WO2026023376A1 - 樹脂粒子及びその用途 - Google Patents

樹脂粒子及びその用途

Info

Publication number
WO2026023376A1
WO2026023376A1 PCT/JP2025/024098 JP2025024098W WO2026023376A1 WO 2026023376 A1 WO2026023376 A1 WO 2026023376A1 JP 2025024098 W JP2025024098 W JP 2025024098W WO 2026023376 A1 WO2026023376 A1 WO 2026023376A1
Authority
WO
WIPO (PCT)
Prior art keywords
weight
resin particles
particles
resin
acid
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
PCT/JP2025/024098
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
晃一 阪部
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Matsumoto Yushi-Seiyaku Co Ltd
Original Assignee
Matsumoto Yushi-Seiyaku Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Matsumoto Yushi-Seiyaku Co Ltd filed Critical Matsumoto Yushi-Seiyaku Co Ltd
Priority to JP2025575629A priority Critical patent/JP7895015B2/ja
Publication of WO2026023376A1 publication Critical patent/WO2026023376A1/ja
Pending legal-status Critical Current
Anticipated expiration legal-status Critical

Links

Classifications

    • A—HUMAN NECESSITIES
    • A61—MEDICAL OR VETERINARY SCIENCE; HYGIENE
    • A61K—PREPARATIONS FOR MEDICAL, DENTAL OR TOILETRY PURPOSES
    • A61K8/00—Cosmetics or similar toiletry preparations
    • A61K8/18—Cosmetics or similar toiletry preparations characterised by the composition
    • A61K8/72—Cosmetics or similar toiletry preparations characterised by the composition containing organic macromolecular compounds
    • A61K8/84—Cosmetics or similar toiletry preparations characterised by the composition containing organic macromolecular compounds obtained by reactions otherwise than those involving only carbon-carbon unsaturated bonds
    • A61K8/85—Polyesters
    • A—HUMAN NECESSITIES
    • A61—MEDICAL OR VETERINARY SCIENCE; HYGIENE
    • A61Q—SPECIFIC USE OF COSMETICS OR SIMILAR TOILETRY PREPARATIONS
    • A61Q1/00—Make-up preparations; Body powders; Preparations for removing make-up
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J3/00—Processes of treating or compounding macromolecular substances
    • C08J3/12—Powdering or granulating
    • C08J3/16—Powdering or granulating by coagulating dispersions

