) and (2) is determined by 1 H-NMR. That is, in the chart obtained by measuring the aliphatic polycarbonate by 1 H-NMR, it is determined from the area ratio of the peaks derived from the structural unit (1) and the structural unit (2).
- the APC of the present disclosure preferably has a glass transition temperature (Tg) of about 35 to 120°C.
- Tg glass transition temperature
- the upper or lower limit of the range is 57, 58, 59, 60, 61, 62, 63, 64, 65, 66, 67, 68, 69, 70, 71, 72, 73, 74, 75, 76, 77, 78, 79, 80, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 100, 101, 102, 103, 104, 105, 106, 107, 108, 109, 110, 111, 112, 113, 114, 115, 116, 117, 118, or 119°C.
- the range is preferably 40 to 115°C, more preferably 60 to 100°C.
- the film forming process is sometimes carried out at around room temperature, in such a case, if the Tg is too high, the energy required for processing becomes excessive. Therefore, in such a case, from the viewpoint of economy and the ease of handling of the film, it is preferable that the film is crystallized at room temperature. It is more preferably 40° C. or lower.
- the glass transition temperature is measured using a differential scanning calorimeter (DSC) under the conditions of a heating rate of 5° C./min, a measurement atmosphere of N 2 and a sample amount of 5 mg.
- DSC differential scanning calorimeter
- the APC of the present disclosure may contain other structural units other than the structural unit (1) and the structural unit (2) as long as the effect is not impaired, or the structural unit (1) and the structural unit (2) It may consist of only
- Examples of structural units other than structural unit (1) and structural unit (2) include structural units in which polyether, polyester, polycarbonate, polyurethane, or polyamide are formed by repeating the structural unit.
- the content of these structural units is preferably 100 mol% or less, more preferably 50 mol% or less, relative to the total molar amount of the structural unit (1) and the structural unit (2). , 25, 24, 23, 22, 21, 20, 19, 18, 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, 4, 3, 2, or 1 mol % or less is more preferable.
- the APC of the present disclosure may contain one or more structural units represented by formula (1), and one or more structural units represented by formula (2) Units may be included.
- a plurality of species here may be, for example, 2, 3, 4, or 5 species. Only one type of structural unit represented by formula (1) may be contained, and only one type of structural unit represented by formula (2) may be contained. Further, only one type of structural unit represented by formula (1) may be contained, and only one type of structural unit represented by formula (2) may be contained. It should be noted that the APC of the present disclosure is preferably a random copolymer.
- a method for producing the APC of the present disclosure includes, for example, a method of polymerizing a predetermined epoxide and carbon dioxide, preferably in the presence of a metal catalyst, to obtain an aliphatic polycarbonate.
- examples of the epoxide used to form the structural unit (1) include cyclopentene oxide, cyclohexene oxide, cyclooctene oxide, cyclododecene oxide, ⁇ -pinene oxide, and 2,3-epoxide.
- examples include norbornene, limonene oxide, dieldrin, etc.
- cyclopentene oxide, cyclohexene oxide, etc. are preferable. These can be used individually by 1 type or in combination of 2 or more types.
- a reactive group can be introduced into the side chain of the aliphatic polycarbonate, and a modification reaction can be carried out using this as a starting point.
- Examples of epoxides used to form the structural unit (2) include ethylene oxide, propylene oxide, 1-butene oxide, 2-butene oxide, isobutylene oxide, 1-pentene oxide, 2-pentene oxide, 1- hexene oxide, 1-octene oxide, 1-dodecene oxide, styrene oxide, 3-phenylpropylene oxide, epichlorohydrin, 3,3,3-trifluoropropylene oxide, 3-naphthylpropylene oxide, 3-phenoxypropylene oxide , 3-naphthoxypropylene oxide, butadiene monoxide, 3-vinyloxypropylene oxide, and 3-trimethylsilyloxypropylene oxide. These can be used individually by 1 type or in combination of 2 or more types. Among them, ethylene oxide and propylene oxide are preferable from the viewpoint of having high reactivity.
- a metal catalyst can be used when polymerizing these epoxides and carbon dioxide.
