WO2001042230A1 - Process for the elimination of materials containing hydrolyzable halides and other high molecular weight materials from epihalohydrin derived epoxy resins - Google Patents

Process for the elimination of materials containing hydrolyzable halides and other high molecular weight materials from epihalohydrin derived epoxy resins Download PDF

Info

Publication number
WO2001042230A1
WO2001042230A1 PCT/US2000/009622 US0009622W WO0142230A1 WO 2001042230 A1 WO2001042230 A1 WO 2001042230A1 US 0009622 W US0009622 W US 0009622W WO 0142230 A1 WO0142230 A1 WO 0142230A1
Authority
WO
WIPO (PCT)
Prior art keywords
epoxy
process according
product
ppm
base
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/US2000/009622
Other languages
English (en)
French (fr)
Inventor
Roger A. Mader
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
3M Innovative Properties Co
Original Assignee
3M Innovative Properties Co
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 3M Innovative Properties Co filed Critical 3M Innovative Properties Co
Priority to JP2001543530A priority Critical patent/JP4907821B2/ja
Priority to EP00925924A priority patent/EP1244644B1/en
Priority to DE60028825T priority patent/DE60028825T2/de
Publication of WO2001042230A1 publication Critical patent/WO2001042230A1/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G59/00—Polycondensates containing more than one epoxy group per molecule; Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups
    • C08G59/14—Polycondensates modified by chemical after-treatment
    • C—CHEMISTRY; METALLURGY
    • C07—ORGANIC CHEMISTRY
    • C07D—HETEROCYCLIC COMPOUNDS
    • C07D301/00—Preparation of oxiranes
    • C07D301/32—Separation; Purification
    • C—CHEMISTRY; METALLURGY
    • C07—ORGANIC CHEMISTRY
    • C07D—HETEROCYCLIC COMPOUNDS
    • C07D303/00—Compounds containing three-membered rings having one oxygen atom as the only ring hetero atom
    • C07D303/02—Compounds containing oxirane rings
    • C07D303/12—Compounds containing oxirane rings with hydrocarbon radicals, substituted by singly or doubly bound oxygen atoms
    • C07D303/18—Compounds containing oxirane rings with hydrocarbon radicals, substituted by singly or doubly bound oxygen atoms by etherified hydroxyl radicals
    • C07D303/20—Ethers with hydroxy compounds containing no oxirane rings
    • C07D303/24—Ethers with hydroxy compounds containing no oxirane rings with polyhydroxy compounds
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G59/00—Polycondensates containing more than one epoxy group per molecule; Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G59/00—Polycondensates containing more than one epoxy group per molecule; Macromolecules obtained by polymerising compounds containing more than one epoxy group per molecule using curing agents or catalysts which react with the epoxy groups
    • C08G59/02—Polycondensates containing more than one epoxy group per molecule
    • C08G59/025—Polycondensates containing more than one epoxy group per molecule characterised by the purification methods used
    • Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y10—TECHNICAL SUBJECTS COVERED BY FORMER USPC
    • Y10S—TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y10S525/00—Synthetic resins or natural rubbers -- part of the class 520 series
    • Y10S525/93—Reaction product of a polyhydric phenol and epichlorohydrin or diepoxide, having a molecular weight of over 5,000, e.g. phenoxy resins

