WO2025095085A1 - 半芳香族ポリアミド樹脂、ポリアミド樹脂組成物、及び半芳香族ポリアミド樹脂の製造方法 - Google Patents
半芳香族ポリアミド樹脂、ポリアミド樹脂組成物、及び半芳香族ポリアミド樹脂の製造方法 Download PDFInfo
- Publication number
- WO2025095085A1 WO2025095085A1 PCT/JP2024/038972 JP2024038972W WO2025095085A1 WO 2025095085 A1 WO2025095085 A1 WO 2025095085A1 JP 2024038972 W JP2024038972 W JP 2024038972W WO 2025095085 A1 WO2025095085 A1 WO 2025095085A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- polyamide resin
- semi
- aromatic polyamide
- mol
- amount
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Links
Classifications
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
- C08G69/00—Macromolecular compounds obtained by reactions forming a carboxylic amide link in the main chain of the macromolecule
- C08G69/02—Polyamides derived from amino-carboxylic acids or from polyamines and polycarboxylic acids
- C08G69/26—Polyamides derived from amino-carboxylic acids or from polyamines and polycarboxylic acids derived from polyamines and polycarboxylic acids
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
- C08G69/00—Macromolecular compounds obtained by reactions forming a carboxylic amide link in the main chain of the macromolecule
- C08G69/02—Polyamides derived from amino-carboxylic acids or from polyamines and polycarboxylic acids
- C08G69/26—Polyamides derived from amino-carboxylic acids or from polyamines and polycarboxylic acids derived from polyamines and polycarboxylic acids
- C08G69/28—Preparatory processes
- C08G69/30—Solid state polycondensation
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
- C08L77/00—Compositions of polyamides obtained by reactions forming a carboxylic amide link in the main chain; Compositions of derivatives of such polymers
- C08L77/06—Polyamides derived from polyamines and polycarboxylic acids
Definitions
- the present invention relates to a semi-aromatic polyamide resin, a polyamide resin composition, and a method for producing a semi-aromatic polyamide resin. More specifically, the present invention relates to a semi-aromatic polyamide resin having excellent fatigue resistance and retention stability during melt processing, and a polyamide resin composition containing the semi-aromatic polyamide resin. The present invention also relates to a method for producing the semi-aromatic polyamide resin.
- Resin materials such as polyamide resins are widely used in parts used in automobiles and industrial machinery. Many resin products are also being put to practical use in sliding components such as gears. In recent years, there has been a trend in product development aimed at miniaturizing sliding components, particularly gears, and increasing their output. To achieve this, it is necessary to increase the torque and rotation speed applied to sliding components, specifically gears. Therefore, sliding components, specifically gears, are required to be used in higher load environments than before, and there is an increasing demand for resin materials with high fatigue resistance that can withstand high loads. Furthermore, such resin materials are also required to have lower water absorption to prevent problems caused by poor meshing due to dimensional changes caused by water absorption.
- Semi-aromatic polyamide resins derived from long-chain aliphatic diamines such as polynonamethylene terephthalamide (hereinafter referred to as PA9T) and polydecamethylene terephthalamide (hereinafter referred to as PA10T), have excellent properties such as heat resistance, rigidity, and sliding properties, as well as high dimensional stability due to low water absorption. For this reason, they are widely used in sliding components, specifically gears.
- the fatigue resistance of semi-aromatic polyamide resins is inferior to that of aliphatic polyamide resins, so there is a demand for improving the fatigue resistance of semi-aromatic polyamide resins.
- the resin materials used for sliding parts, specifically gears are required to have stability during melt processing such as kneading and molding, in other words, retention stability.
- Resin materials with low retention stability experience a drop in resin viscosity due to molecular chains being cut by heat generated during melt processing. This not only reduces mechanical properties such as fatigue resistance, but also leads to poor appearance due to the occurrence of fading, voids, and bumps.
- Patent Document 1 discloses a polyamide resin with a specific viscosity number in which the difference between the amino end group concentration and the carboxyl end group concentration is within a specified range as a semi-aromatic polyamide resin with an increased molecular weight.
- Patent Document 2 discloses a semi-aromatic polyamide resin in which the relationship between the amino end group concentration, the carboxyl end group concentration, and the end concentration in which the amino end group is blocked with carboxylic acid is controlled within a specified range.
- Patent Document 3 discloses a semi-aromatic polyamide resin in which the compatibility is improved by controlling the ratio of the amino end group concentration to the carboxylic acid end group concentration within a specified range in a semi-aromatic polyamide mainly composed of terephthalic acid and 1,10-decanediamine.
- Patent Document 4 discloses that a polyamide resin with excellent retention stability can be obtained by setting the amount of terminal amino groups in a semi-aromatic polyamide resin within a specific range, and further setting the value obtained by dividing the amount of terminal amino groups by the amount of terminal carboxyl groups to a predetermined value or greater.
- Patent Document 4 describes a semi-aromatic polyamide resin with excellent retention stability, but the examples are limited to a semi-aromatic polyamide resin with an intrinsic viscosity [ ⁇ ] of around 1.2 dl/g, and there is no description of a semi-aromatic polyamide resin with a higher intrinsic viscosity, that is, a semi-aromatic polyamide resin with a high molecular weight and excellent retention stability.
- semi-aromatic polyamide resins have poor retention stability during melt processing, and do not provide fatigue resistance.
- semi-aromatic polyamide resins have a high melting point, which means that the temperature during melt processing is high, making them susceptible to decomposition.
- the present invention aims to provide a semi-aromatic polyamide resin that has excellent fatigue resistance and retention stability during melt processing, and also has a high molecular weight.
- the present inventors have conceived the following invention and found that the above problems can be solved. That is, the present invention is as follows.
- a semi-aromatic polyamide resin containing a diamine unit and a dicarboxylic acid unit The diamine units contain 60 to 100 mol % of aliphatic diamine units having 7 to 13 carbon atoms relative to 100 mol % of the diamine units, The dicarboxylic acid unit contains 60 to 100 mol % of an aromatic dicarboxylic acid unit relative to 100 mol % of the carboxylic acid unit, The inherent viscosity ⁇ inh measured in concentrated sulfuric acid at 30° C.
- the semi-aromatic polyamide resin has a ratio of the amount of the terminal amino group [NH 2 ] to the amount of the terminal carboxyl group [COOH], that is, [NH 2 ]/[COOH], of 0.1 or more and less than 1.0.