- metal catalysts include zinc-based catalysts, aluminum-based catalysts, chromium-based catalysts, and cobalt-based catalysts.
- zinc-based catalysts are more preferable because they have high polymerization activity in the polymerization reaction between the epoxide and carbon dioxide.
- an organic zinc catalyst is preferable.
- organic zinc catalysts include zinc acetate, diethyl zinc, dibutyl zinc, etc., as well as compounds such as primary amines, dihydric phenols, aromatic dicarboxylic acids, aromatic hydroxy acids, aliphatic dicarboxylic acids, and aliphatic monocarboxylic acids.
- An organozinc catalyst obtained by reacting with a zinc compound, and the like is preferable because it has a higher polymerization activity. Zinc oxide, glutaric acid and acetic acid are preferred.
- An organic zinc catalyst obtained by reacting with is more preferable.
- the amount of the metal catalyst used in the polymerization reaction is preferably 0.001 parts by mass or more, more preferably 0.01 parts by mass or more, relative to 100 parts by mass of the epoxide. 30 parts by mass or less is preferable, and 20 parts by mass or less is more preferable, from the viewpoint of obtaining an effect commensurate with the amount used.
- the polymerization reaction may optionally be carried out in the presence of a co-catalyst in addition to the metal catalyst.
- promoters include bis(triphenylphosphoranylidene)ammonium chloride (PPNCl), piperidine, bis(triphenylphosphoranylidene)ammonium fluoride (PPNF), bis(triphenylphosphoranylidene)ammonium pentafluorobenzoate ( PPNOBzF ), tetra-n-butylammonium chloride (nBu 4 NCl), tetra-n-butylammonium bromide (nBu 4 NBr), tetra-n-butylammonium iodide (nBu 4 NI), tetra- n-butylammonium acetate (nBu 4 NOAc), tetra-n-butylammonium nitrate (nBu 4 NO 3 ), triethylphosphine (Et 3 P
- the amount of co-catalyst used is preferably 0.1 to 10 mol, more preferably 0.3 to 5 mol, and even more preferably 0.5 to 1.5 mol, relative to 1 mol of the metal catalyst.
- reaction solvent may be used for the polymerization reaction, if necessary.
- reaction solvents include aliphatic hydrocarbon solvents such as pentane, hexane, octane, decane, and cyclohexane; aromatic hydrocarbon solvents such as benzene, toluene, and xylene; methylene chloride, chloroform, carbon tetrachloride, 1, Halogenated carbonization of 1-dichloroethane, 1,2-dichloroethane, ethyl chloride, trichloroethane, 1-chloropropane, 2-chloropropane, 1-chlorobutane, 2-chlorobutane, 1-chloro-2-methylpropane, chlorobenzene, bromobenzene, etc.
- Hydrogen-based solvents such as dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, and anisole; ester-based solvents such as ethyl acetate, n-propyl acetate, and isopropyl acetate; , N-dimethylformamide and N,N-dimethylacetamide; and carbonate solvents such as dimethyl carbonate, ethylmethyl carbonate, diethyl carbonate and propylene carbonate.
- ether-based solvents such as dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, 1,3-dioxolane, and anisole
- ester-based solvents such as ethyl acetate, n-propyl acetate, and isopropyl acetate
- the amount of the reaction solvent used is preferably 100 to 10,000 parts by mass, more preferably 200 to 5,000 parts by mass, more preferably 300 to 1,000 parts by mass, relative to 100 parts by mass of the epoxide, from the viewpoint of allowing the reaction to proceed smoothly. More preferred.
- an autoclave is charged with a predetermined epoxide, a metal catalyst, and, if necessary, a co-catalyst, a reaction solvent, etc., and mixed. After that, carbon dioxide is pressurized to react.
- the amount of carbon dioxide used in the polymerization reaction is preferably 1 to 10 mol, more preferably 1 to 5 mol, and even more preferably 1 to 3 mol, per 1 mol of epoxide. Carbon dioxide may be added all at once, added sequentially, or added continuously.