Definitions

  • the present invention relates to resin particles and their uses.
  • Particles are widely used in cosmetics, paints, optical applications, resins, building materials, and the like.
  • Required particle functions include light diffusion, opacity, coatability, and texture.
  • Particle materials include particles made from a variety of materials, including organic and inorganic substances.
  • Organic particles have a softer texture than inorganic particles, and are therefore preferred for use in cosmetics, paints, and the like, for example, to enhance texture.
  • the optical properties of particles have been explored for use in cosmetics, for example, to achieve a soft-focus effect that reduces the appearance of pores and wrinkles, and to improve brightness.
  • Examples of organic particles include acrylic, styrene, urethane, and silicone polymer particles.
  • Patent Document 1 describes a method for producing polylactic acid-based resin microparticles made of polylactic acid derived from non-petroleum sources, and polylactic acid-based resin microparticles as particles with reduced environmental impact.
  • Patent Document 2 also describes porous resin microparticles made of biodegradable polyester-based thermoplastic resin.
  • these particles are obtained by dissolving the resin component in an organic solvent, which tends to form cavities within the particles.
  • the whiteness increases, making it difficult to maintain the transparency of the coating film.
  • Patent Document 3 also describes approximately spherical resin microparticles with a sphericity of 0.90 to 1.00 and a light scattering index of 0.5 to 1.0. However, because these are solid particles with high sphericity, they have low oil absorption and require the incorporation of large amounts to achieve a certain level of effectiveness. Furthermore, conventional particles have the problem of significant loss during the manufacturing process, resulting in low yield rates.
  • the present invention aims to provide resin particles that can be easily washed away even if they adhere to a surface of a substrate, and the resin particles of the present invention not only improve the efficiency of the production process but also contribute to reducing the maintenance costs of the equipment.
  • the present invention includes the following aspects ⁇ 1> to ⁇ 8>.
  • the resin particles of the present invention can be easily washed away.
  • the resin particles of the present invention contain a polyester resin, have an average circularity of 0.9 or less, and have a loose bulk density of 0.1 to 0.5 g/cm 3 .
  • the reason why the resin particles of the present invention can be easily washed away even after adhesion is not particularly limited, but is thought to be that when the average circularity is 0.9 or less, the particle shape becomes non-uniform and the contact area increases compared to spherical particles, so that when washed away with water or the like, water quickly penetrates the resin particle surface and makes it easy to loosen the resin particles, and when the loose bulk density is 0.1 to 0.5 g/ cm3 , there are many voids between the resin particles, and flow paths for water or the like are efficiently formed.
  • the resin particles (hereinafter sometimes simply referred to as particles) of the present invention will be described below.
  • the average circularity of the particles of the present invention is 0.9 or less.
  • the lower limit of the circularity is preferably 0.20, more preferably 0.25, even more preferably 0.30, and particularly preferably 0.35.
  • the upper limit of the circularity is preferably 0.85, more preferably 0.80, and even more preferably 0.75.
  • 0.20 to 0.85 is preferable, and 0.40 to 0.75 is even more preferable.
  • the circularity is preferably 0.8 or less, more preferably 0.7 or less, and particularly preferably 0.6 or less.
  • the circularity of the particles described in the present invention is determined by the method described in the examples.
  • the particles of the present invention have a loose bulk density of 0.1 to 0.5 g/cm 3.
  • the lower limit of the loose bulk density is preferably 0.12 g/cm 3 , more preferably 0.14 g/cm 3 , even more preferably 0.16 g/cm 3 , and particularly preferably 0.18 g/cm 3.
  • the upper limit of the loose bulk density is preferably 0.45 g/cm 3 , more preferably 0.40 g/cm 3 , and even more preferably 0.35 g/cm 3.
  • 0.12 to 0.45 g/cm 3 is preferred, and 0.18 to 0.35 g/cm 3 is more preferred.
  • the loose bulk density of the particles described in the present invention is determined by the method described in the examples.
  • the apparent specific gravity of the particles of the present invention is preferably 2.0 or less, as this slows the settling rate of the particles.
  • the lower limit of the apparent specific gravity is more preferably 0.85, even more preferably 0.90, and particularly preferably 0.95.
  • the upper limit of the apparent specific gravity is more preferably 1.8, even more preferably 1.6, and particularly preferably 1.4.
  • 0.85 to 1.8 is more preferable, and 0.95 to 1.4 is even more preferable.
  • the apparent specific gravity of the particles described in the present invention is determined by the method described in the Examples.
  • the relative density of the particles of the present invention is preferably 0.6 g/cm 3 or less in terms of increasing the fluidity of the particles.
  • the lower limit of the relative density is more preferably 0.05 g/cm 3 , even more preferably 0.10 g/cm 3 , and particularly preferably 0.15 g/cm 3 .
  • the upper limit of the relative density is more preferably 0.55 g/cm 3 , even more preferably 0.50 g/cm 3 , and particularly preferably 0.45 g/cm 3 .
  • 0.05 to 0.55 g/cm 3 is more preferable, and 0.10 to 0.45 g/cm 3 is even more preferable.
  • the hiding power of the particles of the present invention is preferably 50% or less in terms of transparency when incorporated into a coating film.
  • the upper limit of the hiding power is 30%, more preferably 20%, and particularly preferably 10%.
  • the lower limit of the hiding power is preferably 0%, more preferably 1%.
  • a range of 40% to 0% is preferred, and a range of 20% to 0% is more preferred.
  • the hiding ratio of the particles described in the present invention is determined by the method described in the examples.
