WO2021065221A1 - 焼結部材、及び電磁カップリング - Google Patents
焼結部材、及び電磁カップリング Download PDFInfo
- Publication number
- WO2021065221A1 WO2021065221A1 PCT/JP2020/031031 JP2020031031W WO2021065221A1 WO 2021065221 A1 WO2021065221 A1 WO 2021065221A1 JP 2020031031 W JP2020031031 W JP 2020031031W WO 2021065221 A1 WO2021065221 A1 WO 2021065221A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- sintered member
- mass
- tooth
- cam
- missing
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Images
Classifications
-
- F—MECHANICAL ENGINEERING; LIGHTING; HEATING; WEAPONS; BLASTING
- F16—ENGINEERING ELEMENTS AND UNITS; GENERAL MEASURES FOR PRODUCING AND MAINTAINING EFFECTIVE FUNCTIONING OF MACHINES OR INSTALLATIONS; THERMAL INSULATION IN GENERAL
- F16D—COUPLINGS FOR TRANSMITTING ROTATION; CLUTCHES; BRAKES
- F16D27/00—Magnetically- or electrically- actuated clutches; Control or electric circuits therefor
- F16D27/10—Magnetically- or electrically- actuated clutches; Control or electric circuits therefor with an electromagnet not rotating with a clutching member, i.e. without collecting rings
- F16D27/108—Magnetically- or electrically- actuated clutches; Control or electric circuits therefor with an electromagnet not rotating with a clutching member, i.e. without collecting rings with axially movable clutching members
- F16D27/112—Magnetically- or electrically- actuated clutches; Control or electric circuits therefor with an electromagnet not rotating with a clutching member, i.e. without collecting rings with axially movable clutching members with flat friction surfaces, e.g. discs
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B22—CASTING; POWDER METALLURGY
- B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B22F3/00—Manufacture of workpieces or articles from metallic powder characterised by the manner of compacting or sintering; Apparatus specially adapted therefor ; Presses and furnaces
- B22F3/02—Compacting only
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B22—CASTING; POWDER METALLURGY
- B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B22F3/00—Manufacture of workpieces or articles from metallic powder characterised by the manner of compacting or sintering; Apparatus specially adapted therefor ; Presses and furnaces
- B22F3/10—Sintering only
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B22—CASTING; POWDER METALLURGY
- B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B22F3/00—Manufacture of workpieces or articles from metallic powder characterised by the manner of compacting or sintering; Apparatus specially adapted therefor ; Presses and furnaces
- B22F3/10—Sintering only
- B22F3/1017—Multiple heating or additional steps
- B22F3/1028—Controlled cooling
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B22—CASTING; POWDER METALLURGY
- B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B22F3/00—Manufacture of workpieces or articles from metallic powder characterised by the manner of compacting or sintering; Apparatus specially adapted therefor ; Presses and furnaces
- B22F3/24—After-treatment of workpieces or articles
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B22—CASTING; POWDER METALLURGY
- B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B22F5/00—Manufacture of workpieces or articles from metallic powder characterised by the special shape of the product
- B22F5/08—Manufacture of workpieces or articles from metallic powder characterised by the special shape of the product of toothed articles, e.g. gear wheels; of cam discs
-
- C—CHEMISTRY; METALLURGY
- C21—METALLURGY OF IRON
- C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
- C21D1/00—General methods or devices for heat treatment, e.g. annealing, hardening, quenching or tempering
- C21D1/18—Hardening; Quenching with or without subsequent tempering
-
- C—CHEMISTRY; METALLURGY
- C21—METALLURGY OF IRON
- C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
- C21D6/00—Heat treatment of ferrous alloys
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C33/00—Making ferrous alloys
- C22C33/02—Making ferrous alloys by powder metallurgy
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C33/00—Making ferrous alloys
- C22C33/02—Making ferrous alloys by powder metallurgy
- C22C33/0257—Making ferrous alloys by powder metallurgy characterised by the range of the alloying elements
- C22C33/0264—Making ferrous alloys by powder metallurgy characterised by the range of the alloying elements the maximum content of each alloying element not exceeding 5%
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22C—ALLOYS
- C22C38/00—Ferrous alloys, e.g. steel alloys
- C22C38/18—Ferrous alloys, e.g. steel alloys containing chromium
- C22C38/40—Ferrous alloys, e.g. steel alloys containing chromium with nickel
- C22C38/44—Ferrous alloys, e.g. steel alloys containing chromium with nickel with molybdenum or tungsten
-
- F—MECHANICAL ENGINEERING; LIGHTING; HEATING; WEAPONS; BLASTING
- F16—ENGINEERING ELEMENTS AND UNITS; GENERAL MEASURES FOR PRODUCING AND MAINTAINING EFFECTIVE FUNCTIONING OF MACHINES OR INSTALLATIONS; THERMAL INSULATION IN GENERAL
- F16D—COUPLINGS FOR TRANSMITTING ROTATION; CLUTCHES; BRAKES
- F16D1/00—Couplings for rigidly connecting two coaxial shafts or other movable machine elements
- F16D1/06—Couplings for rigidly connecting two coaxial shafts or other movable machine elements for attachment of a member on a shaft or on a shaft-end
-
- F—MECHANICAL ENGINEERING; LIGHTING; HEATING; WEAPONS; BLASTING
- F16—ENGINEERING ELEMENTS AND UNITS; GENERAL MEASURES FOR PRODUCING AND MAINTAINING EFFECTIVE FUNCTIONING OF MACHINES OR INSTALLATIONS; THERMAL INSULATION IN GENERAL
- F16D—COUPLINGS FOR TRANSMITTING ROTATION; CLUTCHES; BRAKES
- F16D27/00—Magnetically- or electrically- actuated clutches; Control or electric circuits therefor
- F16D27/02—Magnetically- or electrically- actuated clutches; Control or electric circuits therefor with electromagnets incorporated in the clutch, i.e. with collecting rings
- F16D27/09—Magnetically- or electrically- actuated clutches; Control or electric circuits therefor with electromagnets incorporated in the clutch, i.e. with collecting rings and with interengaging jaws or gear-teeth
-
- F—MECHANICAL ENGINEERING; LIGHTING; HEATING; WEAPONS; BLASTING
- F16—ENGINEERING ELEMENTS AND UNITS; GENERAL MEASURES FOR PRODUCING AND MAINTAINING EFFECTIVE FUNCTIONING OF MACHINES OR INSTALLATIONS; THERMAL INSULATION IN GENERAL
- F16D—COUPLINGS FOR TRANSMITTING ROTATION; CLUTCHES; BRAKES
- F16D27/00—Magnetically- or electrically- actuated clutches; Control or electric circuits therefor
- F16D27/10—Magnetically- or electrically- actuated clutches; Control or electric circuits therefor with an electromagnet not rotating with a clutching member, i.e. without collecting rings
-
- F—MECHANICAL ENGINEERING; LIGHTING; HEATING; WEAPONS; BLASTING
- F16—ENGINEERING ELEMENTS AND UNITS; GENERAL MEASURES FOR PRODUCING AND MAINTAINING EFFECTIVE FUNCTIONING OF MACHINES OR INSTALLATIONS; THERMAL INSULATION IN GENERAL
- F16D—COUPLINGS FOR TRANSMITTING ROTATION; CLUTCHES; BRAKES
- F16D27/00—Magnetically- or electrically- actuated clutches; Control or electric circuits therefor
- F16D27/10—Magnetically- or electrically- actuated clutches; Control or electric circuits therefor with an electromagnet not rotating with a clutching member, i.e. without collecting rings
- F16D27/118—Magnetically- or electrically- actuated clutches; Control or electric circuits therefor with an electromagnet not rotating with a clutching member, i.e. without collecting rings with interengaging jaws or gear teeth
-
- F—MECHANICAL ENGINEERING; LIGHTING; HEATING; WEAPONS; BLASTING
- F16—ENGINEERING ELEMENTS AND UNITS; GENERAL MEASURES FOR PRODUCING AND MAINTAINING EFFECTIVE FUNCTIONING OF MACHINES OR INSTALLATIONS; THERMAL INSULATION IN GENERAL
- F16D—COUPLINGS FOR TRANSMITTING ROTATION; CLUTCHES; BRAKES
- F16D27/00—Magnetically- or electrically- actuated clutches; Control or electric circuits therefor
- F16D27/14—Details
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B22—CASTING; POWDER METALLURGY
- B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B22F3/00—Manufacture of workpieces or articles from metallic powder characterised by the manner of compacting or sintering; Apparatus specially adapted therefor ; Presses and furnaces
- B22F3/24—After-treatment of workpieces or articles
- B22F2003/248—Thermal after-treatment
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B22—CASTING; POWDER METALLURGY
- B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B22F2301/00—Metallic composition of the powder or its coating
- B22F2301/35—Iron
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B22—CASTING; POWDER METALLURGY
- B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B22F2998/00—Supplementary information concerning processes or compositions relating to powder metallurgy
- B22F2998/10—Processes characterised by the sequence of their steps
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B22—CASTING; POWDER METALLURGY
- B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B22F2999/00—Aspects linked to processes or compositions used in powder metallurgy
-
- C—CHEMISTRY; METALLURGY
- C21—METALLURGY OF IRON
- C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
- C21D2211/00—Microstructure comprising significant phases
- C21D2211/001—Austenite
-
- C—CHEMISTRY; METALLURGY
- C21—METALLURGY OF IRON
- C21D—MODIFYING THE PHYSICAL STRUCTURE OF FERROUS METALS; GENERAL DEVICES FOR HEAT TREATMENT OF FERROUS OR NON-FERROUS METALS OR ALLOYS; MAKING METAL MALLEABLE, e.g. BY DECARBURISATION OR TEMPERING
- C21D2211/00—Microstructure comprising significant phases
- C21D2211/008—Martensite
-
- F—MECHANICAL ENGINEERING; LIGHTING; HEATING; WEAPONS; BLASTING
- F16—ENGINEERING ELEMENTS AND UNITS; GENERAL MEASURES FOR PRODUCING AND MAINTAINING EFFECTIVE FUNCTIONING OF MACHINES OR INSTALLATIONS; THERMAL INSULATION IN GENERAL
- F16D—COUPLINGS FOR TRANSMITTING ROTATION; CLUTCHES; BRAKES
- F16D2200/00—Materials; Production methods therefor
- F16D2200/0004—Materials; Production methods therefor metallic
- F16D2200/0008—Ferro
- F16D2200/0021—Steel
Definitions
- the present disclosure relates to sintered members and electromagnetic couplings. This application claims priority based on Japanese Application No. 2019-182666 filed on October 3, 2019, and incorporates all the contents described in the Japanese application.