- the working pressure of carbon dioxide used in the polymerization reaction is, for example, preferably 0.1 MPa or higher, more preferably 0.2 MPa or higher, and further preferably 0.5 MPa or higher, from the viewpoint of smoothly proceeding the reaction, which matches the working pressure. From the viewpoint of obtaining an effect, for example, 20 MPa or less is preferable, 10 MPa or less is more preferable, and 5 MPa or less is even more preferable.
- the polymerization reaction temperature in the polymerization reaction is, for example, preferably 0° C. or higher, more preferably 10° C. or higher, and still more preferably 20° C. or higher, from the viewpoint of shortening the reaction time, from the viewpoint of suppressing side reactions and improving the yield. , preferably 100° C. or lower, more preferably 90° C. or lower, and even more preferably 80° C. or lower.
- the polymerization reaction time varies depending on the polymerization reaction conditions, so it cannot be determined unconditionally, but it is usually preferably about 1 to 40 hours.
- the mass average molecular weight (Mw) of the APC of the present disclosure is preferably 100,000 or more and 500,000 or less.
- the upper or lower limit of the range is, for example, , 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, or 490,000.
- the range may be 150,000 or more and 450,000 or less.
- the mass average molecular weight and number average molecular weight of APC of the present disclosure are measured by gel permeation chromatography (GPC) and calculated as standard polystyrene conversion values. More specifically, for example, it is obtained as follows. A tetrahydrofuran solution having a concentration of APC to be measured of 0.3% by mass is prepared, and the solution is subjected to GPC measurement under the following conditions for measurement, and the value is calculated in terms of standard polystyrene. Apparatus used: Gel permeation chromatograph measurement apparatus (manufactured by Waters, product name “waters2695” separation module) Column: TSKgel GMHHR-H (S) x 2 Measurement temperature: 40°C Detector: RI
- the APC of the present disclosure is useful as a film preparation material. Films prepared using the APCs of the present disclosure have excellent elasticity. Film preparation materials comprising APCs of the present disclosure are sometimes referred to as materials of the present disclosure. Films prepared using materials of the present disclosure are sometimes referred to as films of the present disclosure.
- the material of the present disclosure may consist of only the APC of the present disclosure, or may contain components other than the APC of the present disclosure.
- examples of such other components include cross-linking agents, solvents, additives, solvents, pigments, monomer components, inorganic materials, and the like.
- Such ingredients other than APC of the present disclosure can be used singly or in combination of two or more.
- compositions containing the APC of the present disclosure and a cross-linking agent are preferable.
- the composition can be prepared, for example, by appropriately mixing the APC of the present disclosure and a cross-linking agent.
- the composition may be hereinafter referred to as "polycarbonate cross-linking agent composition”.
- cross-linking agents examples include epoxy-based compounds such as ethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, diglycidylaniline, diglycidylamine, epoxidized soybean oil, and glycidyl methacrylate copolymers.
- epoxy-based compounds such as ethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, diglycidylaniline, diglycidylamine, epoxidized soybean oil, and glycidyl methacrylate copolymers.
- Cross-linking agent isocyanate-based cross-linking agent such as tolylene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, cyclohexylene diisocyanate; diphenylmethane-4,4'-bis(1-aziridinecarboxamide), trimethylol aziridine cross-linking agents such as propane-tri- ⁇ -aziridinylpropionate, tetramethylolmethane-tri- ⁇ -aziridinylpropionate, toluene-2,4-bis(1-aziridinecarboxamide); Metal chelate crosslinking agents such as diisopropoxyaluminum monooleyl acetoacetate, monoisopropoxyaluminum bisoleyl acetoacetate, monoisopropoxyaluminum monooleate monoethylacetoacetate
- the amount of the cross-linking agent in the composition is preferably, for example, 0.1 to 20 parts by mass with respect to 100 parts by mass of the aliphatic polycarbonate.
- the lower limit of the range may be, for example, about 0.2, 0.5, 1, 2, 3, 4, or 5 parts by mass.
- the upper limit of the range may be, for example, about 19, 18, 17, 16, 15, 14, 13, 12, 11, or 10 parts by mass.
- 0.5 to 15 parts by mass is more preferable, and 1 to 10 parts by mass is even more preferable.
- a part of the cross-linking agent may react with the aliphatic polycarbonate to form cross-links.
- the composition also contains a crosslinked aliphatic polycarbonate.
