WO1995003341A1 - Polymers of brominated styrene - Google Patents
Polymers of brominated styrene Download PDFInfo
- Publication number
- WO1995003341A1 WO1995003341A1 PCT/US1994/008278 US9408278W WO9503341A1 WO 1995003341 A1 WO1995003341 A1 WO 1995003341A1 US 9408278 W US9408278 W US 9408278W WO 9503341 A1 WO9503341 A1 WO 9503341A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- monomers
- process according
- monomer
- polymerization initiator
- brominated
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
- C08F12/00—Homopolymers and copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and at least one being terminated by an aromatic carbocyclic ring
- C08F12/02—Monomers containing only one unsaturated aliphatic radical
- C08F12/04—Monomers containing only one unsaturated aliphatic radical containing one ring
- C08F12/14—Monomers containing only one unsaturated aliphatic radical containing one ring substituted by hetero atoms or groups containing heteroatoms
- C08F12/16—Halogens
- C08F12/21—Bromine
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
- C08F14/00—Homopolymers and copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and at least one being terminated by a halogen
- C08F14/16—Monomers containing bromine or iodine
Definitions
- the present invention relates generally to polymers of brominated styrene, and more particularly to methods for the solventless bulk polymerization of brominated styrenes.
- brominated styrene A variety of polymers of brominated styrene are known to the art. These brominated polystyrenes are commonly used as flame retardant additives, and are produced by one of two basic methods - the bromination of polystyrene or the polymerization of bromostyrene monomers.
- the materials made by the two production methods are not equivalent.
- bromination of polystyrene will result in undesirable side chain halogenation, causing a reduction in thermal stability or requiring expensive treatment to remove the more labile bromine atoms.
- Polymers prepared by the polymerization of bromostyrene do not have undesirable side chain halogenation, and are preferred for their relatively greater thermal stability.
- a more significant disadvantage of the bromination of polystyrene method is that the brominated polystyrenes produced are limited to copolymer compositions and molecular weights that are readily available.
- the products must be structures that are stable to, and will not interfere with, the bromination process.
- the polymerization of bromostyrene has several advantages over the bromination of polystyrene. As mentioned, it provides a more thermally stable product because side chain halogenation is avoided. Also, this method can be used to produce a continuum of molecular weights and bromine contents not otherwise available. Further, the polymerization can be accomplished without the use of solvents, and is readily adaptable to more economical continuous production processes. In addition, a broad spectrum of copolymer compositions may be produced simply by adjusting the monomer feed. Finally, production of convenient non-dusting pellets (with the option of incorporating auxiliary additives) is a natural by-product of the inventive polymerization process, and may be provided at no additional cost.
- a need also exists for a method of polymerizing bromostyrenes in which the reaction is run to a high degree of completion in a relatively brief period of time. The present invention addresses these needs.
- a process for the solventless polymerization of brominated styrenes comprising the steps of: (a) blending monomers of brominated styrenes with a polymerization initiator; (b) feeding the monomer/polymerization initiator mix into a prepolymerizer wherein the monomers begin to polymerize; and (c) feeding the monomer/polymerization initiator mix and the partially polymerized bromostyrene into a screw-type extruder to drive the polymerization to a high degree of completion in a short period of time.
- the monomers may be preheated before mixing with the initiator, or a heater may be included in the prepolymerizer.
- a second initiator may be used to facilitate polymerization in the extruder reaction zone.
- One object of the present invention is to provide a continuous process for producing brominated styrene homo- and copolymers, wherein the process uses an extruder for at least a portion of the polymerizations.
- a further object of the present invention is to provide a screw-type extruder effective for providing a high degree of conversion from monomer to polymer while maintaining an unexpectedly high molecular weight.
- a further object of the present invention is to provide an improvement to the basic polymerization process in which the early stages of the polymerization are carried out in a prepolymerizer which may optionally be preceded by a preheater.
- Another object of the present invention is to provide an improved polymerization process in which desired additives may be introduced continuously into the brominated polymer during polymerization, thereby avoiding the expense of a separate compounding step.
- An additional object of the present invention is to provide polymers that contain about 50% or more by weight of brominated styrene and that are useful as flame retardant additives.
- a further object of the present invention is to provide a flame retarding polymer comprised predominantly of brominated styrene and having an APHA solution color of less than 500 following heat ageing for eight hours at 243°C in a test tube.
- FIG. 1 is a schematic diagram of one screw extruder used in the processes of the present invention.
- FIG. 2 is a schematic diagram of a second screw extruder used in the processes of the present invention.
- FIG. 3 is a schematic diagram of a third screw extruder used in the processes of the present invention.
