WO2015029621A1 - ハロゲンフリー難燃絶縁電線 - Google Patents

ハロゲンフリー難燃絶縁電線 Download PDF

Info

Publication number
WO2015029621A1
WO2015029621A1 PCT/JP2014/068776 JP2014068776W WO2015029621A1 WO 2015029621 A1 WO2015029621 A1 WO 2015029621A1 JP 2014068776 W JP2014068776 W JP 2014068776W WO 2015029621 A1 WO2015029621 A1 WO 2015029621A1
Authority
WO
WIPO (PCT)
Prior art keywords
mass
inner layer
halogen
resin
parts
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2014/068776
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
太郎 藤田
早味 宏
西川 信也
祐司 越智
堀 賢治
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sumitomo Electric Industries Ltd
Original Assignee
Sumitomo Electric Industries Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sumitomo Electric Industries Ltd filed Critical Sumitomo Electric Industries Ltd
Priority to IN4221DEN2015 priority Critical patent/IN2015DN04221A/en
Priority to EP14839089.1A priority patent/EP3051541A1/en
Priority to BR112015012342A priority patent/BR112015012342A2/pt
Priority to CN201480003191.5A priority patent/CN104813417A/zh
Publication of WO2015029621A1 publication Critical patent/WO2015029621A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Images

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L71/00—Compositions of polyethers obtained by reactions forming an ether link in the main chain; Compositions of derivatives of such polymers
    • C08L71/08—Polyethers derived from hydroxy compounds or from their metallic derivatives
    • C08L71/10—Polyethers derived from hydroxy compounds or from their metallic derivatives from phenols
    • C08L71/12—Polyphenylene oxides
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L23/00—Compositions of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Compositions of derivatives of such polymers
    • C08L23/02—Compositions of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Compositions of derivatives of such polymers not modified by chemical after-treatment
    • C08L23/04—Homopolymers or copolymers of ethene
    • C08L23/08—Copolymers of ethene
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01B—CABLES; CONDUCTORS; INSULATORS; SELECTION OF MATERIALS FOR THEIR CONDUCTIVE, INSULATING OR DIELECTRIC PROPERTIES
    • H01B3/00—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties
    • H01B3/18—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties mainly consisting of organic substances
    • H01B3/28—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties mainly consisting of organic substances natural or synthetic rubbers
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01B—CABLES; CONDUCTORS; INSULATORS; SELECTION OF MATERIALS FOR THEIR CONDUCTIVE, INSULATING OR DIELECTRIC PROPERTIES
    • H01B3/00—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties
    • H01B3/18—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties mainly consisting of organic substances
    • H01B3/30—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties mainly consisting of organic substances plastics; resins; waxes
    • H01B3/42—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties mainly consisting of organic substances plastics; resins; waxes polyesters; polyethers; polyacetals
    • H01B3/427—Polyethers
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01B—CABLES; CONDUCTORS; INSULATORS; SELECTION OF MATERIALS FOR THEIR CONDUCTIVE, INSULATING OR DIELECTRIC PROPERTIES
    • H01B3/00—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties
    • H01B3/18—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties mainly consisting of organic substances
    • H01B3/30—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties mainly consisting of organic substances plastics; resins; waxes
    • H01B3/44—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties mainly consisting of organic substances plastics; resins; waxes vinyl resins; acrylic resins
    • H01B3/441—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties mainly consisting of organic substances plastics; resins; waxes vinyl resins; acrylic resins from alkenes
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01B—CABLES; CONDUCTORS; INSULATORS; SELECTION OF MATERIALS FOR THEIR CONDUCTIVE, INSULATING OR DIELECTRIC PROPERTIES
    • H01B3/00—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties
    • H01B3/18—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties mainly consisting of organic substances
    • H01B3/30—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties mainly consisting of organic substances plastics; resins; waxes
    • H01B3/44—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties mainly consisting of organic substances plastics; resins; waxes vinyl resins; acrylic resins
    • H01B3/442—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties mainly consisting of organic substances plastics; resins; waxes vinyl resins; acrylic resins from aromatic vinyl compounds
    • H—ELECTRICITY
    • H01—ELECTRIC ELEMENTS
    • H01B—CABLES; CONDUCTORS; INSULATORS; SELECTION OF MATERIALS FOR THEIR CONDUCTIVE, INSULATING OR DIELECTRIC PROPERTIES
    • H01B7/00—Insulated conductors or cables characterised by their form
    • H01B7/17—Protection against damage caused by external factors, e.g. sheaths or armouring
    • H01B7/29—Protection against damage caused by extremes of temperature or by flame
    • H01B7/295—Protection against damage caused by extremes of temperature or by flame using material resistant to flame