  • the volume average particle diameter of the resin particles of the present invention is preferably 1 to 50 ⁇ m in terms of fluidity and transparency when incorporated into a coating film.
  • the lower limit of the particle diameter is more preferably 1.5 ⁇ m, even more preferably 2.0 ⁇ m, and particularly preferably 2.5 ⁇ m.
  • the upper limit of the particle diameter is more preferably 40 ⁇ m, even more preferably 35 ⁇ m, and particularly preferably 30 ⁇ m. Also, for example, 1 to 40 ⁇ m is preferred, 1.5 to 30 ⁇ m is more preferred, and 2 to 20 ⁇ m is particularly preferred.
  • the volume average particle diameter of the resin particles is measured by the method described in the Examples.
  • the coefficient of variation CV of the particle size distribution of the resin particles of the present invention is not particularly limited, but is preferably 2 to 70%, as this makes it easier to satisfy the loose bulk density of the present invention.
  • the upper limit of the coefficient of variation CV is preferably 65% or less, more preferably 60% or less, even more preferably 55% or less, and especially preferably 50% or less.
  • the lower limit of the coefficient of variation CV is preferably 3%, more preferably 5%, and especially preferably 7%. Furthermore, for example, 3 to 65% is more preferable, and 5 to 60% is even more preferable.
  • the coefficient of variation CV refers to a value calculated using the following calculation formulas (2) and (3).
  • s is the standard deviation of particle diameters
  • ⁇ x> is the average particle diameter
  • xi is the diameter of the ith particle
  • n is the number of particles.
  • the linseed oil absorption of the resin particles of the present invention is preferably 150 to 500 mL/100 g, as this provides high fluidity and good handleability.
  • the lower limit of the oil absorption is more preferred in order of (1) 160 mL/100 g, (2) 170 mL/100 g, (3) 180 mL/100 g, and (4) 190 mL/100 g (the larger the number in parentheses, the more preferred it is).
  • the upper limit of the oil absorption is more preferred in order of (1) 480 mL/100 g, (2) 460 mL/100 g, (3) 440 mL/100 g, (4) 420 mL/100 g, (5) 400 mL/100 g, (6) 380 mL/100 g, and (7) 360 mL/100 g (the larger the number in parentheses, the more preferred it is). Furthermore, for example, 160 to 480 mL/100 g is more preferable, and 180 to 440 mL/100 g is even more preferable.
  • the linseed oil absorption of the particles is measured using the method described in the Examples.
  • the resin particles of the present invention contain a polyester resin.
  • the polyester resin is not particularly limited, but is preferably at least one selected from aliphatic polyester resins and aliphatic-aromatic polyester resins, with aliphatic polyester resins being particularly preferred, in that they have excellent biodegradability and the relative density can be easily adjusted to 0.6 g/cm or less.
  • the aliphatic polyester resin is not particularly limited as long as the polyhydric alcohol, polycarboxylic acid, and hydroxycarboxylic acid, which are the constituent components of the polyester resin, are aliphatic polyhydric alcohol, aliphatic polycarboxylic acid, and aliphatic hydroxycarboxylic acid, respectively.
  • aliphatic polyesters obtained from constituent components containing a polyhydric alcohol and a polycarboxylic acid are preferred in that the effects of the present application can be more easily obtained.
  • aliphatic polyhydric alcohols include ethylene glycol, 1,3-propanediol, 1,4-butanediol, diethylene glycol, 1,5-pentanediol, 1,6-hexanediol, propylene glycol, dipropylene glycol, triethylene glycol, tetraethylene glycol, 1,2-propanediol, 1,3-butanediol, 2,3-butanediol, neopentyl glycol (2,2-dimethylpropane-1,3-diol), 1,2-hexanediol, 2,5-hexanediol, 2-methyl-2,4-pentanediol, 3-methyl-1,3-pentanediol, 2-ethyl-1,3-hexanediol, 2,2-bis(4-hydroxycyclohexyl)propane, 1,4-cyclohexanediol,
  • Examples of the aliphatic polycarboxylic acid include succinic acid, adipic acid, suberic acid, sebacic acid, azelaic acid, octyl succinic acid, fumaric acid, maleic acid, itaconic acid, decamethylenedicarboxylic acid, anhydrides thereof, etc. These aliphatic polycarboxylic acids may be used alone or in combination of two or more.
  • Examples of aliphatic hydroxycarboxylic acids include lactic acid, glycolic acid, hydroxybutyric acid, hydroxycaproic acid, hydroxydimethylbutyric acid, hydroxymethylbutyric acid, etc. These aliphatic hydroxycarboxylic acids may be used alone or in combination of two or more.
  • Aliphatic polyester resins include, for example, polycaprolactone butylene succinate, polybutylene succinate, polybutylene succinate adipate, polybutylene succinate carbonate, polybutylene adipate, polybutylene succinate lactate, polyethylene succinate, polyethylene adipate, polytetramethylene succinate, polyhydroxyalkanoate, polyhydroxybutyrate, poly(3-hydroxybutyrate-co-3-hydroxyhexanoate), polyhydroxybutyrate valerate, poly(3-hydroxybutyrate-co-3-hydroxyvalerate), poly(3-hydroxybutyrate-co-3-hydroxypropionate), poly(3-hydroxybutyrate-co-4-hydroxybutyrate), poly(3-hydroxybutyrate-co-3-hydroxyacyl), polyhydroxyacyl, and polylactic acid.
  • the proportion of aromatic polycarboxylic acid-derived components in the aliphatic-aromatic polyester resin is preferably 40 unit mol% or less. These aromatic polycarboxylic acids may be used alone or in combination of two or more.
  • polyester resins examples include polybutylene succinate terephthalate, polybutylene adipate terephthalate, polytetramethylene adipate terephthalate, and polybutylene succinate adipate terephthalate.
  • Polyester resin is an environmentally friendly material, so it is preferable that it contains a biodegradable resin, and more preferably it is a biodegradable resin.
  • the polyester resin is not particularly limited, but a weight average molecular weight of 5 ⁇ 10 3 to 1 ⁇ 10 9 is preferred in terms of excellent dispersibility in water.
  • the lower limit of the average molecular weight is more preferred in order of (1) 1 ⁇ 10 4 , (2) 2 ⁇ 10 4 , (3) 3 ⁇ 10 4 , (4) 5 ⁇ 10 4 , (5) 1 ⁇ 10 5 , (6) 2 ⁇ 10 5 , and (7) 3 ⁇ 10 5.
  • the upper limit of the average molecular weight is more preferred in order of (1) 5 ⁇ 10 8, (2) 3 ⁇ 10 8 , (3) 1 ⁇ 10 8 , (4) 5 ⁇ 10 7 , (5) 3 ⁇ 10 7 , and (6) 1 ⁇ 10 7 (the larger the number in parentheses, the more preferred it is).