- FIG. 4 is a schematic diagram of a fourth screw extruder used in the processes of the present invention.
- FIG. 5 is a diagram of a prepolymerizer used in one preferred embodiment of the present invention.
- the present invention provides a process for the continuous bulk polymerization of brominated styrene monomers without the need for hazardous or costly solvents.
- the invention utilizes an extruder as a reaction pot to maintain a very short reaction time while controlling the potentially damaging exother .
- Either a single screw or twin screw extruder may be utilized, with the twin screw design being preferred for reasons of higher productivity, better mixing and the ability to take the reaction to a higher degree of completion.
- the entire reaction may be carried out in the extruder, using an initiator to accelerate the polymerization.
- the initiator is conveniently blended into the monomer with the mixture then being fed into the extruder throat.
- a second addition of monomer plus initiator can be made at a point several barrels downstream from the throat.
- the advantage of this is an increase in productivity; the slower continuous feed at the throat acts as a rear seal for the screw, allowing the faster second feed to be injected under pressure. This avoids the delay of having to wait for the rotating screw elements to carry away low viscosity monomer from the feed throat.
- the screw design of the extruder of the present invention is based on the need to control the reaction by subdividing the polymerization into a series of reaction zones.
- the extruder might be designed to have only one reaction zone.
- Such an extruder might be considered to be a plug flow reactor in which the first barrels are used to heat the monomer to polymerization temperature.
- the middle sections would then contain the highly exothermic runaway polymerization, and the end barrels would further reduce monomer content.
- Deficiencies flowing from this design include the inability to control temperature in the middle sections, as well as the inability to take the reaction to a high degree of completion.
- the inability to control temperature in the middle sections allows excessive temperatures to occur during the major portion of the reaction, eliminating the option of producing higher molecular weight versions of the product and possibly causing thermal degradation.
- the inability to take the reaction to a high degree of completion is probably caused by inadequate monomer mixing.
- the preferred embodiments of the present invention avoid the aforementioned problems by spreading the reaction out over a larger number of barrels. This is accomplished by selecting a screw design comprising at least three reaction zones. Each of the zones is characterized by three types of elements in the following order: (1) forward conveying, (2) neutral mixing, (3) flow impeding.
- the forward conveying elements can be of a normal flighted feeding type, conveying kneading type, or similar design intended to move material through the barrel toward the die.
- the neutral mixing section may consist of neutral kneading blocks, turbine blades or other designs that will mix materials but have little or no conveying effect.
- the last element type is a flow impeding design such as a reverse pumping element or a constricting element - sometimes referred to as a blister - which partially blocks the barrel, causing back pressure.
- the series of reaction zones may be preceded by a number of forward conveying elements. These will help to move material away from the throat, into the reaction zones, and serve to form a rear seal for the screw.
- the reaction zones may also be followed by forward conveying elements in order to move product away from the reaction zones and to develop the pressure required to force product through the die. It has been discovered that the number of required reaction zones is determined in part by the size (screw diameter) of the extruder. For example, in a 57 mm machine acceptable results were achieved with just five reaction zones. In scaling up to a 70 mm extruder however, acceptable results required seven zones, and significant improvements were obtained with a nine-zone design.
- the initiator for the extruder phase of the reaction may be selected from free radical generators well known to the industry.
- the preferred initiators have a reactivity such that they cause rapid polymerization of bromostyrenes to begin at temperatures above approximately 75°C.
- Examples of initiators that may be used to begin polymerizations within the extruder include dicumyl peroxide di-t-butyl peroxide
- the extruder is used to complete the reaction which was begun in a prepolymerizer.
- a prepolymerizer is a vessel through which monomer or mixtures of monomers are continuously introduced while a mixture of monomer and polymer is continuously removed. It is preferred that the contents of the vessel be agitated in some fashion to prevent localized areas of high polymer content. Means for heating the contents are desirable, but are not required if a preheater is used.
- suitable prepolymerizers include stirred tank reactors, static mixing tubes, and even other extruders.
- a low temperature, free radical generator is used to initiate the reaction when a prepolymerizer is utilized.
- the initiator may be selected from peroxides, azo compounds, and other free radical generators known to the industry.
- Preferred initiators have a reactivity such that they cause rapid polymerization of bromostyrenes at temperatures below approximately 100°C. This reactivity is normally expressed in terms of the half life temperature.
- the initiators of the present invention are selected such that at least half of the initiator has decomposed when held for 1 hour at 100°C.
- Examples of products meeting this requirement are benzoyl peroxide t-butylperoctoate t-butylperoxypivalate decanoyl peroxide di(2-ethylhexyl) peroxydicarbonate 2,2'-azobis (2,4-dimethylvaleronitrile) 2,2'-azobis(isobutyronitrile) The most preferred is 2,2'-azobis(2, -dimethylvaleronitrile) .