- Patent Document 1 discloses a driving force transmission device (electromagnetic coupling) that connects and disconnects a propeller shaft of a four-wheel drive vehicle and a rear differential.
- the driving force transmission device includes a first cam mechanism.
- the first cam mechanism includes a main cam (first cam), a pilot cam (second cam), and a cam ball interposed between the main cam and the pilot cam.
- the sintered member according to the present disclosure is It is an annular sintered member and The first surface facing one side in the axial direction, A second surface facing the other side in the axial direction, An inner peripheral surface connected to the inner peripheral edge of the first surface and It has a plurality of tooth groups and a plurality of missing teeth alternately provided along the circumferential direction of the inner peripheral surface.
- the second surface has a plurality of ball grooves arranged in parallel in the circumferential direction.
- Each tooth group has a plurality of spline teeth continuous in the circumferential direction of the peripheral surface.
- the number of the plurality of missing teeth and the number of the plurality of ball grooves are the same.
- the radial formation position of the plurality of missing teeth is within the radial formation range of the plurality of ball grooves.
- the circumferential formation range of the plurality of missing teeth and the circumferential formation range of the plurality of ball grooves overlap.
- the electromagnetic coupling according to the present disclosure is An electromagnetic coupling comprising a first cam, a second cam, and a ball interposed between the first cam and the second cam.
- the first cam is made of the sintered member of the present disclosure.
- FIG. 1 is a perspective view showing the first surface side of the sintered member according to the first and second embodiments.
- FIG. 2 is a perspective view showing the second surface side of the sintered member according to the first and second embodiments.
- FIG. 3 is a plan view showing a part of the first surface side of the sintered member according to the first and second embodiments.
- FIG. 4 is a plan view showing a part of the sintered member according to the first and second embodiments on the second surface side.
- FIG. 5 is a cross-sectional view showing a part of the sintered member cut along the VV cutting line of FIG.
- FIG. 6 is a cross-sectional view showing the electromagnetic coupling according to the first embodiment.
- FIG. 7 shows the sintered member and sample No. 2 according to the second embodiment.
- FIG. 8A shows the sintered member and sample No. 2 according to the second embodiment. It is a micrograph which shows the cross section of the sintered member of 1.
- FIG. 8B shows the sintered member and sample No. 2 according to the second embodiment. It is a micrograph which shows the cross section of the sintered member of 1.
- FIG. 9A shows the sintered member and sample No. 2 according to the second embodiment. 2 is a photomicrograph showing a cross section of the sintered member of 2.
- FIG. 9B shows the sintered member and sample No. 2 according to the second embodiment.
- FIG. 2 is a photomicrograph showing a cross section of the sintered member of 2.
- FIG. 10 is an explanatory diagram illustrating a method of measuring the maximum stress acting on the spline teeth of the sintered member in the analysis example.
- FIG. 11 shows the sample No. It is a micrograph which shows the cross section of the sintered member of 101.
- FIG. 12 shows the sample No. It is a micrograph which shows the cross section of the sintered member of 102.
- the first cam provided in the cam mechanism of the electromagnetic coupling may be composed of a sintered member. Since the first cam mechanically engages with the second cam via the ball, it is desired to have excellent fatigue strength. This is because the first cam having excellent fatigue strength has a long life, so that the electromagnetic coupling can be used for a long period of time.
- one of the purposes of the present disclosure is to provide a sintered member capable of constructing an electromagnetic coupling that can be used for a long period of time.
- Another purpose of this disclosure is to provide an electromagnetic coupling that can be used for a long period of time.
- the sintered member according to the present disclosure can construct an electromagnetic coupling that can be used for a long period of time.
- the electromagnetic coupling according to the present disclosure can be used for a long period of time.
- the first cam provided in the conventional electromagnetic coupling does not have a tooth missing portion on the peripheral surface, and spline teeth are also provided on the peripheral surface in the circumferential direction overlapping the formation range of each ball groove. ing.
- this first cam when an axial load of the sintered member by the second cam of the electromagnetic coupling acts on the sintered member via the ball of the electromagnetic coupling, the present inventor presents the present invention. It was found that stress may be concentrated on the roots of spline teeth.
- the present disclosure is based on the above findings. First, embodiments of the present disclosure will be listed and described.
- the sintered member according to one aspect of the present disclosure is It is an annular sintered member and The first surface facing one side in the axial direction, A second surface facing the other side in the axial direction, An inner peripheral surface connected to the inner peripheral edge of the first surface and It has a plurality of tooth groups and a plurality of missing teeth alternately provided along the circumferential direction of the inner peripheral surface.
- the second surface has a plurality of ball grooves arranged in parallel in the circumferential direction.
- Each tooth group has a plurality of spline teeth continuous in the circumferential direction of the peripheral surface.
- the number of the plurality of missing teeth and the number of the plurality of ball grooves are the same.
- the radial formation position of the plurality of missing teeth is within the radial formation range of the plurality of ball grooves.
- the circumferential formation range of the plurality of missing teeth and the circumferential formation range of the plurality of ball grooves overlap.
- the above sintered member can construct an electromagnetic coupling that can be used for a long period of time.
- the reason is as follows.
- the forming range of the plurality of missing teeth in the circumferential direction and the forming range of the plurality of ball grooves in the circumferential direction overlap, the forming range of each ball groove overlaps on the inner peripheral surface.
- the above-mentioned sintered member constitutes the first cam of the electromagnetic coupling, and the axial load of the sintered member by the second cam of the electromagnetic coupling is applied to the sintered member via the ball of the electromagnetic coupling. Even if it acts on the tooth, the stress concentration is relaxed at the rounded missing tooth portion, and the stress concentration on the tooth root of the spline tooth can be suppressed. Therefore, the sintered member can suppress a decrease in fatigue strength and has a long life.
- the fluctuation range of Vickers hardness up to a depth of 5.0 mm along the direction orthogonal to the surface of the sintered member is 100 HV or less.
- the sintered member has a uniform hardness up to 5.0 mm along a direction orthogonal to the surface, which is a predetermined depth from the surface of the sintered member.
- a sintered member having a non-uniform hardness is easily damaged because a portion having a low hardness can be a mechanical weak point.
- the sintered member having uniform hardness is less likely to be damaged because there are few places where it can be a mechanical weak point.
- the above-mentioned sintered member It contains Ni, Cr, Mo, and C, and has a composition in which the balance is Fe and unavoidable impurities.
- the content of Ni in the sintered member is more than 2% by mass and 6% by mass or less.
- the above sintered member has both high hardness and high toughness. The reason is that although the Ni content is high, it is not excessively high.
- the Cr content is 2% by mass or more and 4% by mass or less.
- the Mo content is 0.2% by mass or more and 0.9% by mass or less.
- the content of C is 0.2% by mass or more and 1.0% by mass or less.
- the above sintered member has high hardness. The reason is that the content of each of the above elements satisfies the above range, although the details will be described later.
- the above-mentioned sintered member It has a multiphase structure of martensite phase and retained austenite phase.
- the area ratio of the retained austenite phase in any cross section of the sintered member is 5% or more.
- the above sintered member has both high hardness and high toughness. The reason is that it has a high hardness martensite phase and a high toughness retained austenite phase. In particular, the sintered member has excellent toughness. The reason is that the area ratio of the tough retained austenite phase is high.
- the electromagnetic coupling according to one aspect of the present disclosure is An electromagnetic coupling comprising a first cam, a second cam, and a ball interposed between the first cam and the second cam.
- the first cam is composed of the sintered member according to any one of the above (1) to (5).
- the above electromagnetic coupling can be used for a long period of time.
- the reason is that the first cam is made of a sintered member having a long life, which can suppress stress concentration on the tooth root of the spline tooth as described above.
- Embodiment 1 [Sintered member]
- the sintered member 1 according to the first embodiment will be described with reference to FIGS. 1 to 5.
- the sintered member 1 is formed in an annular shape (FIG. 1).
- the sintered member 1 has a first surface 11 (FIG. 1), a second surface 12 (FIG. 2), and a peripheral surface 15 (FIG. 1).
- the first surface 11 and the second surface 12 face opposite to each other in the axial direction of the sintered member 1.
- the peripheral surface 15 is an annular surface connected to the inner peripheral edge of the first surface 11.
- One of the features of the sintered member 1 according to this embodiment is that it satisfies the following requirements (a) and (b).
- the shape of the sintered member 1 is a disk shape (FIG. 1).
- a hole 19 is provided in the center of the sintered member 1.
- the hole 19 penetrates along the axial direction of the sintered member 1.
- the sintered member 1 may be provided with a plurality of through holes penetrating the first surface 11 and the second surface 12. This through hole can reduce the weight of the sintered member.
- the first surface 11 is provided on one side of the sintered member 1 in the axial direction (FIG. 1).
