WO2018010108A1 - 一种片状钽粉及其制备方法 - Google Patents
一种片状钽粉及其制备方法 Download PDFInfo
- Publication number
- WO2018010108A1 WO2018010108A1 PCT/CN2016/089874 CN2016089874W WO2018010108A1 WO 2018010108 A1 WO2018010108 A1 WO 2018010108A1 CN 2016089874 W CN2016089874 W CN 2016089874W WO 2018010108 A1 WO2018010108 A1 WO 2018010108A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- powder
- ppm
- nitrogen
- temperature
- flaky
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- C—CHEMISTRY; METALLURGY
- C22—METALLURGY; FERROUS OR NON-FERROUS ALLOYS; TREATMENT OF ALLOYS OR NON-FERROUS METALS
- C22B—PRODUCTION AND REFINING OF METALS; PRETREATMENT OF RAW MATERIALS
- C22B34/00—Obtaining refractory metals
- C22B34/20—Obtaining niobium, tantalum or vanadium
- C22B34/24—Obtaining niobium or tantalum
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B22—CASTING; POWDER METALLURGY
- B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B22F9/00—Making metallic powder or suspensions thereof
- B22F9/16—Making metallic powder or suspensions thereof using chemical processes
- B22F9/18—Making metallic powder or suspensions thereof using chemical processes with reduction of metal compounds
- B22F9/20—Making metallic powder or suspensions thereof using chemical processes with reduction of metal compounds starting from solid metal compounds
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B22—CASTING; POWDER METALLURGY
- B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B22F1/00—Metallic powder; Treatment of metallic powder, e.g. to facilitate working or to improve properties
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B22—CASTING; POWDER METALLURGY
- B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B22F1/00—Metallic powder; Treatment of metallic powder, e.g. to facilitate working or to improve properties
- B22F1/06—Metallic powder characterised by the shape of the particles
- B22F1/068—Flake-like particles
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B22—CASTING; POWDER METALLURGY
- B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B22F1/00—Metallic powder; Treatment of metallic powder, e.g. to facilitate working or to improve properties
- B22F1/14—Treatment of metallic powder
- B22F1/142—Thermal or thermo-mechanical treatment
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B22—CASTING; POWDER METALLURGY
- B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B22F1/00—Metallic powder; Treatment of metallic powder, e.g. to facilitate working or to improve properties
- B22F1/14—Treatment of metallic powder
- B22F1/145—Chemical treatment, e.g. passivation or decarburisation
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01G—CAPACITORS; CAPACITORS, RECTIFIERS, DETECTORS, SWITCHING DEVICES, LIGHT-SENSITIVE OR TEMPERATURE-SENSITIVE DEVICES OF THE ELECTROLYTIC TYPE
- H01G9/00—Electrolytic capacitors, rectifiers, detectors, switching devices, light-sensitive or temperature-sensitive devices; Processes of their manufacture
- H01G9/004—Details
- H01G9/04—Electrodes or formation of dielectric layers thereon
- H01G9/042—Electrodes or formation of dielectric layers thereon characterised by the material
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01G—CAPACITORS; CAPACITORS, RECTIFIERS, DETECTORS, SWITCHING DEVICES, LIGHT-SENSITIVE OR TEMPERATURE-SENSITIVE DEVICES OF THE ELECTROLYTIC TYPE
- H01G9/00—Electrolytic capacitors, rectifiers, detectors, switching devices, light-sensitive or temperature-sensitive devices; Processes of their manufacture
- H01G9/004—Details
- H01G9/04—Electrodes or formation of dielectric layers thereon
- H01G9/048—Electrodes or formation of dielectric layers thereon characterised by their structure
- H01G9/052—Sintered electrodes
- H01G9/0525—Powder therefor
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01G—CAPACITORS; CAPACITORS, RECTIFIERS, DETECTORS, SWITCHING DEVICES, LIGHT-SENSITIVE OR TEMPERATURE-SENSITIVE DEVICES OF THE ELECTROLYTIC TYPE
- H01G9/00—Electrolytic capacitors, rectifiers, detectors, switching devices, light-sensitive or temperature-sensitive devices; Processes of their manufacture
- H01G9/15—Solid electrolytic capacitors
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B22—CASTING; POWDER METALLURGY
- B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B22F9/00—Making metallic powder or suspensions thereof
- B22F9/02—Making metallic powder or suspensions thereof using physical processes
- B22F9/04—Making metallic powder or suspensions thereof using physical processes starting from solid material, e.g. by crushing, grinding or milling
- B22F2009/041—Making metallic powder or suspensions thereof using physical processes starting from solid material, e.g. by crushing, grinding or milling by mechanical alloying, e.g. blending, milling
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B22—CASTING; POWDER METALLURGY
- B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B22F2301/00—Metallic composition of the powder or its coating
- B22F2301/20—Refractory metals
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B22—CASTING; POWDER METALLURGY
- B22F—WORKING METALLIC POWDER; MANUFACTURE OF ARTICLES FROM METALLIC POWDER; MAKING METALLIC POWDER; APPARATUS OR DEVICES SPECIALLY ADAPTED FOR METALLIC POWDER
- B22F2999/00—Aspects linked to processes or compositions used in powder metallurgy
Definitions
- the invention relates to a metal powder and a preparation method thereof, and more particularly to a tantalum powder and a preparation method thereof, in particular to a capacitor grade medium and high pressure tantalum powder and a preparation method thereof.
