WO1998012742A1 - Semiconductor device and method of fabricating the same - Google Patents
Semiconductor device and method of fabricating the same Download PDFInfo
- Publication number
- WO1998012742A1 WO1998012742A1 PCT/JP1997/003267 JP9703267W WO9812742A1 WO 1998012742 A1 WO1998012742 A1 WO 1998012742A1 JP 9703267 W JP9703267 W JP 9703267W WO 9812742 A1 WO9812742 A1 WO 9812742A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- trench
- semiconductor substrate
- film
- oxidation
- formation surface
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- H—ELECTRICITY
- H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- H10W—GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10
- H10W10/00—Isolation regions in semiconductor bodies between components of integrated devices
- H10W10/01—Manufacture or treatment
- H10W10/011—Manufacture or treatment of isolation regions comprising dielectric materials
- H10W10/014—Manufacture or treatment of isolation regions comprising dielectric materials using trench refilling with dielectric materials, e.g. shallow trench isolations
- H10W10/0145—Manufacture or treatment of isolation regions comprising dielectric materials using trench refilling with dielectric materials, e.g. shallow trench isolations of trenches having shapes other than rectangular or V-shape
- H10W10/0147—Manufacture or treatment of isolation regions comprising dielectric materials using trench refilling with dielectric materials, e.g. shallow trench isolations of trenches having shapes other than rectangular or V-shape the shapes being altered by a local oxidation of silicon process, e.g. trench corner rounding by LOCOS
-
- H—ELECTRICITY
- H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- H10W—GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10
- H10W10/00—Isolation regions in semiconductor bodies between components of integrated devices
- H10W10/01—Manufacture or treatment
- H10W10/011—Manufacture or treatment of isolation regions comprising dielectric materials
-
- H—ELECTRICITY
- H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- H10W—GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10
- H10W10/00—Isolation regions in semiconductor bodies between components of integrated devices
- H10W10/10—Isolation regions comprising dielectric materials
-
- H—ELECTRICITY
- H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- H10W—GENERIC PACKAGES, INTERCONNECTIONS, CONNECTORS OR OTHER CONSTRUCTIONAL DETAILS OF DEVICES COVERED BY CLASS H10
- H10W10/00—Isolation regions in semiconductor bodies between components of integrated devices
- H10W10/10—Isolation regions comprising dielectric materials
- H10W10/17—Isolation regions comprising dielectric materials formed using trench refilling with dielectric materials, e.g. shallow trench isolations
Definitions
- This invention relates to a semiconductor device having a trench isolation structure having high reliability, and a method of fabricating the same.
- a LOCOS (Local Oxidation of Silicon) structure is known as a structure for electrically insulating and isolating adjacent devices on a semiconductor substrate. This structure is formed by selectively oxidizing a substrate surface to form a thick thermal oxide film, and has been employed in various semiconductor devices. However, because this LOCOS structure has low processing accuracy, it is not suitable for an insulation/isolation structure of high integration semiconductor devices such as deep submicron devices in which high processing dimensional accuracy is required for the thermal oxide film.
- a so-called "trench isolation structure" by a selective oxidation method which forms shallow trenches in the substrate surface and then selectively oxidizes the trench portions to form the thermal oxide film, has been employed in place of the LOCOS structure as the insulation/isolation structure of semiconductor devices for which high integration density is required, as described in JP-A-63-143835 , for example.
- this trench isolation structure has the advantage that it can form device isolation oxide films having smaller planar dimensions. For this reason, this method is suitable for the fabrication of deep submicron devices for which processing dimensional accuracy of 0.5 urn or below is required.
- a silicon thermal oxide film is formed by oxidizing the surface of a silicon substrate as a semiconductor substrate, for example, a large mechanical stress develops near the interface between the thermal oxide film so formed and the silicon substrate. This is because a part of the silicon substrate (Si) is oxidized and undergoes volume expansion of about twice when it changes to the thermal oxide film (Si0 2 ). When this mechanical stress increases, crystal defects such as dislocation and stacking faults are likely to occur and reliability of the semiconductor devices drops. It has been also clarified that the oxidation reaction itself (diffusion behavior of oxidizing species, reactivity on the oxidation interface, etc) is affected by the stress and the shape of the growing oxide film changes. Since the stress occurs concentratedly near the end points (corner points) of the two-dimensional or three- dimensional shape, careful attention must be paid particularly to the crystal defects and the shape change in this stress concentration field.
- Figs. 1A to ID are schematic views of a fabrication process of a trench isolation structure in a conventional selective oxidation method.