- the second surface 12 is provided on the other side of the sintered member 1 in the axial direction (FIG. 2). That is, the first surface 11 and the second surface 12 are provided on opposite sides of each other in the axial direction of the sintered member 1.
- the shapes of the first surface 11 and the second surface 12 are annular.
- the first surface 11 and the second surface 12 are substantially formed of a plane.
- the first surface 11 and the second surface 12 are substantially orthogonal to the axial direction of the sintered member 1 and parallel to each other.
- the peripheral surface 15 is parallel to the axial direction of the sintered member 1 (FIG. 1).
- the peripheral surface 15 is an inner peripheral surface in this embodiment. That is, the peripheral edge of the peripheral surface 15 on one side in the axial direction of the sintered member 1 is connected to the inner peripheral edge of the first surface 11.
- the peripheral edge of the peripheral surface 15 on the other side in the axial direction of the sintered member 1 is not connected to the inner peripheral edge of the second surface 12 in this embodiment, but is connected to the outer peripheral edge of the third surface 13 described later.
- the peripheral surface 15 is an inner peripheral surface as in the present embodiment, the peripheral edge on the other side of the peripheral surface 15 may be connected to the inner peripheral edge of the second surface 12.
- the peripheral surface 15 may be an outer peripheral surface.
- the peripheral edge on one side of the peripheral surface 15 is connected to the outer peripheral edge of the first surface 11.
- the other peripheral edge of the peripheral surface 15 may be connected to the outer peripheral edge of the second surface 12.
- the third surface 13 is one surface of the sintered member 1 in the axial direction.
- the third surface 13 forms a step corresponding to the length along the axial direction of the peripheral surface 15 with the first surface 11.
- the shape of the third surface 13 is an annular shape.
- the third surface 13 is substantially formed of a flat surface.
- the third surface 13 is substantially parallel to the first surface 11 and the second surface 12.
- Each tooth group 16 is a portion that meshes with the teeth of the mating gear, and is a set of a plurality of spline teeth 16a arranged in parallel along the circumferential direction of the peripheral surface 15 (FIG. 1). The illustration of the mating gear is omitted. Since the peripheral surface 15 of this embodiment is the inner peripheral surface as described above, the tooth group 16 is an internal tooth group. If the peripheral surface 15 is the outer peripheral surface, the tooth group 16 is an external tooth group. The tooth group 16 is provided one by one between the missing tooth portions 17 adjacent to each other in the circumferential direction. The number of tooth groups 16 is the same as the number of missing teeth 17. The number of tooth groups 16 is 3 in this embodiment.
- the number of spline teeth 16a in each tooth group 16 is not particularly limited as long as it is two or more, and can be appropriately selected.
- the number of spline teeth 16a in each tooth group 16 is large, the number of spline teeth 16a that mesh with the mating gear tends to be large. Therefore, the load acting on each spline tooth 16a as it meshes with the mating gear tends to be small.
- the length Lb of the missing tooth portion 17, which will be described later tends to be long. Therefore, as will be described in detail later, even if the first cam 110 (FIG. 6) of the electromagnetic coupling 10 is configured by the sintered member 1, the stress concentration of the spline teeth 16a on the tooth root is likely to be suppressed.
- the number of spline teeth 16a in each tooth group 16 is 8 in this embodiment.
- the length La of each tooth group 16 can be appropriately selected according to the length Lb of the missing tooth portion 17, which will be described later (FIG. 3).
- the length La of the tooth group 16 refers to the length from the spline tooth 16a on one end side of the tooth group 16 to the spline tooth 16a on the other end side on the circumference of the pitch circle Cp of the spline tooth 16a. In FIG. 3, the pitch circle Cp is shown by a broken line.
- the length La of each tooth group 16 may be different from the length Lb of the missing tooth portion 17, or may be the same as the length Lb of the missing tooth portion 17, which will be described later.
- each tooth group 16 When the length La of each tooth group 16 is longer than the length Lb of the missing tooth portion 17, it is easy to increase the number of spline teeth 16a in each tooth group 16. Therefore, the stress acting on each spline tooth 16a tends to be small.
- the length La of each tooth group 16 is shorter than the length Lb of the missing tooth portion 17, the length Lb of the missing tooth portion 17 is long, so that stress concentration on the tooth root of the spline tooth 16a is likely to be suppressed.
- the length a of the tooth group 16 When the length a of the tooth group 16 is equivalent to the length Lb of the missing tooth portion 17, the effect that the stress acting on each spline tooth 16a tends to be small and the stress concentration of the spline tooth 16a on the tooth root are easily suppressed. The effect can be combined in a well-balanced manner.
- the tooth thickness Ta and the tooth groove width Wa of each spline tooth 16a in each tooth group 16 can be appropriately selected according to the tooth groove width and the tooth thickness of the mating gear.
- the tooth thickness Ta of the spline tooth 16a refers to the length of the spline tooth 16a on the circumference of the pitch circle Cp.
- the width Wa of the tooth groove refers to the length between adjacent spline teeth 16a on the circumference of the pitch circle Cp.
- the tooth thickness Ta of each spline tooth 16a is uniform.
- the width Wa of the tooth groove in each tooth group 16 is smaller than the length Lb of the missing tooth portion 17.
- the width Wa of the tooth groove in each tooth group 16 is uniform.
- Each missing tooth portion 17 is a portion that is not provided with a tooth and does not mesh with the tooth of the mating gear (FIG. 1).
- the missing tooth portion 17 is formed of a part of the peripheral surface 15.
- the missing tooth portions 17 are arranged one by one between the tooth groups 16 adjacent to each other in the circumferential direction. That is, the number of missing teeth 17 is the same as the number of ball grooves 12a described later. The number of missing teeth 17 is 3 in this embodiment.
- each missing tooth portion 17 the number of missing spline teeth 16a varies depending on the tooth thickness Ta of the spline tooth 16a, the width Wa of the tooth groove, and the length Lb of the missing tooth portion 17 described later (FIG. 3). As shown by the alternate long and short dash line in FIG. 3, the number of missing spline teeth 16a can be grasped by arranging the spline teeth 16a of the tooth group 16 in the circumferential direction without providing the missing tooth portion 17. At this time, the tooth thickness Ta of each spline tooth 16a is made uniform, and the width Wa of each tooth groove is made uniform.
- the number of missing spline teeth 16a in each missing tooth portion 17 is at least two or more.
- the length Lb of the missing tooth portion 17 tends to be long, it is easy to suppress the stress concentration of the spline tooth 16a on the tooth root.
- the number of missing spline teeth 16a depends on the tooth thickness Ta of the spline teeth 16a, the width Wa of the tooth groove, and the length Lb of the missing tooth portion 17, but is preferably 3 or less, for example.
- the number of missing spline teeth 16a is two in this embodiment. That is, one missing tooth portion 17 is formed by the lack of the two spline teeth 16a, and the two missing teeth are counted as one missing tooth portion 17.
- each missing tooth portion 17 is a portion on the peripheral surface 15 facing each ball groove 12a described later (FIG. 5). That is, the radial formation position of each missing tooth portion 17 is within the radial formation range of each ball groove 12a, and the circumferential formation range of each missing tooth portion 17 and the circumferential direction of each ball groove 12a. The formation range overlaps in the circumferential direction. Unlike the sintered member 1 of the present embodiment, the peripheral surface 15 is not provided with the missing tooth portion 17, and the spline teeth 16a are also provided on the peripheral surface 15 in the circumferential direction overlapping the formation range of each ball groove 12a.
- the first cam 110 of the electromagnetic coupling 10 is configured by the sintered member provided with the above, it is as follows.
- the axial load of the sintered member 1 by the second cam 120 of the electromagnetic coupling 10 acts on the sintered member 1 via the balls 130 of the electromagnetic coupling 10 to form the ball groove 12a.
- Stress concentration occurs at the roots of spline teeth in the circumferential direction that overlaps the range.
- the sintered member 1 of the present embodiment since the forming range of each missing tooth portion 17 in the circumferential direction and the forming range of each ball groove 12a in the circumferential direction overlap, the peripheral surface 15 is formed. There is no root of the spline tooth 16a where stress concentration occurs at a portion in the circumferential direction overlapping the formation range of each ball groove 12a.
- a portion of the peripheral surface 15 in the circumferential direction overlapping the formation range of each ball groove 12a is rounded with a bending diameter larger than the bending diameter of the tooth root of the spline tooth 16a. Therefore, the stress concentration due to the action such as the load is relaxed at the rounded tooth missing portion 17, and the stress concentration of the spline tooth 16a on the tooth root is suppressed.
- the length Lb of each tooth missing portion 17 can be appropriately selected according to the length Lc of each ball groove 12a described later (FIG. 3).
- the length Lb of each missing tooth portion 17 refers to the length between adjacent tooth groups 16 on the circumference of the tooth bottom circle Cr.
- FIG. 3 shows the tooth bottom circle Cr as a alternate long and short dash line.
- the length Lb of each tooth missing portion 17 preferably has a length of 30% or more and 70% or less with respect to the length Lc of each ball groove 12a described later. Since the length Lb of each tooth missing portion 17 has a length of 30% or more with respect to the length Lc of each ball groove 12a, each tooth missing portion 17 has a sufficient length.
- each tooth missing portion 17 has a length of 70% or less with respect to the length Lc of each ball groove 12a, the length of each missing tooth portion 17 does not become excessively long. That is, the length La of the tooth group 16 is not too short.
- the length Lb of each tooth missing portion 17 is shorter than the length Lc of each ball groove 12a (FIG. 4).
- the length Lb of each missing tooth portion 17 is equal.
- Each tooth missing portion 17 is provided within a range overlapping the formation range of each ball groove 12a over the entire length of the length Lb (FIG. 4).