- Metal ruthenium is a valve metal that forms a dense oxide film on the surface and has a unidirectional conductive property.
- the anodic film made of ruthenium metal is stable in chemical properties (especially stable in an acidic electrolyte), high in electrical resistivity (7.5 ⁇ 10 10 ⁇ cm), large in dielectric constant (27.6), and small in leakage current. In addition, it has the advantages of wide operating temperature range (-80 ⁇ 200 °C), high reliability, shock resistance and long service life. It is an ideal material for making small and reliable tantalum capacitors. Because tantalum capacitors have many advantages, they are widely used in electronic equipment such as aerospace, aerospace, communications, computers and mobile phones.
- tantalum powder specially used to make capacitors is called capacitor grade tantalum powder.
- the powder can be divided into high pressure tantalum powder (working voltage greater than 40V), medium pressure tantalum powder (working voltage between 20-40V, including end points) and low pressure tantalum powder (working voltage less than 20V).
- high pressure tantalum powder working voltage greater than 40V
- medium pressure tantalum powder working voltage between 20-40V, including end points
- low pressure tantalum powder working voltage less than 20V.
- the nitrogen doping in the tantalum powder can effectively reduce the oxygen content of the tantalum powder, and at the same time, can reduce the sintering shrinkage rate, increase the porosity, facilitate the immersion of the cathode material, and increase the capacity of the capacitor.
- nitrogen doping in tantalum powder and nitrogen doping in sintered anodes have been an important technique for improving the performance of tantalum powder and tantalum capacitors in the field of tantalum powder production.
- U.S. Patent No. 5,448, 447 discloses the incorporation of 500-7000 ppm of nitrogen in a low CV tantalum powder below 30,000 ⁇ FV/g, above 100V.
- the leakage current is reduced by at least 28% when the high voltage is formed.
- the method of nitrogen doping of the tantalum powder is to carry out nitrogen doping during the deoxidation process in the final step of the manufacturing process, and then no high temperature heat treatment.
- JP-A-2002-30301 discloses a niobium powder having a nitrogen content of 500 to 30,000 ppm and a variation in nitrogen content between particles of less than 100%, which is better than a niobium-free niobium powder. Breakdown voltage.
- the nitrogen doping method of the niobium powder is carried out in a reaction vessel such as a rotary kiln in a final process of a desulfurization process in the manufacturing process, and is heated to 850 ° C in a rotating state to carry out nitrogen doping, and thereafter no heat treatment of 900 ° C or more.
- This patent studies a nitrogen-doping method and a nitrogen-containing niobium powder suitable for high-capacity niobium powders of 30,000 ⁇ FV/g or more.
- Chinese patents CN1363102A and CN100528418C respectively disclose nitrogen-doping methods for niobium and tantalum metal powders, the nitrogen content of which is between 100 and 6000 ppm.
- the nitrogen-doping method described in the two patents is also nitrogen-doped in the final stage, and the nitrogen-doping temperature is 100. °C-600 ° C, and no heat treatment after that.
- Chinese patents CN1433485A and CN1872461A describe a method for producing a nitrogen-containing niobium powder by introducing nitrogen into the metal during the reduction of the metal compound by the reducing agent.
- This nitrogen-doping process is nitrogen-doped at 800 ° C or higher due to the existence of a reduction reaction process, so that the reaction of ruthenium with nitrogen is too fast, resulting in inconsistent nitrogen concentrations in various parts of the reaction vessel, and thus it is difficult to ensure uniform nitrogen-doped between particles.
- the inventors have found through research that the nitrogen-doped powder of the high-capacity tantalum powder of 30000 ⁇ FV/g or more can be improved by using the existing method, but the leakage current and capacity of the tantalum powder are improved, but for 30,000 ⁇ FV/g or less, especially the sheet-like medium-high pressure ⁇
- the powder is nitrogen-doped in the final step without high-temperature heat treatment, and the presence of nitrogen element has no significant effect on the improvement of the medium-high pressure tantalum powder of 30,000 ⁇ FV/g or less, especially the leakage current of the flake powder or the increase of the powder capacity.