Definitions

  • This invention relates to a process for the elimination of undesirable materials from epihalohydrin-derived epoxy resins. More particularly, this invention relates to a process for eliminating materials containing hydrolyzable halides and other high molecular weight materials including those containing hydroxyl functionality from epihalohydrin derived epoxy resins.
  • epichlorohydrin Particularly useful in the preparation of epoxy resins is epichlorohydrin.
  • a dihydric phenol or other active-hydrogen containing material
  • epichlorohydrin is often reacted with epichlorohydrin in the presence of a catalyst.
  • the resulting products include the desired epoxy, high molecular weight materials including oligomers, residual epichlorohydrin, and other contaminants containing hydrolyzable chloride, etc.
  • the preparation of pure epoxies is desirable.
  • High molecular weight materials such as, for example, oligomers or materials containing hydroxyl functionality, may interfere with the epoxy's performance.
  • epihalohydrin-derived epoxies are in the electronics area. Some electronic applications where these epoxies are used include, but are not limited to, conformal coatings, high pressure laminations, castings, die attach adhesives, electrical pottings, encapsulations, and underfills. Hydrolyzable halide is a source of free halide in the presence of moisture. Thus, corrosion caused by a halide is a critical issue in the manufacture of electronic devices. Therefore, elimination of hydrolyzable halides is desirable.
  • Several methods or processes are known for purifying or isolating epoxies. One of these methods is using one or more separation processes such as stripping or distillation.
  • Another method is reacting an alkali metal hydroxide solution or other solvent-based system and water-washing to remove the free chloride or phenolic salts.
  • various methods or processes are known which reduce the amount of hydrolyzable halide in the epoxy product. For example, many methods have been described for the preparation of resins with low levels of hydrolyzable chloride. (See for example, U.S. Patent No. 4,485,221). However, most of these methods involve extraction with an aqueous base and require organic solvents which add expense and decrease process efficiency.
  • the present invention provides a process for eliminating hydrolyzable halides and high molecular weight materials from epihalohydrin-derived epoxies. This process can be conducted by the epoxy manufacturer, or can be conducted on a commercially sold epoxy to reduce the level of or to eliminate hydrolyzable halide and high molecular weight materials present.
  • the present invention comprises a process for eliminating hydrolyzable halides and high molecular weight materials from epihalohydrin-derived epoxy resins comprising the steps of: a) reacting an epoxy resin comprising materials containing hydrolyzable halides with a base wherein said base is present in a quantity which exceeds the molar equivalent based on the materials containing hydrolyzable halide; b) heating the mixture while agitating; c) neutralizing said heated mixture with carbon dioxide to form a crude product; and d) distilling said crude product using molecular distillation to yield a product.
  • Another embodiment of the present invention is a process for eliminating hydrolyzable halides and high molecular weight materials from epihalohydrin-derived epoxy resins comprising the steps of: a) distilling an epoxy resin comprising materials containing hydrolyzable halide using molecular distillation to yield an epoxy distillate; and b) reacting said epoxy distillate with a base wherein said base is present in a quantity which exceeds the molar equivalent based on the materials containing hydrolyzable halide.
  • Another embodiment of the present invention is an epoxy product formed using said contaminant elimination process.
  • the epoxy product formed advantageously has low hydrolyzable halide content. Additionally, the epoxy product can have an epoxide equivalent weight at or near the theoretical value.
  • Yet another embodiment of the present invention is an epoxy derived from epihalohydrin which has low hydrolyzable halide content and which does not contain high molecular weight material.
  • the process of the present invention is solvent-free, relatively inexpensive, versatile, and environmentally-friendly. Moreover, the process of the present invention can be carried out using standard manufacturing equipment and in high volume.
  • the process of the present invention can be done in batch or as a continuous process.
  • the present invention provides a process for eliminating undesirable materials from epoxy resins which are derived from epihalohydrin. These undesirable materials or by-products are defined herein as including materials comprising hydrolyzable halides
  • High molecular weight materials are defined herein as dimers and other materials having a molecular weight greater than the dimer. These high molecular weight materials can be oligomers which can contain hydroxyl groups. Other high molecular weight materials include, but are not limited to, reaction by-products, polymerized epoxies, phenolic salts, etc., and mixtures thereof. Examples of some high molecular weight materials which may be eliminated from some epoxy resins include, but are not limited to:
  • the process of the present invention has many advantages.
  • this process is a relatively inexpensive procedure for preparing epoxy resins which contain very low levels (that is, 0.1 ppm to 100 ppm, preferably less than 10 ppm, and more preferably less than 1 ppm) of hydrolyzable halide.
  • the epoxies of the present invention have an epoxide equivalent weight at or near the theoretical value expected for the specific monomer.
  • low molecular weight halide epoxies such as EPONTM Resin 828 (and its high purity version EPONTM Resin 825), available from Shell Chemical Company, Houston, Texas, is disclosed as having an epoxide equivalent weight of 185-192 (175-180 for EPONTM Resin 825) whereas the theoretical epoxide equivalent weight is 170. (See Shell Resins, SC:235-
  • the process of the present invention is versatile. To purify different epoxy resins, one only needs to change the base in light of the starting epoxy resin. Therefore, the equipment, etc., can remain the same which helps to reduce cost. Further, the required equipment is readily available in the chemical industry.
  • the process advantageously eliminates oligomers and other high molecular weight materials including those high molecular weight materials containing hydroxyl groups which may not be desirable. Side reactions caused by contaminants are substantially or all-together eliminated. This may improve optical clarity and lower the molecular weight which affects the rheological properties of the epoxy and the resultant glass transition temperature of the cured epoxy. Depending on the curative employed, this elimination of by-products containing hydroxyl groups may provide enhanced pot life for the epoxy resin which is advantageous in many applications.
  • Epoxy-resin The epoxy resin that is purified using the present invention includes any epoxy resin which is derived from epihalohydrin or which contains hydrolyzable halides.
  • epoxy resin must be distillable using molecular distillation. Therefore, the epoxy resin must not decompose during the distillation process.
  • the epoxy resins suitable for the present invention can contain materials containing hydrolyzable halides.
  • epoxy resins having hydrolyzable halide contents of 10,000 ppm and epoxy resins having hydrolyzable halide contents of 150 ppm are suitable for the process of the present invention.
  • the epoxy resins of the present invention may include other high molecular weight materials that can contain hydroxyl groups.
  • One example of an epoxy resin suitable for the process of the present invention can be prepared as illustrated below.
  • This epoxy resin contains the desired bisphenol A epoxy product, as well as 1 ,2 chlorohydrin (containing hydrolyzable chloride), and 1 ,3 chlorohydrin
  • epoxy resins useful in the process of the present invention include, but are not limited to, bisphenol A-epichlorohyd ⁇ n epoxy resins, bisphenol F- epichlorohydrin epoxy resins, aliphatic mono glycidyl ethers, aliphatic diglycidyl ethers, aliphatic multifunctional glycidyl ethers, and aliphatic glycidyl esters
  • Examples of useful bisphenol A-epichlorohyd ⁇ n epoxy resins include, but are not limited to, EPONTM Resins 825, 826 and 828, available from Shell Chemical Company, Houston Texas, D E R TM 330, 331, and 332, available from Dow Chemical Company, Midland, Michigan, and ARALDITETM GY 6008, GY 6010, and GY 2600, available from
  • Examples of useful bisphenol F-epichlorohyd ⁇ n epoxy resins include, but are not limited to, EPONTM Resin 862, available from Shell Chemical Company, Houston, Texas, and ARALDITETM GY 281 , GY 282, GY 285, PY 306, and PY 307, available from Ciba Specialty Chemicals, Brewster, New York
  • Examples of useful mono, di and multifunctional glycidyl ether resins include, but are not limited to, HELOXYTM Modifier 107 and HELOXYTM Modifier 48, available from Ciba Specialty Chemicals, Brewster, New York, and EPONTM 1510, available from Shell Chemical Company, Houston Texas Materials having groups which are sensitive to hydrolysis by strong bases such as epoxies having ester linkage are also suitable for the process of the present invention For example, CYTM 184, available from Ciba Specialty Chemicals, Brewster, New York, is suitable for the process of the present invention
  • the process of the present invention comprises the step of treatment of or the reaction of the epoxy resin with a base
  • the base is present in an amount which exceeds the molar equivalent based on the materials comprising hydiolyzable halide This amount depends on the starting epoxy resin For example, if no other acids are present, a theoretical amount of base can be used based on the ppm of hydrolyzable halide In othei situations, for example, 100 percent to 200 percent base is required
