WO2025243391A1 - 半導体装置および半導体装置の製造方法 - Google Patents
半導体装置および半導体装置の製造方法Info
- Publication number
- WO2025243391A1 WO2025243391A1 PCT/JP2024/018675 JP2024018675W WO2025243391A1 WO 2025243391 A1 WO2025243391 A1 WO 2025243391A1 JP 2024018675 W JP2024018675 W JP 2024018675W WO 2025243391 A1 WO2025243391 A1 WO 2025243391A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- layer
- semiconductor device
- silicon crystal
- crystal layer
- bonding
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Links
Classifications
-
- H—ELECTRICITY
- H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- H10D—INORGANIC ELECTRIC SEMICONDUCTOR DEVICES
- H10D30/00—Field-effect transistors [FET]
- H10D30/40—FETs having zero-dimensional [0D], one-dimensional [1D] or two-dimensional [2D] charge carrier gas channels
- H10D30/47—FETs having zero-dimensional [0D], one-dimensional [1D] or two-dimensional [2D] charge carrier gas channels having two-dimensional [2D] charge carrier gas channels, e.g. nanoribbon FETs or high electron mobility transistors [HEMT]
-
- H—ELECTRICITY
- H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
- H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
- H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
- H10P14/20—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials
Definitions
- This disclosure relates to semiconductor devices and methods for manufacturing semiconductor devices, and in particular to semiconductor devices having semiconductor layers made of nitride and methods for manufacturing the same.
- Patent Document 1 using diamond as a heat spreader or heat sink is effective in improving the heat dissipation of semiconductor devices, as diamond has high thermal conductivity.
- the publication also mentions a method of bonding diamond to a semiconductor substrate of a semiconductor device using surface activated bonding. Because diamond has extremely high rigidity, it does not deform during bonding, and many voids tend to form between the semiconductor substrate and diamond. Many voids are particularly likely to form when a SiC substrate is used as the semiconductor substrate. These voids reduce heat dissipation.
- the semiconductor device comprises a substrate, a semiconductor chip including an element region on the substrate, a diamond heat conductor, and a metal layer between the semiconductor chip and the heat conductor, and the substrate has an amorphous region on its back surface.
- the amorphous region and the metal layer are bonded to each other.
- the metal layer and the heat conductor are bonded to each other.
- the element region may include a high electron mobility transistor (HEMT).
- HEMT high electron mobility transistor
- a semiconductor chip and a structure having a heat transfer body are prepared separately.
- the back surface of a semiconductor chip which has an element region formed on the surface of a substrate, is polished. This thins the substrate.
- the structure having a heat transfer body the surface of a diamond heat transfer body is polished. A metal layer is formed on this surface.
- a rare gas beam is irradiated onto the back surface of the semiconductor chip and the surface of the metal layer. As a result, an amorphous region is formed on the back surface of the semiconductor chip.
- the back surface of the semiconductor chip and the surface of the metal layer are activated.
- the back surface of the semiconductor chip and the surface of the metal layer are brought into close contact with each other, thereby bonding them.
- Patent Document 2 discloses a semiconductor device including a HEMT.
- a bonding layer, a SiC layer, and a nitride semiconductor layer are stacked in this order on the main surface of a diamond substrate.
- a source electrode, a drain electrode, and a gate electrode are formed at intervals on the main surface of the nitride semiconductor layer.
- the semiconductor device manufacturing method described in the above-mentioned International Publication may involve the following steps: First, a SiC layer and a nitride semiconductor layer are formed, in that order, on a Si substrate. Next, a HEMT is formed on the nitride semiconductor layer. Next, the entire Si substrate is removed by etching. A diamond substrate is bonded to the exposed SiC layer. According to the above-mentioned International Publication, the bonding is preferably performed using a surface activated bonding method. In this case, first, energetic particles (e.g., Ar particles) are irradiated onto the diamond substrate and the SiC layer in a reduced-pressure, room-temperature atmosphere, thereby removing adsorbed materials from the diamond substrate and the SiC layer.
- energetic particles e.g., Ar particles
- the irradiation of the energetic particles results in the appearance of an amorphous layer primarily composed of C on the diamond substrate, and an amorphous layer primarily composed of C and Si on the SiC layer.
- a bonding layer including the paired amorphous layers.
- a metal layer is provided between the semiconductor chip and the heat transfer body.
- This metal layer increases the parasitic capacitance in the semiconductor device.
- the back surface of the semiconductor chip is polished. As a result, damage caused by polishing is likely to occur to the back surface of the portion of the semiconductor device related to the operation of the HEMT, i.e., the back surface of the nitride semiconductor layer. This damage to the back surface can increase current collapse in the HEMT. In this way, damage to the back surface of the nitride semiconductor layer can degrade the performance of the semiconductor device.
- a nitride semiconductor layer is formed by homoepitaxial growth on a SiC layer provided directly on a Si substrate.
- a silicon crystal layer rather than a SiC layer, may be preferable as an underlayer for homoepitaxial growth. For example, if high in-plane uniformity in the thickness of the underlayer is required, a silicon crystal layer is more likely to meet such requirements than a SiC layer.