- a polyamide resin composition containing a semi-aromatic polyamide resin containing a diamine unit and a dicarboxylic acid unit The diamine units contain 60 to 100 mol % of aliphatic diamine units having 7 to 13 carbon atoms relative to 100 mol % of the diamine units,
- the dicarboxylic acid unit contains 60 to 100 mol % of an aromatic dicarboxylic acid unit relative to 100 mol % of the carboxylic acid unit,
- the semi-aromatic polyamide resin is The weight average molecular weight Mw of the polymer is 40,000 to 90,000 in terms of polymethyl methacrylate as measured by gel permeation chromatography (GPC);
- the amount of terminal amino groups [NH 2 ] is 10 to 70 ⁇ equivalents/g;
- the amount of terminal carboxyl groups [COOH] is 10
- a molded article comprising the polyamide resin composition according to any one of [9] to [15].
- a method for producing a semi-aromatic polyamide resin containing a diamine unit and a dicarboxylic acid unit comprising the steps of: a first reaction step of subjecting a raw material including an aliphatic diamine, an aromatic dicarboxylic acid, and an end-capping agent to a polycondensation reaction to obtain a primary polycondensation reaction product; A second reaction step of solid-state polymerizing the primary polycondensation reaction product to obtain the semi-aromatic polyamide resin, the ratio x/y of the number of moles of amino groups (x) to the number of moles of carboxyl groups (y) contained in the raw material is greater than 1.01 and equal to or less than 1.03; A method for producing a semi-aromatic polyamide resin, wherein the amount of the end-capping agent contained in the raw material is 0.1 to 1.5 mol % relative to 100 mol % of the diamine contained in the raw material.
- the present invention can provide a semi-aromatic polyamide resin that has excellent fatigue resistance and retention stability during melt processing, and has a high molecular weight, and a polyamide resin composition that contains the semi-aromatic polyamide resin.
- the present embodiment is merely an example for embodying the technical idea of the present invention, and the present invention is not limited to the following description.
- preferred embodiments are shown, but a combination of two or more of the individual preferred embodiments is also a preferred embodiment.
- the lower limit and the upper limit can be selectively combined to form a preferred embodiment.
- a numerical range is stated as "XX to YY", it means “XX or more and YY or less”.
- unit means "a structural unit derived from", for example, a “dicarboxylic acid unit” means “a structural unit derived from a dicarboxylic acid”, and a “diamine unit” means “a structural unit derived from a diamine”.
- the semi-aromatic polyamide resin of this embodiment contains diamine units and dicarboxylic acid units.
- the diamine units contain 60 to 100 mol % of diamine units derived from an aliphatic diamine having 7 to 13 carbon atoms relative to 100 mol % of the diamine units
- the dicarboxylic acid units contain 60 to 100 mol % of dicarboxylic acid units derived from an aromatic dicarboxylic acid relative to 100 mol % of the dicarboxylic acid units.
- the diamine units contain 60 to 100 mol % of aliphatic diamine units having 7 to 13 carbon atoms relative to 100 mol % of the diamine units.
- the aliphatic diamine units having 7 to 13 carbon atoms may be linear diamine units and/or branched diamine units. In other words, the aliphatic diamine units having 7 to 13 carbon atoms may be at least one selected from the group consisting of linear diamine units and branched diamine units.
- the aliphatic diamine units having 7 to 13 carbon atoms may contain only one of linear diamine units or branched diamine units, or may contain both linear diamine units and branched diamine units.
- the linear diamine unit may be, for example, a diamine unit derived from at least one selected from the group consisting of 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, 1,12-dodecanediamine, and 1,13-tridecanediamine.
- Examples of the branched diamine units include 2-butyl-2-ethyl-1,5-pentanediamine, 2,2,4-trimethyl-1,6-hexanediamine, 2,4,4-trimethyl-1,6-hexanediamine, 2-methyl-1,8-octanediamine, 3-methyl-1,8-octanediamine, 1,3-dimethyl-1,8-octanediamine, 1,4-dimethyl-1,8-octanediamine, 2,4-dimethyl-1,8-octanediamine, 3,4-dimethyl-1,8-octanediamine, 4,5-dimethyl-1,8-octanediamine,
- the diamine units are derived from at least one selected from the group consisting of 2,2-dimethyl-1,8-octanediamine, 3,3-dimethyl-1,8-octanediamine, 4,4-dimethyl-1,8-octanediamine, 2-methyl-1,9-nonanediamine
- the aliphatic diamine unit having 7 to 13 carbon atoms is preferably a diamine unit derived from at least one selected from the group consisting of 1,9-nonanediamine, 1,10-decanediamine, and 2-methyl-1,8-octanediamine, and more preferably a diamine unit derived from 1,9-nonanediamine and/or a diamine unit derived from 2-methyl-1,8-octanediamine.
- the aliphatic diamine unit having 7 to 13 carbon atoms is more preferably a diamine unit derived from at least one selected from the group consisting of 1,9-nonanediamine and 2-methyl-1,8-octanediamine.
- the aliphatic diamine unit having 7 to 13 carbon atoms is preferably a diamine unit derived from 1,9-nonanediamine and a diamine unit derived from 2-methyl-1,8-octanediamine.
- the aliphatic diamine units having 7 to 13 carbon atoms include both diamine units derived from 1,9-nonanediamine and diamine units derived from 2-methyl-1,8-octanediamine
- the molar ratio of diamine units derived from 1,9-nonanediamine/diamine units derived from 2-methyl-1,8-octanediamine is preferably in the range of 95/5 to 40/60, and more preferably in the range of 90/10 to 50/50.
- the diamine units contain 60 to 100 moles of the aliphatic diamine units having 7 to 13 carbon atoms per 100 moles of the diamine units. From the viewpoints of mechanical properties and heat resistance, the diamine units preferably contain 70 to 100 moles of the aliphatic diamine units having 7 to 13 carbon atoms, more preferably 80 to 100 moles, and even more preferably 90 to 100 moles. The diamine units may contain 100 moles of the aliphatic diamine units having 7 to 13 carbon atoms.
- the diamine unit may contain a diamine unit derived from a diamine other than the aliphatic diamine unit, as long as the effect of the present invention is not impaired.
- the diamine unit derived from the other diamine include a diamine unit derived from at least one diamine selected from the group consisting of an alicyclic diamine and an aromatic diamine.
- the diamine unit derived from the alicyclic diamine includes a diamine unit derived from at least one selected from the group consisting of cyclohexanediamine, methylcyclohexanediamine, isophoronediamine, norbornanedimethylamine, and tricyclodecanedimethyldiamine.
- diamine unit derived from the aromatic diamine examples include a diamine unit derived from at least one selected from the group consisting of p-phenylenediamine, m-phenylenediamine, p-xylylenediamine, m-xylylenediamine, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylsulfone, and 4,4'-diaminodiphenylether.