- the present invention develops a new nitrogen-doping method and develops nitrogen-containing 300. -1800ppm flake powder, which further improves the leakage current and pressure resistance of medium and high pressure flake powder below 30,000 ⁇ FV/g, especially high frequency characteristics, so that medium and high pressure flake powder is better used for high The frequency characteristics require a relatively high field.
- a flaky powder in particular a medium-high pressure flaky powder, which preferably contains nitrogen, phosphorus and/or boron, and is preferably suitable for use in high frequency capacitors;
- Another object is to provide a method of producing the medium and high pressure flakes.
- the method of the present invention is particularly suitable for medium and high pressure flakes of 30,000 ⁇ FV/g or less, it is also suitable for medium and high pressure flakes of more than 30,000 ⁇ FV/g.
- a flaky powder suitable for use in a high frequency capacitor characterized in that the powder contains 300 to 1800 ppm, preferably 400 to 1600 ppm, more preferably 500 to 1500 ppm, most preferably 700 to 1300 ppm of nitrogen; 10 to 100 ppm, preferably 20-80 ppm, more preferably 30-70 ppm of phosphorus; and/or 1-80 ppm, preferably 10-65 ppm, more preferably 20-50 ppm of boron.
- a sheet-like tantalum powder preferably applied to a high-frequency capacitor characterized in that the anode of the electrolytic capacitor made of the powder has a capacity of about 100-250 V and a test frequency of 5000-30,000 HZ. It is 3000 to 30000 ⁇ FV/g.
- the inventors unexpectedly found that the nitrogen content is too low to inhibit sintering and increase the capacity; if the nitrogen content is too high, the hardness of the tantalum powder will increase, which will result in poor briquetting performance and even cause great damage to the abrasive tools. Large wear and tear, thus shortening the service life of the grinding tool, so the nitrogen content is preferably 300 to 1800 ppm.
- the flake powder has an oxygen content of preferably 800 to 3,000 ppm, and the bulk density is not particularly limited, and is preferably 1.4 to 2.0 g/cm 3 , preferably 1.55 to 1.9 g/cm 3 .
- a method for producing flaky powder comprising the steps of:
- the second heat-treated cerium powder is subjected to a second deoxidation, and then optionally subjected to pickling, water washing, drying, and sieving to obtain a flaky enamel powder according to the present invention.
- step 2 during the cooling of the deoxidation treatment of step 2) (special
- the low temperature nitridation of step 3) is started at a temperature below 500 ° C, for example 500 ° C - 240 ° C.
- the deoxidation treatment of step 2) is reheated after cooling to room temperature.
- the tantalum powder used in the step 1) is a sheet-like tantalum powder obtained by any method known in the art, for example, a sheet-like tantalum obtained by vibrating ball milling or stirring ball milling by a vibrating ball mill or a stirring ball mill. powder.
- the heat treatment in step 1) is carried out under vacuum conditions.
- the temperature of the heat treatment is 1200 to 1600 ° C, preferably 1250-1500 ° C, more preferably 1300-1450 ° C.
- the flaky powder of the raw material is obtained by ball milling, pickling and decontamination of the sodium reduced cerium powder to obtain a flaky cerium powder, optionally incorporating phosphorus.
- the deoxidation holding temperature and time of the step 2) or 5) are not particularly limited, and for example, it can be kept at 800 to 1000 ° C (preferably 750 to 980 ° C, 750 to 900 ° C or 850 to 950 ° C) for 3 to 6 hours ( It is preferably 3-5 hours or 4-6 hours).
- the deoxidation in the step 2) is carried out by mixing the niobium powder obtained in the step 1) into the magnesium powder (for example, magnesium powder having a weight of 0.5 to 5 wt% of the niobium powder), and heating to 700 tones in an argon atmosphere. Performed at a temperature of 1000 ° C. A more preferred temperature is 800-900 °C.
- the deoxidation can be completed by mixing the product obtained in the step 1) into the magnesium powder in an amount of 0.5 to 5% by weight based on the weight of the niobium powder, heating in an argon atmosphere to a temperature of 700 to 1000 ° C, and then lowering the temperature.
- the low temperature nitridation in the step 3) means nitriding at a temperature of 500 ° C or lower.
- the low temperature nitriding is specifically carried out by replacing the inert atmosphere with a nitrogen atmosphere after the temperature in the step 2) is lowered to 240 to 500 ° C (for example, 300 to 450 ° C, or about 400 ° C) (preferably maintaining the furnace)
- the internal atmosphere is a positive pressure, for example, 0-0.1 MPa, for example, 0-0.01 MPa), and the heat preservation is 80 ⁇ .
- the cooling is passivated and then discharged.
- the tantalum powder is sieved, pickled, and dried after passivation.
- the second heat treatment in step 4) comprises heating to 1200-1600 ° C under vacuum and for 30-180 minutes, preferably 30-120 minutes.
- the deoxygenation in step 5) can be carried out by any deoxygenation method known in the art.