  • 2 ⁇ 10 4 to 5 ⁇ 10 8 is more preferable, and 3 ⁇ 10 4 to 5 ⁇ 10 8 is even more preferable.
  • Surfactants include, for example, anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, and silicone surfactants.
  • anionic surfactants such as alkyl sulfate ester salts, alkyl ether carboxylate salts, alkyl ether sulfate ester salts, alkyl phosphate ester salts, polyoxyalkylene alkyl ether acetate salts, alkyl sulfonate salts, alkylbenzene sulfonate salts, polyoxyalkylene alkyl ether sulfate salts, polyoxyalkylene alkyl ether phosphate ester salts, higher fatty acid amide sulfonate salts, fatty acid alkali metal salts (e.g., potassium laurate, sodium myristylates, sodium stearate), alkyl sulfosuccinate ester salts, and N-acylamino acid salt
  • organic substances other than organic polymers include waxes, oils, fatty acid metal salts, and amino acid compounds, which can be easily adjusted to a relative density of 0.6 g/cm or less .
  • organic substances include waxes such as carnauba wax, candelilla wax, beeswax, and higher alcohols; oils such as almond oil, olive oil, rice bran oil, squalane, mineral oil, alkanes, and alkyl benzoates; fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, 12-hydroxystearic acid, behenic acid, montanic acid, and cerotic acid; calcium laurate, zinc laurate, zinc myristic acid, zinc palmitate, magnesium stearate, zinc stearate, calcium stearate, aluminum stearate, calcium 12-hydroxystearate, and 12-hydroxystearic acid.
  • Inorganic substances that can easily adjust the hiding power to 50% or less include, for example, wollastonite, sericite, kaolin, mica, clay, talc, bentonite, smectite, alumina silicate, pyrophyllite, montmorillonite, calcium silicate, calcium carbonate, magnesium carbonate, dolomite, calcium sulfate, calcium phosphate, boron nitride, silicon carbide, magnesium silicate, calcium silicate, magnesium aluminometasilicate, magnesium aluminosilicate, hydroxyapatite, titanium oxide, silica, alumina, titanium dioxide, zinc oxide, magnesium oxide, zinc oxide, hydrosaltite, boron nitride, etc., and one or more of these may be used in combination.
  • the resin particles of the present invention are not particularly limited, but preferably have a biodegradation rate of 1% or more after 10 days as measured in accordance with JIS K6950:2000.
  • the lower limits of the biodegradation rate are preferably (1) 3%, (2) 5%, (3) 10%, (4) 15%, (5) 20%, (6) 25%, and (7) 30% in that order (the larger the number in parentheses, the more preferable it is).
  • the resin particles of the present invention can be produced, for example, by a method including step 1 of mixing the above-mentioned polyester resin, a surfactant, a water-soluble polymer, and water to obtain a pre-mixed liquid; step 2 of heating and stirring the pre-mixed liquid obtained in step 1 to obtain a heated dispersion; step 3 of cooling the heated dispersion obtained in step 2; and step 4 of applying an external force to the obtained resin particle dispersion to deform the particles.
  • resin particles of the present invention when the resin particles of the present invention are produced without using organic solvents, resin particles with excellent transparency can be produced, which is preferable. If organic solvents are used, pores tend to form in the resin particles when the organic solvent is removed from the resin particles, resulting in the resulting resin particles having poor transparency. Furthermore, by producing resin particles using water rather than organic solvents, surfactants and water-soluble polymers are more likely to be present at the interface between the resin particles and water during resin particle formation, which is thought to contribute to the surface shape of the resin particles. Furthermore, it is thought that the lipophilic groups of the surfactant affect the resin structure, resulting in resin particles with excellent transparency. Furthermore, not using organic solvents is environmentally friendly and preferable.
  • the surfactant there are no particular limitations on the surfactant, but it is preferable to use a nonionic surfactant with an HLB value of 1 to 13, since this makes it easier to adjust the hiding rate of the resin particles to 50% or less. Furthermore, it is preferable to use an ester type or ester salt type surfactant, since the transparency of the particles is excellent.
  • the surfactant may ultimately be contained within the particles.
  • the presence of the surfactant near the particle surface is thought to have a greater effect on the surface structure, and its increased compatibility with water makes it easier to wash off if it adheres to equipment.
  • the weight percentage of the surfactant in the particles is not particularly limited, but is preferably 0.001 to 10% by weight, with the upper weight percentage more preferably 7% by weight and even more preferably 5% by weight. Meanwhile, the lower weight percentage limit is more preferably 0.005% by weight and even more preferably 0.01% by weight. Furthermore, for example, 0.001 to 7% by weight is more preferred, with 0.001 to 5% by weight being even more preferred.
  • the water-soluble polymer can be any of those described above, and is preferably a water-soluble polymer having a viscosity of 2 to 200,000 mPa ⁇ s in a 4% aqueous solution at 20°C, since this facilitates stable production of resin particles containing the polyester resin of the present invention.
  • the water-soluble polymer is preferably at least one selected from polyvinylpyrrolidone, polyvinyl alcohol, hydroxyethyl cellulose, hydroxypropyl cellulose, methyl cellulose, and carboxymethyl cellulose, and more preferably polyvinyl alcohol.
  • the water-soluble polymer may be ultimately contained in the particles.
  • the presence of the water-soluble polymer in the particles is considered preferable in that it increases affinity with solvents such as water and makes it easier to adjust the hiding power to 50% or less.
  • the weight ratio of the water-soluble polymer in the particles is not particularly limited, but is preferably 0.001 to 10 wt%, with the upper limit of the weight ratio being more preferably 8 wt%, and even more preferably 5 wt%. Meanwhile, the lower limit of the weight ratio is more preferably 0.002 wt%, and even more preferably 0.005 wt%. Furthermore, for example, it is more preferably 0.001 to 8 wt%, and even more preferably 0.001 to 5 wt%.