- compositions containing the APC or polycarbonate cross-linking agent composition of the present disclosure and a solvent and/or additive is preferably included.
- Such compositions can be prepared, for example, by appropriately mixing the APC or polycarbonate crosslinker composition of the present disclosure with solvents and/or additives.
- solvents include toluene, ethyl acetate, butyl acetate, isopropyl alcohol, methyl isobutyl ketone, methyl ethyl ketone, N-methyl-2-pyrrolidone, ethylene glycol ethyl ether, ethylene glycol monobutyl ether, ethylene glycol monoethyl ether acetate, diethylene glycol mono Ethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoisobutyl ether, trimethylpentanediol monoisobutyrate, ethyl carbitol, butyl carbitol, ethyl carbitol acetate, butyl carbitol acetate, terpineol, terpineol acetate, dihydroterpineol, dihydroterpineol acetate, Texanol, isophorone, butyl lactate, diophor
- Additives include cross-linking agents, tackifiers, light stabilizers, silane coupling agents, antistatic agents, antioxidants, UV absorbers, hydrolysis inhibitors, fillers, and plasticizers.
- cross-linking agents include ethylene glycol glycidyl ether, hexamethylene diisocyanate, diphenylmethane diisocyanate and the like.
- the film of the present disclosure is prepared, for example, by heat-press molding the material of the present disclosure.
- the preparation method is not particularly limited.
- the film of the present disclosure preferably has a thickness of, for example, about 0.001 to 5 mm.
- the upper or lower limit of the range is, for example, 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.1, 0.2, 0.3, 0.4, 0 .5, 0.6, 0.7, 0.8, 0.9, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1 .8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3, 3.1 , 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4, 4.1, 4.2, 4.3, 4.4 , 4.5, 4.6, 4.7, 4.8 or 4.9 mm.
- the range may be 0.1-4 mm.
- the film of the present disclosure preferably has a maximum tensile strength measured in accordance with JIS7161 within a specific range. More specifically, the film of the present disclosure preferably has an ultimate tensile strength of 20-40 MPa measured at 23° C. and a tensile speed of 10 mm/min. Satisfying this requirement makes the film easier to handle.
- the upper or lower limit of the range is, for example, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, or 39 MPa. good too.
- the range may be, for example, 21-39 MPa.
- the film of the present disclosure preferably has a tensile modulus of 1000 to 4000 MPa.
- the upper or lower limits of the range are, for example, 3100, 3200, 3300, 3400, 3500, 3600, 3700, 3800 or 3900 MPa.
- the range may be, for example, 1500-3500 MPa.
- the maximum tensile strength and tensile modulus are measured by a tensile test. More specifically, it is measured according to JIS7161 using a precision universal testing machine (autograph). More specifically, it is measured under the conditions of a tensile speed of 10 mm/min and a test temperature of 23°C.
- the film of the present disclosure preferably has a storage modulus E′ at 40° C. of 5 ⁇ 10 8 to 5 ⁇ 10 9 Pa (ie 50 ⁇ 10 8 Pa).
- the upper or lower limit of the range (5 ⁇ 10 8 to 50 ⁇ 10 8 Pa) is, for example, 6 ⁇ 10 8 , 7 ⁇ 10 8 , 8 ⁇ 10 8 , 9 ⁇ 10 8 , 10 ⁇ 10 8 , 11 ⁇ 10 8 , 12 ⁇ 10 8 , 13 ⁇ 10 8 , 14 ⁇ 10 8 , 15 ⁇ 10 8 , 16 ⁇ 10 8 , 17 ⁇ 10 8 , 18 ⁇ 10 8 , 19 ⁇ 10 8 , 20 ⁇ 10 8 , 21 ⁇ 10 8 , 22 ⁇ 10 8 , 23 ⁇ 10 8 , 24 ⁇ 10 8 , 25 ⁇ 10 8 , 26 ⁇ 10 8 , 27 ⁇ 10 8 , 28 ⁇ 10 8 , 29 ⁇ 10 8 , 30 ⁇ 10 8 , 31 ⁇ 10 8 , 32 ⁇ 10 8 , 33 ⁇ 10 8 , 34 ⁇ 10 8 , 35 ⁇ 10 8 , 36 ⁇ 10 8 , 37
- the film of the present disclosure preferably has a loss tangent (tan ⁇ ) at 40°C of less than 1, more preferably 0.005 to 0.7.