- the diamine unit may contain only one type of diamine unit derived from these other diamines, or may contain two or more types.
- the content of the diamine units derived from the other diamines in the diamine units is less than 40 mol % relative to 100 mol % of the diamine units, preferably 30 mol % or less, more preferably 20 mol % or less, and even more preferably 10 mol % or less.
- the content of the diamine units derived from the other diamines in the diamine units is preferably 0 mol% or more and less than 40 mol%, more preferably 0 mol% or more and 30 mol% or less, even more preferably 0 mol% or more and 20 mol% or less, and even more preferably 0 mol% or more and 10 mol% or less, relative to 100 mol% of the diamine units.
- the content of the diamine units derived from the other diamines in the diamine units may be 0 mol%.
- the dicarboxylic acid units contain 60 to 100 mol % of aromatic dicarboxylic acid units relative to 100 mol % of dicarboxylic acid units.
- aromatic dicarboxylic acid unit examples include dicarboxylic acid units derived from at least one selected from the group consisting of terephthalic acid, isophthalic acid, diphenic acid, 4,4'-biphenyldicarboxylic acid, diphenylmethane-4,4'-dicarboxylic acid, diphenylsulfone-4,4'-dicarboxylic acid, 1,2-naphthalenedicarboxylic acid, 1,3-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 1,6-naphthalenedicarboxylic acid, 1,7-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, 2,3-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 2,3-furandicarboxylic acid,
- the aromatic dicarboxylic acid unit is preferably an aromatic dicarboxylic acid unit derived from terephthalic acid.
- the ratio of the aromatic dicarboxylic acid unit contained in the dicarboxylic acid unit is 60 mol% or more relative to 100 mol% of the dicarboxylic acid unit. From the viewpoint of mechanical properties and heat resistance, the ratio of the aromatic dicarboxylic acid unit is preferably 70 mol% or more, more preferably 80 mol% or more, and even more preferably 90 mol% or more. The ratio of the aromatic dicarboxylic acid unit contained in the dicarboxylic acid unit may be 100 mol%.
- the dicarboxylic acid unit preferably contains 70 to 100 mol %, more preferably 80 to 100 mol %, and even more preferably 90 to 100 mol % of aromatic dicarboxylic acid units relative to 100 mol % of dicarboxylic acid units.
- the dicarboxylic acid unit may contain a dicarboxylic acid unit derived from a dicarboxylic acid other than an aromatic dicarboxylic acid, as long as the effect of the present invention is not impaired.
- the other dicarboxylic acid include an aliphatic dicarboxylic acid and an alicyclic dicarboxylic acid.
- dicarboxylic acid unit derived from an aliphatic dicarboxylic acid examples include a dicarboxylic acid unit derived from at least one selected from the group consisting of oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedicarboxylic acid, dodecanedicarboxylic acid, dimethylmalonic acid, 2,2-diethylsuccinic acid, 2,2-dimethylglutaric acid, 2-methyladipic acid, and trimethyladipic acid.
- dicarboxylic acid unit derived from the alicyclic dicarboxylic acid examples include a dicarboxylic acid unit derived from at least one selected from the group consisting of 1,3-cyclopentanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, cycloheptanedicarboxylic acid, cyclooctanedicarboxylic acid, and cyclodecanedicarboxylic acid.
- the dicarboxylic acid unit may contain only one type of dicarboxylic acid unit derived from these other dicarboxylic acids, or may contain two or more types of dicarboxylic acid units derived from these other dicarboxylic acids.
- the content of the dicarboxylic acid units derived from the other dicarboxylic acids contained in the dicarboxylic acid units is less than 40 mol % relative to 100 mol % of the dicarboxylic acid units, preferably 30 mol % or less, more preferably 20 mol % or less, and even more preferably 10 mol % or less.
- the content of the dicarboxylic acid units derived from the other dicarboxylic acid in the dicarboxylic acid units is preferably 0 mol% or more and less than 40 mol%, more preferably 0 mol% or more and 30 mol% or less, even more preferably 0 mol% or more and 20 mol% or less, and even more preferably 0 mol% or more and 10 mol% or less, relative to 100 mol% of the dicarboxylic acid units.
- the content of the diamine units derived from the other dicarboxylic acid in the dicarboxylic acid units may be 0 mol%.
- the ratio of the diamine units and the dicarboxylic acid units in 100 mol% of the semi-aromatic polyamide resin of this embodiment is preferably 70 mol% or more, more preferably 80 mol% or more, even more preferably 90 mol% or more, may be 95 mol% or more, or may even be 100 mol%.
- the ratio of the diamine units and the dicarboxylic acid units in 100 mol% of the semi-aromatic polyamide resin of this embodiment is preferably 70 mol% or more and 100 mol% or less, more preferably 80 mol% or more and 100 mol% or less, even more preferably 90 mol% or more and 100 mol% or less, and may be 95 mol% or more and 100 mol% or less, or may even be 100 mol%.
- the semi-aromatic polyamide resin of this embodiment may further contain aminocarboxylic acid units in addition to the diamine units and dicarboxylic acid units.
- the amino carboxylic acid unit include an amino carboxylic acid unit derived from at least one selected from the group consisting of lactams such as caprolactam and lauryllactam, and amino carboxylic acids such as 11-aminoundecanoic acid and 12-aminododecanoic acid.
- the content of the amino carboxylic acid unit in the semi-aromatic polyamide resin is preferably 30 mol % or less, and more preferably 20 mol % or less, relative to 100 mol % in total of the diamine unit and the dicarboxylic acid unit in the semi-aromatic polyamide resin.
- the content of the aminocarboxylic acid units in the semi-aromatic polyamide resin is preferably 0 mol % or more and 30 mol % or less, more preferably 0 mol % or more and 20 mol % or less, even more preferably 0 mol % or more and 10 mol % or less, and even more preferably 0 mol % or more and 5 mol % or less, relative to 100 mol % of the total of the diamine units and the dicarboxylic acid units in the semi-aromatic polyamide resin.
- the semi-aromatic polyamide resin of this embodiment may also contain structural units derived from trivalent or higher polyvalent carboxylic acids such as trimellitic acid, trimesic acid, and pyromellitic acid, to the extent that melt molding is possible, as long as the effects of the present invention are not impaired.
- End sealing rate In the semi-aromatic polyamide resin of this embodiment, from the viewpoint of melt stability and hydrolysis resistance, it is preferable that the terminal groups of the molecular chain of the semi-aromatic polyamide resin are blocked.
- a terminal blocking agent can be used to block the terminal groups. The details of this terminal blocking agent will be described later.