- the spline teeth 16a on each end side of the tooth group 16 are provided at positions overlapping the ends of the formation range of the ball groove 12a.
- the missing tooth portion 17 facing the ball groove 12a and the spline teeth 16a on each end side of the tooth group 16 are shown by broken lines.
- the length Lb of the tooth missing portion 17 indicates the forming range of the missing tooth portion 17 in the circumferential direction
- the length Lc of the ball groove 12a indicates the forming range of the ball groove 12a in the circumferential direction (FIG. 4). That is, as shown in FIG. 4, the forming range (length Lb) in the circumferential direction of the tooth missing portion 17 and the forming range (length Lc) in the circumferential direction of the ball groove 12a overlap.
- the center of the range of the length Lb of the tooth missing portion 17 and the center of the range of the length Lc of the ball groove 12a are substantially the same, but the center of the range of the length Lb of the tooth missing portion 17 And the center of the range of the length Lc of the ball groove 12a may be deviated. Further, in FIG. 4, the entire range of the length Lb of each tooth missing portion 17 is included in the range of the length Lc of each ball groove 12a, and the entire range of the length Lb of each tooth missing portion 17 is included in each range. Although the case where the ball groove 12a overlaps the length Lc range is illustrated, a part of the length Lb range of each missing tooth portion 17 overlaps the length Lc range of each ball groove 12a. May be good.
- the length Lb of each missing tooth portion 17 becomes the length Lb of each ball groove 12a. It may be longer than the length Lc.
- each of the missing tooth portions 17 on the outer peripheral edge is shifted to the outer peripheral edge side of each ball groove 12a when the missing tooth portions 17 are viewed in a plan view.
- the position of the outer peripheral edge of each missing tooth portion 17 may be displaced toward the inner peripheral edge side of each ball groove 12a.
- the outer peripheral edge of each missing tooth portion 17 may be located exactly in the middle between the outer peripheral edge and the inner peripheral edge of each ball groove 12a.
- each missing tooth portion 17 When the position of the outer peripheral edge of each missing tooth portion 17 is deviated to the inner peripheral edge side of each ball groove 12a, the concentration of stress due to the action such as the load is easily relaxed at the missing tooth portion 17, and the spline tooth It is considered that the stress concentration on the tooth root of 16a is easily suppressed. As described above, the radial formation position of each missing tooth portion 17 is within the radial formation range of each ball groove 12a.
- each ball groove 12a a ball 130 (FIG. 6) provided in the electromagnetic coupling 10 is arranged (FIG. 2).
- the ball grooves 12a are arranged in parallel along the circumferential direction of the second surface 12.
- the ball grooves 12a adjacent to each other in the circumferential direction depend on the number of ball grooves 12a and the length Lc of the ball grooves 12a, they may be provided at intervals in the circumferential direction as in the present embodiment, or may be provided at intervals in the circumferential direction. May be provided so as to be continuous with substantially no interval.
- the fact that the ball grooves 12a are continuous in the circumferential direction without being substantially spaced means, for example, that the ball grooves 12a adjacent to each other in the circumferential direction are continuous with each other through the ends of the ball grooves 12a.
- a second surface 12 is interposed between the ball grooves 12a adjacent to each other in the circumferential direction. The intervals between the ball grooves 12a adjacent to each other in the circumferential direction along the circumferential direction are equal intervals.
- the number of ball grooves 12a is not particularly limited as long as it is two or more, and can be appropriately selected.
- the number of ball grooves 12a may be, for example, 3 to 9.
- the number of ball grooves 12a is 3 in this embodiment.
- the length Lc of each ball groove 12a can be appropriately selected according to the number of ball grooves 12a and the distance between adjacent ball grooves 12a in the circumferential direction. As shown in FIG. 5, the length Lc of each ball groove 12a means the maximum length along the circumferential direction. In this embodiment, the length Lc of each ball groove 12a is longer than the length Lb of each missing tooth portion 17 described above.
- each ball groove 12a is not particularly limited and can be appropriately selected.
- the depth of each ball groove 12a is not uniform and is different.
- the first cam 110 (FIG. 6) of the electromagnetic coupling 10 is composed of the sintered member 1 due to the different depths, the first cam 110 facing each other via the balls 130 will be described in detail later.
- the distance between the cam 120 and the second cam 120 can be narrowed or widened.
- the opening width of each ball groove 12a may be uniform or different (FIG. 2).
- the relationship between the depth of each ball groove 12a and the opening width of each ball groove 12a may satisfy the following relationship.
- the opening width of the deepest part of each ball groove 12a is the widest.
- the opening width of the shallowest portion of each ball groove 12a may be the same as the opening width of the deepest portion, or may be the narrowest.
- each ball groove 12a is a bow shape in this embodiment (FIGS. 2 and 4).
- the depth of each ball groove 12a is inclined so as to become shallower from the center in the circumferential direction toward both ends. That is, the depth at the center of each ball groove 12a in the circumferential direction is the deepest, and the depth at both ends is the shallowest.
- the opening width of each ball groove 12a becomes narrower from the center in the circumferential direction toward both ends. That is, the opening width at the center of each ball groove 12a in the circumferential direction is the widest, and the opening width at both ends in the circumferential direction is the narrowest.
- each ball groove 12a may be inclined so as to become shallower from one end in the circumferential direction toward the other end. In that case, the opening width of each ball groove 12a may become narrower from one end side in the circumferential direction toward the other end side. Further, the opening width of each ball groove 12a may be uniform in the circumferential direction.
- the sintered member 1 is formed by bonding a plurality of iron-based particles to each other.
- Iron-based refers to pure iron or iron-based alloys.
- the iron-based alloy is, for example, one or more additive elements selected from the group consisting of Cu (copper), C (carbon), Ni (nickel), Mo (molybdenum), Mn (manganese), and Cr (chromium).
- the balance is composed of Fe (iron) and impurities.
- Specific iron-based alloys include stainless steel, Fe—C alloys, Fe—Cu—Ni—Mo alloys, Fe—Ni—Mo—Mn alloys, Fe—Cu alloys, and Fe—Cu—C alloys.
- the sintered member 1 made of a specific Fe—Ni—Cr—Mo—C alloy will be described in the second embodiment described later.
- the composition of the sintered member 1 can be confirmed by performing component analysis by ICP emission spectroscopic analysis (Inductively Coupled Plasma Optical Mission Spectrometry: ICP-OES) or the like.
- ICP emission spectroscopic analysis Inductively Coupled Plasma Optical Mission Spectrometry: ICP-OES
- the sintered member 1 of the present embodiment can be manufactured by a method for manufacturing a sintered member including a step of preparing a dust compact and a step of sintering the dust compact. Hereinafter, each step will be described in order.
- This step prepares a powder compact having a plurality of tooth groups, a plurality of missing teeth, and a plurality of ball grooves.
- the plurality of tooth groups, the plurality of missing teeth, and the plurality of ball grooves provided in the dust compact are the plurality of tooth groups 16 and the plurality of missing teeth 17 and the plurality of ball grooves 12a provided in the above-mentioned sintered member 1. It is a street.
- the above-mentioned sintered member 1 is produced by sintering the powder compact prepared in this step. That is, this powder compact corresponds to the above-mentioned sintered member 1 which is not sintered.
- the powder compact is a product obtained by pressure-molding the prepared raw material powder.
- the raw material powder can be appropriately selected so as to have the composition of the sintered member 1 described above.
- For the pressure molding of the raw material powder for example, it is possible to use a mold capable of a near net shape to finish the shape close to the finished product. By this pressure molding, a powder compact having a plurality of tooth groups, a plurality of missing teeth, and a plurality of ball grooves can be obtained.
- the powder compact is also prepared by producing a disk-shaped powder compact and forming a plurality of tooth groups, a plurality of missing teeth, and a plurality of ball grooves by cutting.
- This step sinters the powder compact.
- the above-mentioned sintered member 1 in which the particles of the raw material powder are bonded to each other is obtained.
- a suitable sintering furnace can be used for sintering the powder compact.
- a continuous sintering furnace is suitable for sintering the powder compact.
- the continuous sintering furnace has a sintering furnace and a quenching chamber continuous downstream of the sintering furnace.
- Sintering conditions can be appropriately selected according to the composition of the raw material powder.
- the sintering temperature may be, for example, 1050 ° C or higher and 1400 ° C or lower, and further, 1100 ° C or higher and 1300 ° C or lower.
- the sintering time is, for example, 10 minutes or more and 150 minutes or less, and further includes 15 minutes or more and 60 minutes or less.
- Known conditions can be applied to the sintering conditions.
- the cooling rate in the cooling process of the sintering process can be appropriately selected.
- the sintering member 1 may be rapidly cooled by increasing the cooling rate, or may not be rapidly cooled. If it is rapidly cooled, the heat treatment step described later can be omitted. If it is not rapidly cooled, it may undergo a heat treatment step described later.
- the cooling rate is 1 ° C./sec or higher.
- the cooling rate is 1 ° C./sec or more.
- the sintered member 1 is rapidly cooled. Therefore, since the martensite phase is easily formed, the sintered member 1 having high hardness can be manufactured.
- the cooling rate is further preferably 2 ° C./sec or higher, and particularly preferably 5 ° C./sec or higher.
- the upper limit of the cooling rate is, for example, 1000 ° C./sec, further 500 ° C./sec, and particularly 200 ° C./sec.
- Examples of the cooling method include blowing a cooling gas onto the sintered member 1.
- Examples of the cooling gas include an inert gas such as nitrogen gas and argon gas.
- the method for manufacturing the sintered member may further include at least one step of heat treatment and a step of performing finishing.
- Heat treatment examples of the heat treatment include quenching treatment and tempering treatment. Quenching and tempering improves the mechanical properties, especially hardness and strength of the sintered member 1.