Definitions

  • the present invention does not contain halogen, has an insulation coating that balances insulation resistance, flame retardancy, abrasion resistance, hot water resistance, heat deformation resistance, etc. at a high level, such as harnesses for automobiles and railway vehicles, etc.
  • the present invention relates to a halogen-free flame-retardant insulated electric wire that can be suitably used as:
  • Insulated wires such as harnesses for automobiles and railway vehicles may be exposed to adverse conditions such as temperature changes from cold to high temperatures, vibrations, wind and rain, etc., and may be exposed to heat generation or fire of equipment. Therefore, the insulation coating has mechanical strength, insulation resistance, hot water (stable) resistance, flame resistance, wear resistance, heat deformation resistance, etc. so that it can be used stably even under such adverse conditions. Therefore, it is required to satisfy a predetermined standard, and an acceptance standard based on the ISO standard which is an international standard is defined.
  • Polyvinyl chloride is known as a flame retardant insulating coating material.
  • a method for imparting flame retardancy to an insulating film by adding a halogen-based flame retardant is also known.
  • so-called halogen-free insulating materials that do not use PVC or halogen-based flame retardants have been demanded.
  • the use of a halogen-free insulating material that generates less smoke during combustion is often stipulated from the beginning so that passengers can easily evacuate in the event of a fire.
  • a halogen-free insulating material used as an insulating film a material in which a halogen-free flame retardant such as magnesium hydroxide, aluminum hydroxide, or a nitrogen flame retardant is added to an insulating resin such as a polyolefin resin is also known.
  • a halogen-free flame retardant such as magnesium hydroxide, aluminum hydroxide, or a nitrogen flame retardant is added to an insulating resin such as a polyolefin resin.
  • the halogen-free flame retardant needs to be added in a larger amount than the halogen flame retardant in order to satisfy the flame retardancy, and the insulation film has reduced flexibility, initial elongation and tensile elongation after heat aging. It is easy to cause problems such as degradation.
  • Patent Document 1 contains a thermoplastic resin containing 5% by mass or more of a resin having a carbon-carbon unsaturated bond or a resin having a carbonyl group, a polyfunctional monomer, and a specific type of organophosphorus flame retardant.
  • a flame retardant resin composition in which the content of the polyfunctional monomer and the organic phosphorus flame retardant is within a predetermined range is disclosed, and it is also described that it can be used as an insulating tube or the like.
  • the present invention has a high heat resistance water resistance with high insulation performance that passes the DC stability test required by the EN50306-2 standard, and is a halogen that balances insulation resistance, flame retardancy, wear resistance, and heat deformation resistance at a high level. It is an object to provide a free flame-retardant insulated wire.
  • One aspect of the present invention is an insulated wire having a conductor and a halogen-free insulating layer covering the conductor, the insulating layer comprising: A total of 100 parts by mass of resin obtained by finely dispersing 25-30 parts by mass of a polyphenylene ether resin and 10-30 parts by mass of a styrene elastomer in 40-65 parts by mass of high-density polyethylene having a melt flow rate of 0.60 or less. Component, and a cross-linked product of a resin composition containing 5 to 50% by mass of a phosphinic acid metal salt, 6 to 25% by mass of a phosphoric ester, and 1 to 10% by mass of a polyfunctional monomer based on the resin component.
  • the halogen-free flame retardant insulated wire of the present invention has high heat resistance and water resistance that passes the DC stability test required by EN50306-2 standard, and has insulation resistance, flame resistance, wear resistance, and heat deformation resistance. Is balanced at a high level. Therefore, it can be suitably used as an electric wire used in a high temperature environment such as wiring in an engine room of an automobile.