- the low temperature initiator is used at levels of from about 0.05% to 5% by weight of the monomer, with levels from 0.1% to 2% being preferred.
- accelerants or promoters may be used to reduce the half life temperature (increase the reactivity) of an initiator.
- the combinations of benzoyl peroxide/dimethylaniline and methylethylketone peroxide/cobalt soaps are well known to provide low temperature reactivity.
- the monomer may be 10% to 95% converted to polymer upon exiting the prepolymerizer, with a range of 40% to 95% being preferred.
- a high temperature initiator or blend of initiators may be desirable to complete the polymerization.
- the initiator may be added along with the monomer/polymer mixture, or may be injected several barrels downstream. Examples of suitable free radical generators are listed above (1 hour half lives above 75°C) with 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane being most preferred.
- the brominated monomers may have the general formula
- the most preferred monomer is dibromostyrene (DBS) .
- DBS dibromostyrene
- the bromostyrene monomers comprise from about 1% to about 20% monobromostyrene, from about 0.5% to about 10% tribromostyrene, and from about 70% to about 98.5% dibromostyrene.
- the monomer may also contain various storage stabilizers such as phenols or compounds of sulfur, nitrogen and phosphorus known to the industry to inhibit premature polymerization.
- the stabilizer may be removed prior to polymerization by water washes or by passing the monomer through a bed of activated carbon, silica, alumina or the like. Although water washes are not required, they provide the benefit of producing faster and more consistent reactivity.
- One advantage of the inventive process is the ability to produce a variety of molecular weight polymers within a particular piece of equipment by making only minor changes. It is very desirable and useful to offer these different product variations.
- a low molecular weight brominated polystyrene is known to provide better impact strength in rubber modified polystyrene, while the higher melt viscosity of the high molecular weight versions is preferred for processing characteristics with certain nylons.
- the modification of molecular weight may be accomplished through several different approaches.
- Traditional chain transfer agents such as compounds of sulfur or aliphatic halides may be added to the monomer prior to the start of the reaction.
- 1-dodecanethiol or bromotrichlorometliane are known to be very effective.
- a second approach is to simply increase the loading of initiator used to begin the polymerization. Higher concentrations of active chain initiators increase the competition for available monomer and promote certain chain terminating reactions. Both of these approaches will shorten the average chain length.
- a third way to reduce molecular weight is to conduct the polymerization at a higher temperature. This will also increase the concentration of active initiators, as well as increase the probability of chain terminating reactions occurring before chains have grown to high molecular weight.
- a minor amount of other reactive unsaturated monomers can be mixed into the brominated styrene for the purpose of additional property modification.
- modifications that might be desirable include changes in color, clarity, lubricity, compatibility, melt viscosity, softening point, thermal stability, ultraviolet stability, viscoelastic behavior, polarity, biodegradability and static charge dissipation.
- potential reactive co onomers are ⁇ taleic anhydride, styrene, substituted styrenes such as ⁇ -methylstyrene and chloromethylstyrene, acrylonitrile, methylmethacrylate, acrylic acid, methacrylic acid, butadiene and acryla ide.
- nonreactive additives may be incorporated during the process without the expense of a separate compounding step.
- Metered addition of materials may be accomplished at the feed throat or via a "crammer feeder" attached to any of the extruder barrels while polymerization is being completed in the extruder.
- the product exiting the extruder is therefore a very desirable package of additives in a homogeneous pellet form, produced without the expense of separate blending and compounding steps.
- additives examples include antioxidants, ultraviolet absorbers, antistatic agents, pigments, dyes, nucleating agents, fillers, slip agents, lubricants, antiblocking agents, plasticizers, tougheners and antimicrobials.
- supplemental flame retardants may be incorporated into the package. These may include nonhalogenated materials such as S 2 0 3 , S 2 0 5 , Bi 2 0 3 , Mo0 3 , H 4 N0 3 , trityl compounds, 2,3-dimethyl-2, 3-diphenylbutane, peroxides, and various phosphorous and/or nitrogen containing materials.
- the bromostyrene polymers may also include other halogenated flame retardants which could be used to increase the overall halogen content, improve efficiency or reduce dripping during combustion.
- halogenated additives include decabromodiphenyloxide octabromodiphenyloxide bis(tribromophenoxy)ethane decabromodiphenylethane bisimide of tetrabromophthalic anhydride and ethylenediamine
- molecular weights are given as "M p " , or peak molecular weight versus polystrene standards. This is determined by gel permeation chromatography in which the peak retention time of the bromostyrene polymer is equated with the molecular weight of a polystyrene standard having the same retention time.