  • the resin particles of the present invention preferably contain at least one selected from a surfactant and a water-soluble polymer, as this increases their affinity with solvents such as water.
  • the total weight percentage of the surfactant and water-soluble polymer in the particles is not particularly limited, but is preferably 0.001 to 10% by weight. The lower limit of this weight percentage is more preferred in order of (1) 0.002% by weight, (2) 0.005% by weight, (3) 0.01% by weight, (4) 0.02% by weight, (5) 0.05% by weight, and (6) 0.1% by weight (the larger the number in parentheses, the more preferred it is).
  • this weight percentage is more preferred in order of (1) 7% by weight, (2) 6% by weight, (3) 5% by weight, (4) 4% by weight, and (5) 3% by weight (the larger the number in parentheses, the more preferred it is). Furthermore, for example, 0.001 to 7% by weight is more preferred, and 0.001 to 5% by weight is even more preferred.
  • the resin particles of the present invention are produced by mixing a surfactant and a water-soluble polymer
  • the water-soluble polymer improves the liquid viscosity during production
  • the surfactant improves the efficiency of particle homogenization
  • the surfactant improves the dispersibility of the resin components, resulting in stable resin particles. Therefore, it is even more preferable that the weight ratios of the surfactant and the water-soluble polymer are within the above-mentioned ranges.
  • Step 1 a polyester resin, a surfactant, a water-soluble polymer, and water are mixed to obtain a preliminary mixed solution.
  • the resin particles contain components other than the polyester resin, the surfactant, and the water-soluble polymer, the other components may be added and mixed in this step.
  • the mixing ratio of the polyester resin is not particularly limited, but is preferably 1 to 200 parts by weight per 100 parts by weight of water. A ratio within this range tends to produce resin particles with a more uniform shape, which is preferable because it makes it easier to satisfy the circularity requirement of the present invention and therefore makes it easier to obtain the particle diameter of the present invention.
  • the lower limit of the mixing ratio is more preferably 3 parts by weight, even more preferably 5 parts by weight, and most preferably 10 parts by weight.
  • the upper limit of the mixing ratio is more preferably 180 parts by weight, even more preferably 160 parts by weight, and most preferably 150 parts by weight. Furthermore, for example, 5 to 200 parts by weight is more preferable, and 10 to 180 parts by weight is even more preferable.
  • the mixing ratio of the surfactant is not particularly limited, but is preferably 0.001 to 10 parts by weight per 100 parts by weight of polyester resin, as this makes it easier to obtain the particle size of the present invention. Having this ratio within the above range tends to improve the transparency of the resulting resin particles, making it easier to adjust the hiding ratio to 50% or less.
  • the lower limit of this mixing ratio is preferably 0.01 parts by weight, more preferably 0.05 parts by weight, and especially preferably 0.1 parts by weight.
  • the upper limit of this mixing ratio is more preferably 7 parts by weight, even more preferably 5 parts by weight, and especially preferably 3 parts by weight. Furthermore, for example, 0.001 to 7 parts by weight is more preferred, and 0.01 to 7 parts by weight is even more preferred.
  • the mixing ratio of the water-soluble polymer to water is not particularly limited, but is preferably 0.1 to 100 parts by weight per 100 parts by weight of water, as this facilitates stable production of the polyester resin particles of the present invention. Having this ratio within the above range tends to improve the dispersibility of the resulting resin particles, which is preferable in that it makes it easier to satisfy the circularity requirement of the present invention.
  • the lower limit of this ratio is more preferably 0.5 parts by weight, even more preferably 1 part by weight, and especially preferably 2 parts by weight.
  • the upper limit of this ratio is more preferably 80 parts by weight, even more preferably 70 parts by weight, and especially preferably 60 parts by weight.
  • 0.5 to 100 parts by weight is more preferred, and 1 to 100 parts by weight is even more preferred.
  • Step 2 is a step of heating and stirring the preliminary mixture obtained in step 1 to obtain a heated dispersion.
  • the pressure during heating and stirring in step 2 is not particularly limited, but is preferably 0.1 to 10 MPa.
  • the pressure is preferably equal to or greater than the saturated vapor pressure of water at the heating temperature.
  • the heating temperature is not particularly limited, but is preferably 80 to 200°C. A temperature within this range tends to result in more uniform resin particle shapes, making it easier to stably obtain the particle diameter within the target range of the present invention and satisfy the loose bulk density of the present invention.
  • the temperature is preferably equal to or higher than the softening point or melting point of the polyester resin, more preferably 10°C or higher, even more preferably 20°C or higher, and particularly preferably 30°C or higher.
  • step 2 it is preferable to heat the mixture to a temperature equal to or higher than the softening point or melting point of the polyester resin and stir the mixture under a pressure of 0.1 MPa or more, as this makes it easier to satisfy the circularity requirement of the present invention.
  • the stirring method is not particularly limited, but it is sufficient that the mixture is stirred to an extent that it is mixed.
  • the heating time is not particularly limited, but is preferably 1 to 30 hours. A heating time of 1 hour or more is preferred because more uniform dispersion results and the particle size of the present invention is more easily obtained. A heating time of 30 hours or less tends to improve production efficiency.
  • the lower limit of the heating time is more preferably 2 hours, even more preferably 3 hours, and most preferably 5 hours.