  • the inventor has a two-layer (or multi-layer) insulating coating, On the outer layer side, a polymer alloy, a phosphinic acid metal salt, a phosphate ester and a polyfunctional monomer in which a polyphenylene ether resin and a styrene elastomer are finely dispersed in a high density polyethylene having a melt flow rate of 0.60 or less are predetermined.
  • Halogen-free flame retardant that has high heat resistance and water resistance with high insulation performance that passes the DC stability test required by the EN50306-2 standard, and balances insulation resistance, flame resistance, wear resistance, and heat deformation resistance at a high level It discovered that an insulated wire was obtained and completed this invention.
  • One aspect of the present invention is an insulated wire having a conductor and a halogen-free insulating layer covering the conductor, the insulating layer comprising: A total of 100 parts by mass of resin obtained by finely dispersing 25-30 parts by mass of a polyphenylene ether resin and 10-30 parts by mass of a styrene elastomer in 40-65 parts by mass of high-density polyethylene having a melt flow rate of 0.60 or less. Component, and a cross-linked product of a resin composition containing 5 to 50% by mass of a phosphinic acid metal salt, 6 to 25% by mass of a phosphoric ester, and 1 to 10% by mass of a polyfunctional monomer based on the resin component.
  • the insulation layer of the flame-retardant insulated wire has a multilayer structure having at least two layers of an outer layer on the surface of the insulating layer and an inner layer in contact with the conductor (if necessary, there is another layer between the inner layer and the outer layer). May be)
  • This insulating layer has high hot water resistance (insulation performance is not deteriorated by storage in hot water) and balances insulation resistance, flame retardancy, wear resistance, and heat deformation resistance at a high level.
  • the outer layer mainly contributes to the flame retardancy, while the inner layer contributes to the improvement of hot water resistance.
  • the resin component constituting the outer layer is a polymer alloy obtained by finely dispersing a polyphenylene ether resin as a hard material and a styrene elastomer as a soft component in high-density polyethylene.
  • a high-density polyethylene having a relatively high molecular weight with a melt flow rate (hereinafter referred to as “MFR”) of 0.60 or less is used.
  • the high density polyethylene is polyethylene having a density of 0.942 g / cm 3 or more, and includes both homopolyethylene and polyethylene copolymer.
  • MFR of the high-density polyethylene is smaller, the mechanical strength is higher and the wear resistance is better. Therefore, the wear resistance can be improved by selecting one having an MFR of 0.60 or less. When MFR exceeds 0.60, it becomes difficult to obtain good wear resistance.
  • MFR is a value which shows the fluidity
  • the MFR of high density polyethylene is preferably 0.15 or more and 0.30 or less. Wear resistance is further improved by setting MFR to 0.30 or less. On the other hand, when MFR is smaller than 0.15, the extrusion processability is lowered, which is not preferable.
  • a preferred embodiment of the present invention includes an embodiment in which the high-density polyethylene is a high-density polyethylene having an MFR of 0.15 or more and 0.30 or less.
  • polyphenylene ether resin examples include those made of a single polyphenylene ether resin obtained by oxidative polymerization of 2,6-xylenol.
  • a modified polyphenylene ether resin obtained by melt blending polystyrene with polyphenylene ether can also be used. Use of this modified polyphenylene ether resin is preferable because workability during melt-mixing with high-density polyethylene and styrene-based elastomer is improved, and extrusion processability for forming an insulating coating is improved.
  • the polyphenylene ether-based resin those obtained by appropriately blending a carboxylic acid such as maleic anhydride can be used.
  • styrene elastomers examples include styrene / ethylene butene / styrene copolymers, styrene / ethylene propylene / styrene copolymers, styrene / ethylene / ethylene propylene / styrene copolymers, and styrene / butylene / styrene copolymers.
  • hydrogenated polymers and partially hydrogenated polymers can also be mentioned.
  • transduced carboxylic acid, such as maleic anhydride can also be blended suitably and used.