- the deoxygenation process in step 5) is the same as the deoxygenation process in step 2).
- the deoxygenation process in step 5) is different from the deoxygenation process in step 2).
- the inventors unexpectedly found that if the nitrogen doping treatment is performed at a high temperature of 500 ° C or higher, the diffusion rate of nitrogen increases, the oxide film diffuses rapidly, the tantalum powder is exposed, and the uppermost layer of tantalum and nitrogen are in contact with nitrogen.
- the exothermic reaction of nitrogen proceeds sharply, and even a runaway reaction occurs locally, while the powder of the lower layer is in a state in which nitrogen cannot be rapidly supplied.
- the powder nitrogen content of the surface is very large, while the powder nitrogen content of the lower layer is very small, the difference in nitrogen content between the respective particles becomes very large, and it is possible to form nitride crystals (for example, Ta2Ney TaN) and the like.
- the nitrogen doping treatment is performed only below 500 ° C, and the high temperature heat treatment of 1000 ° C or higher is not followed, the inventors have confirmed that the nitrogen content only stays on the surface of the tantalum powder, the diffusion is not deep enough, and is not more uniform, so for 30000 ⁇ FV. Below /g, especially in the sheet-like medium-high pressure ⁇ powder leakage current improvement or no increase in the powder capacity.
- the method of the present invention combines the characteristics of the existing medium and high pressure tantalum powder production process, performs low temperature nitrogen doping in the deoxidation process, and then performs high temperature heat treatment, thereby avoiding the above problems.
- phosphorus element and/or boron element one element may be selected, or both elements may be simultaneously incorporated, and phosphorus and/or boron may optionally be added before the heat treatment of step 1).
- the compound of the element may also be added together with the magnesium powder in the deoxidation treatment of the step 2), or may be added after the step 5.
- the Feis' average particle size (FSSS/ ⁇ m) used to describe the base metal particles disclosed in this specification was measured by a Fischer sub-sifter, and the oxygen and nitrogen content were analyzed by the US LECO ON-600 oxygen-nitrogen tester. Analysis, the phosphorus content was analyzed by Uninik (Shanghai) Instrument Co., Ltd. 2800 UV/VIS spectrophotometer, and the impurity elements of iron and boron content were analyzed by American Baird DV-5 DC arc photoelectric spectrometer, and the bulk density (SBD, g/) Cm 3 ) is tested according to the method specified in Chinese National Standard GB5060-85.
- the raw materials used in this paper are all commercially available, for example, they can be purchased from Ningxia Dongfang Shengye Co., Ltd.
- the flake powder obtained by the prior art was used as the raw material 1, and the parameters were as shown in Table 1.
- the temperature is raised to 900 ° C for 4 hours, and then cooled to 450 ° C, and then replaced by evacuation, and charged with high purity nitrogen to positive pressure (+ 0.01MPa), and after 60 minutes of heat preservation, after cooling and passivation, it is taken out, and after pickling and impurity removal according to the prior art, it is then charged into a heat treatment furnace, and after being kept at 1430 ° C for 60 minutes, it is cooled and passivated and then discharged, and 60 mesh is passed. Screen and magnetic separation.
- the above powder sample was compression molded, the compact had a density of 5.0 g/cm 3 , the core powder had a weight of 0.20 g, and was sintered at 1600 ° C for 15 minutes to obtain a sintered compact.
- the agglomerates were energized at 150 V in a 0.01% phosphoric acid solution, and the capacity and loss were measured at a test frequency of 5000-30000 Hz.
- the electrical properties of the samples were determined in Table 3.
- Example 2 In the same manner as the raw material used in Example 1, 5 Kg of raw material was taken, 40 ppm of boric acid based on boron element was added, mixed uniformly and subjected to agglomeration treatment, and then placed in a heat treatment furnace, and after being kept at 1450 ° C for 60 minutes, it was cooled and passivated, and then discharged. Screen and magnetic separation. Then, 1.5% of the magnesium powder is added to the weight of the tantalum powder, and under the protection of an inert gas, the temperature is raised to 900 ° C for 4 hours, and then the temperature is lowered and cooled. After passivation, the furnace is removed by acid washing and impurity removal according to the prior art, and then placed in a heat treatment furnace. After being kept at 1430 ° C for 60 minutes, it is cooled and passivated, and then discharged, passed through a 60 mesh sieve and magnetically selected.
- Example 2 The same raw materials as in Example 1 were used, and the parameters were as shown in Table 1. After being agglomerated, they were placed in a heat treatment furnace, and after being kept at 1400 ° C for 60 minutes, they were cooled and passivated, then discharged, and passed through a 60 mesh sieve and magnetically selected. Then, 70 ppm of hexafluorophosphate was added with phosphorus as the phosphorus element, and 2.0% of the magnesium powder was mixed uniformly with the weight of the tantalum powder. Under the protection of the inert gas, the temperature was raised to 880 ° C for 4 hours, and then cooled to 350 ° C after cooling.
