WO1999007934A1 - Procede de production d'etoffes tissees et/ou tricotees utilisant un fil de fixation de la sericine et etoffe tissee et/ou tricotee ainsi obtenue - Google Patents

Procede de production d'etoffes tissees et/ou tricotees utilisant un fil de fixation de la sericine et etoffe tissee et/ou tricotee ainsi obtenue Download PDF

Info

Publication number
WO1999007934A1
WO1999007934A1 PCT/JP1997/002741 JP9702741W WO9907934A1 WO 1999007934 A1 WO1999007934 A1 WO 1999007934A1 JP 9702741 W JP9702741 W JP 9702741W WO 9907934 A1 WO9907934 A1 WO 9907934A1
Authority
WO
WIPO (PCT)
Prior art keywords
woven
knitted fabric
producing
scouring
sericin
Prior art date
Application number
PCT/JP1997/002741
Other languages
English (en)
Japanese (ja)
Inventor
Keiichiro Kanehisa
Original Assignee
Kanehisa Inc.
Sumitomo Corporation
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kanehisa Inc., Sumitomo Corporation filed Critical Kanehisa Inc.
Priority to JP10535548A priority Critical patent/JP3061420B2/ja
Priority to US09/194,716 priority patent/US6302922B1/en
Priority to EP97934712A priority patent/EP1004699A4/fr
Priority to AU37831/97A priority patent/AU3783197A/en
Priority to KR1020007001217A priority patent/KR100338235B1/ko
Priority to PCT/JP1997/002741 priority patent/WO1999007934A1/fr
Publication of WO1999007934A1 publication Critical patent/WO1999007934A1/fr

Abstract

On reforme des étoffes tissées et/ou tricotées au moyen d'une réaction de réticulation de la triazine du squelette en faisant appel à la méthode de fixation de la séricine de la soie brute et ce, afin de renforcer l'irrétrécissabilité, l'auto-défroissabilité et la stabilité des formes de l'étoffe. L'opération achevée, on retire la séricine grâce à un raffinage spécifique. Le procédé de production de ces étoffes tissées et/ou tricotées consiste à transformer et à traiter la soie brute et/ou la fibre cellulosique en faisant intervenir la méthode de fixation précitée, à doubler et à torsader la soie brute et/ou la fibre cellulosique ainsi transformées et traitées à l'aide de la méthode de fixation, à tisser et à tricoter l'étoffe avec les fils ainsi doublés et torsadés, à faire gonfler l'étoffe tissée et/ou tricotée constituant une pièce de vêtement en l'immergeant dans une cuve et, enfin, à procéder à un raffinage enzymatique de l'étoffe dans la cuve. Ce procédé confère à l'étoffe tissée et/ou tricotée des qualités d'irrétrécissabilité, d'auto-défroissabilité et de stabilité des formes.
PCT/JP1997/002741 1996-02-23 1997-08-07 Procede de production d'etoffes tissees et/ou tricotees utilisant un fil de fixation de la sericine et etoffe tissee et/ou tricotee ainsi obtenue WO1999007934A1 (fr)

Priority Applications (6)

Application Number Priority Date Filing Date Title
JP10535548A JP3061420B2 (ja) 1997-08-07 1997-08-07 生糸のセリシン定着糸を用いた織編物の製造方法
US09/194,716 US6302922B1 (en) 1996-02-23 1997-08-07 Process for manufacturing woven or knit fabrics having excellent shrink and crease resistance and shape stability by using sericin fixed yarns of raw silks and the woven or knit fabrics manufactured by the same process
EP97934712A EP1004699A4 (fr) 1997-08-07 1997-08-07 Procede de production d'etoffes tissees et/ou tricotees utilisant un fil de fixation de la sericine et etoffe tissee et/ou tricotee ainsi obtenue
AU37831/97A AU3783197A (en) 1997-08-07 1997-08-07 Method of production of woven/knitted fabrics using sericin fixation yarn and woven/knitted fabric produced by the method
KR1020007001217A KR100338235B1 (ko) 1997-08-07 1997-08-07 세리신이 정착된 생사를 이용한 제직물 또는 편성물의제조 방법 및 이 방법으로 제조된 제직물 또는 편성물
PCT/JP1997/002741 WO1999007934A1 (fr) 1997-08-07 1997-08-07 Procede de production d'etoffes tissees et/ou tricotees utilisant un fil de fixation de la sericine et etoffe tissee et/ou tricotee ainsi obtenue

Applications Claiming Priority (1)