- Example 1 demonstrates the use of a single screw extruder as a continuous prepolymerizer.
- the material exiting the die was collected on dry ice to quench the reaction and was found to contain 20.4% residual monomer, with the polymeric portion having a molecular weight Mschreib of 81,900.
- Example 2 A heated static mixing tube was successfully used as a continuous prepolymerizer.
- the product had an average molecular weight of 77,500, and contained 21% unreacted monomer.
- Partially converted dibromostyrene prepared using a single screw extruder as in Example 1 was collected and ground.
- a blend of 0.5 parts di-t-butylperoxide per 100 parts of monomer/polymer mixture was continuously fed into the same single screw extruder of Example 1, but with a hotter temperature profile. Settings of 210, 210, 220, 220, and 230°C from throat to die were maintained.
- the material going through the extruder had an estimated residence time of 55 seconds and was processed at a rate of 33 pounds per hour.
- the material had an M pc , of 81,400 and contained 13.4% monomer. After the reaction, the molecular weight was 70,000 and the monomer was reduced to 0.5%. Accordingly, it can be seen that the prepolymerizers of Example 1 or 2 could be arranged in tandem with the extruder of Example 3 to provide a continuous process.
- High molecular weight polydibromostyrene was prepared using a 30 mm twin screw extruder as the only reactor.
- the temperature profile was maintained at 160, 155, 185, 205, 205, 220, 230 and 240°C from throat to die while the screw speed was set at 400 rpm's.
- the compositions and rates of feed were:
- the feed throat was located in the first barrel and the injection port was approximately one-fourth of the way towards the die. Experimentation determined that 30 to 35 lbs/hr was the maximum effective feed rate. Increasing monomer flow at either point resulted in flooding of the throat.
- Low molecular weiglit polydibromostyrene was also prepared in the twin screw extruder.
- Example 6 contained 5 reaction zones. This did not provide adequate control of the reaction, spreading it out over just a long enough section to provide only medium molecular weight polymer. And with only 5 mixing areas the monomer content was still too high at the vented barrel to permit vacuum devolatilization without foaming.
- the design in Example 7 increased the number of reaction zones from 5 to 6 by adding a small section of neutral turbine mixers. This reduced the monomer to the point at which a vacuum could be applied, but molecular weight was still in the medium range.
- Example 8 the number of reaction zones was increased from 6 to 7, producing acceptable residual monomer and some improvement in molecular weight. However, it was not until Example 9, increasing the number of reaction zones to nine, that high molecular weight and low residual monomer were achieved.
- a supplemental flame retardant was incorporated into polydibromostyrene during continuous production.
- DBDPO decabromodiphenyloxide
- the temperature profile was maintained at approximately 140, 150, 180, 180, 200, 220, 230 and 240°C from throat to die. Screw speed was 400 rpm.
- the polymeric portion of the product had an M ps of 59,800, while the overall composition had a monomer content of 0.88%.
- the product had a calculated bromine content of 66% (compared with 60% for the neat homopolymer). Accordingly, less of the blend would be required as a flame retarding additive, making it a more efficient and valuable product while being produced at no greater of a manufacturing cost than the homopolymer itself.
- An inorganic synergist was also incorporated during continuous polymerization.
- a prepolymerizer was used to increase the production rate of DBS homopolymer.
- a prepolymerizer was constructed as shown in FIG. 5. In essence it was an elongated stirred tank reactor consisting of a 2 inch jacketed pipe containing a full length stir shaft fitted with a variety of blade types. Heating/cooling was accomplished by pumping oil of the desired temperature through the jacket. Monomer plus peroxide was continuously pumped into the bottom of the reactor and overflowed from the top directly into the twin screw extruder described in Example 4. The temperature profile of the extruder was 200, 210, 210, 210, 210, 220, 220 and 220°C with a screw speed of 400 rpm's. Oil temperature to the prepolymerizer was 145°C. A high temperature peroxide was injected neat into the extruder to complete the reaction.
- a preheater and a low temperature initiator were used to further increase productivity and to reduce the peak temperature.
- Example 12 The equipment in Example 12 was modified by adding a preheater to the system directly before the prepolymerizer.
- the preheater consisted of a 3 ft. long single pass stainless steel heat exchanger using recirculated tempered water as the heat source. Dibromostyrene monomer was passed through the preheater, warming it to about 70°C before it entered the prepolymerizer. The low temperature initiator was injected into the monomer just before it entered the prepolymerizer. Oil temperature to the prepolymerizer was reduced to 135°C. A high temperature peroxide was injected neat into the extruder to complete the reaction.