- an oxidation prevention film 3 is first deposited to a surface of a silicon substrate 1 through a pad oxide film (silicon thermal oxide film) 2, then the oxidation prevention film 3, the pad oxide film 2 and the silicon substrate 1 of the area, where a device isolation oxide film is desired to be formed, are partially removed to form a trench (Fig. IB), and the silicon thermal oxide film 5 is formed by oxidizing the trench surface.
- a gate oxide film 6 , a gate electrode 7, an inter-layer insulating film 8, a buried insulating film 9, a first layer wiring 10 and a second layer inter-layer insulating film 11 are serially formed.
- the end points (corner points) essentially exist near the trench upper end portion or the trench lower end portion of the substrate. Therefore, the stress concentration field is formed near the end point (corner point) due to thermal oxidation. Because such a stress concentration field is formed, the shape of the substrate, particularly near the trench upper end portion, is oxidized in some cases into a pointed shape 4 having an acute angle as shown in Fig. 1C.
- an electronic circuit such as transistors, capacitors, etc, is formed in a device formation area covered with the oxide protective film 3 as shown in Fig. ID. If such an acute angle portion 4 remains on the substrate surface, however, the concentration of electric field occurs at this portion during the circuit operation and deteriorates the breakdown voltage characteristics of the transistors, the capacitances, etc, that constitutes the circuit, as pointed out by A. Bryant et al . in "Technical Digest of IEDM '94", pp. 671-674.
- the present invention is directed to provide a semiconductor device which does not invite deterioration of breakdown voltage characteristics of transistors and capacitances constituting a circuit but has high reliability, and a method of fabricating such a semiconductor device.
- the object described above can be accomplished by preventing a substrate shape in the proximity of the upper end portion of a device isolation trench on a surface of a semiconductor substrate from becoming an acute angle.
- a method of fabricating a semiconductor device for accomplishing the object described above includes the following steps.
- a silicon substrate, etc, may be used as the semiconductor substrate.
- the film thickness of the oxidation prevention film must be such that all the oxide prevention films are not oxidized in the oxidation steps of the post- steps (4 ) , (7) , etc.
- a polycrystalline silicon thin film, a silicon nitride film, etc, may be used as the oxidation prevention film. Since easily oxidizable materials such as the polycrystalline silicon thin film have low restriction force to volume expansion of the new grown silicon oxide film from the silicon substrate with oxidation, the stress concentration at the trench upper end portion can be reduced. Since difficultly oxidizable materials such as the silicon nitride film have a small oxidation quantity in the oxidation process, the film thickness can be reduced.
- This trench can be formed by an ordinary lithography method using a photoresist and etching, for example .
- Step to remove corners formed by trench on circuit formation surface of semiconductor substrate This step is not always necessary, but if the corners are removed by this step, the oxidation step (7) of the post-step becomes unnecessary in most cases.
- Step to oxidize trench portion formed in semiconductor substrate The trench portion is oxidized by several to dozens of nm by oxidation. Due to this oxidation, the bird's beak is grown at the trench portion and a radius of curvature is formed at the corners at the trench upper end portion.
- Step to bury buried insulating film into oxidized trench The trench portion is oxidized by several to dozens of nm by oxidation. Due to this oxidation, the bird's beak is grown at the trench portion and a radius of curvature is formed at the corners at the trench upper end portion.
- the material used as the buried insulating film is essentially an insulating material and has a low dielectric constant.
- a material having a high dielectric constant is used, a coupling capacitance which is formed when a wiring material is deposited on this insulating film at a post-step becomes great.
- a silicon oxide film, etc, is a preferred burying material, and polycrystalline silicon or the like is not preferred.
- Step to remove buried insulating film formed on oxidation prevention film The buried insulating film is etched back by chemical-mechanical polishing (CMP) or dry etching.
- CMP chemical-mechanical polishing
- the oxidation prevention film serves as an etching stopper and has also the function of preventing etching of the semiconductor substrate below the oxidation prevention film.
- This step grows the radius of curvature of the trench upper end portion of the semiconductor substrate to a sufficient radius of curvature for preventing the increase of the leakage current.
- This oxidation step provides also the effect that the buried insulating film is made compact . This step is not necessary if the radius of curvature at the trench upper end portion of the semiconductor substrate has become sufficient to prevent the increase of the leakage current due to the oxidation step ( 4) .
- This step may be executed before the step (6) or the next step (8).
- this step is executed after the next step (8), the surface of the semiconductor substrate is simultaneously oxidized, too, but the oxide film formed on the surface of the semiconductor substrate is removed after completion of additional oxidation and in this way, the step of forming the device isolation oxide film is completed.
- the formation step of the device isolation oxide film is completed by this step. Therefore, a semiconductor device is formed by forming a circuit such as transistors on the semiconductor substrate on which the device isolation oxide film is formed.