- a silicon-on-insulator (SOI) substrate having a structure in which an insulating layer and a silicon crystal layer serving as an underlayer are stacked in order on a Si substrate, a silicon crystal layer suitable for the underlayer can be easily prepared. Furthermore, when a semiconductor device is manufactured using the above-mentioned SOI substrate, it is also easy to remove the Si substrate, which will ultimately become unnecessary. In contrast, according to WO 2023/048160, when the entire Si substrate is removed by etching, the surface where the etching stops consists of the SiC layer, so it can be difficult to stop the etching precisely at the desired position. As a result, damage is caused to the back surface of the nitride semiconductor layer, which can lead to a decrease in the performance of the semiconductor device.
- SOI silicon-on-insulator
- the present disclosure has been made to solve the above-mentioned problems, and its purpose is to provide a semiconductor device and a method for manufacturing a semiconductor device that can suppress degradation of the performance of the semiconductor device due to damage to the back surface of the nitride semiconductor layer.
- the semiconductor device comprises a diamond substrate, a bonding layer made of an amorphous material and disposed directly on the diamond substrate, a silicon crystal layer bonded to the diamond substrate at least via the bonding layer, a buffer layer made of a nitride containing aluminum atoms and disposed on the bonding layer at least via the silicon crystal layer, and a nitride semiconductor layer disposed directly on the buffer layer and having a composition different from that of the buffer layer.
- the method for manufacturing a semiconductor device comprises: a) forming a buffer layer made of a nitride containing aluminum atoms directly or indirectly on a silicon crystal layer, the silicon crystal layer being disposed directly on an oxide layer, the oxide layer being disposed on a support substrate; b) forming a nitride semiconductor layer on the buffer layer, the nitride semiconductor layer having a composition different from that of the buffer layer; c) forming a semiconductor device structure on the nitride semiconductor layer; d) providing a protective substrate on the semiconductor device structure via an adhesive layer; e) removing the support substrate after d); f) bonding the silicon crystal layer and the polished surface of a diamond substrate to each other via at least a bonding layer, the bonding layer being disposed directly on the polished surface of the diamond substrate and on the silicon crystal layer directly or via the oxide layer; and g) removing the adhesive layer and the protective substrate.
- the buffer layer is disposed on the bonding layer with at least a silicon crystal layer interposed between them. Therefore, during the manufacture of the semiconductor device, the silicon crystal layer can continue to protect the buffer layer until the structure including the nitride semiconductor layer is bonded to the diamond substrate using the bonding layer. This allows the buffer layer to continue to protect the back surface of the nitride semiconductor layer from damage caused by any manufacturing process. This makes it possible to suppress degradation of the performance of the semiconductor device due to damage to the back surface of the nitride semiconductor layer.
- FIG. 1 is a cross-sectional view schematically showing a configuration of a semiconductor device according to a first embodiment.
- FIG. 2 is a top view schematically showing the configuration of the semiconductor device of FIG. 1;
- FIG. 2 is a flow chart schematically showing a method for manufacturing the semiconductor device according to FIG. 1;
- 2 is a cross-sectional view schematically showing a first step in the method for manufacturing the semiconductor device according to FIG. 1;
- 2 is a top view schematically showing a first step in the method for manufacturing the semiconductor device shown in FIG. 1;
- 2 is a cross-sectional view schematically showing a second step in the method for manufacturing the semiconductor device according to FIG. 1; 1.
- FIG. 4 is a cross-sectional view schematically showing a third step in the method for manufacturing the semiconductor device according to FIG.
- FIG. 4 is a cross-sectional view schematically showing a fourth step in the method for manufacturing the semiconductor device according to FIG. 1.
- FIG. 4 is a cross-sectional view schematically showing a fifth step in the method for manufacturing the semiconductor device according to FIG. 1.
- FIG. 4 is a cross-sectional view schematically showing a sixth step in the method for manufacturing the semiconductor device according to FIG. 1.
- FIG. 4 is a cross-sectional view schematically showing a seventh step in the method for manufacturing the semiconductor device according to FIG. 1.
- FIG. 4 is a cross-sectional view schematically showing an eighth step in the method for manufacturing the semiconductor device according to FIG. 1.
- FIG. 4 is a cross-sectional view schematically showing a ninth step in the method for manufacturing the semiconductor device according to FIG. 1.
- FIG. 4 is a cross-sectional view schematically showing a tenth step in the method for manufacturing the semiconductor device in FIG.
- FIG. 1 is a graph schematically showing the relationship between a drain voltage Vds and a drain current Ids in a semiconductor device.
- 1 is a graph showing a relationship between applied power P and a temperature rise ⁇ T in a current-carrying region in a semiconductor device;
- FIG. 1 is a graph schematically showing the relationship between the thickness of a silicon crystal layer and the rate of temperature rise Rth in a semiconductor device.
- FIG. 10 is a cross-sectional view schematically showing a configuration of a semiconductor device according to a second embodiment.
- FIG. 11 is a cross-sectional view schematically showing a configuration of a semiconductor device according to a third embodiment.
- FIG. 20 is a flow chart schematically showing a method for manufacturing the semiconductor device according to FIGS. 19A to 19C. 20 is a cross-sectional view schematically showing a step in the method
- First Embodiment 1 and 2 are a cross-sectional view and a top view, respectively, that schematically show the configuration of a semiconductor device 100 according to the first embodiment.
- the surface electrodes 14 are given a dotted pattern to make them easier to identify.
- the semiconductor device 100 includes a diamond substrate 16, a bonding layer 15, a silicon crystal layer 11, a buffer layer 12, and a nitride semiconductor layer 13.
- the diamond substrate 16, the bonding layer 15, the silicon crystal layer 11, the buffer layer 12, and the nitride semiconductor layer 13 may be stacked in this order as shown in FIG. 1 .