- the quenching treatment may be a carburizing quenching treatment.
- Known conditions can be applied to the quenching treatment (carburizing and quenching treatment) and the tempering treatment.
- the dimensions of the sintered member 1 are adjusted to the design dimensions.
- the finishing process include sizing and polishing the surface of the sintered member 1. In particular, the polishing process tends to reduce the surface roughness of the sintered member 1.
- the sintered member 1 according to the embodiment can be suitably used for, for example, a cam component constituting a cam mechanism of an electromagnetic coupling.
- An example of the electromagnetic coupling according to this embodiment will be described with reference to FIG.
- the electromagnetic coupling 10 connects and disconnects, for example, the propeller shaft of an automobile and the rear differential gear.
- the electromagnetic coupling 10 includes a cam mechanism having a first cam 110, a second cam 120, and a ball 130.
- FIG. 6 shows only the cam mechanism for convenience of explanation. In addition to these members, the electromagnetic coil, armature, first clutch, second clutch, etc. provided in the electromagnetic coupling 10 are not shown.
- FIG. 6 is a cross-sectional view showing a state in which the cam mechanism is cut at the same position as the cross-sectional view shown in FIG.
- the first cam 110 is composed of the above-mentioned sintered member 1. That is, the first cam 110 has a plurality of tooth groups 16 and a plurality of missing teeth 17.
- the second surface 12 includes a plurality of ball grooves 12a.
- the first surface 11 of the first cam 110 is located on the side opposite to the second cam 120 side, and the second surface 12 of the first cam 110 is located on the second cam 120 side.
- the second cam 120 has a ball groove 121 in which the ball 130 is arranged.
- the ball 130 is interposed between the ball groove 12a of the first cam 110 and the ball groove 121 of the second cam 120.
- the distance between the first cam 110 and the second cam 120 may be widened or narrowed as shown in FIG. 6, although not shown, depending on the presence or absence of energization of the electromagnetic coil.
- the second cam 120 rotates via the armature, the second clutch, etc. as the electromagnetic coil is energized.
- the ball 130 is dragged by the ball groove 121 of the second cam 120 and moves from the deepest portion to the shallowest portion of the ball groove 12a in the first cam 110.
- the movement of the ball 130 pushes the first cam 110 toward the first surface 11 side via the ball 130.
- the first cam 110 is separated from the second cam 120, and the distance between the first cam 110 and the second cam 120 is widened.
- the propeller shaft and the rear differential gear are connected via the first clutch or the like.
- the rotation of the second cam 120 at the time of energization is released.
- the second cam 120 rotates on the side opposite to that when the power is turned on.
- the ball 130 is dragged by the ball groove 121 of the second cam 120 and moves from the shallowest portion to the deepest portion of the ball groove 12a in the first cam 110.
- the movement of the ball 130 releases the pressing force on the first surface 11 side of the first cam 110 via the ball 130.
- the first cam 110 approaches the second cam 120 side, and the distance between the first cam 110 and the second cam 120 is narrowed. When the above interval is narrowed, the connection between the propeller shaft and the rear differential gear via the first clutch or the like is cut off.
- the sintered member 1 according to the present embodiment can construct an electromagnetic coupling 10 that can be used for a long period of time.
- each ball groove 12a is formed on the peripheral surface 15.
- the sintered member 1 according to the present embodiment constitutes the first cam 110 of the electromagnetic coupling 10, and the axial load of the sintered member 1 by the second cam 120 of the electromagnetic coupling 10 is applied to the electromagnetic cup. Even if it acts on the sintered member 1 via the ball 130 of the ring 10, the stress concentration is relaxed by the rounded missing tooth portion 17, and the stress concentration of the spline tooth 16a on the tooth root can be suppressed. .. Therefore, the sintered member 1 according to the present embodiment can suppress a decrease in fatigue strength and has a long life.
- the electromagnetic coupling 10 according to the present embodiment can be used for a long period of time because the first cam 110 is formed by the sintered member 1 having a long life because the stress concentration of the spline teeth 16a on the tooth root can be suppressed. is there.
- Embodiment 2 >> [Sintered member]
- the sintered member 1 according to the second embodiment will be described with reference to FIGS. 1 to 5, 7, 8A, 8B, 9A, and 9B.
- the sintered member 1 according to the second embodiment is different from the sintered member 1 according to the first embodiment in that it mainly has a specific composition, structure, and characteristics.
- the appearance of the sintered member 1 according to the second embodiment is the same as that of the sintered member 1 according to the first embodiment.
- the following description will focus on the differences from the first embodiment. The description of the configuration similar to that of the first embodiment will be omitted.
- composition of the sintered member 1 contains Ni, Cr, Mo, and C, and the balance is composed of Fe and unavoidable impurities.
- Ni enhances the toughness of the sintered member 1. Since Ni can improve hardenability in the manufacturing process of the sintered member 1, it also contributes to increasing the hardness of the sintered member 1.
- the manufacturing process of the sintered member 1 may be simply referred to as a manufacturing process.
- the Ni content is preferably more than 2% by mass and 6% by mass or less. When the Ni content exceeds 2% by mass, the sintered member 1 has excellent toughness. The reason is that the content of Ni is high. Due to the high content of Ni, a part of Ni is alloyed with Fe, and the rest of Ni is not alloyed and exists as pure Ni. The portion existing as pure Ni contributes to the improvement of toughness.
- the sintered member 1 When the Ni content is 6% by mass or less, the sintered member 1 has excellent hardness. The reason is that the amount of Ni is not excessively large, so that the decrease in hardness can be suppressed. Therefore, when the Ni content satisfies the above range, the sintered member 1 can have both high hardness and high toughness.
- the Ni content is further preferably 2.5% by mass or more and 5.5% by mass or less, and particularly preferably 3% by mass or more and 5% by mass or less.
- the Ni content means the content of Ni in the sintered member 1 when the total content of the elements contained in the sintered member 1 is 100% by mass. This point is the same for Cr, Mo, and C, which will be described later.
- the Cr content is preferably, for example, 2% by mass or more and 4% by mass or less. When the Cr content is 2% by mass or more, the sintered member 1 has excellent hardness. When the Cr content is 4% by mass or less, the decrease in toughness of the sintered member 1 can be suppressed.
- the Cr content is further preferably 2.2% by mass or more and 3.8% by mass or less, and particularly preferably 2.5% by mass or more and 3.5% by mass or less.
- Mo Mo increases the hardness of the sintered member 1. This is because Mo can improve hardenability in the manufacturing process.
- the Mo content is preferably, for example, 0.2% by mass or more and 0.9% by mass or less. When the Mo content is 0.2% by mass or more, the sintered member 1 has excellent hardness. When the Mo content is 0.9% by mass or less, the decrease in toughness of the sintered member 1 can be suppressed.
- the Mo content is further preferably 0.3% by mass or more and 0.8% by mass or less, and particularly preferably 0.4% by mass or more and 0.7% by mass or less.
- (C) C improves the hardness of the sintered member 1.
- C tends to cause a liquid phase of Fe—C to appear in the manufacturing process.
- the liquid phase of Fe-C tends to round the corners of the pores. Therefore, the sintered member 1 has few acute-angled portions of pores that cause a decrease in hardness. Therefore, the hardness of the sintered member 1 tends to increase.
- the content of C is preferably, for example, 0.2% by mass or more and 1.0% by mass or less. When the C content is 0.2% by mass or more, the sintered member 1 has a high hardness. This is because the liquid phase of Fe—C appears sufficiently in the manufacturing process, and it is easy to effectively round the corners of the pores.
- the sintered member 1 When the C content is 1.0% by mass or less, the sintered member 1 is excellent in dimensional accuracy. This is because it is easy to prevent the liquid phase of Fe—C from being excessively generated in the manufacturing process.
- the content of C is further preferably 0.3% by mass or more and 0.95% by mass or less, and particularly preferably 0.4% by mass or more and 0.9% by mass or less.
- the structure of the sintered member 1 preferably has a mixed phase structure of a martensite phase and a retained austenite phase (FIGS. 8A, 8B, 9A, 9B).
- 8A, 8B, 9A, and 9B are micrographs of a cross section of the sintered member 1, as will be described in detail later.
- the white part at the tip of the arrow in each figure is the retained austenite phase, and the part around the retained austenite phase is the martensite phase.
- the sintered member 1 has a martensite phase and thus has a high hardness.
- the sintered member 1 has a retained austenite phase, so that it has high toughness.
- the area ratio of the retained austenite phase is preferably 5% or more, for example. Then, since the area ratio of the highly tough retained austenite phase is high, the sintered member 1 is excellent in toughness.
- the area ratio of the retained austenite phase is preferably 50% or less, for example. Then, the area ratio of the retained austenite phase does not become too large. That is, the area ratio of the martensite phase tends to increase. Therefore, the sintered member 1 has high hardness and high toughness.
- the area ratio of the retained austenite phase is further preferably 10% or more and 45% or less, and particularly preferably 15% or more and 40% or less.
- the area ratio of the retained austenite phase refers to the ratio of the total area of the retained austenite phase to the total area of the micrograph in the cross section of the sintered member 1, as will be described in detail later.
- the sintered member 1 preferably has a high hardness. It is preferable that the sintered member 1 has a large Vickers hardness and a small fluctuation range of the Vickers hardness (circles shown in the graph of FIG. 7). Details of the graph of FIG. 7 will be described later.
- the Vickers hardness of the sintered member 1 is preferably 615 HV or more.
- the fluctuation range of the Vickers hardness of the sintered member 1 is preferably 100 HV or less.
- the sintered member 1 has a high hardness and a uniform hardness from the surface to the predetermined depth.