- a semiconductor device for accomplishing the afore-mentioned objects is a semiconductor device having a device isolation oxide film which is formed on a circuit formation surface of a semiconductor substrate and is a trench isolation structure, wherein an angle ⁇ between the circuit formation surface of the semiconductor substrate and the side surface of the semiconductor substrate in a depth-wise direction of the trench constituting the trench isolation structure is within the range of 90° ⁇ ⁇ ⁇ 180°. Because this structure can prevent field concentration at the trench upper end portion, it can prevent the increase of a leakage current resulting from deterioration of withstand voltage characteristics of the circuit such as transistors and capacitances formed on the semiconductor substrate.
- the coupling capacitance of wirings constituted on the semiconductor substrate can be reduced by burying the inside of the trench by an insulating material having a low dielectric constant such as a silicon oxide, and reliability of the semiconductor device can be further improved.
- Figs. 1A, IB, 1C and ID are schematic views, each showing a fabrication process of a trench isolation structure in a selective oxidation method according to the prior art
- Figs. 2A to 2N are schematic views, each showing a fabrication process of an MOS transistor according to the first embodiment of the present invention
- Fig. 3 is a flowchart showing the fabrication process of the MOS transistor according to the first embodiment of the present invention.
- Figs. 4A to 4N are schematic views, each show- ing a fabrication process of an MOS transistor according to the second embodiment of the present invention
- Fig. 5 is a flowchart showing the fabrication process of the MOS transistor according to the second embodiment of the present invention.
- Figs. 6A to 6N are schematic views, each show- ing a fabrication process of an MOS transistor according to the third embodiment of the present invention ?
- Fig. 7 is a flowchart of the fabrication process of the MOS transistor according to the third embodiment of the present invention
- Figs. 8A to 8N are schematic views, each showing a fabrication process of an MOS transistor according to the fourth embodiment of the present invention.
- Fig. 9 is a flowchart of the fabrication process of the MOS transistor according to the fourth embodiment of the present invention.
- FIG. 2A to 2N are schematic views of the fabrication process of the MOS transistor according to the first embodiment
- Fig. 3 is a flowchart of the fabrication process of this MOS transistor.
- the fabrication process of the MOS transistor of this first embodiment is as follows.
- a surface of a silicon substrate 1 is thermally oxidized so as to form a pad oxide film 2 having a thickness of 10 to several tens of nm [Fig. 2B and Fig. 3 (101) to (102)].
- a polycrystalline silicon thin film 18 is deposited on the pad oxide film 2 to a thickness of about 10 to 200 nm [Fig. 2B, Fig. (103)].
- This poly- crystalline silicon thin film 18 is used as an oxidation prevention film when a device isolation thermal oxide film 5 is formed.
- the polycrystalline silicon film 18 may be directly deposited on the silicon substrate 1 by omitting the formation of the pad oxide film 2.
- the following description is based on the assumption that the pad oxide film 2 is formed. Therefore, the process step relating to the pad oxide film 2 is not necessary when the formation of the pad oxide film 2 is omitted.
- a photoresist 19 is formed on the polycrystalline silicon film 18 [Fig. 2B, Fig. 3 (104)].
- thermal oxide is carried out so as to form an oxide film 5 by oxidizing the trench portion formed in the surface of the silicon substrate 1 to several to dozens of nm [Figs. 2E and 2F, Fig. 3 (108) to (109)].
- a sufficient film thickness of the polycrystalline silicon thin film 18 deposited as the oxidation prevention film must be secured so that it can function as the oxidation prevention film for preventing the surface side of the polysilicon thin film 18 from being fully oxidized at the time of thermal oxidation and preventing the silicon substrate 1 below this polycrystalline silicon thin film 18 from being oxidized entirely.
- the pad oxide film 2 is preferably formed.
- an insulating film 9 such as a silicon oxide film is deposited by chemical vapor deposition, sputtering, etc, in order to completely bury the inside of the trench covered by the thermal oxidation film (hereinafter, the insulating film 9 for burying the inside of the trench will be called the "buried insulating film 9" [Fig. 2G, Fig. 3 (110)].
- the material used for this buried insulating film 9 is an insulating material and preferably has a low dielectric constant. For, when a material having a high dielectric constant is used, a coupling capacitance formed when a wiring material is deposited on this film in a post-step becomes greater.
- polycrystalline silicon as the burying material.
- the buried insulating film 9 is then etched back by chemical-mechanical polishing (CMP) or dry etching [Fig. 2G, Fig. 3 (111)].