- a semiconductor device structure ES is provided on a primary surface FM1 of the nitride semiconductor layer 13.
- the semiconductor device structure ES may include a surface electrode 14.
- the semiconductor device structure ES has a HEMT structure, and the surface electrode 14 includes multiple electrode portions, namely, a gate electrode portion 14a, a source electrode portion 14b, and a drain electrode portion 14c.
- the semiconductor device structure ES may include an insulating film in addition to the surface electrode 14.
- the semiconductor device structure ES may also include a protective film for protecting its surface.
- the insulating film may be made of, for example, SiN, Al 2 O 3 , or SiO 2 .
- the protective film may be made of, for example, polyimide.
- the diamond substrate 16 is made of a single crystal diamond, a mosaic diamond, or a polycrystalline diamond.
- a mosaic diamond is made up of multiple single crystal diamonds bonded together in the in-plane direction (the lateral direction in Figure 1).
- the diamond substrate 16 may have a thickness of 50 ⁇ m or more and 600 ⁇ m or less.
- the bonding layer 15 is disposed directly on the diamond substrate 16 and is made of an amorphous material.
- the material of the bonding layer 15 may be a single-layer material or a laminated material.
- the bonding layer 15 may include an amorphous carbon layer disposed directly on the diamond substrate 16.
- the amorphous carbon layer may have a thickness of 1 nm or less.
- the bonding layer 15 may include a silicon-containing layer.
- the silicon-containing layer may be laminated on the amorphous carbon layer.
- the silicon-containing layer is a layer containing silicon atoms.
- the silicon-containing layer may further contain carbon atoms and/or oxygen atoms. Therefore, the material of the silicon - containing layer is, for example, Si, SiOx (X>0), SiC, or SiCxOy (X>0, Y>0).
- the thickness of the bonding layer 15 is preferably 1 nm or more and 10 nm or less, and more preferably 1 nm or more and 5 nm or less.
- the bonding layer 15 has a first interface IF1 in contact with the diamond substrate 16 and a second interface IF2 opposite the first interface IF1.
- the second interface IF2 is the interface between the bonding layer 15 and the silicon crystal layer 11.
- the first interface IF1 may have an arithmetic mean roughness of 0.5 nm or less.
- the upper surface of the diamond substrate 16 in FIG. 1 (corresponding to the main surface FM3 in FIG. 12) may have an arithmetic mean roughness of 0.5 nm or less.
- the second interface IF2 may have an arithmetic mean roughness of 0.5 nm or less.
- the back surface FB2 of the silicon crystal layer 11 may have an arithmetic mean roughness of 0.5 nm or less.
- the silicon crystal layer 11 is bonded to the diamond substrate 16 via at least the bonding layer 15. In the first embodiment, the silicon crystal layer 11 is directly bonded to the bonding layer 15.
- the silicon crystal layer 11 may be a single-crystal Si layer.
- the silicon crystal layer 11 serves as a base layer when the buffer layer 12 and the nitride semiconductor layer 13 are grown in sequence, in other words, as a growth substrate.
- the thickness of the silicon crystal layer 11 is preferably 0.5 ⁇ m or more and 20.0 ⁇ m or less, and more preferably 0.5 ⁇ m or more and 5.0 ⁇ m or less.
- the silicon crystal layer 11 may have a resistivity of 5000 ⁇ -cm or less.
- the buffer layer 12 is disposed on the bonding layer 15 with at least the silicon crystal layer 11 interposed therebetween. In the first embodiment, the buffer layer 12 is disposed directly on the silicon crystal layer 11.
- the thickness of the buffer layer 12 is preferably 2 ⁇ m or less.
- the buffer layer 12 is made of a nitride containing aluminum atoms. The nitride may also contain gallium atoms.
- the material of the buffer layer 12 may be a single-layer material or a laminated material made up of multiple materials with different compositions. Specifically, the material of the buffer layer 12 is, for example, AlGaN or AlN.
- the component ratio of Al atoms in the composition of the buffer layer 12 may be different from the component ratio of Al atoms in the composition of the nitride semiconductor layer 13.
- the nitride semiconductor layer 13 is disposed directly on the buffer layer 12. Taking into account the effect on heat dissipation performance, the thickness of the nitride semiconductor layer 13 is preferably 10 ⁇ m or less.
- the nitride semiconductor layer 13 has a composition different from that of the buffer layer 12.
- the material of the nitride semiconductor layer 13 may contain aluminum atoms, but does not necessarily have to.
- the material of the nitride semiconductor layer 13 may be a single-layer material or a multi-layer material.
- the single-layer material may be SiN, GaN, AlGaN, InAlN, or AlN, and may be doped with impurities such as Fe and/or C.
- the multi-layer material may be two or more of the above-mentioned materials.
- the material of the surface electrode 14 may be a single metal element or an alloy.
- the single metal element may be one element selected from the group consisting of Cu, Ti, Al, Au, Ni, Nb, Pd, Pt, Cr, W, Ta, and Mo.
- the alloy may be AlSi, AlCu, AuGe, AuGa, or AuSn.
- the material of the surface electrode 14 may be a laminate using two or more of the above-mentioned materials. If the surface electrode 14 includes multiple electrode portions, the materials of the multiple electrode portions may be the same or different.
- Figure 3 is a flow diagram that schematically illustrates the manufacturing method MM1 of the semiconductor device 100 ( Figure 1).