- the above powder sample was compression-molded, the density of the compact was 5.0 g/cm 3 , and the weight of the core powder was 0.20 g, and sintered at 1700 ° C for 15 minutes in a vacuum furnace of 10 -3 Pa to obtain a sintered compact.
- the agglomerates were energized at 140 V in a 0.01% phosphoric acid solution, and the capacity and loss were measured at a test frequency of 5000-30000 Hz.
- the electrical properties of the samples were determined in Table 3.
- Example 2 The same as the raw materials used in Example 2, after being agglomerated, charged into a heat treatment furnace, incubated at 1400 ° C for 60 min, cooled and passivated, and then discharged, passed through a 60 mesh sieve and magnetically selected, and blended into 2.0% by weight of niobium powder.
- the magnesium powder is uniformly mixed. Under the protection of inert gas, the temperature is raised to 880 ° C for 4 h, and then the temperature is lowered. After cooling and passivation, the furnace is discharged, and after pickling and impurity removal according to the prior art, it is then charged into the heat treatment furnace at 1400 ° C. After 60 minutes of heat preservation, it was cooled and passivated, and then discharged, passed through a 60 mesh sieve and magnetically selected.
- the flake powder obtained by the prior art was used as the raw material 2, and its properties are shown in Table 1.
- Table 1 Take 5Kg, add 80ppm ammonium dihydrogen phosphate in terms of phosphorus element, mix well and after the agglomeration treatment, put it into the heat treatment furnace, heat it at 1380 °C for 60min, then pass the cooling passivation, then go out, pass 60 mesh sieve and magnetic separation, Then, 2.5% of the magnesium powder is added to the weight of the tantalum powder, and under the protection of an inert gas, the temperature is raised to 860 ° C for 4 hours, then cooled to 320 ° C, and then replaced by evacuation, and charged with high purity nitrogen to positive pressure (+0.01).
- the above powder sample was compression molded, the compact had a density of 5.0 g/cm 3 , the core powder had a weight of 0.15 g, and was sintered at 1500 ° C for 20 minutes to obtain a sintered compact.
- the agglomerates were energized at 140 V in a 0.01% phosphoric acid solution, and the capacity and loss were measured at a test frequency of 5000-30000 Hz.
- the electrical properties of the samples were determined in Table 3.
- Example 3 In the same manner as the raw material used in Example 3, 5 kg was added, 80 ppm of ammonium dihydrogen phosphate was added as phosphorus, mixed uniformly and subjected to agglomeration treatment, and then placed in a heat treatment furnace, and after being kept at 1380 ° C for 60 minutes, it was cooled and passivated and then discharged. After 60 mesh sieve and magnetic separation, and then 2.5% of magnesium powder by weight of niobium powder, under the protection of inert gas, the temperature is raised to 860 ° C for 4 h, then cooled, cooled and passivated, and then discharged, using the prior art. After pickling and impurity removal, it is placed in a heat treatment furnace, and after being kept at 1450 ° C for 60 min, it is cooled and passivated, and then discharged, passed through a 60 mesh sieve and magnetically selected.
- the flake powder obtained by the prior art was used as the raw material 3, and its properties are shown in Table 1.
- Take 5Kg add 40ppm boric acid based on boron element, mix well and after the agglomeration treatment, put it into the heat treatment furnace, heat it at 1520 °C for 60min, then pass the cooling passivation, then go out, pass 60 mesh sieve and magnetic separation, then mix 1.5% of the magnesium powder by weight of niobium powder, under the protection of inert gas, the temperature is raised to 920 ° C for 4 h, cooled to 420 ° C after cooling, and then replaced by high-purity nitrogen to positive pressure (+0.01 MPa). After 60 minutes of heat preservation, it is cooled and passivated and then discharged.
- the above powder sample was compression-molded, the density of the compact was 6.0 g/cm 3 , the weight of the core powder was 3 g, and the sintered block obtained by sintering at 1700 ° C for 30 minutes was energized at 150 V in a 0.01% phosphoric acid solution at 5000-30000 Hz. The capacity and loss were measured at the test frequency, and the electrical properties of the samples were determined in Table 3.
- Example 4 The same materials as used in Example 4 were used. Take 5Kg of raw material and add 40ppm based on boron The boric acid is uniformly mixed and subjected to agglomeration treatment, then placed in a heat treatment furnace, heated at 1520 ° C for 60 min, cooled and passivated, and then discharged, passed through a 60 mesh sieve and magnetically selected, and then blended with 1.5% by weight of niobium powder. The powder was heated to 920 ° C for 4 h under the protection of an inert gas, and then cooled.