- the sintered member 1 is less likely to be damaged because there are few places where it can be a mechanical weak point as compared with the sintered member having a non-uniform hardness. Since the Vickers hardness fluctuation range of the sintered member 1 is small, the sintered member 1 is subjected to a sinter hardening process in which it is rapidly cooled in the cooling process of the sintering process. Since the sintered member 1 is subjected to a sinter hardening treatment, it is not quenched and tempered after sintering. The fluctuation range of the Vickers hardness of the sintered member 1 that has not been subjected to the sinter hardening treatment and has been quenched and tempered after sintering is, for example, more than 100 HV.
- the Vickers hardness of the sintered member 1 is more preferably 620 HV or more, and particularly preferably 625 HV or more.
- the fluctuation range of the Vickers hardness is more preferably 75 HV or less, and particularly preferably 50 HV.
- the Vickers hardness of the sintered member 1 is the average of the Vickers hardness measured at a plurality of points from the surface of the sintered member 1 to a predetermined depth in the cross section of the sintered member 1, as will be described in detail later. ..
- the fluctuation range of the Vickers hardness of the sintered member 1 is the maximum value and the minimum value of the Vickers hardness measured from the surface to a predetermined depth in the cross section of the sintered member 1, as will be described in detail later. The difference between.
- the sintered member 1 preferably has high toughness. Specifically, in the Ono-type rotary bending fatigue test described later, it is preferable that the stress amplitude that can withstand the 107 times repeated bending test is large and the bending fatigue strength is excellent.
- the stress amplitude that can withstand the 107-fold repeated bending test is preferably 420 MPa or more.
- the stress amplitude that can withstand the 107-fold repeated bending test is preferably 423 MPa or more, and particularly preferably 425 MPa or more.
- the sintered member 1 of the present embodiment is manufactured by a method for manufacturing a sintered member including a step of preparing a dust compact and a step of sintering the dust compact, similar to the above-described method for manufacturing a sintered member. it can.
- the step of preparing is the same as the above-mentioned step of preparing, in that a powder compact having a plurality of tooth groups, a plurality of missing teeth, and a plurality of ball grooves is prepared.
- the step of preparing is different from the above-mentioned step of preparing in that a powder containing an iron-based alloy powder, Ni powder, and C powder is used as the raw material powder of the powder compact. In the sintering process, it is rapidly cooled in the cooling process.
- the iron-based alloy powder contains Cr and Mo, and has a composition in which the balance is Fe and unavoidable impurities.
- the Cr and Mo contents in the iron-based alloy are maintained even after the sintering step described later. That is, the contents of Cr and Mo in the iron-based alloy are maintained in the above-mentioned sintered member 1.
- the Cr content in the iron-based alloy is, for example, preferably 2% by mass or more and 4% by mass or less, more preferably 2.2% by mass or more and 3.8% by mass or less, and particularly 2.5% by mass. It is preferably 3.5% by mass or more and 3.5% by mass or less.
- the Mo content in the iron-based alloy is preferably, for example, 0.2% by mass or more and 0.9% by mass or less, and further preferably 0.3% by mass or more and 0.8% by mass or less. In particular, 0.4% by mass or more and 0.7% by mass or less is preferable.
- the reason for setting the Cr and Mo contents in the above range is as described above.
- the content of Cr and Mo refers to the content of Cr and Mo in the iron-based alloy when the total content of the elements contained in the iron-based alloy is 100% by mass.
- the average particle size of the iron-based alloy powder is, for example, 50 ⁇ m or more and 150 ⁇ m or less. Iron-based alloy powders having an average particle size within the above range are easy to handle and pressure-molded. An iron-based alloy powder having an average particle size of 50 ⁇ m or more can easily secure fluidity. An iron-based alloy powder having an average particle size of 150 ⁇ m or less can easily obtain a sintered member 1 having a dense structure. Further, the average particle size of the iron-based alloy powder is 55 ⁇ m or more and 100 ⁇ m or less.
- the "average particle size" is a particle size (D50) at which the cumulative volume in the volume particle size distribution measured by a laser diffraction type particle size distribution measuring device is 50%. This point is the same for the average particle diameters of Ni powder and C powder described later.
- Ni powder examples include pure Ni powder.
- the content of Ni powder is maintained even after the sintering step described later. That is, the content of Ni powder is maintained in the above-mentioned sintered member 1.
- the content of Ni powder is more than 2% by mass and 6% by mass or less, more preferably 2.5% by mass or more and 5.5% by mass or less, and particularly 3% by mass or more and 5% by mass or less. preferable. Due to the high content of Ni powder, a part of Ni can be alloyed with Fe by the sintering step, and the rest of Ni can be made to exist as pure Ni without being alloyed. Moreover, a multiphase structure of the martensite phase and the retained austenite phase can be formed.
- the content of Ni powder refers to the content of Ni powder in the raw material powder when the total content of the raw material powder is 100% by mass.
- the average particle size of Ni powder affects the distribution of the retained austenite phase.
- the average particle size of the Ni powder is, for example, 1 ⁇ m or more and 40 ⁇ m or less.
- Ni powder having an average particle size of 40 ⁇ m or less tends to evenly distribute the retained austenite phase.
- Ni powder having an average particle size of 1 ⁇ m or more is easy to handle, so that manufacturing workability can be improved.
- the average particle size of the Ni powder is 1 ⁇ m or more and 30 ⁇ m or less, and particularly 1 ⁇ m or more and 20 ⁇ m or less.
- the C powder becomes a liquid phase of Fe—C in the heating process of the sintering step, and the corners of the pores in the sintering member 1 are rounded to improve the hardness of the sintering member 1.
- the content of C powder is maintained even after the sintering step described later, as in the case of Ni powder and the like. That is, the content of the C powder in the raw material powder is maintained in the above-mentioned sintered member 1.
- the content of the C powder is, for example, preferably 0.2% by mass or more and 1.0% by mass or less, further preferably 0.3% by mass or more and 0.95% by mass or less, and particularly 0.4% by mass. % Or more and 0.9% by mass or less are preferable.
- the average particle size of the C powder is preferably smaller than the average particle size of the iron-based alloy powder.
- the C powder which is smaller than the iron-based alloy powder, is likely to be uniformly dispersed in the iron-based alloy powder, so that alloying is likely to proceed.
- the average particle size of the C powder is, for example, 1 ⁇ m or more and 30 ⁇ m or less, and further includes 10 ⁇ m or more and 25 ⁇ m or less. From the viewpoint of forming a liquid phase of Fe—C, it is preferable that the average particle size of the C powder is large, but if it is too large, the time for the liquid phase to appear becomes long, and the pores become too large, resulting in defects.
- the raw material powder may contain a lubricant.
- the lubricant enhances the lubricity of the raw material powder during molding and improves the moldability.
- Types of lubricants include, for example, higher fatty acids, metal soaps, fatty acid amides, higher fatty acid amides and the like.
- Known lubricants can be used as these lubricants.
- the form of the lubricant may be any form such as solid, powder, or liquid. At least one of these can be used alone or in combination as the lubricant.
- the content of the lubricant in the raw material powder is, for example, 0.1% by mass or more and 2.0% by mass or less, and further 0.3% by mass or more and 1.5% by mass, when the raw material powder is 100% by mass.
- the following can be mentioned, and in particular, 0.5% by mass or more and 1.0% by mass or less can be mentioned.
- the raw material powder may contain an organic binder.
- organic binder Known organic binders can be used.
- the content of the organic binder is 0.1% by mass or less when the raw material powder is 100% by mass.
- the proportion of the metal powder contained in the molded product can be increased, so that it is easy to obtain a dense powder compact.
- the organic binder is not contained, it is not necessary to degreas the powder compact in a subsequent step.
- the cooling rate in the cooling process of the sintering step is 1 ° C./sec or more.
- the sintered member 1 is rapidly cooled. Therefore, a mixed phase structure of the martensite phase and the retained austenite phase is likely to be formed. Therefore, the sintered member 1 having excellent hardness and toughness is manufactured.
- the higher the C content the easier it is for the martensite phase to be formed, so that the sintered member 1 having high hardness is manufactured.
- the larger the amount of Ni powder the easier it is for the retained austenite phase to be formed, so that the highly tough sintered member 1 can be easily manufactured.
- the sintered member 1 having a small fluctuation range of Vickers hardness from the surface to a predetermined depth. Specifically, the sintered member 1 having a fluctuation range of Vickers hardness of 50 HV or less is manufactured.
- the preferred cooling rate is as described above.
- the sintered member 1 according to the present embodiment can have both high hardness and high toughness in addition to the effects of the first embodiment. This is because the sintered member 1 is excellent in toughness due to a high Ni content, and can suppress a decrease in hardness because the Ni content is not excessively high. Moreover, the sintered member 1 has a mixed phase structure of a high-hardness martensite phase and a high-toughness retained austenite phase. Further, the sintered member 1 has a uniform hardness from the surface to a predetermined depth. This is because the sintered member 1 has a small fluctuation range of the Vickers hardness. Therefore, the sintered member 1 according to the present embodiment can be suitably used for the first cam 110 (FIG. 6) provided in the above-mentioned electromagnetic coupling 10.
- the first member of No. 1 was composed of the sintered member 1 described with reference to FIGS. 1 to 5. That is, the first member of this model has a plurality of tooth groups and a plurality of missing teeth on the inner peripheral surface connected to the first surface, and has a plurality of ball grooves on the second surface.
- the plurality of tooth groups, the plurality of missing tooth portions, and the plurality of ball grooves of the first member are appropriately formed by forming the plurality of tooth groups 16 and the plurality of missing tooth portions 17 and the plurality of ball grooves 12a of FIGS. 1 to 5. You can refer to it.
- the number of tooth groups was 3, and the number of spline teeth in each tooth group was 8.
- the number of missing teeth was set to 3, which is the same as the number of tooth groups.