- Figures 4 and 5 are a cross-sectional view and a top view, respectively, that schematically illustrate the first step in the manufacturing method of the semiconductor device 100.
- Figures 6 to 14 are cross-sectional views that schematically illustrate the second to tenth steps in the manufacturing method of the semiconductor device 100, respectively.
- an SOI substrate 10 is formed.
- the SOI substrate 10 is composed of a silicon crystal layer 11, an oxide layer 19, and a support substrate 20.
- the oxide layer 19 is disposed on the support substrate 20.
- the silicon crystal layer 11 is disposed directly on the oxide layer 19.
- the thickness of the support substrate 20 is preferably 500 ⁇ m or more and 700 ⁇ m or less.
- the thickness of the oxide layer 19 is preferably 0.1 ⁇ m or more and 2.0 ⁇ m or less.
- the support substrate 20 is typically a Si substrate.
- the silicon crystal layer 11 preferably has an in-plane uniformity within 10%.
- such in-plane uniformity is satisfied in an SOI substrate 10 (wafer) having a diameter of about 50 millimeters (2 inches) or more.
- the in-plane uniformity of the silicon crystal layer 11 may be calculated based on the thickness at, for example, nine measurement points PM (FIG. 5) shown in FIG. 5.
- One of the measurement points may be approximately the center of the wafer.
- the other eight measurement points may be selected at approximately equiangular intervals (in other words, at approximately 45° intervals) on the boundary between the ineffective area at the outer edge of the wafer and the effective area inside it.
- the maximum, minimum, and average thickness values at these measurement points are used to calculate the following equation:
- In-plane uniformity (%) (maximum value - minimum value) / (average value x 2) x 100
- the in-plane uniformity may be calculated by:
- the silicon crystal layer 11 is bonded to the support substrate 20 via the oxide layer 19, and then the silicon crystal layer 11 is given the desired thickness and in-plane uniformity by grinding and polishing.
- the silicon crystal layer 11 may be deposited on the oxide layer 19 instead of being bonded thereto, and a dopant such as boron or phosphorus may be added to adjust the resistivity.
- a technique known as SIMOX separation by implanted oxygen
- the silicon crystal layer 11 and oxide layer 19 may be formed on the surface of the support substrate 20 by implanting a high concentration of oxygen ions into the interior of a single-crystal silicon substrate and then performing a high-temperature heat treatment.
- the following description of the manufacturing method will be given assuming that the support substrate 20 is a single-crystal Si substrate and the oxide layer is a silicon oxide film.
- a buffer layer 12 made of nitride is formed directly or indirectly on the silicon crystal layer 11 of the SOI substrate 10.
- the buffer layer 12 is formed directly on the silicon crystal layer 11.
- a nitride semiconductor layer 13 having a composition different from that of the buffer layer 12 is formed on the buffer layer 12. These are formed by, for example, metal organic chemical vapor deposition (MOCVD) or the like.
- MOCVD metal organic chemical vapor deposition
- step ST30 FIG. 3
- a semiconductor element structure ES is formed on the main surface FM1 of the nitride semiconductor layer 13.
- a protective substrate 18 is provided on the main surface FM1 (FIG. 7) on which the semiconductor element structure ES is provided, via an adhesive layer 17.
- the adhesive layer 17 may be made of an adhesive material containing resin.
- the protective substrate 18 is provided temporarily to protect the semiconductor element structure ES.
- the thickness of the protective substrate 18 is, for example, 500 ⁇ m or more.
- the material of the protective substrate 18 is preferably one that has high strength, and is also preferably transparent if light irradiation is used to harden the adhesive layer 17.
- the material of the protective substrate 18 is, for example, sapphire, quartz, or SiC.
- step ST50 the support substrate 20 (FIG. 8) is removed as shown in FIG. 9.
- This removal process is performed by proceeding from the main surface FM4 (FIG. 8) of the support substrate 20 and stopping on the oxide layer 19, thereby exposing the main surface FM5 of the oxide layer 19.
- This removal process may be performed by grinding, dry etching, or wet etching. It is easy to ensure a sufficient etching selectivity of the support substrate 20, such as a single-crystal Si substrate, to the oxide layer 19, such as a silicon oxide film. Therefore, it is easy to remove the support substrate 20 by etching without significantly sacrificing the oxide layer 19.
- an alkaline solution such as KOH, NaOH, or ammonia is used.
- step ST61 in step ST61 (FIG. 3), wet etching is performed with a higher etching rate for the material of the oxide layer 19 than for the material of the silicon crystal layer 11.
- the oxide layer 19 (FIG. 9) is removed while leaving the silicon crystal layer 11, as shown in FIG. 10.
- the surface roughness of the back surface FB2 of the silicon crystal layer 11 after the oxide layer 19 is removed roughly corresponds to the surface roughness of the back surface FB2 (FIG. 4) of the silicon crystal layer 11 before the oxide layer 19 is removed. It is preferable that these surface roughnesses have an arithmetic mean roughness of 0.5 nm or less.
- an activation process may be performed on the back surface FB2 of the silicon crystal layer 11. Specifically, an ion beam of a rare gas element (e.g., He, Ar, Xe, or Ne) is irradiated onto the back surface FB2. This removes impurities and deposits on the back surface FB2 and exposes dangling bonds on the irradiated surface.
- a rare gas element e.g., He, Ar, Xe, or Ne
- a diamond substrate 16 having a main surface FM3 is prepared.
- the diamond substrate 16 is preferably fabricated by chemical vapor deposition (CVD).