- the proportion of blocked terminal groups among all terminal groups of the molecular chain of the semi-aromatic polyamide resin is called the terminal blocking rate. This terminal blocking rate is preferably 5 mol% or more, and more preferably 10 mol% or more.
- the terminal blocking rate is preferably 40 mol% or less, and more preferably 30 mol% or less.
- the terminal blocking rate is preferably 5 to 40 mol%, more preferably 10 to 30 mol%, and even more preferably 10 to 20 mol%.
- the terminal capping rate of the semi-aromatic polyamide resin can be calculated by measuring the amount of terminal carboxyl groups, the amount of terminal amino groups, and the amount of terminal groups capped with a terminal capping agent in the semi-aromatic polyamide resin, and then calculating it from the following formula (1):
- A represents the total amount of terminal groups (usually equal to twice the number of molecules of the semi-aromatic polyamide resin)
- B represents the total amount of terminal carboxyl groups and terminal amino groups.
- Terminal sealing rate (%) [(AB)/A] x 100 Formula (1)
- the amount of each of the terminal groups in the semi-aromatic polyamide resin of the present embodiment is a value calculated from the integral value of the characteristic signal of each terminal group by subjecting the semi-aromatic polyamide resin dissolved in deuterated 1,1,1,3,3,3-hexafluoroisopropanol to 1H -NMR analysis at 600 MHz and 50° C. More specifically, it can be determined by the method described in the Examples.
- the inherent viscosity ⁇ inh of the semi-aromatic polyamide resin of this embodiment is 1.6 to 3.0 dl/g.
- the inherent viscosity ⁇ inh is preferably 1.7 dl/g or more, more preferably 1.8 dl/g or more, and even more preferably 1.9 dl/g or more.
- the semi-aromatic polyamide resin can be made to have excellent fatigue resistance.
- the inherent viscosity ⁇ inh is preferably 2.7 dl/g or less, more preferably 2.5 dl/g or less, and even more preferably 2.3 dl/g or less.
- the semi-aromatic polyamide resin can be made to have excellent moldability and retention stability.
- the inherent viscosity ⁇ inh is preferably 1.7 to 2.7 dl/g, more preferably 1.7 to 2.5 dl/g, even more preferably 1.8 to 2.5 dl/g, even more preferably 1.9 to 2.5 dl/g, and most preferably 1.9 to 2.3 dl/g.
- the inherent viscosity ⁇ inh can be determined by measuring the flow time of a solution in which concentrated sulfuric acid is used as a solvent at a concentration of 0.2 g/dl and a temperature of 30° C. More specifically, it can be determined by the method described in the examples.
- the amount of terminal amino groups [NH 2 ] of the semi-aromatic polyamide resin of this embodiment is 10 to 70 ⁇ equivalents/g.
- the amount of terminal amino groups [NH 2 ] is preferably 15 ⁇ equivalents/g or more, more preferably 20 ⁇ equivalents/g or more, even more preferably 30 ⁇ equivalents/g or more, and even more preferably 40 ⁇ equivalents/g or more.
- the amount of terminal amino groups [NH 2 ] is in the above range, the inherent viscosity ⁇ inh indicating the molecular weight of the semi-aromatic polyamide resin is in the desired range, so that the fatigue resistance is more excellent.
- the amount of terminal amino groups [NH 2 ] is preferably 60 ⁇ equivalents/g or less, more preferably 50 ⁇ equivalents/g or less, and even more preferably 45 ⁇ equivalents/g or less.
- the amount of the terminal amino group [NH 2 ] is preferably 10 to 60 ⁇ equivalents/g, more preferably 10 to 50 ⁇ equivalents/g, even more preferably 15 to 50 ⁇ equivalents/g, and even more preferably 15 to 45 ⁇ equivalents/g.
- the amount of terminal carboxyl groups [COOH] of the semi-aromatic polyamide resin of this embodiment is 10 to 90 ⁇ equivalents/g.
- the amount of terminal carboxyl groups [COOH] is preferably 20 ⁇ equivalents/g or more, more preferably 30 ⁇ equivalents/g or more, even more preferably 40 ⁇ equivalents/g or more, and even more preferably 55 ⁇ equivalents/g or more.
- the amount of terminal carboxyl groups [COOH] is in the above range, the inherent viscosity ⁇ inh indicating the molecular weight of the semi-aromatic polyamide resin is in the desired range, so that the fatigue resistance is more excellent.
- the amount of terminal carboxyl groups [COOH] is preferably 85 ⁇ equivalents/g or less, more preferably 80 ⁇ equivalents/g or less.
- the amount of the terminal carboxyl group [COOH] is preferably 20 to 85 ⁇ equivalents/g, more preferably 30 to 80 ⁇ equivalents/g, even more preferably 40 to 80 ⁇ equivalents/g, and even more preferably 55 to 80 ⁇ equivalents/g.
- the amount of terminal amino groups [ NH2 ] refers to the amount of terminal amino groups (unit: ⁇ equivalents/g) contained in 1 g of the semi-aromatic polyamide resin
- the amount of terminal carboxyl groups [COOH] refers to the amount of terminal carboxyl groups (unit: ⁇ equivalents/g) contained in 1 g of the semi-aromatic polyamide resin.
- the amount of terminal amino groups [NH 2 ] and the amount of terminal carboxyl groups [COOH] of the semi-aromatic polyamide resin of the present embodiment are values calculated from the integral value of the characteristic signal of each terminal group when the semi-aromatic polyamide resin is dissolved in deuterated 1,1,1,3,3,3-hexafluoroisopropanol and subjected to 1 H-NMR analysis under conditions of 600 MHz and 50° C. More specifically, they can be determined by the method described in the Examples.
- the ratio [NH 2 ]/[COOH] of the amount of terminal amino groups [NH 2 ] to the amount of terminal carboxyl groups [COOH] of the semi-aromatic polyamide resin of this embodiment is 0.1 or more and less than 1.0.
- the ratio [NH 2 ]/[COOH] is preferably 0.2 to 0.9, more preferably 0.2 to 0.8, even more preferably 0.2 to 0.7, and even more preferably 0.3 to 0.7.
- the ratio [NH 2 ]/[COOH] is within the above range, the inherent viscosity ⁇ inh indicating the molecular weight of the semi-aromatic polyamide resin is in the desired range, so that the fatigue resistance is more excellent.
- crosslinking and hydrolysis between terminal amino groups during melt processing are suppressed, and the semi-aromatic polyamide resin has excellent retention stability.