  • the epoxy resin may be combined with a base at room temperature to form a mixture or in other situations, the epoxy resin may be pre-heated. Thus, the heating and agitation step may occur prior to and during the reaction with the base, simultaneously with the base treatment step, or after the base is added to the epoxy resin. This order is dictated by the starting epoxy resin.
  • suitable bases include, but are not limited to, hydroxides such as potassium hydroxide in water, sodium hydroxide, and lithium hydroxide, hydrides such as lithium hydride, sodium hydride (optionally in mineral oil), and potassium hydride, alkoxides such as primary, secondary, and tertiary (for example, potassium t-butoxide in THF) alkoxides such as sodium ethoxide, carbonates such as potassium carbonate and sodium carbonate, and quaternary ammonium salts.
  • hydroxides such as potassium hydroxide in water, sodium hydroxide, and lithium hydroxide
  • hydrides such as lithium hydride, sodium hydride (optionally in mineral oil), and potassium hydride
  • alkoxides such as primary, secondary, and tertiary (for example, potassium t-butoxide in THF) alkoxides such as sodium ethoxide
  • carbonates such as potassium carbonate and sodium carbonate
  • quaternary ammonium salts such as
  • the base strength and the temperature are such that the halohydrin closes to the epoxy and under which the epoxy does not polymerize.
  • potassium t-butoxide in THF was suitable at
  • non-nucleophilic bases such as sodium hydride are believed to have the advantageous effect of closing the halohydrin without reacting appreciably with other base (hydrolytically) sensitive functionality such as esters. Without being bound by theory, the following is believed to occur:
  • the process of the present invention preferably comprises the following steps: (a) distilling an epoxy resin comprising materials containing hydrolyzable halide using molecular distillation to yield an epoxy distillate; and (b) reacting said epoxy distillate with a base wherein said base is present in a quantity which exceeds the molar equivalent based on the materials containing hydrolyzable halide.
  • the initial distillation step removes moisture along with high molecular weight materials containing hydroxyl functionality.
  • the product can either be neutralized with water and carbon dioxide to remove residual sodium hydride before distillation or can be distilled directly without neutralization.
  • the mixture is heated to a temperature suitable for reaction of the halohydrin to form the epoxy while agitated.
  • the mixture may be heated using a heat mantel.
  • the mixture is heated between 20 °C to 200 °C for 1 minute to 12 hours.
  • the temperature and time depend upon the starting epoxy resin, base strength and solubility, the catalytic activity of the base towards epoxy polymerization, and commercial viability. This heating and mixing can occur a ter the epoxy resin and base are combined, prior to and during the base treatment step, or simultaneously with the addition of the base and base treatment step.
  • the mixture is usually heated to alter the viscosity which in turn helps the dispersion of the base.
  • the heated mixture is then neutralized, if required, using carbon dioxide to form a crude product. With the hydrides, this neutralization step may not be required. Optionally, at this point, residual salts may be removed from the crude product by filtration.
  • the crude product is isolated by molecular distillation to yield the product.
  • a rolled film evaporator or wipe film evaporator may be used.
  • the crude product is distributed across a vertical heated surface by an efficient, self-cleaning roller wiper system into a uniform thin film.
  • the evaporated material travels a short distance to an internal condenser.
  • a smaller vacuum is used with low operating temperatures. (See UIC Inc., "Short Path Vacuum Distillation from Laboratory to Production", 1997).
  • a wipe film evaporator a wiper is used instead of the self-cleaning roller wiper.
  • the distillation conditions depend on the boiling point of the crude product.
  • Noncondensible materials which may be in the starting materials, that is, the epoxy resin, are removed during molecular distillation.
  • the yielded epoxy product has low levels of hydrolyzable halide, that is, from 1 to 100 ppm, preferably less than 10 ppm, more preferably less than 1 ppm.
  • the yielded product is preferably free of high molecular weight materials.
  • High molecular weight material-free is defined herein as having no dimers and materials having higher molecular weight than the dimer.
  • the epoxide equivalent weight is at or near the theoretical epoxide equivalent weight (that is, within 2 percent, preferably within 1 percent of the theoretical epoxide equivalent weight)
  • the epoxy product of the present invention has a higher cured glass transition temperature than the less pure version which is advantageous
  • the epoxy product of the present invention is also more predictable due to product consistency
  • the viscosity is lower than the less pure version of the same epoxy resin
  • Residual base may inhibit cationically cured epoxies