- the upper or lower limit of the range is, for example, 0.01, 0.015, 0.02, 0.025, 0.03, 0.035, 0.04, 0.045, 0.05, 0.06, 0.07,0.08,0.09,0.1,0.15,0.2,0.25,0.3,0.35,0.4,0.45,0.5,0. It may be 55, 0.6 or 0.65.
- the range may be from 0.01 to 0.5, or for example from 0.01 to 0.1.
- the storage elastic modulus E' and loss tangent (tan ⁇ ) at 40°C are measured using a dynamic viscoelasticity measuring device (for example, a universal testing machine (manufactured by TA Instruments, RSA-G2)). More specifically, it is measured under the conditions of a vibration frequency of 10 Hz, a test temperature increase rate of 5° C./min, and a test piece size of 40 mm ⁇ 5 mm.
- a dynamic viscoelasticity measuring device for example, a universal testing machine (manufactured by TA Instruments, RSA-G2)
- Organozinc catalyst 81 g (1.00 mol) of zinc oxide, 132 g (1.00 mol) of glutaric acid, and 1000 g of toluene were placed in a 1.5 L separable flask equipped with a condenser, thermometer and stirrer. planted. Then, the temperature was raised to 60° C. under a nitrogen atmosphere, and the mixture was stirred at the same temperature for 8 hours to react. After that, it was cooled to room temperature, suction filtered, and then dried at 90° C. and 1.0 kPa abs for 1 hour to obtain 196 g (powder) of an organozinc catalyst. The powder was used as an organozinc catalyst for the production of aliphatic polycarbonates.
- Example 1 Preparation of Aliphatic Polycarbonate
- 27.3 g of the above organozinc catalyst 690 g of toluene, 5 g (0.05 mol) of cyclohexene oxide, and 90 g of propylene oxide (1.0 g) were added. 55 mol) and carbon dioxide were added, the reaction system was adjusted to 60° C. and 0.99 MPa, and the polymerization reaction was carried out for 24 hours while replenishing the consumed carbon dioxide.
- the autoclave was cooled and depressurized to obtain a white polymer slurry. This was filtered, concentrated, purified with methanol, and dried under reduced pressure to obtain 149 g of an aliphatic polycarbonate (polymer yield: 90%).
- Table 1 summarizes the raw materials and yields of each polycarbonate obtained.
- a structural unit derived from cyclohexene oxide is sometimes referred to as a CHO unit.
- a structural unit derived from propylene oxide is sometimes referred to as a PO unit.
- the mass-average molecular weight (Mw) and number-average molecular weight (Mn) of the aliphatic polycarbonate are values converted to standard polystyrene and measured under the following conditions by introducing a tetrahydrofuran solution having a polymer concentration of 0.3% by mass into a measuring device.
- Apparatus used Gel permeation chromatograph (Wa ters, product name “waters2695” separation module) Column: TSKgel GMHHR-H (S) x 2 Measurement temperature: 40°C Detector: RI
- DSC dynamic viscoelasticity measurement
- DSC differential scanning calorimeter
- step (ii) Place the SUS (stainless steel) plate prepared in step (i) in a hot press machine at a predetermined temperature (130 to 200° C.) and preheat for 5 minutes.
- Bombing was carried out about 10 times to defoam and press for about 20 seconds (pressure 150 kgf/cm 2 ).
- the film was peeled off from the SUS plate by cold pressing at 15°C.
- Table 2 summarizes the measurement results for the polycarbonate of each example and the film made using it.