- the main surface FM3 of the diamond substrate 16 is polished. This polishing is preferably performed so that the main surface FM3 has an arithmetic mean roughness of 0.5 nm or less.
- a bonding layer 15 is formed on the main surface FM3 ( FIG. 12 ) of the diamond substrate 16. Therefore, the bonding layer 15 is disposed directly on the main surface FM3 ( FIG. 12 ) of the diamond substrate 16, i.e., on the polished surface of the diamond substrate 16.
- the main surface FM3 ( FIG. 12 ) of the diamond substrate 16 is first activated. Specifically, the main surface FM3 of the diamond substrate 16 is irradiated with an ion beam of a rare gas element (e.g., He, Ar, Xe, or Ne). This removes impurities and deposits on the main surface FM3 and exposes dangling bonds on the irradiated surface.
- a rare gas element e.g., He, Ar, Xe, or Ne
- the vicinity of the main surface FM3 of the diamond substrate 16 is amorphized, thereby forming an amorphous carbon layer on the diamond substrate 16 as at least a part of the bonding layer 15.
- the bonding layer 15 may then be further formed by deposition on this amorphous carbon layer. This deposition is carried out by sputtering using, for example, Si, SiO 2 or SiC as a target material.
- the silicon crystal layer 11 and the main surface FM3 (FIG. 12), which is the polished surface of the diamond substrate 16 are bonded to each other via at least the bonding layer 15.
- the bonding layer 15 is disposed directly on the silicon crystal layer 11.
- the structure including the diamond substrate 16 (FIG. 13) and the structure including the silicon crystal layer 11 (FIG. 10) are bonded to each other via the bonding layer 15.
- This bonding is preferably performed by room-temperature pressure bonding.
- the surfaces to be bonded preferably have atomic-level smoothness. Specifically, the arithmetic mean roughness of the surfaces to be bonded is preferably 0.5 nm or less.
- room-temperature pressure bonding generally involves concerns about partial delamination, the bonding layer 15 functions to prevent this. Furthermore, room-temperature pressure bonding does not require heating for bonding, so warping due to thermal stress can be avoided.
- step ST80 ( Figure 3) the adhesive layer 17 and protective substrate 18 are removed ( Figure 1). Specifically, by peeling off the adhesive layer 17, the adhesive layer 17 and protective substrate 18 are separated from the portion that will become the semiconductor device 100 ( Figure 1). This results in the semiconductor device 100.
- Figure 15 is a graph showing the relationship between drain voltage Vds and drain current Ids in a semiconductor device 100 having a HEMT structure.
- the solid line shows the characteristics when no pulse is applied
- the dashed line shows the characteristics when a pulse is applied.
- the decrease in drain current Ids (see the arrow in the figure) is related to current collapse caused by carrier traps on the back surface of the nitride semiconductor layer 13, in other words, back surface collapse.
- the silicon crystal layer 11 is left in place until the semiconductor device 100 is completed, thereby reliably protecting the back surface of the nitride semiconductor layer 13. This suppresses back surface collapse, thereby suppressing the decrease in drain current Ids.
- the silicon crystal layer 11 is located between the semiconductor element structure ES and the diamond substrate 16, heat dissipation characteristics are sacrificed to some extent.
- the dashed line in the figure corresponds to a device in which the diamond substrate 16 is omitted from the semiconductor device 100 ( Figure 1). In this device, the heat dissipation enhancement provided by the diamond substrate 16 is not achieved, resulting in a very large temperature rise ⁇ T.
- the lower of the two solid lines in the figure corresponds to a device in which the silicon crystal layer 11 is omitted from the semiconductor device 100 ( Figure 1).
- the heat dissipation enhancement provided by the diamond substrate 16 is achieved without being impeded by the silicon crystal layer 11, resulting in a significant reduction in the temperature rise ⁇ T.
- the upper of the two solid lines in the figure corresponds to a semiconductor device having both the diamond substrate 16 and the silicon crystal layer 11.
- the heat dissipation characteristics deteriorate.
- the diamond substrate 16 has a very large heat dissipation promotion effect, so as long as the silicon crystal layer 11 is not excessively thick, this heat dissipation promotion effect can be fully enjoyed.
- the bonding layer 15 is very thin and has little effect on heat dissipation, so reference to the bonding layer 15 has been omitted in the above description.
- Figure 17 is a graph that schematically shows the relationship between the thickness of the silicon crystal layer 11 of the semiconductor device 100 and the rate of temperature rise Rth per 1 W/mm in the semiconductor device 100.
- the thickness of the silicon crystal layer 11 is 20.0 ⁇ m or less, it is possible to avoid excessive sacrifice of heat dissipation characteristics due to the presence of the silicon crystal layer 11.
- its thickness is preferably 0.5 ⁇ m or more.
- its thickness is preferably 0.5 ⁇ m or more and 20.0 ⁇ m or less.
- the silicon crystal layer 11 is removed by etching and/or grinding the bottom of the structure shown in FIG. 10 and the removal process can be stopped when the back surface consisting of the buffer layer 12 is exposed, and a diamond substrate 16 is bonded to the back surface via a bonding layer 15, a semiconductor device without the silicon crystal layer 11 can be obtained.
- the silicon crystal layer 11 does not impair heat dissipation.