Application Number Priority Date Filing Date Title
PCT/JP1997/002741 WO1999007934A1 (fr) 1997-08-07 1997-08-07 Procede de production d'etoffes tissees et/ou tricotees utilisant un fil de fixation de la sericine et etoffe tissee et/ou tricotee ainsi obtenue

Publications (1)

Publication Number Publication Date
WO1999007934A1 true WO1999007934A1 (fr) 1999-02-18

Family

ID=14180936

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP1997/002741 WO1999007934A1 (fr) 1996-02-23 1997-08-07 Procede de production d'etoffes tissees et/ou tricotees utilisant un fil de fixation de la sericine et etoffe tissee et/ou tricotee ainsi obtenue

Country Status (5)

Country Link
EP (1) EP1004699A4 (fr)
JP (1) JP3061420B2 (fr)
KR (1) KR100338235B1 (fr)
AU (1) AU3783197A (fr)
WO (1) WO1999007934A1 (fr)

Cited By (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN110055756A (zh) * 2019-05-07 2019-07-26 四川丝玛帛科技有限公司 蚕丝的多维交联固胶方法
CN114622412A (zh) * 2022-03-02 2022-06-14 杭州路先非织造股份有限公司 一种热粘合制备丝胶整理水刺非织造布的方法

Families Citing this family (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
GB0126118D0 (en) 2001-10-31 2002-01-02 Vollrath Friedrich W L Precursor feedstock for forming filaments
KR100443462B1 (ko) * 2002-02-28 2004-08-09 성광물산(주) 티셔츠의 에리 형태안정화 가공방법
KR100693384B1 (ko) * 2005-06-24 2007-03-09 한양대학교 산학협력단 폴리락틱애시드 섬유의 정련방법
NZ592338A (en) 2008-09-26 2012-11-30 Oncomed Pharm Inc Frizzled-binding agents and uses thereof
KR100933549B1 (ko) 2009-05-07 2009-12-23 정은주 실크생사를 이용한 편직용 실크사 및 그 실크사에 의한 실크원단과 실크편직제품

Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS50126909A (fr) * 1974-03-29 1975-10-06
JPS5520034B2 (fr) * 1972-04-18 1980-05-30
JPS63126910A (ja) * 1986-11-11 1988-05-30 Satoshi Aoki 絹繊維の再生方法
JPH0411084A (ja) * 1990-04-28 1992-01-16 Kanebo Ltd 特殊表面絹布およびその製造方法
JPH0995865A (ja) * 1995-09-27 1997-04-08 Heian Yushi Kagaku Kogyo Kk セリシン定着繭及びセリシン定着糸
JPH09119033A (ja) * 1995-10-27 1997-05-06 Matsuoka Kigyo Kk 潜在捲縮性生糸およびその製造方法、ならびにその潜在捲縮性生糸から得られる捲縮性絹糸

Patent Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS5520034B2 (fr) * 1972-04-18 1980-05-30
JPS50126909A (fr) * 1974-03-29 1975-10-06
JPS63126910A (ja) * 1986-11-11 1988-05-30 Satoshi Aoki 絹繊維の再生方法
JPH0411084A (ja) * 1990-04-28 1992-01-16 Kanebo Ltd 特殊表面絹布およびその製造方法
JPH0995865A (ja) * 1995-09-27 1997-04-08 Heian Yushi Kagaku Kogyo Kk セリシン定着繭及びセリシン定着糸
JPH09119033A (ja) * 1995-10-27 1997-05-06 Matsuoka Kigyo Kk 潜在捲縮性生糸およびその製造方法、ならびにその潜在捲縮性生糸から得られる捲縮性絹糸

Non-Patent Citations (1)

* Cited by examiner, † Cited by third party
Title
See also references of EP1004699A4 *

Cited By (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN110055756A (zh) * 2019-05-07 2019-07-26 四川丝玛帛科技有限公司 蚕丝的多维交联固胶方法
CN114622412A (zh) * 2022-03-02 2022-06-14 杭州路先非织造股份有限公司 一种热粘合制备丝胶整理水刺非织造布的方法
CN114622412B (zh) * 2022-03-02 2023-08-01 杭州路先非织造股份有限公司 一种热粘合制备丝胶整理水刺非织造布的方法

Also Published As

Publication number Publication date
AU3783197A (en) 1999-03-01
KR20010022623A (ko) 2001-03-26
JP3061420B2 (ja) 2000-07-10
KR100338235B1 (ko) 2002-05-27
EP1004699A4 (fr) 2000-11-08
EP1004699A1 (fr) 2000-05-31