Landscapes
- Chemical & Material Sciences (AREA)
- Health & Medical Sciences (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Medicinal Chemistry (AREA)
- Polymers & Plastics (AREA)
- Organic Chemistry (AREA)
- Engineering & Computer Science (AREA)
- Manufacturing & Machinery (AREA)
- Materials Engineering (AREA)
- Polyesters Or Polycarbonates (AREA)
- Organic Low-Molecular-Weight Compounds And Preparation Thereof (AREA)
Priority Applications (3)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| CN202280008578.4A CN116670205A (zh) | 2021-03-29 | 2022-03-11 | 膜及其制备用材料 |
| JP2023510843A JPWO2022209775A1 (cg-RX-API-DMAC7.html) | 2021-03-29 | 2022-03-11 | |
| KR1020237021504A KR20230161419A (ko) | 2021-03-29 | 2022-03-11 | 필름 및 그 조제용 재료 |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2021-055523 | 2021-03-29 | ||
| JP2021055523 | 2021-03-29 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2022209775A1 true WO2022209775A1 (ja) | 2022-10-06 |
Family
ID=83456209
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2022/011006 Ceased WO2022209775A1 (ja) | 2021-03-29 | 2022-03-11 | フィルム及びその調製用材料 |
Country Status (4)
| Country | Link |
|---|---|
| JP (1) | JPWO2022209775A1 (cg-RX-API-DMAC7.html) |
| KR (1) | KR20230161419A (cg-RX-API-DMAC7.html) |
| CN (1) | CN116670205A (cg-RX-API-DMAC7.html) |
| WO (1) | WO2022209775A1 (cg-RX-API-DMAC7.html) |
Citations (7)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH01210146A (ja) * | 1987-12-14 | 1989-08-23 | Arco Chem Technol Inc | 金属鋳物の製造に使用する模型を製造する方法 |
| JP2000256454A (ja) * | 1999-03-08 | 2000-09-19 | Takasago Internatl Corp | 光学活性ポリカーボネートおよびその製造方法 |
| JP2012224675A (ja) * | 2011-04-15 | 2012-11-15 | Sumitomo Seika Chem Co Ltd | ポリカーボネート樹脂組成物 |
| JP2012530794A (ja) * | 2009-06-18 | 2012-12-06 | エスケー イノベーション シーオー., エルティーディー. | 酸素及び水分遮断用樹脂組成物及びそれを利用したシート |
| JP2013538898A (ja) * | 2010-09-01 | 2013-10-17 | エスケー イノベーション シーオー., エルティーディー. | ペーパコーティング用組成物 |
| WO2017119330A1 (ja) * | 2016-01-04 | 2017-07-13 | 住友精化株式会社 | 樹脂表面粗化用組成物 |
| WO2017175778A1 (ja) * | 2016-04-08 | 2017-10-12 | 住友精化株式会社 | 隔壁形成用脂肪族ポリカーボネート樹脂、隔壁材料、基板及びその製造方法、配線基板の製造方法、並びに、配線形成方法 |
Family Cites Families (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US4665136A (en) * | 1986-04-07 | 1987-05-12 | Air Products And Chemicals, Inc. | Process for producing novel block alkylene polycarbonate copolymers |
| KR20160012726A (ko) | 2014-07-25 | 2016-02-03 | 주식회사 엘지화학 | 폴리알킬렌 카보네이트의 제조 방법 |
| KR101906208B1 (ko) | 2017-04-13 | 2018-12-05 | 부산대학교 산학협력단 | 맥문동 추출물, 감초 및 계피를 유효성분으로 포함하는, 변비의 예방 또는 치료용 약학적 조성물 |
| TWI849041B (zh) | 2019-01-24 | 2024-07-21 | 日商住友精化股份有限公司 | 脂肪族聚碳酸酯、脂肪族聚碳酸酯組成物及其等之用途 |
-
2022
- 2022-03-11 JP JP2023510843A patent/JPWO2022209775A1/ja active Pending
- 2022-03-11 KR KR1020237021504A patent/KR20230161419A/ko not_active Withdrawn
- 2022-03-11 CN CN202280008578.4A patent/CN116670205A/zh active Pending
- 2022-03-11 WO PCT/JP2022/011006 patent/WO2022209775A1/ja not_active Ceased