- the number of missing spline teeth was set to 2 in each missing tooth portion.
- the number of ball grooves was three.
- Analysis model No. 101 Analysis model No.
- the first member of the analysis model No. 101 has no missing tooth on the inner peripheral surface connected to the first surface, and has a plurality of spline teeth parallel to each other in the circumferential direction of the inner peripheral surface. It was the same as the first member of 1.
- the number of spline teeth was 30.
- the number of ball grooves was three.
- FIG. 10 is a cross-sectional view showing a state in which each member is cut at the same position as the cross-sectional view shown in FIG.
- the second member 220 is composed of the second cam 120 described with reference to FIG. That is, the second member 220 has a ball groove 121 in which the ball 230 is arranged.
- the ball 230 is interposed between the ball groove 12a in the first member 210 and the ball groove 121 in the second member 220 of each analysis model.
- the ball 230 was arranged at a position slightly deviated from the deepest portion of the ball groove 12a in the first member 210 so as not to move from that position.
- the first jig 310 was arranged on the outer peripheral edge side of the first surface 11 of the first member 210.
- the second jig 320 was arranged on the outer peripheral edge side of the second member 220 opposite to the ball groove 121 and facing the ball 230.
- the first jig 310 and the second jig 320 pressed the first member 210 and the second member 220 along the axial direction of the first member 210.
- the maximum stress acting on the spline teeth of the first member 210 was investigated by FEM analysis.
- Workbench Mechanical manufactured by ANSYS was used as software.
- Test example In the test example, the hardness and toughness of the sintered member were evaluated.
- Sample No. 1 Sample No. 2
- Sample No. 1 Sample No. The sintered member of No. 2 was produced through a step of preparing a raw material powder, a step of producing a powder compact, and a step of sintering the powder compact.
- the iron-based alloy powder contains Cr and Mo, and has a plurality of iron alloy particles whose balance is Fe and unavoidable impurities.
- Table 1 shows the Cr content and the Mo content in the iron-based alloy. That is, the Cr content in the iron-based alloy is 3.0% by mass, and the Mo content in the iron-based alloy is 0.5% by mass. “-” Shown in Table 1 indicates that the corresponding element is not contained.
- Table 1 shows the contents of Ni powder and C powder in the raw material powder.
- Sample No. In No. 1 the content of Ni powder is 3% by mass, the content of C powder is 0.65% by mass, and the content of Fe powder is the balance.
- Sample No. In No. 2 the content of Ni powder is 4% by mass, the content of C powder is 0.75% by mass, and the content of Fe powder is the balance.
- the raw material powder was pressure-molded to prepare a powder compact.
- the molding pressure was 700 MPa.
- the dust compact was sintered to produce a sintered member.
- a continuous sintering furnace having a sintering furnace and a continuous quenching chamber downstream of the sintering furnace was used for sintering the powder compact.
- the sintering temperature was 1300 ° C. and the sintering time was 15 minutes.
- Sample No. 101, sample No. 102 Sample No. 101, sample No. The sintered member of 102 had the sample No. 1 except that the content of Ni powder and the content of C powder in the prepared raw material powder were different. It was produced in the same manner as the sintered member of 1. Specifically, the sample No. In 101, the content of Ni powder in the raw material powder was set to 1% by mass, and the content of C powder in the raw material powder was set to 0.7% by mass. Sample No. In 102, the content of Ni powder in the raw material powder was 2% by mass, and the content of C powder in the raw material powder was 0.7% by mass.
- Sample No. 110 Sample No. The sintered member of 110 was sample No. 1 except for the following points (a) to (e). It was produced in the same manner as in 2.
- E After the step of sintering, quenching and tempering were performed.
- the iron-based alloy powder contains Cu, Mo, and Ni, and has a plurality of iron alloy particles whose balance is Fe and unavoidable impurities.
- the Cu content in the iron-based alloy is 1.5% by mass.
- the Mo content in the iron-based alloy is 0.5% by mass.
- the content of Ni in the iron-based alloy is 4% by mass.
- Sample No. In 110, the content of C powder in the raw material powder is 0.5% by mass, and the content of Fe powder is the balance.
- the sintered member was slowly cooled without quenching.
- the cooling rate is about 0.5 ° C./sec.
- the apparent density (g / cm3) of each sample in the sintered member was measured by the Archimedes method. The apparent density was determined by "(dry weight of the sintered member) / ⁇ (dry weight of the sintered member)-(weight of the oil-immersed material of the sintered member in water) ⁇ x water density".
- the weight of the oil-immersed material of the sintered member in water is the weight of the member in which the sintered member immersed in oil and impregnated with oil is immersed in water.
- the number of N was set to 3.
- the average of the measurement results of the three sintered members was taken as the apparent density of the sintered members of each sample. The results are shown in Table 1.
- the hardness of the sintered member was evaluated by determining the Vickers hardness of the sintered member and the fluctuation range of the Vickers hardness from the surface of the sintered member to a predetermined depth.
- the Vickers hardness was measured in accordance with JIS Z 2244 (2009).
- the test piece was cut out from the sintered member.
- the shape of the test piece was rectangular.
- the size of the test piece was 55 mm ⁇ 10 mm ⁇ thickness 10 mm.
- the test piece was cut out so that one surface in the thickness direction of the test piece was composed of the surface of the sintered member.
- the Vickers hardness at 11 points was measured from the surface of the test piece to the predetermined depth in the cross section of the test piece.
- the surface of the test piece was one surface in the thickness direction of the test piece described above.
- the predetermined depth was 5.0 mm along the direction orthogonal to the surface of the test piece.
- the breakdown of the measurement points is 0.1 mm from the surface and 10 points at intervals of 0.5 mm from the surface.
- the number of N was set to 3.
- the average Vickers hardness at all measurement points of the three test pieces was taken as the Vickers hardness of the sintered member.
- the difference between the maximum value and the minimum value of the average Vickers hardness at each measurement point of the three test pieces was defined as the fluctuation range of the Vickers hardness of the sintered member. The results are shown in Table 1.
- sample No. 2 As a representative, sample No. 2. Sample No. 101, sample No. In the 110 sintered members, the average Vickers hardness at each measurement point of the three test pieces is shown by a circle, a cross, and a black diamond in FIG. 7. The horizontal axis of the graph of FIG. 7 indicates the depth (mm) from the surface, and the vertical axis indicates the Vickers hardness (HV).
- the Ono-type rotary bending fatigue test was performed in accordance with JIS Z 2274 (1978) using FTO-100 manufactured by Tokyo Testing Machine Co., Ltd. as a testing machine.
- the test piece was cut out from the sintered member.
- the test piece was a test piece conforming to JIS Z 2274 (1978) No. 1 test piece.
- the shape of the test piece is dumbbell-shaped.
- This test piece has a pair of large diameter portions and a small diameter portion. Each large diameter portion is provided at both ends in the axial direction of the test piece.
- the shape of each large diameter portion is columnar.
- the diameter of each large diameter portion is uniform in the axial direction of the large diameter portion.
- the small diameter portion is provided between the two large diameter portions. Both large diameter parts and small diameter parts are continuous.
- the shape of the small diameter portion is columnar.
- the small diameter portion has a parallel portion and a pair of curved portions.
- the parallel portion is a portion having a uniform diameter along the axial direction at the center of the small diameter portion in the axial direction.
- Each curved portion is a portion connecting the parallel portion and the large diameter portion, and is a portion whose diameter increases from the parallel portion side to the large diameter portion side.
- the axial length of the test piece was 90.18 mm.
- the axial length of each large diameter portion was 27.5 mm, and the axial length of the small diameter portion was 35.18 mm.
- the diameter of the large diameter portion was 12 mm.
- the diameter of the parallel portion was 8 mm.
- the length of the parallel portion is 16 mm.
- the rotation speed was set to 3400 rpm.
- the maximum stress amplitude at which the test piece did not break when repeatedly bent 107 times was measured.
- the number of N was set to 3.
- the average of the stress amplitudes of the three test pieces was taken as the stress amplitude of the sintered member. The results are shown in Table 1.
- the cross section of the sintered member was an arbitrary cross section.
- the cross section was exposed as follows.
- a resin molded body was prepared in which a sample piece obtained by cutting a part of a sintered member was embedded in an epoxy resin.
- the resin molded body was polished.
- the polishing process was performed in two stages. As the first step, the resin of the resin molded product is polished until the cut surface of the sintered member is exposed. As the second step, the exposed cut surface is polished. Polishing is mirror polishing. That is, the cross section to be observed is a mirror-polished surface.
- FIGS. 8A and 8B, 9A and 9B, 11 and 12 show the sample No. 1. Sample No. 2. Sample No. 101, sample No. A photomicrograph of a cross section of the sintered member of 102 is shown. The size of the micrographs of FIGS. 8A, 9A, 11 and 12, is about 2.82 mm ⁇ 2.09 mm. The size of the micrographs of FIGS. 8B and 9B is about 1.38 mm ⁇ 1.02 mm.
- each micrograph shows the retained austenite phase with arrows.
- the white part at the tip of this arrow is the retained austenite phase.
- the area around the white area is the martensite phase. Note that FIG. 11 does not have an arrow because no retained austenite phase is observed.
- the area ratio of the retained austenite phase in the above five samples was determined.
- the ratio of the total area of the retained austenite phase to the total area of the measurement field of view was determined by using a portable X-ray residual stress measuring device ⁇ -X360 manufactured by Pulsetech Industries.
- the number of measurement fields was set to two.
- the size of the measurement field of view was 2 mm in diameter.
- the average of the ratio of the total area of the retained austenite phase in each measurement field of view was taken as the area ratio of the retained austenite phase.
- Table 1 The results are shown in Table 1.
- sample No. 1 sample No. 1
- Sample No. 2 is the sample No. 101, sample No. 102, sample No.