  • the upper limit of the heating time is more preferably 25 hours, even more preferably 20 hours, and most preferably 15 hours.
  • Step 3 is a step of cooling the heated dispersion obtained in step 2.
  • the cooling method is not particularly limited, but it is preferable to cool the heated dispersion obtained in step 2 to 5 to 50° C.
  • the cooling rate is not particularly limited, but rapid cooling or natural cooling by air cooling or the like may be used.
  • stirring may be continued at the stirring speed of step 2, or stirring may be stopped.
  • the dispersion after cooling is an aqueous dispersion containing resin particles.
  • Step 4 is a step of applying a mechanical external force to the resin particles obtained in step 3 to deform the resin particles.
  • the deformation method is not particularly limited, but a method in which a physical force is applied to the particles is preferred because it is easier to satisfy the circularity requirement of the present invention.
  • the method for applying the mechanical external force is not particularly limited, but examples include mixing and stirring with glass beads, using a ball mill, a bead mill, and a vibration dryer.
  • the form of the resin particles in step 4 may be a dispersion, a wet powder, or a dry powder.
  • the resin particles of the present invention may be used in the form of a dispersion, a wet powder, or a dry powder.
  • the wet powder can be obtained by dehydrating the dispersion liquid in step 3 using, for example, a centrifuge, a pressure press, a vacuum dehydrator, or the like.
  • the dispersion liquid in step 3 may be subjected to a dehydration treatment after a measure to reduce the liquid viscosity has been taken.
  • the method for reducing the liquid viscosity is not particularly limited, and examples thereof include a method of diluting the liquid by adding water, a method of salting out the water-soluble components, and a method of decomposing the water-soluble components with an oxidizing agent or an enzyme.
  • the value of the liquid viscosity is not particularly limited as long as it allows dehydration treatment to be carried out.
  • the liquid viscosity is preferably 1,000 mPa s or less, more preferably 500 mPa s or less, and particularly preferably 100 mPa s or less, from the viewpoints that aggregation of resin particles can be suppressed in the subsequent drying step and the hiding ratio can be easily adjusted to 50% or less.
  • the dry powder can be obtained by drying the wet powder using a tray dryer, an indirect heating dryer, a fluidized bed dryer, a vacuum dryer, a vibration dryer, a flash dryer, etc.
  • the dispersion obtained in step 3 can be dried using a spray dryer, a fluidized bed dryer, etc. to obtain a dry powder.
  • the dry powder may be classified by air classification, screen classification, or the like.
  • the resin particles of the present invention can be used in cosmetics, paints, optical applications, resins, building materials, etc.
  • the resin particles of the present invention are excellent in transparency and can therefore be suitably used in cosmetics and coating compositions.
  • the weight ratio of the resin particles to the entire coating composition is not particularly limited, but is preferably 0.1 to 30% by weight, more preferably 0.5 to 20% by weight, and even more preferably 1 to 10% by weight.
  • volume average particle size Measurement was carried out using a laser diffraction scattering particle size distribution measuring device (Microtrac particle size distribution meter (model 9320-HRA), manufactured by Nikkiso Co., Ltd.) by irradiating with ultrasonic waves for 120 seconds by a wet measurement method.
  • the volume average particle size was adopted as the value at which the cumulative frequency in volume-based measurement was 50% (D50).
  • the average circularity was calculated using a dynamic particle image analyzer (HydroInsight, manufactured by Spectris). Specifically, the measurement method was as follows: 200 mg of a resin particle sample was added to a beaker containing 20 mL of ion-exchanged water, and the mixture was treated in an ultrasonic bath for 1 minute to prepare a sample solution. Water was circulated in advance at 2500 rpm in the Hydro MV dispersion unit of the Mastersizer 3000 connected to Hydro Insight, and the sample solution was added until a predetermined concentration was reached, and measurement was performed. (Measurement conditions) Lens: Standard lens (particle size measurement range: 1 to 300 ⁇ m) Camera gain:50 Dark threshold: 80 Min sharpness:30 Number of particles measured: 10,000
  • the hiding ratio was measured according to the following procedure based on the hiding test paper method described in JIS K 5600-4-1: 1999.
  • the coating mixture used for evaluation was prepared according to the following procedure. Binder resin: 70 parts by weight of water-based glossy transparent urethane resin for buildings (manufactured by Sunday Paint, model number Sunday-037902) Resin particles: 30 parts by weight
  • the resulting coating mixture was applied to an opacity test paper (vertical black and white A type) so that the coating thickness after drying would be 100 ⁇ m, thereby preparing a sample.
  • the relative density in this application is the mass of resin particles contained in a unit volume compared to the apparent specific gravity, which is the theoretical specific gravity of the material.
  • the cleaning property evaluation in this application is an index showing the ease of cleaning resin particles adhering to equipment, etc.
  • the cleaning property evaluation was performed under the following conditions. The better the cleaning property, the better the cleaning property when resin particles adhere to equipment.
  • Sample Preparation 1 g of resin particles was dispersed in 10 g of water and placed in a 10 mL centrifuge tube. Thereafter, the centrifuge tube was shaken up and down 30 times or more to obtain a uniform aqueous dispersion of resin particles.
  • Standing The sample prepared in (1) was left standing for 24 hours. During this standing period, the resin particles naturally settled and aggregated at the bottom of the container.