- the polymer produced under these conditions had an M 1 n b c of 64,000 with a residual monomer of 0.35%.
- the introduction of the preheater and low temperature initiator had several beneficial effects. For example, production rates were significantly increased over the 71.4 lbs/hr of the previous Example. This was accomplished by preheating the materials to near reaction temperature before entering the prepolymerizer, making the prepolymerizer more efficient. Also, the peak temperature within the prepolymerizer was reduced. The higher temperature peroxide used in Example 12 required that the reactants be heated to approximately 145°C to provide rapid polymerization. The exothermic polymer formation resulted in peak temperatures as high as 280°C. This is not desirable since low levels of thermal decomposition will occur, lowering product quality.
- the initiator of the current Example caused the reaction to begin at a lower temperature. Since the heat of polymerization is independent of the temperature at which the reaction begins, the lower initiation provided a peak exotherm of around 200°C, well below the point of thermal decom
- a copolymer of dibromostyrene was prepared using the design of this invention.
- the thermal stability of a DBS homopolymer, PDBS was compared with that of a polymeric material obtained by bromination of polystyrene (BrPS) .
- BrPS polystyrene
- a sample of each material was placed in a test tube which was then inserted into a heating block maintained at 243°C. The contents were held at temperature and exposed to air for 8 hours, after which the samples were cooled and removed by breaking away the glass. Colors of the heat treated materials were determined by dissolving them in toluene and comparing them with APHA standards.
- the PDBS demonstrated significantly less color formation, indicating less thermal decomposition.
Landscapes
- Chemical & Material Sciences (AREA)
- Health & Medical Sciences (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Medicinal Chemistry (AREA)
- Polymers & Plastics (AREA)
- Organic Chemistry (AREA)
- Addition Polymer Or Copolymer, Post-Treatments, Or Chemical Modifications (AREA)
- Compositions Of Macromolecular Compounds (AREA)
- Polymerisation Methods In General (AREA)
Priority Applications (4)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP50533495A JP3499558B2 (ja) | 1993-07-22 | 1994-07-22 | 臭素化スチレンのポリマー |
| DE69421080T DE69421080T2 (de) | 1993-07-22 | 1994-07-22 | Polymere aus bromiertem styrol |
| EP94922686A EP0710255B1 (en) | 1993-07-22 | 1994-07-22 | Polymers of brominated styrene |
| AU73710/94A AU7371094A (en) | 1993-07-22 | 1994-07-22 | Polymers of brominated styrene |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| US08/095,865 | 1993-07-22 | ||
| US08/095,865 US5304618A (en) | 1993-07-22 | 1993-07-22 | Polymers of brominated styrene |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO1995003341A1 true WO1995003341A1 (en) | 1995-02-02 |
Family
ID=22253940
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/US1994/008278 Ceased WO1995003341A1 (en) | 1993-07-22 | 1994-07-22 | Polymers of brominated styrene |
Country Status (7)
| Country | Link |
|---|---|
| US (2) | US5304618A (enExample) |
| EP (1) | EP0710255B1 (enExample) |
| JP (1) | JP3499558B2 (enExample) |
| AU (1) | AU7371094A (enExample) |
| DE (1) | DE69421080T2 (enExample) |
| IL (1) | IL110245A0 (enExample) |
| WO (1) | WO1995003341A1 (enExample) |
Cited By (13)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US5677390A (en) * | 1996-09-26 | 1997-10-14 | Albemarle Corporation | Process for brominating polystyrenic resins |
| US5686538A (en) * | 1996-09-26 | 1997-11-11 | Albemarle Corporation | Process for brominating polystyrenic resins |
| US5767203A (en) * | 1996-09-26 | 1998-06-16 | Albemarle Corporation | Process for brominated styrenic polymers |
| US5916978A (en) * | 1996-09-26 | 1999-06-29 | Albemarle Corporation | Process for brominated styrenic polymers |