- Table 1 Main impurity content and physical properties of the raw materials used in the present invention
- Table 2 Main impurity content and physical properties of samples of the examples and comparative examples of the present invention
- Table 3 Main electrical performance indexes of the samples of the examples and comparative examples of the present invention under high frequency test
- the leakage current of the sample of the example was significantly lower than that of the comparative example, for example, by at least 10%, and the capacity was remarkably improved, for example, by 5% or more. This has great advantages for high-frequency powders and is also unexpected.
- the tantalum powder obtained in the examples had a small density ratio before and after sintering, and suppressed excessive shrinkage due to sintering, so that the capacity was high under high-frequency test conditions, and the leak current was relatively small.
- the tantalum powder obtained in the comparative example was not subjected to high-temperature treatment after nitrogen doping, so that the shrinkage due to sintering was large, and the capacity was low under high-frequency test conditions, and the leak current was relatively large.
Landscapes
- Engineering & Computer Science (AREA)
- Chemical & Material Sciences (AREA)
- Power Engineering (AREA)
- Chemical Kinetics & Catalysis (AREA)
- General Chemical & Material Sciences (AREA)
- Materials Engineering (AREA)
- Microelectronics & Electronic Packaging (AREA)
- Manufacturing & Machinery (AREA)
- Organic Chemistry (AREA)
- Metallurgy (AREA)
- Mechanical Engineering (AREA)
- Nanotechnology (AREA)
- Physics & Mathematics (AREA)
- Thermal Sciences (AREA)
- Powder Metallurgy (AREA)
- Manufacture Of Metal Powder And Suspensions Thereof (AREA)
- Manufacture And Refinement Of Metals (AREA)
- Inorganic Compounds Of Heavy Metals (AREA)
Priority Applications (9)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| US16/317,394 US20190308247A1 (en) | 2016-07-13 | 2016-07-13 | Flaked tantalum powder and preparation method thereof |
| CN201680086461.2A CN109312424A (zh) | 2016-07-13 | 2016-07-13 | 一种片状钽粉及其制备方法 |
| EP16908436.5A EP3486338B1 (en) | 2016-07-13 | 2016-07-13 | Flaky tantalum powder and method for preparing the same |
| PCT/CN2016/089874 WO2018010108A1 (zh) | 2016-07-13 | 2016-07-13 | 一种片状钽粉及其制备方法 |
| MX2019000450A MX2019000450A (es) | 2016-07-13 | 2016-07-13 | Polvo de tantalio escamoso y metodo de preparacion del mismo. |
| KR1020197004021A KR20190028745A (ko) | 2016-07-13 | 2016-07-13 | 박편화된 탄탈륨 분말 및 이의 제조방법 |
| IL264192A IL264192B2 (en) | 2016-07-13 | 2016-07-13 | Flaked tantalum powder and preparation method thereof |
| JP2019501516A JP6977021B2 (ja) | 2016-07-13 | 2016-07-13 | 薄片状タンタル粉末およびその調製方法 |
| RU2019103885A RU2734851C2 (ru) | 2016-07-13 | 2016-07-13 | Хлопьевидный порошкообразный тантал и способ его получения |
Applications Claiming Priority (1)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| PCT/CN2016/089874 WO2018010108A1 (zh) | 2016-07-13 | 2016-07-13 | 一种片状钽粉及其制备方法 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2018010108A1 true WO2018010108A1 (zh) | 2018-01-18 |
Family
ID=60952280
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/CN2016/089874 Ceased WO2018010108A1 (zh) | 2016-07-13 | 2016-07-13 | 一种片状钽粉及其制备方法 |
Country Status (9)