  • elastomer which is a block copolymer of styrene and a rubber component because the extrusion processability, tensile elongation at break and flexibility are improved.
  • Preferred block copolymers include styrene / ethylene / butylene / styrene block copolymers (SEBS) having a styrene / ethylene / butylene ratio of 30:70 to 60:40, and styrene / ethylene / butylene / ethylene block copolymers. (SEBC), styrene-ethylene / ethylene / propylene-styrene block copolymer (SEEPS), and the like.
  • the resin component is a polymer alloy obtained by finely dispersing a polyphenylene ether resin and a styrene elastomer in high density polyethylene. Finely dispersed means a state in which polyphenylene ether-based resin and styrene-based elastomer are uniformly dispersed in a submicron size in high-density polyethylene. In order to obtain uniform dispersion, it is preferable to mix with a high shear type twin-screw kneading extruder.
  • the content of the high-density polyethylene is 40 to 65 parts by mass
  • the content of the polyphenylene ether resin is 25 to 30 parts by mass
  • the content of the styrene elastomer is 10 parts by mass.
  • the content of the high density polyethylene is less than 40 parts by mass, it is difficult to finely disperse the polyphenylene ether resin and the styrene elastomer in the high density polyethylene to make a polymer alloy, and the wear resistance is lowered.
  • the content of the high-density polyethylene exceeds 65 parts by mass, the flame retardancy decreases.
  • Polyphenylene ether resin is a hard material with high heat resistance and high flame retardancy.
  • the styrenic elastomer imparts flexibility to the resin composition. Therefore, when the content of the styrene-based elastomer is less than 10 parts by mass, the flexibility is lowered, and when it exceeds 30 parts by mass, the wear resistance is lowered. When the content of the polyphenylene ether-based resin exceeds 30 parts by mass, the flexibility decreases, and when it is less than 25 parts by mass, the heat resistance, wear resistance, and flame retardancy decrease.
  • Resin component is cross-linked, and as a result of cross-linking, heat resistance and mechanical strength are improved.
  • the crosslinking method include a method by irradiation with ionizing radiation.
  • ionizing radiation include electromagnetic waves such as ⁇ -rays, X-rays, and ultraviolet rays, and particle beams such as ⁇ -rays.
  • ease of control, ease of use of the radiation source, penetration thickness of ionizing radiation, and speed of crosslinking treatment From the viewpoint of the above, an electron beam is preferable.
  • the resin composition forming the outer layer contains a phosphinic acid metal salt, a phosphate ester and a polyfunctional monomer in addition to the above resin components.
  • the phosphinic acid metal salt is a compound represented by the following formula (I).
  • R 1 and R 2 are each an alkyl group having 1 to 6 carbon atoms or an aryl group having 12 or less carbon atoms
  • M is calcium, aluminum or zinc
  • phosphinic acid metal salts include aluminum salts of organic phosphinic acids such as EXOLIT OP1230, EXOLIT OP1240, EXOLIT OP930, and EXOLIT OP935 manufactured by Clariant, or blends of aluminum phosphinic acid such as EXOLIT OP1312 and melamine polyphosphate. You can use things.
  • the content of the phosphinic acid metal salt is 5 to 50% by mass of the resin component (5 to 50 parts by mass with respect to 100 parts by mass of the resin component).
  • the content of the phosphinic acid metal salt is less than 5% by mass, the flame retardancy of the insulating layer becomes insufficient.
  • mechanical strength falls and abrasion resistance etc. become inadequate.
  • Phosphoric acid ester is added to the resin composition to act as a flame retardant.
  • the content of the phosphate ester is 6 to 25% by mass with respect to the resin component. When it is less than 6% by mass, the flame retardancy is insufficient, and when it exceeds 25% by mass, the mechanical properties of the insulating layer are deteriorated.
  • a phosphate ester having a high phosphorus content or a phosphate ester having a high molecular weight and a high melting point is preferable as a phosphate ester because it has a large effect of improving flame retardancy. Accordingly, condensed phosphate esters are preferred. In particular, bisphenol A bis-diphenyl phosphate can be preferably used.