- CMP chemical-mechanical polishing
- the polycrystalline silicon thin film 18 used as the oxidation prevention film functions as an etching stopper and plays the role of preventing the silicon substrate 1 below the polycrystalline silicon thin film 18 from being etched.
- the formation step of the device isolation oxide film is completed by removing the polycrystalline silicon thin film 18 and the pad oxide film 2 [Fig. 2H, Fig. 3 (113)].
- thermal oxidation is again carried out (hereinafter called "additional oxidation") after the buried insulating film 9 is etched back from the next product lot [Fig. 21, Fig. 3 (112)].
- a weak boundary layer of the coupling portion deposited by chemical vapor deposition or sputtering to the trench sidewalls and the upper surface of the trench exists at the trench upper end portion 12, and the oxidation seeds can diffuse at a relatively high rate along this weak boundary layer.
- the oxidation seeds are supplied to the trench upper end portion 12 within a short time (10 or more minutes at the oxidation temperature of 850°C), so that only the portions in the proximity of the trench upper end portion 12 are oxidized preferentially and the formation of the radius of curvature of the trench upper end portion 12 is promoted.
- this additional oxidation provides the effect of rendering the buried insulating film 9 compact.
- the formation step of the device isolation oxide film is completed by removing the polycrystalline silicon thin film 18 and the pad oxide film 2 [Fig. 2M, Fig. 3 (113)].
- This additional oxidation may be carried out after the polycrystalline silicon thin film 18 is removed.
- the surface of the silicon substrate 1 is simultaneously oxidized, too, but the formation step of the device isolation oxide film is completed by removing this oxide film formed on the surface of the silicon substrate 1 after the additional oxidation is completed.
- Transistor structures, etc, are formed on the silicon substrate 1 [Figs. 2J, K, L, N(h), Fig. 3 (114) to (122)].
- Conventional fabrication technologies of the transistor structure, etc, can be employed without particular limitation, and a typical fabrication proces of the MOS transistor structure will be explained next by way of example.
- These thin films can be formed by CVD, or the like, for example.
- the silicon oxide film may be formed by thermal oxidation of the silicon substrate 1.
- An impurity is implanted and a first layer wiring 10, an inter-layer insulating film 11, etc, are formed.
- an inter-layer insulating film 14, a wiring 15 and an insulting film 16 are formed, whenever necessary.
- the MOS transistor described above can be used for memory circuits such as a DRAM (Dynamic Random Access Memory) or arithmetic operation circuits such as logic devices.
- memory circuits such as a DRAM (Dynamic Random Access Memory) or arithmetic operation circuits such as logic devices.
- the first embodiment described above can prevent the acute angle portions from remaining near the trench upper end portions of the silicon substrate when the trench isolation structure is formed as the device isolation oxide film structure, can prevent the increase of the leakage current or the drop of withstand voltage characteristics of the MOS transistor resulting from the field concentration in the proximity of the gate electrode film, by forming the radius portions or the obtuse angle portions near the trench upper end portion of the silicon substrate, and can improve electrical reliability of the transistor.
- the trench upper end portion of the silicon substrate before thermal oxidation is substantially orthogonal in the first embodiment, there is the case where the radius of curvature near the trench upper end portion of the silicon substrate is not sufficient.
- FIGS. 4A to 4N are schematic views showing the fabrication process of the MOS transistor according to the second embodiment
- Fig. 5 is a flowchart of the fabrication process of the MOS transistor of this embodiment.
- the fabrication process of the MOS transistor of the second embodiment modifies the fabrication step (4) of the first embodiment in the following way. Since the fabrication steps other than the step (4) are the same as those of the first embodiment, the detailed explanation will be omitted.
- the angle of the trench sidewalls near the trench lower end portion need not always be 90 degrees and a predetermined inclination (substantially within the range of 60 to 90 degrees) [Figs. 4C, D, E, Fig. 5 (205) to (207)] may be formed.
- the etching step that is, isotropic etching and anisotropic etching, at the time of formation of the shallow trench becomes more complicated.
- the isotropic etching portion 13 is disposed at the trench upper end portion of the silicon substrate at the time of formation of the shallow trench as described above, oxidation of the trench upper end portion of the silicon substrate 1 by first thermal oxidation (formation of the radius of curvature) is promoted, and the necessity for additional oxidation becomes lower.
- FIGS. 6A to 6N are schematic views of the fabrication process of the MOS transistor according to the third embodiment and Fig. 7 is a flowchart of the fabrication process of the MOS transistor of this embodiment.
- the fabrication process of the MOS transistor according to the third embodiment is as follows. (1) The surface of the silicon substrate 1 is thermally oxidized and the pad oxide film 2 having a thickness of 10 to dozens of nm is formed [Figs. 6B, Fig. 7 (301) to (302)].