| Country | Link |
|---|---|
| US (1) | US20190308247A1 (enExample) |
| EP (1) | EP3486338B1 (enExample) |
| JP (1) | JP6977021B2 (enExample) |
| KR (1) | KR20190028745A (enExample) |
| CN (1) | CN109312424A (enExample) |
| IL (1) | IL264192B2 (enExample) |
| MX (1) | MX2019000450A (enExample) |
| RU (1) | RU2734851C2 (enExample) |
| WO (1) | WO2018010108A1 (enExample) |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN115223798A (zh) * | 2022-07-29 | 2022-10-21 | 长春维鸿东光电子器材有限公司 | 一种轴向引出有机高分子钽固定电容器的制造方法 |
Families Citing this family (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN113199021B (zh) * | 2021-04-09 | 2022-12-13 | 宁波职业技术学院 | 一种建筑材料用高性能镁合金复合粉体及其制备方法 |
| WO2023074413A1 (ja) * | 2021-10-28 | 2023-05-04 | パナソニックIpマネジメント株式会社 | 陽極体およびその製造方法、ならびに、電解コンデンサおよびその製造方法 |
| CN114210973B (zh) | 2021-12-15 | 2023-03-24 | 宁夏东方钽业股份有限公司 | 一种钽粉的生产方法以及由该方法得到的钽粉 |
| CN117020215B (zh) | 2021-12-15 | 2025-12-12 | 宁夏东方钽业股份有限公司 | 采用碱土金属还原氧化钽生产电容器用钽粉的方法 |
| CN117182085A (zh) * | 2023-10-16 | 2023-12-08 | 中国振华(集团)新云电子元器件有限责任公司(国营第四三二六厂) | 一种片状钽粉制作方法、电容器及电子设备 |
Citations (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN1236177A (zh) * | 1993-04-26 | 1999-11-24 | 卡伯特公司 | 电容器级钽粉、由其得到的电容器及其在制造电容器阳极中的应用 |
| JP2002030301A (ja) * | 2000-07-12 | 2002-01-31 | Showa Kyabotto Super Metal Kk | 窒素含有金属粉末およびその製造方法ならびにそれを用いた多孔質焼結体および固体電解コンデンサ |
| CN1433485A (zh) * | 2000-02-08 | 2003-07-30 | 卡伯特超金属株式会社 | 含氮的钽或铌粉末的制备和固体电解质电容器 |
| CN1872461A (zh) * | 2001-08-15 | 2006-12-06 | 卡伯特超金属株式会社 | 含氮金属粉末及其制造方法和采用该粉末的多孔质烧结体及固体电解电容器 |
| CN101234425A (zh) * | 2008-01-11 | 2008-08-06 | 宁夏东方钽业股份有限公司 | 含氮均匀的阀金属粉末及其制造方法,阀金属坯块和阀金属烧结体以及电解电容器的阳极 |
Family Cites Families (11)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| DE3140248C2 (de) * | 1981-10-09 | 1986-06-19 | Hermann C. Starck Berlin, 1000 Berlin | Verwendung von dotiertem Ventilmetallpulver für die Herstellung von Elektrolytkondensatoranoden |
| US5211741A (en) * | 1987-11-30 | 1993-05-18 | Cabot Corporation | Flaked tantalum powder |
| CN1023548C (zh) * | 1989-11-20 | 1994-01-19 | 宁夏有色金属冶炼厂 | 电容器级钽粉的生产方法 |
| DE69516556T2 (de) * | 1994-01-26 | 2000-09-07 | H.C. Starck, Inc. | Verfahren zum Nitrieren von Tantalpulver |
| CN1080319C (zh) * | 1997-02-19 | 2002-03-06 | H·C·施塔克公司 | 无碱金属和无氟的钽粉及其制造方法 |
| BRPI9911008B1 (pt) * | 1998-05-06 | 2018-09-25 | H.C. Starck Gmbh | processo para a produção de capacitor de pós de metal, pó de nióbio, anodo de capacitor, pó de liga para uso na fabricação de capacitores eletrolíticos, processo para a fabricação de pó de liga |
| CN1258417C (zh) * | 1998-05-06 | 2006-06-07 | H·C·施塔克公司 | 金属粉末的制备方法 |
| CN100491022C (zh) * | 2000-03-01 | 2009-05-27 | 卡伯特公司 | 氮化的电子管金属及其制造方法 |
| CN101579743B (zh) * | 2003-06-10 | 2014-11-26 | 卡伯特公司 | 钽粉及其制造方法 |
| CN102120258B (zh) * | 2011-02-14 | 2012-12-26 | 宁夏东方钽业股份有限公司 | 钽粉的热处理方法 |
| JP6077274B2 (ja) * | 2012-11-15 | 2017-02-08 | グローバルアドバンストメタルジャパン株式会社 | 窒素含有タンタル粉末およびその製造方法 |
-
2016
- 2016-07-13 RU RU2019103885A patent/RU2734851C2/ru active
- 2016-07-13 EP EP16908436.5A patent/EP3486338B1/en active Active
- 2016-07-13 IL IL264192A patent/IL264192B2/en unknown
- 2016-07-13 KR KR1020197004021A patent/KR20190028745A/ko not_active Ceased
- 2016-07-13 CN CN201680086461.2A patent/CN109312424A/zh active Pending
- 2016-07-13 US US16/317,394 patent/US20190308247A1/en not_active Abandoned