  • phosphate esters include resorcinol bis-dixylenyl phosphate, resorcinol bis-diphenyl phosphate, triphenyl phosphate, triphenyl phosphate, trimethyl phosphate, triethyl phosphate, tricresidyl phosphate, trixylenyl phosphate , Cresyl phenyl phosphate, cresyl 2,6-xylenyl phosphate, 2-ethylhexyl diphenyl phosphate, 1,3 phenylene bis (diphenyl phosphate), 1,3 phenylene bis (di 2,6 xylenyl phosphate Fate), bisphenol A bis (diphenyl phosphate), octyl diphenyl phosphate, diethylene ethyl ester phosphate, dihydroxypropylene butyl ester Terphosphate, ethylene disodium ester phosphate, t-butyl
  • the polyfunctional monomer acts as a crosslinking aid when the resin component is crosslinked by irradiation with ionizing radiation.
  • the polyfunctional monomer those having a plurality of carbon-carbon double bonds in the molecule such as trimethylolpropane trimethacrylate, triallyl cyanurate, triallyl isocyanurate and the like can be preferably used.
  • the polyfunctional monomer is preferably liquid at normal temperature. Of these, trimethylolpropane trimethacrylate is preferred because of its high compatibility with resin components.
  • the content of the polyfunctional monomer is 1 to 10% by mass with respect to the resin component. When it is less than 1% by mass, the crosslinking efficiency is poor and the properties such as heat resistance are lowered. On the other hand, if it exceeds 10% by mass, the mechanical properties deteriorate.
  • the resin composition forming the outer layer can be prepared by mixing these materials using a known melt mixer such as a single-screw kneading extruder, a twin-screw kneading extruder, a pressure kneader, or a Banbury mixer.
  • a known melt mixer such as a single-screw kneading extruder, a twin-screw kneading extruder, a pressure kneader, or a Banbury mixer.
  • a polymer alloy in which a polyphenylene ether-based resin and a styrene-based elastomer are finely dispersed in high-density polyethylene can be formed by mixing the above-described essential components at a specified ratio using a known melt mixer.
  • any of low-density polyethylene, medium-density polyethylene, and high-density polyethylene can be used, but among these, high-density polyethylene is preferable because of its high wear resistance.
  • the polyethylene forming the inner layer is cross-linked. Crosslinking can be performed in the same manner as the crosslinking of the resin component constituting the outer layer. When cross-linking is performed by ionizing radiation irradiation, a method of forming an outer layer and an inner layer with a resin before cross-linking, and then irradiating the insulated wire with ionizing radiation to simultaneously cross-link the outer layer and inner layer resins is efficient and preferable.
  • the mechanical strength of the insulating layer, in particular, the heat deformation resistance is improved.
  • the degree of crosslinking is preferably such that the gel fraction is 50% or more.
  • the gel fraction is a percentage of the weight of the sample before immersion after the sample is immersed in xylene at 120 ° C. and heated for 24 hours, and then the insoluble matter is separated and dried. Means the calculated value.
  • the resin for forming the inner layer a resin having a tertiary carbon in the chemical structure and being radiation decomposable, such as polypropylene, is not preferable.
  • a crosslinking aid such as the above-mentioned polyfunctional monomer may be added to the inner layer.
  • additives such as an antioxidant, an antioxidant, a processing stabilizer, and a colorant may be appropriately added to both the outer layer and the inner layer. These additives may be added alone or in combination of two or more.
  • the thickness of the inner layer is 10 to 85% of the total thickness of the inner layer and the outer layer, and preferably 15 to 80%. If it is less than 10%, the hot water resistance decreases, and hot water resistance that passes the DC stability test required by the EN50306-2 standard cannot be obtained. On the other hand, if it exceeds 85%, the flame retardancy decreases.
  • the thickness of the outer layer is preferably 0.03 mm or more, more preferably 0.04 mm or more.
  • the thickness of the inner layer is preferably 0.03 mm or more.
  • the thickness of the outer layer is less than 0.03 mm, the flame retardancy is insufficient.
  • the thickness of the inner layer is less than 0.03 mm, the hot water resistance is lowered, and the DC stability test required by the EN50306-2 standard is likely to occur. Therefore, a preferred embodiment of the present invention includes an embodiment in which the outer layer has a thickness of 0.03 mm or more and the inner layer has a thickness of 0.03 mm or more.