Patent Citations (7)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH01210146A (ja) * | 1987-12-14 | 1989-08-23 | Arco Chem Technol Inc | 金属鋳物の製造に使用する模型を製造する方法 |
| JP2000256454A (ja) * | 1999-03-08 | 2000-09-19 | Takasago Internatl Corp | 光学活性ポリカーボネートおよびその製造方法 |
| JP2012530794A (ja) * | 2009-06-18 | 2012-12-06 | エスケー イノベーション シーオー., エルティーディー. | 酸素及び水分遮断用樹脂組成物及びそれを利用したシート |
| JP2013538898A (ja) * | 2010-09-01 | 2013-10-17 | エスケー イノベーション シーオー., エルティーディー. | ペーパコーティング用組成物 |
| JP2012224675A (ja) * | 2011-04-15 | 2012-11-15 | Sumitomo Seika Chem Co Ltd | ポリカーボネート樹脂組成物 |
| WO2017119330A1 (ja) * | 2016-01-04 | 2017-07-13 | 住友精化株式会社 | 樹脂表面粗化用組成物 |
| WO2017175778A1 (ja) * | 2016-04-08 | 2017-10-12 | 住友精化株式会社 | 隔壁形成用脂肪族ポリカーボネート樹脂、隔壁材料、基板及びその製造方法、配線基板の製造方法、並びに、配線形成方法 |
Also Published As
| Publication number | Publication date |
|---|---|
| KR20230161419A (ko) | 2023-11-27 |
| CN116670205A (zh) | 2023-08-29 |
| JPWO2022209775A1 (cg-RX-API-DMAC7.html) | 2022-10-06 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| EP2707224B1 (en) | Polymer compositions and methods | |
| JP5381977B2 (ja) | ヒドロキシ化合物の製造方法、ならびにプレポリマーおよびポリウレタンの製造方法 | |
| CN107108873B (zh) | 聚碳酸酯树脂 | |
| CN103097425B (zh) | 制备多元醇混合物的方法 | |
| US7919656B2 (en) | Linear amine functionalized poly(trimethylene ether) compositions | |
| TW201920329A (zh) | 製造熱塑性聚唑烷酮聚合物之方法(二) | |
| CN111094380A (zh) | 生产热塑性聚噁唑烷酮聚合物的方法 | |
| KR102448348B1 (ko) | 폴리옥사졸리디논 화합물의 합성 방법 | |
| JP2019536848A (ja) | 廃棄原料由来の新規の高分子量ポリマー | |
| US12030987B2 (en) | Aliphatic polycarbonate | |
| CN103502304A (zh) | 具有所期望的支化度的支化芳香族聚碳酸酯树脂的制造方法 | |
| EP3357949A1 (en) | Method for the production of polyoxazolidinone polymer compounds | |
| US12049535B2 (en) | Polyol composition comprising anhydrosugar alcohols and anhydrosugar alcohol polymer | |
| CN107922569B (zh) | 用于制备开环聚合产物的方法 | |
| WO2009106774A1 (fr) | Nouveaux allongeurs de chaines pour formulations d'elastomeres de polyurethanes | |
| CN116670205A (zh) | 膜及其制备用材料 | |
| EP4255947B1 (en) | Method for the production of thermoplastic polyoxazolidinone polymers | |
| TWI603995B (zh) | 以二甲基碳酸酯製備之共聚物及其製備方法 | |
| KR102292023B1 (ko) | 폴리카보네이트 수지 및 그 제조 방법 | |
| JP2022041689A (ja) | 熱可塑性樹脂、ジヒドロキシ化合物 | |
| CN112996835A (zh) | 生产热塑性聚噁唑烷酮聚合物的方法 | |
| JPS5922916A (ja) | 脂肪族ポリイソシアヌレ−ト重合体の製造方法 | |
| EP4008736A1 (en) | Method for the production of thermoplastic polyoxazolidinone polymers | |
| CN115667358A (zh) | 具有特定比例的酯基团的聚酯碳酸酯 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 22779996 Country of ref document: EP Kind code of ref document: A1 |
|
| ENP | Entry into the national phase |
Ref document number: 2023510843 Country of ref document: JP Kind code of ref document: A |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 202280008578.4 Country of ref document: CN |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| 122 | Ep: pct application non-entry in european phase |
Ref document number: 22779996 Country of ref document: EP Kind code of ref document: A1 |
|
| WWW | Wipo information: withdrawn in national office |