- the weight average molecular weight of the semi-aromatic polyamide resin of this embodiment is preferably 40,000 or more, more preferably 45,000 or more, and even more preferably 50,000 or more, from the viewpoint of fatigue resistance. Also, the weight average molecular weight of the semi-aromatic polyamide resin is preferably 90,000 or less, more preferably 80,000 or less, and even more preferably 70,000 or less, from the viewpoint of moldability. The weight average molecular weight of the semi-aromatic polyamide resin is preferably 40,000 to 90,000, more preferably 45,000 to 80,000, and even more preferably 50,000 to 70,000.
- the semi-aromatic polyamide resin of this embodiment preferably has a weight average molecular weight (hereinafter also referred to as Mw) decrease rate of 20% or less before and after melt kneading. This makes it possible to improve the retention stability.
- Mw weight average molecular weight
- the melt kneading may be performed by melt kneading only the semi-aromatic polyamide resin alone, or by mixing it with other components and melt kneading it as a composition.
- the decrease rate of the weight average molecular weight is calculated by the following formula (2).
- Mw 0 is the weight average molecular weight before melt kneading
- Mw 1 is the weight average molecular weight after melt kneading at a cylinder temperature of 320 to 325°C using a twin-screw extruder.
- Reduction rate of weight average molecular weight (Mw 0 ⁇ Mw 1 ) ⁇ 100/Mw 0 (2)
- the decrease rate of the weight average molecular weight is more preferably 18% or less, and even more preferably 15% or less.
- the melt-kneading is carried out using a twin-screw extruder "BTN-32-S2-30-L" manufactured by Plastics Engineering Research Institute Co., Ltd. as the twin-screw extruder, at a cylinder temperature of 320 to 325°C and a residence time of 1 to 5 minutes, and more specifically, can be carried out by the method described in the Examples.
- the weight average molecular weight of the semi-aromatic polyamide resin is a value determined by gel permeation chromatography (GPC) in terms of a standard polymethyl methacrylate molecular weight. More specifically, it can be determined by the method described in the examples.
- the semi-aromatic polyamide resin of this embodiment preferably has a melting point of 250°C or more, more preferably 280°C or more, and even more preferably 290°C or more.
- the semi-aromatic polyamide resin can be made to have excellent heat resistance.
- the upper limit of the melting point of the semi-aromatic polyamide resin is preferably 330°C or less, more preferably 320°C or less, and even more preferably 310°C or less.
- the melting point of the semi-aromatic polyamide resin is preferably 250 to 330°C, more preferably 280 to 320°C, even more preferably 290 to 320°C, and even more preferably 290 to 310°C.
- the melting point of the semi-aromatic polyamide resin is a value determined as a peak temperature of an endothermic peak that appears when the temperature is raised at a rate of 10° C./min using a differential scanning calorimetry (DSC) analyzer. More specifically, it can be determined by the method described in the Examples.
- the semi-aromatic polyamide resin of this embodiment preferably has a heat of fusion ⁇ Hm of 20 mJ/mg or more, more preferably 30 mJ/mg or more, and even more preferably 40 mJ/mg or more.
- a heat of fusion ⁇ Hm of 20 mJ/mg or more, more preferably 30 mJ/mg or more, and even more preferably 40 mJ/mg or more.
- the heat of fusion ⁇ Hm of the semi-aromatic polyamide resin is preferably as high as possible, but from the viewpoint of moldability, it is preferably 80 mJ/mg or less, more preferably 70 mJ/mg or less, and even more preferably 60 mJ/mg or less.
- the heat of fusion ⁇ Hm is preferably 20 to 80 mJ/mg, more preferably 30 to 70 mJ/mg, even more preferably 30 to 60 mJ/mg, even more preferably 40 to 60 mJ/mg, and even more preferably 40 to 50 mJ/mg.
- the heat of fusion ⁇ Hm of the semi-aromatic polyamide resin is a value determined as the peak area of an endothermic peak appearing when the temperature is raised at a rate of 10° C./min using a differential scanning calorimetry (DSC) analyzer. More specifically, it can be determined by the method described in the Examples.
- DSC differential scanning calorimetry
- a raw material containing an aliphatic diamine, an aromatic dicarboxylic acid, and an end-capping agent is melt-polymerized and polycondensed.
- a preparation step for preparing the raw material may be provided before the first reaction step.
- the raw material preferably contains an aliphatic diamine, an aromatic dicarboxylic acid, and an end-capping agent.
- the raw material preferably contains a catalyst and other components as necessary.
- the ratio (x/y) of the number of moles of amino groups (x) and the number of moles of carboxyl groups (y) contained in the raw material is greater than 1.01 and not more than 1.03, preferably 1.015 to 1.025, and more preferably 1.02 to 1.03.
- the number of moles of amino groups (x) is the sum of the number of moles of amino groups derived from the aliphatic diamine, the terminal blocking agent having an amino group, and other components
- the number of moles of carboxyl groups (y) is the sum of the number of moles of carboxyl groups derived from the aromatic carboxylic acid, the terminal blocking agent having a carboxyl group, and other components.
- the raw material contains an end-capping agent.
- the amount of the terminal blocking agent contained in the raw material is preferably 5.0 mol% or less, more preferably 3.0 mol% or less, and even more preferably 1.5 mol% or less, based on 100 mol% of the diamine units contained in the raw material. Also, it is preferably 0.1 mol% or more, more preferably 0.5 mol% or more, and even more preferably 0.7 mol% or more.
- the amount of the terminal blocking agent is preferably 0.1 to 5.0 mol%, more preferably 0.5 to 3.0 mol%, and even more preferably 0.7 to 1.5 mol%, based on 100 mol% of the diamine units contained in the raw material.
- a monofunctional compound that is reactive with the amino group or carboxyl group at the end of the molecular chain of the semi-aromatic polyamide resin can be used.
- Specific examples include monocarboxylic acids, acid anhydrides, monoisocyanates, monoacid halides, monoesters, monoalcohols, and monoamines. From the viewpoints of reactivity and stability of terminal blocking, monocarboxylic acids are preferred as terminal blocking agents for amino groups. Furthermore, monoamines are preferred as terminal blocking agents for carboxyl groups. From the viewpoints of ease of handling, monocarboxylic acids are more preferred as terminal blocking agents.
- the monocarboxylic acid used as the terminal blocking agent is not particularly limited as long as it is reactive with amino groups, and examples thereof include aliphatic monocarboxylic acids such as acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, pivalic acid, and isobutyric acid; alicyclic monocarboxylic acids such as cyclopentane carboxylic acid and cyclohexane carboxylic acid; aromatic monocarboxylic acids such as benzoic acid, toluic acid, ⁇ -naphthalene carboxylic acid, ⁇ -naphthalene carboxylic acid, methylnaphthalene carboxylic acid, and phenyl acetic acid; and any mixtures thereof.