Similar Documents

Publication Publication Date Title
US6302922B1 (en) Process for manufacturing woven or knit fabrics having excellent shrink and crease resistance and shape stability by using sericin fixed yarns of raw silks and the woven or knit fabrics manufactured by the same process
WO1999007934A1 (fr) Procede de production d'etoffes tissees et/ou tricotees utilisant un fil de fixation de la sericine et etoffe tissee et/ou tricotee ainsi obtenue
TW200304516A (en) Stretch fabrics with improved chemical resistance and durability
JP3529089B2 (ja) 精製セルロース繊維織編物の加工方法
JP2000119973A (ja) 生糸のセリシン定着法を用いて製造された織編物
EP1599630B1 (fr) Procede de production d'un tissu de fibre lyocell teint et apprete
JPH0995865A (ja) セリシン定着繭及びセリシン定着糸
JP4195689B2 (ja) 綿と再生セルロース繊維とからなる複合繊維製品の製造方法
JP4799021B2 (ja) ナイロン繊維又は羊毛に用いられる染料で非染色性の糸を染色可能とする方法
CN1262713A (zh) 利用丝胶固定的纱线制造机织或针织织物的方法和由此方法制造的机织或针织织物
KR100483809B1 (ko) 이염성 셀룰로오스 직편물의 제조방법
JP2780747B2 (ja) 木綿繊維含有繊維製品及びその製造方法
JPH0711575A (ja) セルロース系繊維含有繊維製品及びその製造方法
JPH0411085A (ja) 特殊表面絹布およびその製造方法
JP2000054268A (ja) 溶剤紡糸セルロース繊維布帛の加工方法
JP2780746B2 (ja) 天然セルロース系繊維含有繊維製品の製造方法
WO1999046439A1 (fr) Procede de preparation de la laine utilisant la fixation par sericine de soie grege et rembourrages produits suivant ce procede
JP2001329464A (ja) 防縮性、形態安定性に優れたウオッシャブルウ−ルの製造方法及びそれによって製造された織編物
CN1332289A (zh) 生产耐收缩性及定形性好的可洗羊毛织品的方法及其织品
KR100367703B1 (ko) 방축성, 형태 안정성이 우수한 워셔블 울 직편물의 제조방법 및 그로부터 제조된 직편물
JPH09256271A (ja) 木綿繊維含有繊維製品およびその製造方法
JP3458909B2 (ja) 木綿繊維含有繊維製品及びその製造方法
JPH09195164A (ja) 木綿繊維含有繊維製品
JPH09296354A (ja) 木綿含有起毛または/およびパイル織編物の製造方法
JPH08170269A (ja) 絹製品

Legal Events

Date Code Title Description
WWE Wipo information: entry into national phase

Ref document number: 97182338.3

Country of ref document: CN

WWE Wipo information: entry into national phase

Ref document number: 09194716

Country of ref document: US

AK Designated states

Kind code of ref document: A1

Designated state(s): AL AM AT AU AZ BB BG BR BY CA CH CN CZ DE DK EE ES FI GB GE HU IS JP KE KG KR KZ LK LR LS LT LU LV MD MG MK MN MW MX NO NZ PL PT RO RU SD SE SG SI SK TJ TM TR TT UA UG US UZ VN

AL Designated countries for regional patents

Kind code of ref document: A1

Designated state(s): GH KE LS MW SD SZ UG ZW AM AZ BY KG KZ MD RU TJ TM AT BE CH DE DK ES FI FR GB GR IE IT LU MC NL PT SE BF BJ CF CG CI CM GA GN ML MR NE SN TD TG

ENP Entry into the national phase

Ref document number: 1999 194716

Country of ref document: US

Date of ref document: 19990305

Kind code of ref document: A

DFPE Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed before 20040101)
121 Ep: the epo has been informed by wipo that ep was designated in this application
WWE Wipo information: entry into national phase

Ref document number: 1020007001217

Country of ref document: KR

WWE Wipo information: entry into national phase

Ref document number: 1997934712

Country of ref document: EP

WWP Wipo information: published in national office

Ref document number: 1997934712

Country of ref document: EP

REG Reference to national code

Ref country code: DE

Ref legal event code: 8642

NENP Non-entry into the national phase

Ref country code: CA

WWP Wipo information: published in national office

Ref document number: 1020007001217

Country of ref document: KR

WWG Wipo information: grant in national office

Ref document number: 1020007001217

Country of ref document: KR

WWW Wipo information: withdrawn in national office

Ref document number: 1997934712

Country of ref document: EP