- a silicon nitride film 17 having high oxidation resistance is deposited to a thickness of 10 to 200 nm on the pad oxide film 2 [Fig. 6B, Fig. 7 (303)].
- This silicon nitride film 17 is used as an oxidation prevention film when the device isolation oxide film 5 is formed.
- the silicon nitride film 17 having high oxidation resistance may be directly formed on the silicon substrate 1 by omitting the formation of the pad oxide film 2.
- the silicon nitride film 17 is deposited through the pad oxide film 2 and te polycrystalline silicon thin film, or through only the polycrystalline silicon thin film. in either case, the silicon nitride film 17 exists on the outermost surface of the structure.
- the following description is based on the assumption that the polycrystalline silicon thin film and the pad oxide film 2 are formed. Therefore, when the formation of the polycrystalline silicon thin film and the pad oxide film 2 is omitted, the process steps relating to the polycrystalline silicon thin film and the pad oxide film 2 are not necessary.
- the photoresist 19 is formed on the silicon nitride film 17 [Fig. 6B, Fig. 7 (304)]. (4) After the photoresist 19 of the area in which the device isolation film is to be formed is removed by an ordinary lithography method, the silicon nitride film 17, the pad oxide film 2 and the polycrystlaline silicon film are removed by etching.
- the photoresist is removed, and the shallow trench is formed in the surface of the silicon substrate 1 by dry etching.
- isotropic etching is applied to the portions near the trench end portion so as to form the radius of curvature in the proximity of the trench upper end and then anisotropic etching is applied to form the trench shape having the slope portion like the isotropic etching portion 13.
- the angle of the trench sidewalls near the trench lower end portion need not always be 90 degrees, and a predetermined inclina- tion (substantially within the range of 60 to 90 degrees) may be formed, as well [Figs. 6C , D, E, Fig. 7 (305) to (308)].
- the film thickness of the silicon nitride film 17 as the oxidation prevention film must be a film thickness sufficient to function as the oxidation prevention film to prevent the silicon nitride film 17 from being completely oxidized at the time of thermal oxidation and to prevent the silicon substrate 1 below the silicon nitride film 17 from being completely oxidized.
- the film thickness can be made thinner than the polycrystalline silicon thin film 18 used in the first and second embodiments.
- the pad oxide film 2 silicon in the proximity of the upper end portion of the silicon substrate 1 keeping contact with the pad oxide film 2 and the lower end of the polycrystalline thin film are serially oxidized from the trench end, and the so-called "bird's beak" is formed, so that the radius of curvature near the upper end of the silicon substrate 1 is promoted. From this aspect, the pad oxide film 1 is preferably formed.
- the insulating film 9 such as a silicon oxide film is deposited to bury the inside of the trench by chemical vapor deposition, sputtering, etc, in order to fully bury the inside of the trench covered by the thermal oxidation film (hereinafter, the insulating film 9 for burying the inside of the trench will be called the "buried insulating film 9" [Fig. 6G, Fig. 7 (310)].
- the material used for the burying insulating film 9 is preferably a material having an insulating property and a low dielectric constant.
- a material having a high dielectric constant is used, a coupling capacitance formed when a wiring material is deposited on the film material in the post-process becomes great. From this aspect, the use of polycrystalline silicon as the burying material is not preferred.
- the formation process of the device isolation oxide film is completed by etching back the buried insulating film 9 and then removing the remaining silicon nitride film 17, polycrystalline silicon and pad oxide film 2 [Figs. 6H, I, Fig. 7 (313)].
- thermal oxidation is again carried out (hereinafter called "additional oxidation") before the buried insulating film 9 is etched back [Fig. 6L, Fig. 7 (312)]. in this case, since the buried insulating film
- oxidation proceeds from portions near the trench upper end portion 12 and the inside of the trench is hardly oxidized for the following reason. in other words, thermal oxidation inside the trench is carried out through the buried insulating film 9 but in this case, a longer time is necessary for the oxidation seeds to diffuse inside the buried insulating film 9 before reaching the silicon substrate 1 than when the silicon substrate is directly oxidized. Therefore, oxidation does not substantially proceed within a short time of several minutes near the bottom of the trench.
- a weak boundary layer of the coupling portion of the buried insulating film 9 deposited to the trench sidewalls and the trench upper surface by chemical vapor deposition or sputtering exists at the trench upper end portion 12.
- the oxidation seeds can diffuse at a relatively high rate along this weak boundary layer, so that the oxidation seeds are supplied to the trench upper end portion 12 within a short time (10 minutes or more at an oxidation temperature of 850°C), the portions near the trench upper end portion 12 are oxidized preferentially and the formation of the radius of curvature of the trench upper end portion 12 is promoted.