  • the thickness of the insulating layer can be appropriately selected according to the conductor diameter.
  • the insulated wire of the present invention is excellent in wear resistance, the required characteristics can be obtained even when the thickness of the insulating layer is 0.25 mm or less. Can be satisfied. When the thickness of the insulating layer is 0.25 mm or less, wiring in a narrow portion is possible and handling is easy.
  • Examples of the conductor constituting the insulated wire include copper and aluminum having excellent conductivity.
  • the conductor may be a single wire or a stranded wire of a plurality of strands.
  • the insulating coating can be formed using a known extruder such as a melt extruder.
  • the outer layer resin composition may be coated to crosslink the resin.
  • the resin composition of the outer layer may be coated thereon, and then the inner layer and outer layer resins may be crosslinked simultaneously by irradiation with ionizing radiation.
  • the inner and outer layer resins (compositions) may be simultaneously coated on the conductor wires, and then the inner layer and outer layer resins may be simultaneously crosslinked by irradiation with ionizing radiation.
  • Bisphenol A bis-diphenyl phosphate manufactured by Daihachi Chemical Co., CR741 TMPTMA: Trimethylolpropane trimethacrylate
  • Phosphinic acid metal salt Exolit OP930 (manufactured by Clariant)
  • Magnesium hydroxide Kisuma 5P (manufactured by Kyowa Chemical) -Hindered phenolic antioxidant: Irganox 1010 (BASF)
  • Examples 1 to 4 and Comparative Examples 1 to 7 Preparation of resin composition pellets
  • the components for the outer layer and inner layer were mixed according to the formulation shown in Tables 1 and 2.
  • Hot water resistance test based on ISO6722
  • a 25m insulated wire wound three or more times is immersed in 1% saline solution at 85 ° C, and a 48V DC voltage is applied between the electrode immersed in the saline solution and the insulated wire. Then energize for 7 days.
  • a 7-day energization is performed 5 times, and a case where the insulation resistance after energization for a total of 35 days is 10 9 ⁇ ⁇ mm or more is considered acceptable.
  • the halogen-free flame-retardant insulated wires of Examples 1 to 4 that satisfy the constituent requirements of the present invention have high hot water resistance, insulation resistance, flame resistance, wear resistance, The heat deformability is excellent.
  • Comparative Example 1 in which the thickness of the inner layer is 89%, which exceeds 85% of the total thickness of the inner layer and the outer layer, the flame retardancy is low and the standard is not satisfied.
  • Comparative Examples 2 and 3 in which the thickness of the inner layer is less than 10% of the total thickness of the inner layer and the outer layer, the hot water resistance does not satisfy the standard according to EN50306-2 DC stability test.
  • the comparative example 4 which does not contain a phosphinic acid metal salt, a flame retardance is inadequate.
  • Comparative Example 5 in which polypropylene was used instead of high-density polyethylene, the wear resistance was insufficient. It is thought that polypropylene is difficult to be crosslinked. In Comparative Example 5, the adhesive strength between the inner layer and the outer layer was insufficient. This is probably because crosslinking is not performed, and the types of resins in the inner layer and the outer layer are different.
  • Comparative Example 6 using EVA as a resin component, the wear resistance was insufficient. Further, Comparative Example 7 using the cross-linked polyethylene for the outer layer and the resin composition of the outer layer of Example 1 for the inner layer had insufficient flame retardancy. This is probably because the cross-linked polyethylene having low flame retardancy is used as the outer layer.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Physics & Mathematics (AREA)
  • Spectroscopy & Molecular Physics (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Organic Chemistry (AREA)
  • Insulated Conductors (AREA)
  • Compositions Of Macromolecular Compounds (AREA)
  • Organic Insulating Materials (AREA)
PCT/JP2014/068776 2013-08-27 2014-07-15 ハロゲンフリー難燃絶縁電線 Ceased WO2015029621A1 (ja)

