JPS6253423A - 紡機用メタリツクワイヤ - Google Patents

紡機用メタリツクワイヤ

Info

Publication number
JPS6253423A
JPS6253423A JP18905985A JP18905985A JPS6253423A JP S6253423 A JPS6253423 A JP S6253423A JP 18905985 A JP18905985 A JP 18905985A JP 18905985 A JP18905985 A JP 18905985A JP S6253423 A JPS6253423 A JP S6253423A
Authority
JP
Japan
Prior art keywords
metallic wire
wires
alloy steel
spinning machine
martensite
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP18905985A
Other languages
English (en)
Inventor
Shigeki Kanazawa
金沢 茂樹
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to JP18905985A priority Critical patent/JPS6253423A/ja
Publication of JPS6253423A publication Critical patent/JPS6253423A/ja
Pending legal-status Critical Current

Abstract

(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。

Description

【発明の詳細な説明】 産業上の利用分野 本発明は紡績工程の主として梳綿機に使用する、紡機用
メタリックワイヤの改良に関するものである。
従来の技術および問題点 従来、梳綿機は1時間当りの生産量が809程度の条件
で紡出されていた。
しかし、最近の高速高生産領域のきびしい紡出条件下で
は、紡出したスライノ(の品質向上と摩針周期の延長、
つまり省力化が要求され、また安定操業と経済的な面か
ら高耐摩耗性で寿命が長く、スライバ中のネップが少な
いことが要求されている。従って、従来この耐摩耗性、
摩針周期の延長を計る。ために0.8%〜1.1%の炭
素鋼材に焼入を施し九ものが使用されているが、耐摩耗
性が不十分で寿命の点で上記要件を満足するもの力!得
られないという問題点があった。
問題点を解決するための手段 本発明は上記問題点を解消するものであシ、Q、Or元
素を含有する合金鋼線を素材として、熱処理によシマル
チンサイト基地中にOrの硬い炭化物を分散させた耐摩
耗性の高いメタリックワイヤを提供するものである。
以下本発明の1実施例を説明する。
実施例 Ct−1,0% 、Or ’k 1.5%含んだ軸受鋼
を、球状化焼鈍し、所定のメタリックワイヤの形状に成
形し、900〜950℃の条件下で焼入れし、200〜
230℃にて焼戻しを行って耐摩耗性に優れたメタリッ
クワイヤを得た。
メタリックワイヤ形成素材として用いる合金鋼線中に含
まれるC量は0.13〜1.5%、Cr量は0、6〜3
.0%の範囲内にあることが望ましく、少ないと耐摩耗
性向上に有効なるクロム炭化物が少なくなり、又それ以
上に多いと加工性が悪くなる。
作  用 上記本発明の紡機用メタリックワイヤを用いて、下記の
条件下で高速高生産紡出を行なった結果について説明す
る。
シリンダ回転数  450 rpm ドツファ回転数   86 rpm 紡出ゲレy     530 gr/6YD生  産 
 量        50即/hr糸  番  手  
     M8〜20′8本発明の詳細な説明するため
に、図面に梳綿機の生産量とスライバ中のネップ数の関
係を示す。人は本発明の紡機用メタリックワイヤ、Bは
従来のメタリックワイヤの場合を示す。
スライバ中のネップ数が管理限界に来た時にメタリック
ワイヤの歯先を砥石にて置針するが、本発明の紡機用メ
タリックワイヤを用いると置針周期が従来の2倍以上に
なることがわかる。
又、従来の紡機用メタリックワイヤはネップ数が急速に
多く、歯先を置針しても動面稜線の摩耗の九めに使用初
期の如き少ないネップ数とならないが、本発明の紡機用
メタリックワイヤは歯先の置針により著しくネップ数を
減少させることができる。
発明の効果 本発明の紡機用メタリックワイヤは上記の構成よシなる
ため耐摩耗性を著るしく向上し、スフ4フ品質を長らく
維持することができる。
また、メタリックワイヤの歯先の置針周期が従来の2倍
以上となるため梳綿機の保全を容易とする等の優れた効
果を有する発明である。
【図面の簡単な説明】
図面は梳綿機の生産量とネップ数との関係を示す曲線図
である。 A・・・本発明の紡機用メタリックワイヤB・・・従来
の紡機用メタリックワイヤま胤屋

Claims (1)

    【特許請求の範囲】
  1. C含有量0.6%〜1.5%、Cr含有量0.6%〜3
    .0%である合金鋼線材を所定のメタリックワイヤ形状
    に成形し、熱処理によつて該メタリックワイヤのマルテ
    ンサイト基地中に球状化したクロム炭化物を分散せしめ
    てなることを特徴とする紡機用メタリックワイヤ。
JP18905985A 1985-08-27 1985-08-27 紡機用メタリツクワイヤ Pending JPS6253423A (ja)