- the formation process of the device isolation oxide film is completed by etching back the buried insulating film 9 and then removing the remaining silicon nitride film 17, polycrystalline silicon and pad oxide film 2 [Fig. 6M, Fig. 7 (313)].
- this additional oxidation need not always be carried out before etch-back of the buried insulating film 9, and may be carried out after etch- back of the buried insulating film 9 in accordance with the product specification required for products in the same way as in the first embodiment.
- a transistor structure, etc, is formed on the silicon substrate 1 [Figs. 6J to 6N, Fig. 7 (314) to (322)].
- the silicon oxide film may be formed by the thermal oxidation of the silicon substrate 1.
- a metal film such as a tungsten film and a silicide thin film, or their laminate body, is formed, unnecessary portions are removed by etching, etc, to form the gate electrode 7.
- An impurity is implanted and a first layer wiring 10, an inter-layer insulating film 11, etc, are formed. Wirings of the second layer et seq, and an insulating film are formed further, whenever necessary.
- the MOS transistor described above can be used for memory circuits such as a DRAM (Dynamic Random Access Memory), an SRAM or arithmetic operation circuits such as logic devices (Static Random Access Memory), etc.
- the third embodiment prevents the acute angle portions from remaining in the proximity of the trench upper end portion of the silicon substrate when forming the trench isolation structure as the device isolation oxide film structure but forms the radius of curvature portion or the obtuse angle portion near the trench upper end portion of the silicon substrate. Therefore, this embodiment can prevent the increase of the leakage current of the MOS transistor or the drop of the breakdown voltage characteristics resulting from the field concentration near the end portion of the gate electrode, and can improve electrical reliability of the transistor .
- the third embodiment uses the silicon nitride film 17 having high oxidation resistance as the oxidation prevention film, the film thickness of the oxidation prevention film can be reduced, and removal of this oxidation prevention film in the final process step becomes easier.
- the etching process at the time of the formation of the shallow trench gets complicated in this third embodiment in the same way as in the second embodiment, but because the isotropic etching portion 13 is disposed at the trench upper end portion of the silicon substrate 1 when the shallow trench is formed as described above, oxidation of the trench upper end portion of the silicon substrate 1 is promoted in the initial thermal oxidation process and the necessity for additional oxidation becomes lower.
- Figs. 8A to 8N are schematic views of the fabrication process of the MOS transistor of the fourth embodiment and Fig. 9 is a flowchart of the fabrication process of the MOS transistor in this embodiment.
- the fabrication process of the MOS transistor of the fourth embodiment modifies the fabrication step (4) of the first embodiment in the following way. Since the fabrication steps other than the step (4) are the same as those of the first embodiment, the detailed explanation will be omitted.
- the photoresist in the area in which the device isolation film is to be formed is removed by an ordinary lighography method, the silicon nitride film 17, the pad oxide film 2 and the polycrystalline silicon thin film are removed by etching.
- the photoresist is removed and the shallow trench is formed in the surface of the silicon substrate 1 by dry etching.
- the angle of the trench sidewalls near the trench lower end portion need not always be 90 degrees and a predetermined inclination (substantially within the range of 760 to 90 degrees) may be formed [Figs. 8C, D, E, Fig. 9 (405) to (408)].
- the fourth embodiment uses the silicon nitride film 17 having high oxidation resistance as the oxidation prevention film in the same way as in the third embodiment, the film thickness of the oxidation prevention film can be reduced, and removal of the oxidation prevention film in the final process step becomes easier.
- the fourth embodiment can easily form the trench by anisotropic etching alone, and has high productivity.
- the embodiments of the present invention can provide a semiconductor device which does not invite deterioration of the transistors constituting the circuit and the breakdown voltage characteristics of the capacitance, and a method of fabricating the semiconductor device.