Priority Applications (4)

Application Number Priority Date Filing Date Title
IN4221DEN2015 IN2015DN04221A (enExample) 2013-08-27 2014-07-15
EP14839089.1A EP3051541A1 (en) 2013-08-27 2014-07-15 Halogen-free flame-retardant insulated wire
BR112015012342A BR112015012342A2 (pt) 2013-08-27 2014-07-15 fio elétrico isolado retardante de chamas livre de halogênio
CN201480003191.5A CN104813417A (zh) 2013-08-27 2014-07-15 无卤阻燃绝缘电线

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2013175883A JP2015046258A (ja) 2013-08-27 2013-08-27 ハロゲンフリー難燃絶縁電線
JP2013-175883 2013-08-27

Publications (1)

Publication Number Publication Date
WO2015029621A1 true WO2015029621A1 (ja) 2015-03-05

Family

ID=52586196

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2014/068776 Ceased WO2015029621A1 (ja) 2013-08-27 2014-07-15 ハロゲンフリー難燃絶縁電線

Country Status (6)

Country Link
EP (1) EP3051541A1 (enExample)
JP (1) JP2015046258A (enExample)
CN (1) CN104813417A (enExample)
BR (1) BR112015012342A2 (enExample)
IN (1) IN2015DN04221A (enExample)
WO (1) WO2015029621A1 (enExample)

Families Citing this family (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP6836246B2 (ja) * 2015-10-30 2021-02-24 イタルマッチ ケミカルズ ソチエタ ペル アツィオーニITALMATCH CHEMICALS S.p.A. 熱可塑性衝撃改良スチレン系ポリマーをベースとした、環境にやさしい難燃性組成物および成形材料
JP6418137B2 (ja) * 2015-11-25 2018-11-07 住友電気工業株式会社 難燃性樹脂組成物及び難燃性ケーブル
JP6418138B2 (ja) * 2015-11-25 2018-11-07 住友電気工業株式会社 難燃性樹脂組成物および難燃性ケーブル
CN107808710B (zh) * 2016-09-09 2021-09-28 日立金属株式会社 绝缘电线及电缆
JPWO2019176886A1 (ja) * 2018-03-13 2020-12-03 株式会社フジクラ ケーブル及びワイヤハーネス
CN115975331A (zh) * 2023-02-27 2023-04-18 昆山浩恩高分子材料有限公司 耐刮擦无卤阻燃热塑性弹性体线缆材料组合物及其制备方法

Citations (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2002124138A (ja) * 2000-10-16 2002-04-26 Auto Network Gijutsu Kenkyusho:Kk 絶縁電線
JP2011099084A (ja) 2009-10-06 2011-05-19 Sumitomo Electric Ind Ltd 難燃性樹脂組成物及びそれを用いた絶縁電線、フラットケーブル、成形品
JP2013161590A (ja) * 2012-02-03 2013-08-19 Sumitomo Electric Ind Ltd ハロゲンフリー難燃絶縁電線