- aliphatic monocarboxylic acids such as acetic acid, propionic acid, butyric acid, valeric
- At least one selected from the group consisting of acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecanoic acid, myristic acid, palmitic acid, stearic acid, and benzoic acid is preferred in terms of reactivity, stability of the blocked terminal, and price.
- the monoamine used as the terminal blocking agent is not particularly limited as long as it is reactive with carboxyl groups, and examples thereof include aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, and dibutylamine; alicyclic monoamines such as cyclohexylamine and dicyclohexylamine; aromatic monoamines such as aniline, toluidine, diphenylamine, and naphthylamine; and any mixtures thereof.
- aliphatic monoamines such as methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, and dibutylamine
- At least one selected from the group consisting of butylamine, hexylamine, octylamine, decylamine, stearylamine, cyclohexylamine, and aniline is preferred in terms of reactivity, high boiling point, stability of blocked terminals, and price.
- a catalyst When producing the semi-aromatic polyamide resin of this embodiment, a catalyst can be added.
- the amount of the catalyst used is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and preferably 1.0% by mass or less, and more preferably 0.5% by mass or less, based on the total mass of the raw materials. If the amount of the catalyst used is above the lower limit, polymerization proceeds well. If the amount is below the upper limit, impurities derived from the catalyst are less likely to be generated, and for example, when the polyamide resin composition containing the semi-aromatic polyamide resin of the present invention is extrusion molded, problems due to the impurities can be prevented.
- the amount of the catalyst used is preferably 0.01 to 1.0% by mass, more preferably 0.05 to 0.5% by mass, based on the total mass of the raw materials.
- phosphoric acid, phosphorous acid, hypophosphorous acid, salts or esters thereof can be used.
- the salts or esters include salts of phosphoric acid, phosphorous acid or hypophosphorous acid with metals such as potassium, sodium, magnesium, vanadium, calcium, zinc, cobalt, manganese, tin, tungsten, germanium, titanium and antimony; ammonium salts of phosphoric acid, phosphorous acid or hypophosphorous acid; ethyl esters, isopropyl esters, butyl esters, hexyl esters, isodecyl esters, octadecyl esters, decyl esters, stearyl esters and phenyl esters of phosphoric acid, phosphorous acid or hypophosphorous acid.
- a primary polycondensation reaction product is obtained.
- a raw material containing an aliphatic diamine, an aromatic dicarboxylic acid, and an end-capping agent is polycondensed by melt polymerization to obtain a primary polycondensation reaction product.
- the raw material may contain an aliphatic diamine, an aromatic dicarboxylic acid, and an end-capping agent, and may be mixed all at once or may be mixed by adding a part of it separately later.
- the polymerization temperature is preferably 200 to 270°C, more preferably 240 to 260°C.
- the degree of polymerization of the primary polycondensation reaction product is increased, and the occurrence of fusion or aggregation of the polycondensation reaction product during the solid-phase polymerization in the subsequent step and the collapse of the molar balance between the dicarboxylic acid component and the diamine component can be suppressed.
- a semi-aromatic polyamide resin is obtained.
- the semi-aromatic polyamide resin is obtained by solid-state polymerization of the primary polycondensation reaction product.
- a method of solid-state polymerization it is preferable to carry out solid-state polymerization of the primary polycondensation reaction product at a temperature of 200° C. or higher and lower than the melting point of the semi-aromatic polyamide resin.
- the solid-state polymerization temperature is the reaction temperature during solid-state polymerization, and is more preferably 215° C. or higher, and even more preferably 230° C. or higher.
- heating and stirring in which the mixture is stirred while being heated is preferable.
- any method that can uniformly heat and stir may be used, and for example, a horizontal heating and stirring device may be used. If the solid-state polymerization temperature is lower than 200°C, it takes a long time to reach the desired molecular weight (inherent viscosity ⁇ inh ), and the productivity decreases.
- the solid-state polymerization temperature is equal to or higher than the melting point of the primary polycondensation reactant, the primary polycondensation reactant is likely to undergo fusion, aggregation, adhesion to the vessel wall, coloring, or the molar balance is easily disrupted due to the volatilization of the dicarboxylic acid component and diamine component constituting the primary polycondensate during solid-state polymerization. Therefore, it is preferable to carry out the solid-state polymerization of the primary polycondensation reactant within a temperature range of 100°C lower to 40°C lower than the melting point of the primary polycondensate.
- the semi-aromatic polyamide resin may be a polyamide resin composition.
- the polyamide resin composition contains at least the semi-aromatic polyamide resin.
- the polyamide resin composition preferably contains the semi-aromatic polyamide resin in an amount of 50% by mass or more and less than 100% by mass, more preferably 60 to 99.5% by mass, even more preferably 70 to 99% by mass, and even more preferably 80 to 99% by mass.
- the polyamide resin composition can have excellent retention stability during molding and excellent heat aging resistance.
- the polyamide resin composition of the present embodiment preferably contains the semi-aromatic polyamide resin and a crystal nucleating agent.
- the polyamide resin composition preferably contains 0.01 to 10 parts by mass of a nucleating agent relative to 100 parts by mass of the semi-aromatic polyamide resin, more preferably 0.1 to 5 parts by mass, even more preferably 1 to 5 parts by mass, and even more preferably 1 to 3 parts by mass.
- crystal nucleating agent examples include metal oxides such as zinc oxide, magnesium oxide, iron oxide, antimony oxide, titanium oxide, alumina, and silica, inorganic salts such as sodium carbonate, potassium carbonate, calcium carbonate, zinc carbonate, magnesium carbonate, calcium silicate, lead silicate, magnesium silicate, calcium phosphate, lead phosphate, calcium sulfate, and barium sulfate, clays such as talc, kaolin, mica, and acid clay, organic acid salts such as calcium oxalate, calcium benzoate, magnesium stearate, and zinc salicylate, high-melting point polymers such as polyamide 6T and polyamide 46, powder simple substances such as zinc powder, aluminum powder, graphite powder, and carbon black, p-t-butylbenzoic aluminum, bis(4-t-butylphenyl)sodium phosphate, 2,2'-methylenebis(4,6-di-t-butylphenyl)sodium phosphate, and di
- the average particle size of the crystal nucleating agent is preferably 0.01 to 20 ⁇ m or less, more preferably 0.5 to 15 ⁇ m or less, and even more preferably 1 to 10 ⁇ m or less.
- the average particle size of the crystal nucleating agent can be obtained by the following method. A molded product made of a polyamide resin composition containing a crystal nucleating agent is dissolved in a solvent such as formic acid in which polyamide is soluble.
- the insoluble component obtained is observed with an optical microscope or a scanning electron microscope, and the average value of the maximum Feret diameter of 100 or more crystal nucleating agents can be taken as the average particle size.