Landscapes
- Element Separation (AREA)
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP8/244445 | 1996-09-17 | ||
| JP24444596A JP3611226B2 (ja) | 1996-09-17 | 1996-09-17 | 半導体装置及びその製造方法 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO1998012742A1 true WO1998012742A1 (en) | 1998-03-26 |
Family
ID=17118766
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP1997/003267 Ceased WO1998012742A1 (en) | 1996-09-17 | 1997-09-16 | Semiconductor device and method of fabricating the same |
Country Status (6)
| Country | Link |
|---|---|
| JP (1) | JP3611226B2 (enExample) |
| KR (1) | KR100425064B1 (enExample) |
| CN (1) | CN1161837C (enExample) |
| MY (1) | MY129438A (enExample) |
| TW (1) | TW360945B (enExample) |
| WO (1) | WO1998012742A1 (enExample) |
Cited By (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO1998036452A1 (en) * | 1997-02-18 | 1998-08-20 | Hitachi, Ltd. | Semiconductor device and process for producing the same |
| WO1999044223A3 (en) * | 1998-02-27 | 1999-10-28 | Lsi Logic Corp | Process of shallow trench isolating active devices to avoid sub-threshold kinks arising from corner effects without additional processing |
| SG82695A1 (en) * | 1999-06-01 | 2001-08-21 | Hitachi Ltd | Process for producing semiconductor device and semiconductor device produced thereby |
| US7221030B2 (en) | 2002-08-30 | 2007-05-22 | Fujitsu Limited | Semiconductor device |
Families Citing this family (3)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US5811346A (en) * | 1997-04-14 | 1998-09-22 | Vlsi Technology, Inc. | Silicon corner rounding in shallow trench isolation process |
| US7539963B2 (en) * | 2003-10-24 | 2009-05-26 | Fujitsu Microelectronics Limited | Semiconductor device group and method for fabricating the same, and semiconductor device and method for fabricating the same |
| KR100584776B1 (ko) * | 2004-03-05 | 2006-05-29 | 삼성전자주식회사 | 반도체 장치의 액티브 구조물 형성 방법, 소자 분리 방법및 트랜지스터 형성 방법 |
Citations (6)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US4839306A (en) * | 1987-03-24 | 1989-06-13 | Oki Electric Industry Co., Ltd. | Method of manufacturing a trench filled with an insulating material in a semiconductor substrate |
| EP0459397A2 (en) * | 1990-05-28 | 1991-12-04 | Kabushiki Kaisha Toshiba | Semiconductor device having a trench for device isolation and method of fabricating the same |
| US5236861A (en) * | 1991-08-16 | 1993-08-17 | Sony Corporation | Manufacturing method of metal-insulator-semiconductor device using trench isolation technique |
| US5316965A (en) * | 1993-07-29 | 1994-05-31 | Digital Equipment Corporation | Method of decreasing the field oxide etch rate in isolation technology |
| EP0660391A2 (en) * | 1993-12-20 | 1995-06-28 | Kabushiki Kaisha Toshiba | Semiconductor device with a trench isolation region and method of manufacturing the same |
| US5536675A (en) * | 1993-12-30 | 1996-07-16 | Intel Corporation | Isolation structure formation for semiconductor circuit fabrication |
-
1996
- 1996-09-17 JP JP24444596A patent/JP3611226B2/ja not_active Expired - Fee Related
-
1997
- 1997-09-15 TW TW086113393A patent/TW360945B/zh not_active IP Right Cessation
- 1997-09-16 WO PCT/JP1997/003267 patent/WO1998012742A1/en not_active Ceased
- 1997-09-16 KR KR10-1999-7002156A patent/KR100425064B1/ko not_active Expired - Fee Related
- 1997-09-16 CN CNB971980063A patent/CN1161837C/zh not_active Expired - Fee Related
- 1997-09-16 MY MYPI97004289A patent/MY129438A/en unknown
Patent Citations (6)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US4839306A (en) * | 1987-03-24 | 1989-06-13 | Oki Electric Industry Co., Ltd. | Method of manufacturing a trench filled with an insulating material in a semiconductor substrate |
| EP0459397A2 (en) * | 1990-05-28 | 1991-12-04 | Kabushiki Kaisha Toshiba | Semiconductor device having a trench for device isolation and method of fabricating the same |
| US5236861A (en) * | 1991-08-16 | 1993-08-17 | Sony Corporation | Manufacturing method of metal-insulator-semiconductor device using trench isolation technique |
| US5316965A (en) * | 1993-07-29 | 1994-05-31 | Digital Equipment Corporation | Method of decreasing the field oxide etch rate in isolation technology |
| EP0660391A2 (en) * | 1993-12-20 | 1995-06-28 | Kabushiki Kaisha Toshiba | Semiconductor device with a trench isolation region and method of manufacturing the same |
| US5536675A (en) * | 1993-12-30 | 1996-07-16 | Intel Corporation | Isolation structure formation for semiconductor circuit fabrication |