  • Other low hydrolyzable halide epoxy resins such as EPONTM Resin 1462, available from Shell Chemical Company, which have some residual base are described as having a yellow color (a Gardner Color Scale value of less than 3)
  • the epoxy product of the present invention is colorless For example, using the Gardner test (ASTM D1544- 80), the Gardner Color Scale value is less than 0 1 for EPONTM Resin 828
  • the process of the present invention can be batch or continuous
  • the epoxy products of the present invention are suitable in optical applications where clarity is an important property As indicated above, a low Gardner Color value is obtainable
  • the epoxy products of the present invention are suitable as a primer for other epoxy materials for aircraft and automotive applications where corrosion resistance may be important Additionally, these epoxy products may be particularly useful as either a primer or adhesive on other metallic surfaces where corrosion is an issue
  • the epoxy products of the present invention are also particularly suitable for high temperature applications where a high glass transition temperature is desirable
  • the test method used to determine the hydrolyzable chloride content in epoxy resins utilizes ion chromatography and is based on ASTM D 1726-90.
  • the test procedure was as follows: A boiled-out (18 Mohm water), empty 250 mL iodine flask was electronically tared. The epoxy sample (6 - 8 grams) was added to the flask, and the weight was recorded to the nearest 0.0001 gram. Blanks were carried, but with no sample added. 50 mL of THF and 10 mL of 0.1 N KOH/MeOH were added to the flask, and the mixture was heated at reflux for about 30 minutes and cooled to room temperature. 20 mL ultrapure water was added next along with 2.00 mL of NaCl solution (0.005 N) by means of a pipette. The solvents were then evaporated by gently heating via steamplate at about
  • the test procedure for determining epoxide equivalent weight uses a stable titrant, perchloric acid which generates hydrobromic acid in situ by its action on either tetrabutylammonium bromide or tetrabutylammonium iodide.
  • a weighed sample of 0.5-0.9 meq epoxy in 50 ml chloroform is dissolved.
  • 10 ml of 10 percent tetrabutylammonium bromide (or iodide) is added and then 10-20 ml of acetic acid is added.
  • the sample is then titrated with 0.1 N HCIO4 to the potentiometric endpoint.
  • the epoxide equivalent weight was 170 (theoretical value is 170).
  • EPONTM Resin 862 (available from Shell Chemical Company) was distilled on a rolled film evaporator (model number KDL4) at about 170°C and about .001 mm vacuum. 354 grams of distillate and 178 grams of residue were obtained. The distillate was kept under a nitrogen atmosphere and transferred to a flask equipped with a mechanical stirrer, nitrogen inlet, and temperature probe. 0.56 grams of 60 percent sodium hydride in mineral oil was added to the flask and the mixture was heated to about 80°C at which point there was a slow evolution of hydrogen gas. The temperature was increased to about 100°C and the mixture was held at that temperature until no more gas evolution was detected (about two hours).
  • Example 3 The reaction mixture was cooled to about 70°C and dry ice added followed by 0.4 milliliters of water. More dry ice was added and the mixture cooled to room temperature.
  • the crude product was distilled on a rolled film evaporator at about 170°C and about .001 mm vacuum to give 214 grams of clear product.
  • the level of hydrolyzable chloride was reduced from 126 ppm to ⁇ .5 ppm as analyzed using the method disclosed in Example 1. Using the analysis method of Example 1, the epoxide equivalent weight was 157.8 (theoretical value is 157).
  • Example 3 The level of hydrolyzable chloride was reduced from 126 ppm to ⁇ .5 ppm as analyzed using the method disclosed in Example 1. Using the analysis method of Example 1, the epoxide equivalent weight was 157.8 (theoretical value is 157).
  • Heloxy Modifier 107 (337 grams) was treated with 0.53 grams of 60 percent sodium hydride in mineral oil and heated to about 80 °C for about 7 hours. Work-up with dry ice and water as described in the previous examples gave a crude product which was distilled on a rolled film evaporator (model number
  • Example 6 In a 1 liter three-neck round bottom flask, equipped with a mechanical stirrer, nitrogen inlet, and temperature probe, was added 650 grams of D.E.R. 313M (407 ppm hydrolyzable chloride) available from Dow Chemical Company, Midland, Michigan. This mixture was heated to about 70 °C and a premix of 4.0 grams of 50 percent aqueous potassium hydroxide was added. The resulting mixture was heated for about 4 hours and then dry ice was added and the mixing continued for about 30 minutes. This mixture was then cooled to room temperature. This gave a crude product which was distilled on a rolled film evaporator (model number KDL4) at about 185 °C at about .001 mm vacuum to give 433 grams of clear colorless material. Analysis showed that the hydrolyzable chloride was reduced to 13.9 ppm using the analysis method disclosed in Example 1. Using the analysis method of Example 1, the epoxide equivalent weight was 166.7 (theoretical value is 170).