  • Example 1 300 parts by weight of water, 100 parts by weight of polybutylene succinate adipate, 0.5 parts by weight of sorbitan monolaurate, and 20 parts by weight of polyvinyl alcohol were mixed and placed in a 1 L pressure-resistant container, which was then sealed. The internal temperature of the container was raised to 130°C, and the mixture was stirred at 250 rpm for 5 hours under a pressure of 0.4 MPa. The mixture was then cooled to 30°C, and an oxidizing agent was added to obtain an aqueous dispersion (1) of approximately spherical resin particles.
  • the obtained aqueous dispersion (1) of approximately spherical resin particles was transferred to a 1 L glass beaker, and 100 parts by weight of water and 1,000 parts by weight of glass beads having a diameter of 5 mm were added thereto, followed by mixing for 12 hours at 300 rpm using a Three-One motor equipped with an anchor blade (blade diameter 20 mm) at 30°C under atmospheric pressure to obtain an aqueous dispersion (1) of flat resin particles.
  • the obtained aqueous dispersion (1) was dehydrated by filtration, dried at 50°C, and classified to obtain flat resin particles 1.
  • the evaluation results of the obtained resin particles 1 are shown in Table 1. An electron microscope photograph of the resin particles 1 is shown in FIG.
  • Resin particles 1 contained 98.8% by weight of polyester resin, 0.2% by weight of sorbitan monolaurate, and 1.0% by weight of polyvinyl alcohol.
  • Example 2 Flat resin particles 2 were obtained in the same manner as in Example 1, except that the processing time for the step of deforming the resin particles was changed to 6 hours.
  • Resin particles 2 contained 98.8% by weight of polyester resin, 0.3% by weight of sorbitan monostearate, and 0.9% by weight of polyvinyl alcohol.
  • Example 3 Flat resin particles 3 were obtained in the same manner as in Example 1, except that the processing time for the step of deforming the resin particles was changed to 18 hours.
  • the particles 3 contained 99.1% by weight of polyester resin, 0.1% by weight of sorbitan monolaurate, and 0.8% by weight of polyvinyl alcohol.
  • Example 4 An aqueous dispersion (4) of approximately spherical resin particles was obtained in the same manner as in Example 1, except that polybutylene succinate adipate was replaced with polybutylene succinate.
  • the obtained aqueous dispersion (4) of approximately spherical resin particles was treated for 24 hours using a bead mill (Dynomill Multilab 0.6 type, manufactured by Shinmaru Enterprises) whose casing was filled with zirconia beads having a diameter of 0.3 mm, to obtain an aqueous dispersion (4) of flat resin particles.
  • the obtained aqueous dispersion (4) was dehydrated by filtration, dried at 50°C, and classified to obtain flat resin particles 4.
  • Particle 4 contained 99.4% by weight of polyester resin, 0.1% by weight of sorbitan monolaurate, and 0.5% by weight of polyvinyl alcohol.
  • Example 5 An aqueous dispersion (5) of approximately spherical resin particles was obtained in the same manner as in Example 1, except that polybutylene succinate adipate was changed to polybutylene adipate terephthalate and 0.3 g of sorbitan monolaurate was used. The obtained aqueous dispersion (5) of approximately spherical resin particles was dehydrated by filtration, dried at 50°C, and classified to obtain approximately spherical resin particles (5).
  • Example 6 Flat resin particles 6 were obtained in the same manner as in Example 1, except that polybutylene succinate adipate was changed to polytetramethylene adipate terephthalate and the amount of sorbitan monolaurate was changed to 0.25 g.
  • the content of the polyester resin in the particles 6 was 98.8% by weight, the content of sorbitan monolaurate was 0.3% by weight, and the content of polyvinyl alcohol was 0.9% by weight.
  • Example 7 Flat resin particles 7 were obtained in the same manner as in Example 1, except that the amount of polybutylene succinate adipate was changed from 100 parts by weight to 70 parts by weight and the amount of polyhydroxyalkanoate was changed to 30 parts by weight. Resin particles 7 contained 98.5% by weight of polyester resin, 0.4% by weight of sorbitan monolaurate, and 1.1% by weight of polyvinyl alcohol.
  • Example 8 Flat resin particles 8 were obtained in the same manner as in Example 1, except that the amount of polybutylene succinate adipate was changed from 100 parts by weight to 20 parts by weight and the amount of low-density polyethylene was changed to 80 parts by weight. Resin particles 8 contained 19.7% by weight of polyester resin, 78.6% by weight of low-density polyethylene, 0.5% by weight of sorbitan monolaurate, and 1.2% by weight of polyvinyl alcohol.
  • Comparative Example 1 Approximately spherical resin particles 10 were obtained in the same manner as in Example 1, except that the step of deforming the particles with glass beads was omitted.
  • Comparative Example 2 Matsumoto Microsphere MHB-R (manufactured by Matsumoto Yushi Seiyaku Co., Ltd., average particle size 11 ⁇ m), which is PMMA crosslinked hollow particles, was used as the resin particles.
  • Comparative Example 3 30 parts by weight of polybutylene succinate adipate and 970 parts by weight of 3-methoxy-3-methyl-1-butanol were mixed and placed in a 1 L pressure vessel, which was then sealed. The temperature inside the vessel was raised to 140°C, and the mixture was stirred at 400 rpm for 2.0 hours under a pressure of 0.1 MPa, and then cooled to 25°C to obtain a dispersion of resin particles. The mixture was then dehydrated by filtration and dried at 50°C to obtain porous resin particles 3.
  • Comparative Example 4 Flat resin particles 11 were obtained in the same manner as in Example 1, except that the amount of polybutylene succinate adipate was changed from 100 parts by weight to 60 parts by weight and calcium carbonate was changed to 40 parts by weight.
  • the particles of Examples 1 to 9 contained polyester resin, had a circularity of 0.9 or less, and a loose bulk density of 0.1 to 0.5 g/cm 3 , and were therefore particles that could be easily washed away.
  • the particles of Comparative Examples 1 to 4 were not particles of the present invention, and therefore when they adhered to the equipment, they were difficult to clean, which reduced the efficiency of the manufacturing process.
  • the resin particles of the present invention can be easily washed away, which increases production efficiency and reduces waste and equipment maintenance costs.