- 2016-07-13 MX MX2019000450A patent/MX2019000450A/es unknown
- 2016-07-13 WO PCT/CN2016/089874 patent/WO2018010108A1/zh not_active Ceased
- 2016-07-13 JP JP2019501516A patent/JP6977021B2/ja active Active
Patent Citations (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN1236177A (zh) * | 1993-04-26 | 1999-11-24 | 卡伯特公司 | 电容器级钽粉、由其得到的电容器及其在制造电容器阳极中的应用 |
| CN1433485A (zh) * | 2000-02-08 | 2003-07-30 | 卡伯特超金属株式会社 | 含氮的钽或铌粉末的制备和固体电解质电容器 |
| JP2002030301A (ja) * | 2000-07-12 | 2002-01-31 | Showa Kyabotto Super Metal Kk | 窒素含有金属粉末およびその製造方法ならびにそれを用いた多孔質焼結体および固体電解コンデンサ |
| CN1872461A (zh) * | 2001-08-15 | 2006-12-06 | 卡伯特超金属株式会社 | 含氮金属粉末及其制造方法和采用该粉末的多孔质烧结体及固体电解电容器 |
| CN101234425A (zh) * | 2008-01-11 | 2008-08-06 | 宁夏东方钽业股份有限公司 | 含氮均匀的阀金属粉末及其制造方法,阀金属坯块和阀金属烧结体以及电解电容器的阳极 |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN115223798A (zh) * | 2022-07-29 | 2022-10-21 | 长春维鸿东光电子器材有限公司 | 一种轴向引出有机高分子钽固定电容器的制造方法 |
Also Published As
| Publication number | Publication date |
|---|---|
| KR20190028745A (ko) | 2019-03-19 |
| EP3486338A4 (en) | 2020-02-26 |
| IL264192B1 (en) | 2023-08-01 |
| CN109312424A (zh) | 2019-02-05 |
| RU2019103885A3 (enExample) | 2020-08-13 |
| EP3486338B1 (en) | 2023-06-21 |
| IL264192B2 (en) | 2023-12-01 |
| US20190308247A1 (en) | 2019-10-10 |
| JP2019527300A (ja) | 2019-09-26 |
| JP6977021B2 (ja) | 2021-12-08 |
| IL264192A (enExample) | 2019-02-28 |
| RU2019103885A (ru) | 2020-08-13 |
| MX2019000450A (es) | 2019-09-23 |
| RU2734851C2 (ru) | 2020-10-23 |
| EP3486338A1 (en) | 2019-05-22 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP6977021B2 (ja) | 薄片状タンタル粉末およびその調製方法 | |
| CN117020215B (zh) | 采用碱土金属还原氧化钽生产电容器用钽粉的方法 | |
| CN104858436B (zh) | 高可靠高比容电解电容器用钽粉的制备方法 | |
| CN103894601B (zh) | 一种改善了耐电压性能的高压钽粉末的制备方法 | |
| CN114210973B (zh) | 一种钽粉的生产方法以及由该方法得到的钽粉 | |
| JPH07508618A (ja) | 改良されたタンタル粉末の製造方法及びその粉末から得られる高キャパシタンスで電気漏れの少ない電極 | |
| JP2014015683A (ja) | 金属粉末の熱処理方法およびそれにより製造された製品 | |
| CZ305376B6 (cs) | Nitridovaný práškový kov s nízkým elektrochemickým potenciálem, způsob jeho výroby a anoda kondenzátoru s jeho obsahem | |
| EP3184205B1 (en) | Preparation method for composite tantalum powder | |
| JP2002206105A (ja) | タンタル粉末の製法、タンタル粉末およびタンタル電解コンデンサ | |
| KR20260053523A (ko) | 고전압 탄탈륨 분말과 이의 제조 방법, 및 커패시터 애노드 | |
| WO2013058018A1 (ja) | コンデンサの陽極体の製造方法 | |
| CN1478287A (zh) | 用于电容器的粉末、其烧结体及使用该烧结体的电容器 | |
| CN104209511A (zh) | 一种耐高压钽粉及其制备方法 | |
| JP4986272B2 (ja) | ニオブ粉、その焼結体及びコンデンサ | |
| JPWO2001081029A1 (ja) | ニオブ粉、その焼結体及びコンデンサ | |
| CN103878364A (zh) | 一种改善了耐电压性能的中压钽粉的制备方法 | |
| CN106392060A (zh) | 一种混合钽粉及其制备方法 | |
| CN104209512B (zh) | 一种中压钽粉及其制备方法 | |
| WO2013172453A1 (ja) | コンデンサ素子の製造方法 | |
| WO2013094252A1 (ja) | タングステンコンデンサの陽極及びその製造方法 | |
| CN118492364A (zh) | 一种耐高电压钽粉末的团化方法、由该方法制备的钽粉末以及由该钽粉末制备的电容器 | |
| JPWO2015107749A1 (ja) | タングステン固体電解コンデンサ素子の製造方法 | |
| CN118832171A (zh) | 一种高压钽粉的制备方法、由该钽粉制备的阳极和电容器 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 16908436 Country of ref document: EP Kind code of ref document: A1 |
|
| ENP | Entry into the national phase |
Ref document number: 2019501516 Country of ref document: JP Kind code of ref document: A |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| ENP | Entry into the national phase |
Ref document number: 20197004021 Country of ref document: KR Kind code of ref document: A |
|
| ENP | Entry into the national phase |