- the Feret diameter is the distance between two straight lines when the crystal nucleating agent is sandwiched between two parallel straight lines.
- the crystal nucleating agent may be treated with a silane coupling agent, a titanium coupling agent, or the like, as necessary.
- the silane coupling agent is not particularly limited, but examples thereof include aminosilane-based coupling agents such as ⁇ -aminopropyltriethoxysilane, ⁇ -aminopropyltrimethoxysilane, and N- ⁇ -(aminoethyl)- ⁇ -aminopropylmethyldimethoxysilane; mercaptosilane-based coupling agents such as ⁇ -mercaptopropyltrimethoxysilane and ⁇ -mercaptopropyltriethoxysilane; epoxysilane-based coupling agents; and vinylsilane-based coupling agents. These silane coupling agents may be used alone or in combination of two or more.
- the polyamide resin composition of the present embodiment preferably contains the semi-aromatic polyamide resin and an antioxidant.
- the polyamide resin composition preferably contains 0.01 to 5 parts by mass, more preferably 0.05 to 3 parts by mass, and even more preferably 0.1 to 2 parts by mass of an antioxidant relative to 100 parts by mass of the semi-aromatic polyamide resin.
- an antioxidant By containing the antioxidant in the above range, a polyamide resin composition having excellent retention stability during molding and excellent heat aging resistance can be obtained.
- antioxidants examples include organic antioxidants such as phenol-based antioxidants, phosphorus-based antioxidants, sulfur-based antioxidants, and amine-based antioxidants, and inorganic antioxidants such as copper compounds and halides.
- the antioxidant may be used alone or in combination of two or more kinds.
- the antioxidants from the viewpoint of excellent heat aging resistance, at least one selected from the group consisting of a phenol-based antioxidant, an amine-based antioxidant, and a combination of a copper compound and a halide is preferred.
- phenol-based antioxidant examples include 2,2-thio-diethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexane-1,6-diyl bis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide)], pentaerythrityl-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylene bis(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide triethylene glycol bis(3-tert-butyl-4-hydroxy-5-methylphenyl)propionate, hexamethylene bis(3-(3,5-di-tert 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris(4-
- the phenol-based antioxidant is preferably at least one selected from N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxyphenyl)propionamide and 3,9-bis ⁇ 2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl ⁇ -2,4,8,10-tetraoxaspiro[5.5]undecane.
- the phosphorus-based antioxidants include, for example, monosodium phosphate, disodium phosphate, trisodium phosphate, sodium phosphite, calcium phosphite, magnesium phosphite, manganese phosphite, pentaerythritol-type phosphite compounds, trioctyl phosphite, trilauryl phosphite, octyl diphenyl phosphite, trisisodecyl phosphite, phenyl diisodecyl phosphite, phenyl di(tridecyl)phosphite, diphenyl isooctyl phosphite, diphenyl isodecyl phosphite, diphenyl isodecyl phosphite, diphenyl (tridecyl)phosphite, triphenyl
- sulfur-based antioxidants examples include distearyl 3,3'-thiodipropionate, pentaerythrityl tetrakis (3-lauryl thiopropionate), 2-mercaptobenzimidazole, didodecyl 3,3'-thiodipropionate, ditridecyl 3,4'-thiodipropionate, 2,2-bis[[3-(dodecylthio)-1-oxopropoxy]methyl]-1,3-propanediyl ester, and the like.
- amine-based antioxidant examples include 4,4'-bis( ⁇ , ⁇ -dimethylbenzyl)diphenylamine (such as "Nocrak CD” manufactured by Ouchi Shinko Chemical Industry Co., Ltd. and "Naugard 445" manufactured by Addiband Japan Co., Ltd.), N,N'-di-2-naphthyl-p-phenylenediamine (such as "Nocrak White” manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), N,N'-diphenyl-p-phenylenediamine (such as "Nocrak DP” manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), N-phenyl-1-naphthylamine (such as "Nocrak PA” manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), N-phenyl-N'-isopropyl-p-phenylenediamine (such as "Nocrak 810-NA” manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), N
- Examples of the copper compound include copper halides, copper acetate, copper propionate, copper benzoate, copper adipate, copper terephthalate, copper isophthalate, copper salicylate, copper nicotinate, copper stearate, and copper complex salts coordinated with chelating agents such as ethylenediamine and ethylenediaminetetraacetic acid.
- Examples of the copper halide include copper iodide; copper bromides such as copper (I) bromide and copper (II) bromide; and copper chlorides such as copper (I) chloride.
- At least one selected from the group consisting of copper halides and copper acetate is preferred, at least one selected from the group consisting of copper iodide, copper bromide, copper chloride, and copper acetate is more preferred, and at least one selected from the group consisting of copper iodide, copper bromide, and copper acetate is even more preferred, from the viewpoint of excellent heat aging resistance and suppression of metal corrosion of the screw and cylinder during extrusion.
- any halide that does not fall under the category of copper compounds can be used, and a salt of a metal element of Group 1 or Group 2 of the Periodic Table of Elements and a halogen is preferred.
- a salt of a metal element of Group 1 or Group 2 of the Periodic Table of Elements and a halogen is preferred.
- potassium iodide, potassium bromide, potassium chloride, sodium iodide, sodium chloride, etc. can be mentioned.
- at least one selected from the group consisting of potassium iodide and potassium bromide is preferred, and potassium iodide is more preferred, from the viewpoint that the obtained polyamide resin composition has excellent high-temperature heat resistance such as heat aging resistance and can suppress metal corrosion.
- the copper compound and the halide are preferably used in combination from the viewpoint that the resulting polyamide resin composition has excellent high-temperature heat resistance, such as heat aging resistance.
- the polyamide resin composition of this embodiment may contain a semi-aromatic polyamide resin and at least one selected from the group consisting of a crystal nucleating agent and an antioxidant.
- the polyamide resin composition of this embodiment preferably contains a sliding property improver.
- the polyamide resin composition preferably contains 0.01 to 10 parts by mass of the sliding property improver relative to 100 parts by mass of the semi-aromatic polyamide resin, more preferably 0.05 to 7 parts by mass, even more preferably 0.1 to 5 parts by mass, and even more preferably 1 to 4 parts by mass. This can improve the sliding property of a molded article made of the polyamide resin composition.