Landscapes

  • Chemical & Material Sciences (AREA)
  • Organic Chemistry (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • General Chemical & Material Sciences (AREA)
  • Epoxy Resins (AREA)
  • Epoxy Compounds (AREA)
PCT/US2000/009622 1999-12-07 2000-04-11 Process for the elimination of materials containing hydrolyzable halides and other high molecular weight materials from epihalohydrin derived epoxy resins Ceased WO2001042230A1 (en)

Priority Applications (3)

Application Number Priority Date Filing Date Title
JP2001543530A JP4907821B2 (ja) 1999-12-07 2000-04-11 加水分解性ハロゲン化物および他の高分子量材料を含有する材料をエピハロヒドリン誘導エポキシ樹脂から除去する方法
EP00925924A EP1244644B1 (en) 1999-12-07 2000-04-11 Process for the elimination of materials containing hydrolyzable halides and other high molecular weight materials from epihalohydrin derived epoxy resins
DE60028825T DE60028825T2 (de) 1999-12-07 2000-04-11 Verfahren zur entfernung von hydrolysierbare halogenide enthaltenden materialien und von anderen hochmolekularen materialien aus von epihalohydrin abgeleiteten epoxyharzen

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
US45455899A 1999-12-07 1999-12-07
US09/454,558 1999-12-07

Publications (1)

Publication Number Publication Date
WO2001042230A1 true WO2001042230A1 (en) 2001-06-14

Family

ID=23805102

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/US2000/009622 Ceased WO2001042230A1 (en) 1999-12-07 2000-04-11 Process for the elimination of materials containing hydrolyzable halides and other high molecular weight materials from epihalohydrin derived epoxy resins

Country Status (6)

Country Link
US (1) US6620907B2 (enExample)
EP (1) EP1244644B1 (enExample)
JP (1) JP4907821B2 (enExample)
KR (1) KR100693849B1 (enExample)
DE (1) DE60028825T2 (enExample)
WO (1) WO2001042230A1 (enExample)

Cited By (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US6620907B2 (en) 1999-12-07 2003-09-16 3M Innovative Properties Company Process for the elimination of materials containing hydrolyzable halides and other high molecular weight materials from epihalohydrin derived epoxy resins
US9456513B2 (en) 2009-02-25 2016-09-27 3M Innovative Properties Company Article with gasket having moisture transmission resistivity and method

Families Citing this family (25)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
AU2003234394A1 (en) * 2002-05-23 2003-12-12 3M Innovative Properties Company Nanoparticle filled underfill
US6777460B2 (en) * 2002-12-23 2004-08-17 3M Innovative Properties Company Curing agents for cationically curable compositions
JP2005314512A (ja) * 2004-04-28 2005-11-10 Japan Epoxy Resin Kk 液状エポキシ樹脂およびその製造方法、エポキシ樹脂組成物およびその硬化体
US7491287B2 (en) * 2006-06-09 2009-02-17 3M Innovative Properties Company Bonding method with flowable adhesive composition
US20080152921A1 (en) * 2006-12-20 2008-06-26 3M Innovative Properties Company Thermally B-Stageable Composition for Rapid Electronic Device Assembly
US20110039982A1 (en) * 2008-05-22 2011-02-17 Hefner Jr Robert E Epoxy resins and processes for preparing the same
JP2012219081A (ja) * 2011-04-12 2012-11-12 Toray Fine Chemicals Co Ltd 高純度ジグリシジルアミン系エポキシ化合物およびその製造方法
JP5951963B2 (ja) * 2011-11-07 2016-07-13 旭化成株式会社 エポキシ樹脂の製造方法及び該製造方法を用いて得られたエポキシ樹脂
JP2014040508A (ja) * 2012-08-21 2014-03-06 Asahi Kasei E-Materials Corp エポキシ樹脂の製造方法
JP2014065835A (ja) * 2012-09-26 2014-04-17 Asahi Kasei E-Materials Corp エポキシ樹脂の製造方法
CN105793312A (zh) * 2013-12-18 2016-07-20 蓝立方知识产权有限责任公司 蒸馏酚醛环氧树脂
US9695271B2 (en) * 2013-12-18 2017-07-04 Blue Cube Ip Llc Distilled epoxy novolac resins
EP3350284B1 (en) 2015-09-15 2019-02-27 3M Innovative Properties Company Additive stabilized composite nanoparticles
CN108026444B (zh) 2015-09-15 2020-08-04 3M创新有限公司 添加剂稳定的复合纳米粒子
EP3377591A1 (en) 2015-11-18 2018-09-26 3M Innovative Properties Company Copolymeric stabilizing carrier fluid for nanoparticles
CN108699433B (zh) 2016-02-17 2020-08-14 3M创新有限公司 具有稳定含氟化合物共聚物的量子点
KR20220065086A (ko) 2016-04-01 2022-05-19 쓰리엠 이노베이티브 프로퍼티즈 컴파니 플루오로케미칼 안정화제를 갖는 양자점
WO2017200824A1 (en) 2016-05-20 2017-11-23 3M Innovative Properties Company Quantum dots with mixed amine and thiol ligands
CN109476986B (zh) 2016-07-20 2022-07-01 3M创新有限公司 用于量子点的稳定苯乙烯聚合物
KR20190031505A (ko) 2016-07-20 2019-03-26 쓰리엠 이노베이티브 프로퍼티즈 컴파니 양자점을 위한 안정화 스티렌계 중합체
WO2018052777A1 (en) 2016-09-14 2018-03-22 3M Innovative Properties Company Fast curing optical adhesive
WO2018167645A1 (en) 2017-03-14 2018-09-20 3M Innovative Properties Company Additive stabilized composite nanoparticles
JP7595404B2 (ja) * 2019-03-07 2024-12-06 味の素株式会社 樹脂組成物
CN118515631A (zh) * 2023-02-20 2024-08-20 中国石油化工股份有限公司 一种双酚a二缩水甘油醚的分离纯化方法
WO2026110649A1 (ja) * 2024-11-22 2026-05-28 株式会社Adeka エポキシ樹脂、エポキシ樹脂の製造方法、エポキシ蒸留物、エポキシ蒸留物の製造方法、硬化性組成物、硬化物及び硬化物の製造方法

Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0028810A2 (en) * 1979-11-08 1981-05-20 The Dow Chemical Company Solvent-free process for preparing liquid epoxy resins
EP0303901A2 (en) * 1987-08-13 1989-02-22 The Dow Chemical Company Method for reducing the aliphatic halide content of epoxy resins
EP0441284A2 (en) * 1990-02-08 1991-08-14 The Dow Chemical Company Process for reducing the undesirable halide content of epoxyresins
WO1997044335A1 (en) * 1996-05-21 1997-11-27 Exxon Chemical Patents Inc. Purification of glycidyl esters by thin film evaporation

Family Cites Families (20)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
DE203056C (enExample)
US3213113A (en) 1965-10-19 Removal of aldehydes from ethylene oxide
US3309384A (en) 1961-10-02 1967-03-14 Celanese Coatings Co Preparation of low viscosity epoxide resins
US3291758A (en) 1963-05-31 1966-12-13 Gen Electric Superconductive materials
US3417050A (en) 1965-05-04 1968-12-17 Celanese Coatings Co Epoxide resin process
GB1509354A (en) * 1976-04-24 1978-05-04 Maruzen Oil Co Ltd Process for purifying halogenated alkenyl-phenol polymers
US4395542A (en) 1982-01-19 1983-07-26 Ciba-Geigy Corporation Process for removing trace amounts of epichlorohydrin from heat sensitive glycidyl products
US4447598A (en) 1983-04-07 1984-05-08 The Dow Chemical Company Method of preparing epoxy resins having low hydrolyzable chloride contents
US4485221A (en) 1983-11-03 1984-11-27 Ciba-Geigy Corporation Process for making epoxy novolac resins with low hydrolyzable chlorine and low ionic chloride content
US4535150A (en) 1984-12-04 1985-08-13 Celanese Corporation Process for preparing epoxy resins having low hydrolyzable chlorine contents
US4668807A (en) 1984-12-21 1987-05-26 Ciba-Geigy Corporation Process for reducing the content of hydrolyzable chlorine in glycidyl compounds
US4810776A (en) 1986-07-14 1989-03-07 Ciba-Geigy Corporation Process for producing epoxy resin having a low-EHC-content from chlorine-substituted crude epoxy resin of high EHC-content and apparatus for automatically controlling such process
US4829104A (en) 1986-07-18 1989-05-09 The Dow Chemical Company Controlled film build epoxy coatings applied by cathodic electrodeposition
US4895755A (en) 1986-09-15 1990-01-23 The Dow Chemical Company Halogenated advanced epoxy resins
JPH0368568A (ja) 1989-08-09 1991-03-25 Nissan Chem Ind Ltd 低塩素含有エポキシ化合物の製造方法
JPH0662596B2 (ja) * 1990-04-19 1994-08-17 ダイソー株式会社 エポキシ化合物の精製方法
JPH05331155A (ja) * 1992-06-01 1993-12-14 Sanyo Chem Ind Ltd グリシジルエーテルの製造法
JP3811831B2 (ja) * 1996-07-04 2006-08-23 東都化成株式会社 ビスフェノール型固形エポキシ樹脂、その製造方法及び塗料組成物
JPH11269159A (ja) * 1998-03-20 1999-10-05 New Japan Chem Co Ltd グリシジル化合物の精製方法
WO2001042230A1 (en) 1999-12-07 2001-06-14 3M Innovative Properties Company Process for the elimination of materials containing hydrolyzable halides and other high molecular weight materials from epihalohydrin derived epoxy resins

Patent Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0028810A2 (en) * 1979-11-08 1981-05-20 The Dow Chemical Company Solvent-free process for preparing liquid epoxy resins
EP0303901A2 (en) * 1987-08-13 1989-02-22 The Dow Chemical Company Method for reducing the aliphatic halide content of epoxy resins
EP0441284A2 (en) * 1990-02-08 1991-08-14 The Dow Chemical Company Process for reducing the undesirable halide content of epoxyresins
WO1997044335A1 (en) * 1996-05-21 1997-11-27 Exxon Chemical Patents Inc. Purification of glycidyl esters by thin film evaporation