| US6133381A (en) * | 1996-09-26 | 2000-10-17 | Albelmarle Corporation | Brominated polystyrenic flame retardants |
| US6232393B1 (en) | 1996-09-26 | 2001-05-15 | Albemarle Corporation | Polymers flame retarded with brominated polystyrenic resins |
| US6232408B1 (en) | 1996-09-26 | 2001-05-15 | Albemarle Corporation | Brominated polstyrenic resins |
| US6235831B1 (en) | 1996-09-26 | 2001-05-22 | Albemarle Corporation | Polymer compositions containing brominated polystyrenic resins |
| US6235844B1 (en) | 1996-09-26 | 2001-05-22 | Albemarle Corporation | Brominated polystyrenic resins |
| US6326439B1 (en) | 1996-09-26 | 2001-12-04 | Albemarle Corporation | Process for brominating polystyrenic resins |
| USRE37902E1 (en) | 1996-06-14 | 2002-11-05 | Albemarle Corporation | Brominated polystyrene having improved thermal stability and color and process for the preparation thereof |
| US6518368B2 (en) | 1996-06-14 | 2003-02-11 | Albemarle Corporation | Brominated polystyrene having improved thermal stability and color and process for the preparation thereof |
| US6521714B2 (en) | 1996-09-26 | 2003-02-18 | Albemarle Corporation | Brominated polystyrenic resins |
Families Citing this family (17)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US6037401A (en) * | 1996-02-26 | 2000-03-14 | Dsm N.V. | Flame retardant polyamide composition |
| US5723549A (en) * | 1996-06-14 | 1998-03-03 | Ferro Corporation | Process for the preparation of brominated polystyrene having improved color characteristics |
| CN1122046C (zh) * | 1997-11-18 | 2003-09-24 | 阿尔伯麦尔公司 | 制备具有改进颜色性能的溴化聚苯乙烯方法 |
| US6277314B1 (en) | 1998-02-04 | 2001-08-21 | Flextech Packaging, Ltd. | System and method for producing polymeric film |
| CN1518580A (zh) | 2000-09-22 | 2004-08-04 | ��Ļ���Ű˾ | 改良的阻燃剂-聚酰胺组合物 |
| US7202296B2 (en) * | 2003-12-19 | 2007-04-10 | Albemarle Corporation | Flame retardant compositions and their use |
| US7612156B2 (en) | 2004-09-30 | 2009-11-03 | Chemtura Corporation | Polymers of bromostyrenes having controlled molecular weight |
| CA2687508C (en) * | 2007-06-07 | 2016-05-24 | Albemarle Corporation | Low molecular weight brominated polymers and their use in thermoplastic formulations |
| CN100567234C (zh) * | 2008-03-14 | 2009-12-09 | 山东天一化学有限公司 | 一种三溴苯乙烯的制备方法 |
| CN101240047B (zh) * | 2008-03-14 | 2010-06-09 | 山东天一化学有限公司 | 一种聚三溴苯乙烯的制备方法 |
| US8993684B2 (en) | 2008-06-06 | 2015-03-31 | Albemarle Corporation | Low molecular weight brominated polymers, processes for their manufacture and their use in thermoplastic formulations |
| JP6133406B2 (ja) * | 2012-05-07 | 2017-05-24 | ビーエーエスエフ ソシエタス・ヨーロピアBasf Se | 混合ニーダを運転する方法 |
| WO2015162609A1 (en) * | 2014-04-23 | 2015-10-29 | Bromine Compounds Ltd. | Process for the polymerization of pentabromobenzyl (meth) acrylate, the polymer obtained and uses thereof |
| CN106117409A (zh) * | 2016-06-20 | 2016-11-16 | 山东大学 | 一种聚溴化苯乙烯的制备方法 |
| EP3590977B1 (de) * | 2018-07-05 | 2020-09-30 | Karlsruher Institut für Technologie | Lösungsmittelfreies polymerisierbares gemisch, verfahren zur herstellung eines funktionalisierten polymers und funktionalisiertes polymer |
| US11670836B2 (en) * | 2020-10-29 | 2023-06-06 | Advanced Semiconductor Engineering, Inc. | Semiconductor device package |
| EP4741429A1 (en) | 2024-11-12 | 2026-05-13 | LANXESS Corporation | Low molecular weight polybromostyrene as flame retardant, process of manufacture and applications thereof |
Citations (7)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| DE1112631B (de) * | 1959-08-26 | 1961-08-10 | Basf Ag | Verfahren zur kontinuierlichen Blockpolymerisation von Styrol |
| US3058929A (en) * | 1958-07-24 | 1962-10-16 | Dow Chemical Co | Method of polymerizing a vinyl aromatic monomer in the presence of an organic bromide and an organic peroxide and a self-extinguishing vinyl aromatic polymer containing same |
| JPS4926951A (enExample) * | 1972-07-12 | 1974-03-09 | ||