Landscapes

  • Health & Medical Sciences (AREA)
  • Life Sciences & Earth Sciences (AREA)
  • Chemical & Material Sciences (AREA)
  • Veterinary Medicine (AREA)
  • Public Health (AREA)
  • General Health & Medical Sciences (AREA)
  • Animal Behavior & Ethology (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Organic Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Medicinal Chemistry (AREA)
  • Dispersion Chemistry (AREA)
  • Birds (AREA)
  • Epidemiology (AREA)
  • Processes Of Treating Macromolecular Substances (AREA)
PCT/JP2025/024098 2024-07-24 2025-07-04 樹脂粒子及びその用途 Pending WO2026023376A1 (ja)

Priority Applications (1)

Application Number Priority Date Filing Date Title
JP2025575629A JP7895015B2 (ja) 2024-07-24 2025-07-04 樹脂粒子及びその用途

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2024118311 2024-07-24
JP2024-118311 2024-07-24

Publications (1)

Publication Number Publication Date
WO2026023376A1 true WO2026023376A1 (ja) 2026-01-29

Family

ID=98565601

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2025/024098 Pending WO2026023376A1 (ja) 2024-07-24 2025-07-04 樹脂粒子及びその用途

Country Status (2)

Country Link
JP (1) JP7895015B2 (cg-RX-API-DMAC7.html)
WO (1) WO2026023376A1 (cg-RX-API-DMAC7.html)

Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2003103517A (ja) * 2001-09-28 2003-04-09 Teijin Chem Ltd 熱可塑性樹脂組成物の製造方法
JP2018158571A (ja) * 2017-03-21 2018-10-11 株式会社リコー 立体造形用樹脂粉末、立体造形物の製造方法、及び立体造形物の製造装置
WO2019189420A1 (ja) * 2018-03-29 2019-10-03 積水化成品工業株式会社 ポリエチレンテレフタレート系樹脂粒子
WO2023139987A1 (ja) * 2022-01-18 2023-07-27 松本油脂製薬株式会社 粒子、及びその用途

Family Cites Families (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN119923429A (zh) * 2022-09-21 2025-05-02 积水化成品工业株式会社 树脂颗粒及其用途

Patent Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2003103517A (ja) * 2001-09-28 2003-04-09 Teijin Chem Ltd 熱可塑性樹脂組成物の製造方法
JP2018158571A (ja) * 2017-03-21 2018-10-11 株式会社リコー 立体造形用樹脂粉末、立体造形物の製造方法、及び立体造形物の製造装置
WO2019189420A1 (ja) * 2018-03-29 2019-10-03 積水化成品工業株式会社 ポリエチレンテレフタレート系樹脂粒子
WO2023139987A1 (ja) * 2022-01-18 2023-07-27 松本油脂製薬株式会社 粒子、及びその用途

Also Published As

Publication number Publication date
JP7895015B2 (ja) 2026-07-24
JPWO2026023376A1 (cg-RX-API-DMAC7.html) 2026-01-29

Similar Documents

Publication Publication Date Title
TWI719772B (zh) 含乙酸纖維素之粒子、化妝品組成物及含乙酸纖維素之粒子之製造方法
JP7454108B2 (ja) 粒子、及びその用途
JP6921293B1 (ja) 樹脂ビーズ、樹脂ビーズの製造方法、及び樹脂ビーズを用いた製品
TWI337893B (en) Modifying powder, liquid compositions and molded products containing the modifying powder, and method for producing the modifying powder
WO2024032316A1 (zh) 可降解微珠及其制备方法与应用
JP7857323B2 (ja) 生分解性球状粒子及びその製造方法
JP7377924B1 (ja) ポリマー粒子及びその用途
JPWO2004055099A1 (ja) 複合硬化シリコーン粉末、その製造方法および水性組成物
JP5133478B2 (ja) 生分解性ポリエステル樹脂微粒子の製造方法
JP7443614B1 (ja) 樹脂粒子及びその用途
JP7678855B2 (ja) ポリマー粒子及びその用途
JP7542703B2 (ja) 樹脂粒子及びその用途
JP7617217B2 (ja) ポリエステル系樹脂粒子及びその用途
JP7443605B2 (ja) ポリマー粒子及びその用途
CN118660926A (zh) 粒子及其用途
JP5665332B2 (ja) 複合粒子の製造方法
JP2007071415A (ja) 吸収剤の製造法
CN108137950B (zh) 中空聚合物组合物
JP2026080775A (ja) 熱可塑性高分子粒子、熱可塑性高分子粒子の水性分散液、及び、その製造方法
WO2023119927A1 (ja) 多孔質粒子、化粧品組成物及び多孔質粒子の製造方法
JP2026074482A (ja) 複合粒子及びその用途
TWI766843B (zh) 中空聚合物組合物
TWI859571B (zh) 可降解微珠及其製備方法與應用
JP7392905B1 (ja) 経時安定性に優れた抗微生物性を有する金属微粒子含有分散液
JPH0532524A (ja) 多孔質球状アパタイト粒子の製造方法

Legal Events

Date Code Title Description
ENP Entry into the national phase

Ref document number: 2025575629

Country of ref document: JP

Kind code of ref document: A

WWE Wipo information: entry into national phase

Ref document number: 2025575629

Country of ref document: JP

121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 25844280

Country of ref document: EP

Kind code of ref document: A1