- the buffer layer 12 is typically very thin, it is very difficult to control the removal process to stop when the buffer layer 12 is exposed. Especially in mass production, the buffer layer 12 is easily lost, exposing the back surface of the silicon crystal layer 11. In order to bond the diamond substrate 16 to this back surface via the bonding layer 15 with sufficient strength, the back surface must be highly smooth.
- the buffer layer 12 is disposed on the bonding layer 15 with at least the silicon crystal layer 11 interposed therebetween. Therefore, in the manufacture of the semiconductor device 100, the silicon crystal layer 11 can continue to protect the buffer layer 12 until the configuration shown in FIG. 14 is obtained in step ST71 (FIG. 3), in other words, until the structure including the nitride semiconductor layer 13 is bonded to the diamond substrate 16 using the bonding layer 15. This allows the buffer layer 12 to continue to protect the back surface of the nitride semiconductor layer 13 from damage caused by any manufacturing process.
- the buffer layer 12 can continue to protect the back surface of the nitride semiconductor layer 13 from damage caused by a polishing process for smoothing or an ion beam irradiation process for activation. This makes it possible to suppress degradation of the performance of the semiconductor device 100 caused by damage to the back surface of the nitride semiconductor layer 13.
- the bonding layer 15 is made of an amorphous material. This mitigates the reduction in bonding strength caused by lattice mismatch at the bonding interface. From this perspective, it is particularly preferable that the bonding layer 15 include an amorphous carbon layer that is in direct contact with the diamond substrate 16.
- the silicon crystal layer 11 is directly bonded to the bonding layer 15. This prevents a reduction in heat dissipation caused by a component placed between the silicon crystal layer 11 and the bonding layer 15.
- the buffer layer 12 can be more reliably protected during the manufacture of the semiconductor device 100. This makes it possible to more reliably suppress a decrease in the performance of the semiconductor device 100, specifically current collapse, caused by damage to the back surface of the nitride semiconductor layer 13.
- the thickness of the silicon crystal layer 11 20.0 ⁇ m or less, preferably 5.0 ⁇ m or less, it is possible to prevent the silicon crystal layer 11 from having an excessively adverse effect on the heat dissipation from the nitride semiconductor layer 13 to the diamond substrate 16.
- the silicon crystal layer 11 be 20.0 ⁇ m or less, the rigidity of the silicon crystal layer 11 can be reduced. As a result, even if the diamond substrate 16 has a slight warp, the silicon crystal layer 11 can be easily bonded along the warp.
- This bonding process is usually performed by bonding the SOI substrate 10, which includes the portion that will become the silicon crystal layer 11 of the semiconductor device 100, to the diamond substrate 16. It is preferable that the in-plane thickness uniformity of the silicon crystal layer 11 on the SOI substrate 10 be within 10%.
- the buffer layer 12 is disposed directly on the silicon crystal layer 11. This avoids a reduction in heat dissipation caused by a component disposed between the buffer layer 12 and the silicon crystal layer 11.
- the silicon crystal layer 11 may have a resistivity of 5000 ⁇ cm or less. In this case, the occurrence of current collapse in the silicon crystal layer 11 can be suppressed.
- the bonding layer 15 may include an amorphous carbon layer disposed directly on the diamond substrate 16. This amorphous carbon layer may be formed in conjunction with activating the surface of the diamond substrate 16.
- the bonding layer 15 may include a silicon-containing layer.
- the silicon-containing layer may be, for example, a Si layer, a SiO 2 layer, or a laminate thereof formed by a sputtering method using Si or SiO 2.
- the silicon-containing layer does not need to be a semiconductor layer to which a dopant is added, and therefore can have high resistivity. This can suppress leakage current in the semiconductor device 100.
- the thickness of the bonding layer 15 1 nm or more it becomes easier to ensure sufficient bonding strength by the bonding layer 15.
- the diamond substrate 16 is made of single crystal diamond, mosaic diamond, or polycrystalline diamond. Although single crystal diamond, mosaic diamond, and polycrystalline diamond have different grain boundary configurations, they all have high thermal conductivity. Therefore, all of these are suitable materials for the diamond substrate 16. In particular, the thermal conductivity of single crystal diamond and mosaic diamond is the highest of any natural solid.
- the diamond substrate 16 may have a thickness of 50 ⁇ m or more and 600 ⁇ m or less. This thickness range is suitable for achieving high heat dissipation properties with the diamond substrate 16.
- the arithmetic mean roughness of each of the first interface IF1 and the second interface IF2 of the bonding layer 15 may be 0.5 nm or less.
- the process from FIG. 9 to FIG. 10, i.e., the process of removing the oxide layer 19 while leaving the silicon crystal layer 11, is performed by wet etching.
- wet etching which removes the oxide layer 19 while leaving the silicon crystal layer 11, can be performed with a high selectivity.
- the surface roughness of the interface between the silicon crystal layer 11 and the oxide layer 19 becomes roughly the same as the surface roughness of the interface between the silicon crystal layer 11 and the adhesive layer 17. Therefore, if the former is kept sufficiently small, the latter can also be made sufficiently small. In this case, there is no need to perform smoothing processes such as polishing after wet etching.
- the in-plane thickness uniformity of the silicon crystal layer 11 included therein can easily be kept within 10%.
- variation in the effect of the silicon crystal layer 11 on heat dissipation characteristics can be sufficiently suppressed.
- ⁇ Second Embodiment> 18 is a cross-sectional view schematically illustrating a configuration of a semiconductor device 101 according to a second embodiment.