- the Vickers hardness was high, the fluctuation range of the Vickers hardness was small, and the stress amplitude was large.
- the sample No. 1 As shown in FIGS. 8A, 8B, 9A, and 9B, the sample No. 1. Sample No. It was found that the sintered member of No. 2 had a mixed phase structure of a martensite phase and a retained austenite phase. On the other hand, as shown in FIGS. 11 and 12, the sample No. 101, sample No. It was found that the sintered member of 102 was substantially composed of the martensite phase, with little or no retained austenite phase. Sample No. 1. Sample No. The area ratio of the retained austenite phase in the sintered member of No. 2 is the sample No. 101, sample No. It was higher than the area ratio of the retained austenite phase in the sintered member of 102.
Landscapes
- Engineering & Computer Science (AREA)
- Mechanical Engineering (AREA)
- Chemical & Material Sciences (AREA)
- General Engineering & Computer Science (AREA)
- Manufacturing & Machinery (AREA)
- Materials Engineering (AREA)
- Metallurgy (AREA)
- Organic Chemistry (AREA)
- Physics & Mathematics (AREA)
- Electromagnetism (AREA)
- Thermal Sciences (AREA)
- Crystallography & Structural Chemistry (AREA)
- Mechanical Operated Clutches (AREA)
- Powder Metallurgy (AREA)
Priority Applications (5)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2021550403A JP7179269B2 (ja) | 2019-10-03 | 2020-08-17 | 焼結部材、及び電磁カップリング |
| CN202080064883.6A CN114402147B (zh) | 2019-10-03 | 2020-08-17 | 烧结部件及电磁耦合器 |
| US17/762,734 US12392382B2 (en) | 2019-10-03 | 2020-08-17 | Sintered member and electromagnetic coupling |
| KR1020227010810A KR102720408B1 (ko) | 2019-10-03 | 2020-08-17 | 소결 부재 및 전자 커플링 |
| DE112020004757.1T DE112020004757T5 (de) | 2019-10-03 | 2020-08-17 | Sinterglied und elektromagnetische Kuppelung |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2019182666 | 2019-10-03 | ||
| JP2019-182666 | 2019-10-03 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2021065221A1 true WO2021065221A1 (ja) | 2021-04-08 |
Family
ID=75338190
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2020/031031 Ceased WO2021065221A1 (ja) | 2019-10-03 | 2020-08-17 | 焼結部材、及び電磁カップリング |
Country Status (7)
| Country | Link |
|---|---|
| US (1) | US12392382B2 (cg-RX-API-DMAC10.html) |
| JP (1) | JP7179269B2 (cg-RX-API-DMAC10.html) |
| KR (1) | KR102720408B1 (cg-RX-API-DMAC10.html) |
| CN (1) | CN114402147B (cg-RX-API-DMAC10.html) |
| DE (1) | DE112020004757T5 (cg-RX-API-DMAC10.html) |
| TW (1) | TWI877231B (cg-RX-API-DMAC10.html) |
| WO (1) | WO2021065221A1 (cg-RX-API-DMAC10.html) |
Families Citing this family (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP1666420S (cg-RX-API-DMAC10.html) * | 2019-10-03 | 2020-08-24 |
Citations (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPS60172599A (ja) * | 1984-02-17 | 1985-09-06 | 凸版印刷株式会社 | 液圧転写用転写紙 |
| JPH07158417A (ja) * | 1993-10-14 | 1995-06-20 | Toyota Motor Corp | 内燃機関のバルブタイミング制御装置 |
| JP2002178092A (ja) * | 2000-12-13 | 2002-06-25 | Aichi Steel Works Ltd | 欠歯領域を有する歯形状部品の製造方法 |
| JP2017133660A (ja) * | 2016-01-29 | 2017-08-03 | 武蔵精密工業株式会社 | 伝動装置 |
Family Cites Families (10)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH0138344Y2 (cg-RX-API-DMAC10.html) | 1985-11-08 | 1989-11-16 | ||
| US5142943A (en) * | 1991-09-30 | 1992-09-01 | Hughes Leon D | Clutch drive differential system |
| JP3395327B2 (ja) * | 1994-03-09 | 2003-04-14 | 三菱マテリアル株式会社 | 内ヘリカルギヤの製造方法および製造装置 |
| ATE279671T1 (de) * | 1997-07-15 | 2004-10-15 | Aimbridge Pty Ltd | Zahnradprofil für planetengetriebe, planetengetriebe und winden die ein planetengetriebe verwenden |
| DE102008031512A1 (de) * | 2008-07-03 | 2010-01-07 | Schaeffler Kg | Vorspanneinheit |
| JP2012167783A (ja) | 2011-02-16 | 2012-09-06 | Jtekt Corp | 駆動力伝達装置 |
| JP6566337B2 (ja) | 2014-03-05 | 2019-08-28 | 株式会社リコー | 画像形成装置 |
| JP2019019862A (ja) * | 2017-07-14 | 2019-02-07 | 日本電産シンポ株式会社 | 波動歯車装置 |
| EP3667120B1 (en) * | 2017-08-09 | 2022-03-30 | Harmonic Drive Systems Inc. | Wave gear device |
| US20190219147A1 (en) * | 2018-01-17 | 2019-07-18 | ILJIN USA Corporation | Gear for a torque transmission device and method for making the gear |
-
2020
- 2020-08-17 US US17/762,734 patent/US12392382B2/en active Active
- 2020-08-17 WO PCT/JP2020/031031 patent/WO2021065221A1/ja not_active Ceased
- 2020-08-17 JP JP2021550403A patent/JP7179269B2/ja active Active
- 2020-08-17 DE DE112020004757.1T patent/DE112020004757T5/de active Pending
- 2020-08-17 KR KR1020227010810A patent/KR102720408B1/ko active Active
- 2020-08-17 CN CN202080064883.6A patent/CN114402147B/zh active Active
- 2020-09-26 TW TW109133478A patent/TWI877231B/zh active
Patent Citations (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPS60172599A (ja) * | 1984-02-17 | 1985-09-06 | 凸版印刷株式会社 | 液圧転写用転写紙 |
| JPH07158417A (ja) * | 1993-10-14 | 1995-06-20 | Toyota Motor Corp | 内燃機関のバルブタイミング制御装置 |
| JP2002178092A (ja) * | 2000-12-13 | 2002-06-25 | Aichi Steel Works Ltd | 欠歯領域を有する歯形状部品の製造方法 |
| JP2017133660A (ja) * | 2016-01-29 | 2017-08-03 | 武蔵精密工業株式会社 | 伝動装置 |
Also Published As
| Publication number | Publication date |
|---|---|
| JP7179269B2 (ja) | 2022-11-29 |
| JPWO2021065221A1 (cg-RX-API-DMAC10.html) | 2021-04-08 |
| US12392382B2 (en) | 2025-08-19 |
| TWI877231B (zh) | 2025-03-21 |
| CN114402147A (zh) | 2022-04-26 |
| KR102720408B1 (ko) | 2024-10-21 |
| DE112020004757T5 (de) | 2022-06-15 |
| CN114402147B (zh) | 2023-12-15 |
| KR20220054863A (ko) | 2022-05-03 |
| US20220333653A1 (en) | 2022-10-20 |
| TW202120223A (zh) | 2021-06-01 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP4789837B2 (ja) | 鉄系焼結体及びその製造方法 | |
| JP6688287B2 (ja) | プレアロイ鉄基粉末、プレアロイ鉄基粉末を含有する鉄基粉末混合物、及び鉄基粉末混合物からプレス成形および焼結した部品を製造する方法 | |
| JP6722511B2 (ja) | 浸炭用焼結鋼、浸炭焼結部材およびそれらの製造方法 | |
| JP6194613B2 (ja) | 摺動部材用鉄基焼結合金およびその製造方法 | |
| JP2005213649A (ja) | 粉末金属から部品を製造する方法 | |
| CN105899315A (zh) | 烧结机械部件及其制造方法 | |
| JP2019019362A (ja) | 焼結部材、及び焼結部材の製造方法 | |
| JP7179269B2 (ja) | 焼結部材、及び電磁カップリング | |
| US7041149B2 (en) | Sintered sprocket for silent chain and production method therefor | |
| JP7188434B2 (ja) | 焼結バルブガイド及びその製造方法 | |
| JP2020172698A (ja) | 焼結部品の製造方法、及び焼結部品 | |
| JP2020172697A (ja) | 焼結部品の製造方法、及び焼結部品 | |
| JP6842345B2 (ja) | 耐摩耗性鉄基焼結合金の製造方法 | |
| KR102810038B1 (ko) | 소결 부재 및 소결 부재의 제조 방법 | |
| JP6444621B2 (ja) | 焼結機械部品 | |
| JP7114817B2 (ja) | 焼結材、及び焼結材の製造方法 | |
| KR102647464B1 (ko) | 철기 합금 소결체 및 분말 야금용 철기 혼합 가루 | |
| US20220105564A1 (en) | Sintered material, gear, and method for producing sintered material | |
| JPH10317090A (ja) | 鉄合金焼結体部品とその製法 | |
| WO2015111338A1 (ja) | 焼結機械部品及びその製造方法 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 20872110 Country of ref document: EP Kind code of ref document: A1 |
|
| ENP | Entry into the national phase |
Ref document number: 2021550403 Country of ref document: JP Kind code of ref document: A |
|
| ENP | Entry into the national phase |
Ref document number: 20227010810 Country of ref document: KR Kind code of ref document: A |
|
| 122 | Ep: pct application non-entry in european phase |
Ref document number: 20872110 Country of ref document: EP Kind code of ref document: A1 |
|
| WWG | Wipo information: grant in national office |
Ref document number: 17762734 Country of ref document: US |