Family Cites Families (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US8658898B2 (en) * 2009-04-13 2014-02-25 Yazaki Corporation Resin composition for heat-resistant electrical wire, and heat-resistant electrical wire
US9234088B2 (en) * 2011-03-17 2016-01-12 Sumitomo Electric Industries, Ltd. Non-halogen flame-retardant resin composition, and insulated electric wire and tube using the same
JP5218706B1 (ja) * 2011-06-29 2013-06-26 東レ株式会社 ポリフェニレンスルフィド樹脂組成物およびそれからなる成形品

Patent Citations (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2002124138A (ja) * 2000-10-16 2002-04-26 Auto Network Gijutsu Kenkyusho:Kk 絶縁電線
JP2011099084A (ja) 2009-10-06 2011-05-19 Sumitomo Electric Ind Ltd 難燃性樹脂組成物及びそれを用いた絶縁電線、フラットケーブル、成形品
JP2013161590A (ja) * 2012-02-03 2013-08-19 Sumitomo Electric Ind Ltd ハロゲンフリー難燃絶縁電線

Also Published As

Publication number Publication date
EP3051541A1 (en) 2016-08-03
IN2015DN04221A (enExample) 2015-10-16
CN104813417A (zh) 2015-07-29
BR112015012342A2 (pt) 2017-07-11
JP2015046258A (ja) 2015-03-12

Similar Documents

Publication Publication Date Title
JP5549675B2 (ja) ノンハロゲン難燃性樹脂組成物およびそれを用いた電線・ケーブル
CN103620700B (zh) 无卤阻燃绝缘电线
JP5825536B2 (ja) ノンハロゲン難燃性樹脂組成物並びにこれを用いた絶縁電線及びチューブ
JP5569363B2 (ja) 絶縁電線およびその製造方法
JP5556183B2 (ja) 難燃性樹脂組成物及びそれを用いた絶縁電線、フラットケーブル、成形品
KR101601286B1 (ko) 고난연 전자 기기 전선용 고분자 조성물과 이를 이용한 전선
CN104240809A (zh) 无卤阻燃性电线电缆
JP2015046258A (ja) ハロゲンフリー難燃絶縁電線
US20140141240A1 (en) Halogen-free resin composition, electric wire and cable
CN103842431B (zh) 耐热阻燃树脂组合物、绝缘电线和管
CN105038087A (zh) 高抗撕无卤阻燃电动汽车电线电缆料及电线电缆生产方法
JP2014067657A (ja) ノンハロゲン難燃性絶縁電線
JP2010118207A (ja) ハロゲンフリー難燃絶縁電線
JP5105242B2 (ja) 難燃性樹脂組成物並びにこれを用いた絶縁電線及びフラットケーブル
WO2015040941A1 (ja) ハロゲンフリー難燃絶縁電線および難燃絶縁チューブ
JP2016103414A (ja) 電線被覆材組成物、絶縁電線及びワイヤーハーネス
CN104220511A (zh) 无卤阻燃树脂组合物、以及使用该无卤阻燃树脂组合物的电线和电缆
JP2017160328A (ja) ハロゲンフリー難燃性樹脂組成物及びハロゲンフリー難燃絶縁電線
CN103219076A (zh) 无卤阻燃绝缘电线
KR101778803B1 (ko) 고내열성 전선용 절연 조성물
TW201504339A (zh) 無鹵素阻燃絕緣電線

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 14839089

Country of ref document: EP

Kind code of ref document: A1

REEP Request for entry into the european phase

Ref document number: 2014839089

Country of ref document: EP

WWE Wipo information: entry into national phase

Ref document number: 2014839089

Country of ref document: EP

REG Reference to national code

Ref country code: BR

Ref legal event code: B01A

Ref document number: 112015012342

Country of ref document: BR

NENP Non-entry into the national phase

Ref country code: DE

ENP Entry into the national phase

Ref document number: 112015012342

Country of ref document: BR

Kind code of ref document: A2

Effective date: 20150527