- the semiconductor device 101 differs from the semiconductor device 100 (FIG. 1: first embodiment) in that the semiconductor device 101 includes a silicon compound layer 21 between the silicon crystal layer 11 and the buffer layer 12. Therefore, in the second embodiment, the buffer layer 12 is indirectly disposed on the silicon crystal layer 11 via the silicon compound layer 21.
- the silicon compound layer 21 may be any one of a silicon carbide layer, a silicon oxide layer, and a silicon nitride layer. Alternatively, the silicon compound layer 21 may be a layer formed by stacking two or more of these layers.
- crystal growth of the buffer layer 12 and the nitride semiconductor layer 13 can be performed on the silicon compound layer 21.
- a silicon compound layer 21 suitable for crystal growth of the buffer layer 12 lattice defects during the crystal growth can be further reduced.
- FIG. 19 is a cross-sectional view schematically illustrating the configuration of a semiconductor device 102 according to a third embodiment.
- the semiconductor device 102 differs from the semiconductor device 100 (FIG. 1: first embodiment) in that it includes an oxide layer 19.
- the oxide layer 19 is disposed between the silicon crystal layer 11 and the bonding layer 15.
- the oxide layer 19 is in direct contact with the silicon crystal layer 11 and is also directly bonded to the bonding layer 15. Therefore, the silicon crystal layer 11 is indirectly bonded to the bonding layer 15 via the oxide layer 19.
- the silicon crystal layer 11 is also bonded to the diamond substrate 16 via the oxide layer 19 and the bonding layer 15.
- the oxide layer 19 may be made of SiO 2 .
- the oxide layer 19 may have a thickness of 0.1 ⁇ m or more and 1.0 ⁇ m or less.
- the second interface IF2 of bonding layer 15 is the interface with oxide layer 19, unlike semiconductor device 100 ( Figure 1: Embodiment 1).
- the arithmetic mean roughness of second interface IF2 be 0.5 nm or less. This increases the bonding strength between bonding layer 15 and oxide layer 19.
- FIG 20 is a flow diagram that schematically illustrates a manufacturing method MM2 for the semiconductor device 102 ( Figure 19).
- the steps up to step S50 are performed to form the configuration shown in Figure 9.
- step S62 Figure 20
- the main surface FM5 of the oxide layer 19 is polished. This results in the main surface FM5 being the polished surface.
- a polished surface is formed as the main surface FM5 of the oxide layer 19.
- This polishing is preferably precision polishing using chemical mechanical polishing (CMP).
- CMP chemical mechanical polishing
- this polishing be controlled so that the thickness of the oxide layer 19 after polishing is 0.1 ⁇ m or more and 1.0 ⁇ m or less.
- step ST72 the bonding layer 15 is disposed on the silicon crystal layer 11 with the oxide layer 19 interposed therebetween, and is disposed directly on the polished surface of the oxide layer 19, which serves as the main surface FM5.
- step S80 is performed in the same manner as in the manufacturing method MM1 (FIG. 3: embodiment 1) described above, thereby forming the semiconductor device 102 (FIG. 19).
- the configuration other than the above is substantially the same as that of the first embodiment described above, and therefore the same or corresponding elements are denoted by the same reference numerals and their description will not be repeated.
- the silicon compound layer 21 ( Figure 18) described in the second embodiment may be applied to the semiconductor device 102 ( Figure 19).
- the buffer layer 12 is disposed on the bonding layer 15 via not only the silicon crystal layer 11 but also the oxide layer 19. Therefore, during the manufacture of the semiconductor device 102, until the configuration shown in FIG. 21 is obtained, in other words, until the structure including the nitride semiconductor layer 13 is bonded to the diamond substrate 16 using the bonding layer 15, not only the silicon crystal layer 11 but also the oxide layer 19 can continue to protect the buffer layer 12. This allows the buffer layer 12 to continue to protect the back surface of the nitride semiconductor layer 13 from damage caused by any manufacturing process. This prevents performance degradation of the semiconductor device 102 due to damage to the back surface of the nitride semiconductor layer 13. In particular, when ion beam processing is performed immediately before bonding to the structure including the diamond substrate 16, damage to the nitride semiconductor layer 13 caused by the ion beam can be prevented not only by the buffer layer 12 and silicon crystal layer 11 but also by the oxide layer 19.
- the bonding layer 15 is bonded to the oxide layer 19.
- the bonding layer 15 made of an amorphous material is more likely to have a better lattice match with the oxide layer 19 than with the silicon crystal layer 11. Therefore, the bonding strength can be increased compared to when the bonding layer 15 is bonded to the silicon crystal layer 11.
- the oxide layer 19 of the semiconductor device 102 may be a SiO 2 layer having a thickness of 0.1 ⁇ m or more. Although the thermal conductivity of SiO 2 is relatively low, if the thickness is not excessively large, ie, 1.0 ⁇ m or less, it is possible to avoid a significant decrease in heat dissipation caused by the oxide layer 19 being interposed between the nitride semiconductor layer 13 and the diamond substrate 16.
- a polishing step for forming a polished surface is performed, but this step is performed on the oxide layer 19. This makes it possible to suppress damage caused by the polishing step to the nitride semiconductor layer 13.