Cited By (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US6620907B2 (en) 1999-12-07 2003-09-16 3M Innovative Properties Company Process for the elimination of materials containing hydrolyzable halides and other high molecular weight materials from epihalohydrin derived epoxy resins
US9456513B2 (en) 2009-02-25 2016-09-27 3M Innovative Properties Company Article with gasket having moisture transmission resistivity and method

Also Published As

Publication number Publication date
JP4907821B2 (ja) 2012-04-04
US6620907B2 (en) 2003-09-16
US20020022709A1 (en) 2002-02-21
DE60028825T2 (de) 2007-01-18
EP1244644A1 (en) 2002-10-02
JP2003516399A (ja) 2003-05-13
KR100693849B1 (ko) 2007-03-13
KR20020058082A (ko) 2002-07-12
DE60028825D1 (de) 2006-07-27
EP1244644B1 (en) 2006-06-14

Similar Documents

Publication Publication Date Title
US6620907B2 (en) Process for the elimination of materials containing hydrolyzable halides and other high molecular weight materials from epihalohydrin derived epoxy resins
CA1210189A (en) Process for the preparation of epoxide resins by the advancement method
EP0103282B1 (en) A process for preparing glycidyl derivatives of compounds having at least one aromatic hydroxyl group or aromatic amine group
EP0203473A2 (en) Process for the preparation of epoxy resins
EP0091836B1 (en) A process for production of an epoxidized polyether
US4831101A (en) Polyglycidyl ethers from purified epihalohydrin
US4313886A (en) Process for preparing liquid epoxy resins
JP3644761B2 (ja) 脂肪族ポリグリシジルエーテルの製造方法
EP3122734B1 (en) Epoxy resin compositions
US4273921A (en) Water-soluble epoxy resins and process for their preparation
JPH09183829A (ja) エポキシ樹脂、エポキシ樹脂組成物及びその硬化物
US4250100A (en) Water-soluble epoxy resins and process for their preparation
US4110354A (en) Water-soluble epoxy resins and process for their preparation
JP7061538B2 (ja) ジグリシジルアミン系エポキシ化合物の精製方法
EP0028810A2 (en) Solvent-free process for preparing liquid epoxy resins
KR20050053336A (ko) 2-하이드록시아이소부티르산글리시딜의 제조방법
JPS61171728A (ja) 新規臭素含有エポキシ樹脂およびその製法
JPH09110847A (ja) 環状テルペン骨格含有モノエポキシ化合物およびこれを反応性希釈剤として使用したエポキシ樹脂組成物
JP2000143769A (ja) 液状エポキシ樹脂、液状エポキシ樹脂の製造方法、エポキシ樹脂組成物及びその硬化物
JP2022102229A (ja) エポキシ化合物の製造方法
JPH06345846A (ja) エポキシ樹脂及びその製造法、樹脂組成物及びその硬化物
JPS6424818A (ja) ノボラック型樹脂及びその製法
JP2002284841A (ja) エポキシ樹脂、エポキシ樹脂混合物、エポキシ樹脂組成物及びその硬化物
JPS5973577A (ja) ポリエポキシ化合物の製造方法
JPH07165883A (ja) エポキシ樹脂及びその製造方法

Legal Events

Date Code Title Description
AK Designated states

Kind code of ref document: A1

Designated state(s): BR CN JP KR SG

AL Designated countries for regional patents

Kind code of ref document: A1

Designated state(s): AT BE CH CY DE DK ES FI FR GB GR IE IT LU MC NL PT SE

DFPE Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed before 20040101)
121 Ep: the epo has been informed by wipo that ep was designated in this application
ENP Entry into the national phase

Ref country code: JP

Ref document number: 2001 543530

Kind code of ref document: A

Format of ref document f/p: F

WWE Wipo information: entry into national phase

Ref document number: 1020027007142

Country of ref document: KR

WWE Wipo information: entry into national phase

Ref document number: 2000925924

Country of ref document: EP

WWP Wipo information: published in national office

Ref document number: 1020027007142

Country of ref document: KR

WWP Wipo information: published in national office

Ref document number: 2000925924

Country of ref document: EP

WWG Wipo information: grant in national office

Ref document number: 2000925924

Country of ref document: EP

WWG Wipo information: grant in national office

Ref document number: 1020027007142

Country of ref document: KR