Cited By (8)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO1998036452A1 (en) * | 1997-02-18 | 1998-08-20 | Hitachi, Ltd. | Semiconductor device and process for producing the same |
| US6242323B1 (en) | 1997-02-18 | 2001-06-05 | Hitachi, Ltd. | Semiconductor device and process for producing the same |
| US6559027B2 (en) | 1997-02-18 | 2003-05-06 | Hitachi, Ltd. | Semiconductor device and process for producing the sme |
| WO1999044223A3 (en) * | 1998-02-27 | 1999-10-28 | Lsi Logic Corp | Process of shallow trench isolating active devices to avoid sub-threshold kinks arising from corner effects without additional processing |
| SG82695A1 (en) * | 1999-06-01 | 2001-08-21 | Hitachi Ltd | Process for producing semiconductor device and semiconductor device produced thereby |
| US6635945B1 (en) | 1999-06-01 | 2003-10-21 | Hitachi, Ltd. | Semiconductor device having element isolation structure |
| US6858515B2 (en) * | 1999-06-01 | 2005-02-22 | Renesas Technology Corp. | Process for producing semiconductor device and semiconductor device produced thereby |
| US7221030B2 (en) | 2002-08-30 | 2007-05-22 | Fujitsu Limited | Semiconductor device |
Also Published As
| Publication number | Publication date |
|---|---|
| JP3611226B2 (ja) | 2005-01-19 |
| MY129438A (en) | 2007-04-30 |
| KR20000036123A (ko) | 2000-06-26 |
| CN1161837C (zh) | 2004-08-11 |
| CN1231064A (zh) | 1999-10-06 |
| TW360945B (en) | 1999-06-11 |
| KR100425064B1 (ko) | 2004-03-30 |
| JPH1092919A (ja) | 1998-04-10 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| US7915173B2 (en) | Shallow trench isolation structure having reduced dislocation density | |
| US8294236B2 (en) | Semiconductor device having dual-STI and manufacturing method thereof | |
| US5770875A (en) | Large value capacitor for SOI | |
| US6737330B2 (en) | Isolation structure and fabricating method therefor | |
| US6518641B2 (en) | Deep slit isolation with controlled void | |
| US20020031871A1 (en) | Method for increasing a very-large-scale-integrated (vlsi) capacitor size on bulk silicon and silicon-on-insulator (soi) wafers | |
| US5723381A (en) | Formation of self-aligned overlapping bitline contacts with sacrificial polysilicon fill-in stud | |
| US20040142534A1 (en) | Semiconductor device having trench isolation structure and method of fabricating the same | |
| KR19990023196A (ko) | 트렌치 절연 구조 형성 방법과 반도체 디바이스 및 그의 제조방법 | |
| US20130009276A1 (en) | Methods of filling isolation trenches for semiconductor devices and resulting structures | |
| JP2002026143A (ja) | トレンチ側壁に酸化物層を形成する方法 | |
| US6682986B2 (en) | Method of forming shallow trench isolation and method of manufacturing a semiconductor device using the same | |
| US20020127818A1 (en) | Recess-free trench isolation structure and method of forming the same | |
| JPH08274163A (ja) | Soi材料上の集積回路及びその製法 | |
| KR100307651B1 (ko) | 반도체장치의제조방법 | |
| KR100251280B1 (ko) | 샐로우 트랜치 아이솔레이션 방법 | |
| US6335556B1 (en) | Semiconductor device and method for manufacturing semiconductor device | |
| US6849521B2 (en) | Method for manufacturing a semiconductor device | |
| JP3611226B2 (ja) | 半導体装置及びその製造方法 | |
| KR19980041816A (ko) | 디봇 형성을 최소화하는 방법 및 집적 회로 칩 | |
| US6238997B1 (en) | Method of fabricating shallow trench isolation | |
| US6350659B1 (en) | Process of making semiconductor device having regions of insulating material formed in a semiconductor substrate | |
| US6239476B1 (en) | Integrated circuit isolation structure employing a protective layer and method for making same | |
| KR100305026B1 (ko) | 반도체소자의 제조방법 | |
| JP2000031489A (ja) | 半導体装置の製造方法 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| WWE | Wipo information: entry into national phase |
Ref document number: 97198006.3 Country of ref document: CN |
|
| AK | Designated states |
Kind code of ref document: A1 Designated state(s): CN KR SG US |
|
| AL | Designated countries for regional patents |
Kind code of ref document: A1 Designated state(s): AT BE CH DE DK ES FI FR GB GR IE IT LU MC NL PT SE |
|
| DFPE | Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed before 20040101) | ||
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application | ||
| WWE | Wipo information: entry into national phase |
Ref document number: 1019997002156 Country of ref document: KR |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 09254939 Country of ref document: US |
|
| 122 | Ep: pct application non-entry in european phase | ||
| WWP | Wipo information: published in national office |
Ref document number: 1019997002156 Country of ref document: KR |
|
| WWG | Wipo information: grant in national office |
Ref document number: 1019997002156 Country of ref document: KR |