| JPS5896627A (ja) * | 1981-12-04 | 1983-06-08 | Nippon Ester Co Ltd | 連続重合方法 |
| WO1986003508A1 (en) * | 1984-12-05 | 1986-06-19 | General Electric Company | Thermoplastics containing brominated homopolymer |
| US4758644A (en) * | 1985-02-19 | 1988-07-19 | Mitsui Toatsu Chemicals, Inc. | Bromostyrene composition |
| US5274029A (en) * | 1990-09-10 | 1993-12-28 | Kelley Joseph M | Styrene polymerization process |
Family Cites Families (9)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| BE624340A (enExample) * | 1961-11-02 | |||
| US3534012A (en) * | 1969-05-01 | 1970-10-13 | Dow Chemical Co | Anionic polymerization of nuclear halogenated styrenes |
| US3794471A (en) * | 1971-08-16 | 1974-02-26 | Monsanto Co | Continuous polymerization apparatus |
| NL7812460A (nl) * | 1978-12-22 | 1980-06-24 | Stamicarbon | Broombevattend polymeer en werkwijze voor het bereiden van een broombevattend polymeer. |
| US4518194A (en) * | 1983-11-23 | 1985-05-21 | Kirkham Robert L | Automatic truck bed cover assembly |
| US4755573A (en) * | 1985-11-15 | 1988-07-05 | General Electric Company | Cationic polymerization of bromoalkenyl aromatic compounds with aromatic chain transfer agent, and products |
| US4728463A (en) * | 1986-08-18 | 1988-03-01 | Ethyl Corporation | Brominated fire retardant composition |
| US5223594A (en) * | 1987-07-08 | 1993-06-29 | Hitachi, Ltd. | Flame-retardant resin composition containing a bromostyrene prepolymer |
| WO1992004387A1 (en) * | 1990-09-06 | 1992-03-19 | Great Lakes Chemical Corporation | Flame retardant brominated styrene-based latices |
-
1993
- 1993-07-22 US US08/095,865 patent/US5304618A/en not_active Expired - Lifetime
-
1994
- 1994-03-22 US US08/215,803 patent/US5369202A/en not_active Expired - Fee Related
- 1994-07-07 IL IL110245A patent/IL110245A0/xx unknown
- 1994-07-22 EP EP94922686A patent/EP0710255B1/en not_active Expired - Lifetime
- 1994-07-22 DE DE69421080T patent/DE69421080T2/de not_active Expired - Lifetime
- 1994-07-22 AU AU73710/94A patent/AU7371094A/en not_active Abandoned
- 1994-07-22 WO PCT/US1994/008278 patent/WO1995003341A1/en not_active Ceased
- 1994-07-22 JP JP50533495A patent/JP3499558B2/ja not_active Expired - Fee Related
Patent Citations (7)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US3058929A (en) * | 1958-07-24 | 1962-10-16 | Dow Chemical Co | Method of polymerizing a vinyl aromatic monomer in the presence of an organic bromide and an organic peroxide and a self-extinguishing vinyl aromatic polymer containing same |
| DE1112631B (de) * | 1959-08-26 | 1961-08-10 | Basf Ag | Verfahren zur kontinuierlichen Blockpolymerisation von Styrol |
| JPS4926951A (enExample) * | 1972-07-12 | 1974-03-09 | ||
| JPS5896627A (ja) * | 1981-12-04 | 1983-06-08 | Nippon Ester Co Ltd | 連続重合方法 |
| WO1986003508A1 (en) * | 1984-12-05 | 1986-06-19 | General Electric Company | Thermoplastics containing brominated homopolymer |
| US4758644A (en) * | 1985-02-19 | 1988-07-19 | Mitsui Toatsu Chemicals, Inc. | Bromostyrene composition |
| US5274029A (en) * | 1990-09-10 | 1993-12-28 | Kelley Joseph M | Styrene polymerization process |
Non-Patent Citations (1)
| Title |
|---|
| See also references of EP0710255A4 * |
Cited By (16)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| USRE37902E1 (en) | 1996-06-14 | 2002-11-05 | Albemarle Corporation | Brominated polystyrene having improved thermal stability and color and process for the preparation thereof |
| US6518368B2 (en) | 1996-06-14 | 2003-02-11 | Albemarle Corporation | Brominated polystyrene having improved thermal stability and color and process for the preparation thereof |
| US6232393B1 (en) | 1996-09-26 | 2001-05-15 | Albemarle Corporation | Polymers flame retarded with brominated polystyrenic resins |
| US6232408B1 (en) | 1996-09-26 | 2001-05-15 | Albemarle Corporation | Brominated polstyrenic resins |
| US5852132A (en) * | 1996-09-26 | 1998-12-22 | Albemarle Corporation | Process for brominating polystyrenic resins |