Landscapes
- Recrystallisation Techniques (AREA)
Priority Applications (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| PCT/JP2024/018675 WO2025243391A1 (ja) | 2024-05-21 | 2024-05-21 | 半導体装置および半導体装置の製造方法 |
| JP2024563355A JP7642176B1 (ja) | 2024-05-21 | 2024-05-21 | 半導体装置および半導体装置の製造方法 |
Applications Claiming Priority (1)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| PCT/JP2024/018675 WO2025243391A1 (ja) | 2024-05-21 | 2024-05-21 | 半導体装置および半導体装置の製造方法 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2025243391A1 true WO2025243391A1 (ja) | 2025-11-27 |
Family
ID=94825637
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2024/018675 Pending WO2025243391A1 (ja) | 2024-05-21 | 2024-05-21 | 半導体装置および半導体装置の製造方法 |
Country Status (2)
| Country | Link |
|---|---|
| JP (1) | JP7642176B1 (cg-RX-API-DMAC7.html) |
| WO (1) | WO2025243391A1 (cg-RX-API-DMAC7.html) |
Citations (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2010258352A (ja) * | 2009-04-28 | 2010-11-11 | Oki Data Corp | 半導体薄膜素子の製造方法並びに半導体ウエハ、及び、半導体薄膜素子 |
| JP2018206955A (ja) * | 2017-06-05 | 2018-12-27 | 富士通株式会社 | 半導体装置、電源装置、増幅器及び半導体装置の製造方法 |
| JP6771706B1 (ja) * | 2020-03-23 | 2020-10-21 | 三菱電機株式会社 | 窒化物半導体装置およびその製造方法 |
| WO2024058180A1 (ja) * | 2022-09-12 | 2024-03-21 | 公立大学法人大阪 | 半導体装置形成用基板、半導体積層構造体、半導体装置、半導体装置形成用基板の製造方法、半導体積層構造体の製造方法及び半導体装置の製造方法 |
-
2024
- 2024-05-21 WO PCT/JP2024/018675 patent/WO2025243391A1/ja active Pending
- 2024-05-21 JP JP2024563355A patent/JP7642176B1/ja active Active
Patent Citations (4)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2010258352A (ja) * | 2009-04-28 | 2010-11-11 | Oki Data Corp | 半導体薄膜素子の製造方法並びに半導体ウエハ、及び、半導体薄膜素子 |
| JP2018206955A (ja) * | 2017-06-05 | 2018-12-27 | 富士通株式会社 | 半導体装置、電源装置、増幅器及び半導体装置の製造方法 |
| JP6771706B1 (ja) * | 2020-03-23 | 2020-10-21 | 三菱電機株式会社 | 窒化物半導体装置およびその製造方法 |
| WO2024058180A1 (ja) * | 2022-09-12 | 2024-03-21 | 公立大学法人大阪 | 半導体装置形成用基板、半導体積層構造体、半導体装置、半導体装置形成用基板の製造方法、半導体積層構造体の製造方法及び半導体装置の製造方法 |
Also Published As
| Publication number | Publication date |
|---|---|
| JPWO2025243391A1 (cg-RX-API-DMAC7.html) | 2025-11-27 |
| JP7642176B1 (ja) | 2025-03-07 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP5031365B2 (ja) | エピタキシャル成長層の形成方法 | |
| JP5031364B2 (ja) | エピタキシャル成長層の形成方法 | |
| JP6772711B2 (ja) | 半導体積層構造体および半導体デバイス | |
| US10826459B2 (en) | Heterostructure and method of fabrication | |
| CN108140541B (zh) | SiC复合基板的制造方法 | |
| KR102047864B1 (ko) | 단결정 재료 사용의 개선된 효율을 갖는 유사 기판 | |
| JP5271279B2 (ja) | 高熱消散基板を製造する方法 | |
| CN104798206B (zh) | 具有工程衬底的iii族氮化物晶体管 | |
| WO2018016350A1 (ja) | 半導体基板及びその製造方法 | |
| WO2017043528A1 (ja) | SiC複合基板の製造方法及び半導体基板の製造方法 | |
| JP7279552B2 (ja) | 電子デバイス用基板およびその製造方法 | |
| CN104781907B (zh) | Iii族氮化物复合衬底及其制造方法、层叠的iii族氮化物复合衬底、iii族氮化物半导体器件及其制造方法 | |
| KR102885393B1 (ko) | 복합 기판 및 그 제조 방법 | |
| KR20220133902A (ko) | 질화갈륨/다이아몬드 웨이퍼 | |
| EP2849207B1 (en) | Heat dissipation substrate and method for producing same | |
| WO2012128268A1 (ja) | 圧電デバイス、圧電デバイスの製造方法 | |
| US11738539B2 (en) | Bonded substrate including polycrystalline diamond film | |
| US12076973B2 (en) | Bonded substrate including polycrystalline diamond film | |
| US20170221705A1 (en) | Composite substrate, semiconductor device, and method for manufacturing thereof | |
| JP4370862B2 (ja) | 積層基板の洗浄方法および基板の貼り合わせ方法 | |
| CN113013061A (zh) | 一种利用有机薄膜进行化合物半导体加工的方法 | |
| CN113841223B (zh) | 半导体基板的制造方法和半导体装置的制造方法 | |
| KR102049248B1 (ko) | 희생층을 이용한 GaN 결정층 분리 방법 | |
| JP7642176B1 (ja) | 半導体装置および半導体装置の製造方法 | |
| JP6248395B2 (ja) | Iii族窒化物複合基板およびその製造方法、積層iii族窒化物複合基板、ならびにiii族窒化物半導体デバイスおよびその製造方法 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| ENP | Entry into the national phase |
Ref document number: 2024563355 Country of ref document: JP Kind code of ref document: A |