| US5916978A (en) * | 1996-09-26 | 1999-06-29 | Albemarle Corporation | Process for brominated styrenic polymers |
| US6133381A (en) * | 1996-09-26 | 2000-10-17 | Albelmarle Corporation | Brominated polystyrenic flame retardants |
| US6207765B1 (en) | 1996-09-26 | 2001-03-27 | Albemarle Corporation | Process for brominated styrenic polymers |
| US5677390A (en) * | 1996-09-26 | 1997-10-14 | Albemarle Corporation | Process for brominating polystyrenic resins |
| US5852131A (en) * | 1996-09-26 | 1998-12-22 | Albemarle Corporation | Process for brominating polystyrenic resins |
| US6235831B1 (en) | 1996-09-26 | 2001-05-22 | Albemarle Corporation | Polymer compositions containing brominated polystyrenic resins |
| US6235844B1 (en) | 1996-09-26 | 2001-05-22 | Albemarle Corporation | Brominated polystyrenic resins |
| US6326439B1 (en) | 1996-09-26 | 2001-12-04 | Albemarle Corporation | Process for brominating polystyrenic resins |
| US5767203A (en) * | 1996-09-26 | 1998-06-16 | Albemarle Corporation | Process for brominated styrenic polymers |
| US5686538A (en) * | 1996-09-26 | 1997-11-11 | Albemarle Corporation | Process for brominating polystyrenic resins |
| US6521714B2 (en) | 1996-09-26 | 2003-02-18 | Albemarle Corporation | Brominated polystyrenic resins |
Also Published As
| Publication number | Publication date |
|---|---|
| EP0710255A1 (en) | 1996-05-08 |
| DE69421080D1 (de) | 1999-11-11 |
| IL110245A0 (en) | 1994-10-21 |
| EP0710255B1 (en) | 1999-10-06 |
| US5369202A (en) | 1994-11-29 |
| JPH09502210A (ja) | 1997-03-04 |
| US5304618A (en) | 1994-04-19 |
| EP0710255A4 (en) | 1997-03-26 |
| JP3499558B2 (ja) | 2004-02-23 |
| DE69421080T2 (de) | 2000-04-13 |
| AU7371094A (en) | 1995-02-20 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| US5304618A (en) | Polymers of brominated styrene | |
| WO2009107765A1 (ja) | 熱可塑性共重合体の製造方法 | |
| US5221787A (en) | Method of preparing maleic anhydride terpolymers | |
| KR100893873B1 (ko) | 내열 특성이 우수한 열가소성 공중합 수지의 연속 제조방법 | |
| EP3262088B1 (en) | Continuous process for preparation of high heat resistance copolymers | |
| JP2009191096A (ja) | 熱可塑性樹脂組成物の製造方法 | |
| Villalobos et al. | Bulk and solution processes | |
| JP5058407B2 (ja) | 場合によりエチレン性不飽和ニトリルを含有した、ビニル芳香族ポリマーの生産プロセス | |
| JP4325475B2 (ja) | メタクリル系重合体及びその製造方法 | |
| JPS6243409A (ja) | 熱可塑性樹脂の製造方法 | |
| US5880232A (en) | Process for producing styrene based polymer and molded articles comprising the polymer | |
| JPS5919576B2 (ja) | ゴム変性スチレン系樹脂の製造方法 | |
| KR100309807B1 (ko) | 고무개질 스티렌 수지의 제조방법 | |
| CN114106250A (zh) | 一种弹性体树脂组合物及其制备方法 | |
| JPS58132002A (ja) | メタクリレ−ト系共重合体の連続的製造方法 | |
| JPH07116262B2 (ja) | α−メチルスチレン共重合体の製造方法 | |
| JPH04146907A (ja) | スチレン―アクリロニトリル共重合体の製造法 | |
| AU464207B2 (en) | Process for producing transparent rubber modified plastics | |
| JPH06145215A (ja) | マレイミド系共重合体の製造方法 | |
| JP2970951B2 (ja) | ゴム変性スチレン系樹脂のゴム含有量調整方法 | |
| JPS5915348B2 (ja) | スチレン系樹脂組成物 | |
| JPH0334482B2 (enExample) | ||
| JPS62197408A (ja) | 熱可塑性共重合体樹脂組成物 | |
| JPH03199252A (ja) | スチレン系樹脂組成物 | |
| JPH01201307A (ja) | メタクリル重合体の製造法 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| AK | Designated states |
Kind code of ref document: A1 Designated state(s): AU CA JP KR NO RU |
|
| AL | Designated countries for regional patents |
Kind code of ref document: A1 Designated state(s): AT BE CH DE DK ES FR GB GR IE IT LU MC NL PT SE |
|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application | ||
| DFPE | Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed before 20040101) | ||
| WWE | Wipo information: entry into national phase |
Ref document number: 1994922686 Country of ref document: EP |
|
| WWP | Wipo information: published in national office |
Ref document number: 1994922686 Country of ref document: EP |
|
| NENP | Non-entry into the national phase |
Ref country code: CA |
|
| WWG | Wipo information: grant in national office |
Ref document number: 1994922686 Country of ref document: EP |