- the sliding property improver may, for example, be a fluororesin such as polytetrafluoroethylene, polytetrafluoroethylene-perfluoroalkoxyethylene copolymer, or polytetrafluoroethylene-polyhexafluoropropylene copolymer; polyolefins such as (high molecular weight) polyethylene, oxidized polyethylene, acid-modified (ultra-high molecular weight) polyethylene, polypropylene, acid-modified polypropylene, copolymerized polyolefins, or acid-modified copolymerized polyolefins; polydimethylsiloxane, polymethylphenylsiloxane, amino-modified polydimethylsiloxane, epoxy-modified polydimethylsiloxane, alcohol-modified polydimethylsiloxane, carboxymethyl ...
- fluororesin such as polytetrafluoroethylene, polytetrafluoroethylene-
- silicones examples include silicon-modified polydimethylsiloxane and fluorine-modified polydimethylsiloxane; layered inorganic compounds such as graphite and molybdenum disulfide; inorganic fibers such as glass fibers, potassium titanate whiskers, zinc oxide whiskers, and boronate whiskers; organic fibers such as LCP fibers, aramid fibers, and carbon fibers; inorganic particles such as alumina, talc, and silica; phosphates such as metaphosphates, pyrophosphates, calcium phosphate, calcium hydrogen phosphate, barium phosphate, lithium phosphate, calcium metaphosphate, and zinc pyrophosphate; mineral oils such as spindle oil, turbine oil, machine oil, and dynamo oil; and montanic acid salts such as calcium montanic acid. These sliding property improvers may be used alone or in combination of two or more.
- fluororesin polyethylene oxide, acid-modified (ultra-high molecular weight) polyethylene, acid-modified copolymer polyolefin, molybdenum disulfide, and aramid fiber are preferred from the viewpoint of their great effect in reducing the amount of wear and the coefficient of friction.
- the polyamide resin composition of this embodiment preferably contains a semi-aromatic polyamide resin and at least one selected from the group consisting of a crystal nucleating agent, an antioxidant, and a sliding property improver. In this case, too, it is possible to contain them in the above-mentioned preferred content.
- the polyamide resin composition of this embodiment may contain other additives as necessary, such as a lubricant, an inorganic filler, an impact modifier, a release agent, a colorant, a plasticizer, an ultraviolet absorber, a light stabilizer, an oxygen absorber, a hydrogen sulfide absorbent, a flame retardant, a flame retardant assistant, an antistatic agent, a crystallization retarder, and an organic fibrous filler.
- the content of the other additives is not particularly limited as long as it does not impair the effects of the present invention, but is preferably 0.01 to 200 parts by mass, and more preferably 0.02 to 100 parts by mass, relative to 100 parts by mass of the semi-aromatic polyamide resin.
- the content of the lubricant is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.1 to 3 parts by mass, relative to 100 parts by mass of the semi-aromatic polyamide resin. This can improve the fluidity of the polyamide resin composition and the appearance and releasability of a molded article made of the polyamide resin composition.
- the lubricants include, for example, higher fatty acids having 8 or more carbon atoms, such as stearic acid, palmitic acid, behenic acid, erucic acid, oleic acid, lauric acid, montanic acid, etc.; higher fatty acid metal salts, such as calcium stearate, aluminum stearate, zinc stearate, magnesium stearate, calcium montanate, sodium montanate, aluminum montanate, zinc montanate, magnesium montanate, calcium behenate, sodium behenate, zinc behenate, calcium laurate, zinc laurate, calcium palmitate, etc.; higher fatty acid esters, such as stearyl alcohol, behenyl alcohol, lauryl alcohol, etc.; higher fatty acid amides, such as stearic acid amide, oleic acid amide, erucic acid amide, ethylene bisstearylamide, ethylene bisoleylamide, N-stearylstearylamide, N-stearylerucamide,
- metal stearates, metal montanates, ethylene bisstearylamides, and polyolefins are preferred from the viewpoint of excellent heat resistance and moldability.
- the inorganic fillers include, for example, fibrous fillers such as glass fibers, carbon fibers, calcium silicate fibers, potassium titanate fibers, aluminum borate fibers, and wollastonite; glass flakes, silicon nitride, hydrotalcite zeolite, boehmite, aluminum hydroxide, calcium silicate, sodium aluminosilicate, carbon nanotubes, graphene, brass, copper, silver, nickel, iron, calcium fluoride, montmorillonite, expandable fluoromica, and apatite. These inorganic fillers may be used alone or in combination of two or more.
- fibrous fillers such as glass fibers, carbon fibers, calcium silicate fibers, potassium titanate fibers, aluminum borate fibers, and wollastonite
- glass flakes silicon nitride, hydrotalcite zeolite, boehmite, aluminum hydroxide, calcium silicate, sodium aluminosilicate, carbon nanotubes, graphene, brass, copper, silver,
- the inorganic fillers at least one selected from fibrous fillers is preferred from the viewpoint of excellent moldability and mechanical strength.
- the polyamide resin composition of this embodiment is a polyamide resin composition containing a semi-aromatic polyamide resin containing diamine units and dicarboxylic acid units, wherein the diamine units contain 60 to 100 mol % of aliphatic diamine units having 7 to 13 carbon atoms relative to 100 mol % of the diamine units, and the dicarboxylic acid units contain 60 to 100 mol % of aromatic dicarboxylic acid units relative to 100 mol % of the carboxylic acid units.
- the semi-aromatic polyamide resin has a weight average molecular weight Mw of 40,000 to 90,000 in terms of polymethyl methacrylate as measured by gel permeation chromatography (GPC), a terminal amino group amount [NH 2 ] of 10 to 70 ⁇ equivalents/g, a terminal carboxyl group amount [COOH] of 10 to 90 ⁇ equivalents/g, and a ratio of the terminal amino group amount [NH 2 ] to the terminal carboxyl group amount [COOH], [NH 2 ]/[COOH], of 0.1 or more and less than 1.0.
- GPC gel permeation chromatography
- a preferred embodiment of the semi-aromatic polyamide resin contained in the polyamide resin composition of this embodiment, which is another embodiment, is the same as the preferred embodiment described in the above-mentioned [Semi-aromatic polyamide resin].
- the amount of terminal amino groups [NH 2 ] and the amount of terminal carboxyl groups [COOH] in the semi-aromatic polyamide resin contained in the polyamide resin composition of this embodiment, which is another embodiment are values calculated by titration.
- the amount of terminal amino groups [NH 2 ] is a value calculated by titration using 0.01 or 0.1 N HCl aqueous solution with thymol blue as an indicator
- the amount of terminal carboxyl groups [COOH] is a value calculated by titration using 0.01 or 0.1 N potassium hydroxide/ethanol solution with a potentiometric titrator. More specifically, they can be determined by the method described in the examples.
- the polyamide resin composition of this embodiment which is another aspect, preferably contains at least one selected from the group consisting of a crystal nucleating agent, an antioxidant, a sliding property improver, and a lubricant.
- the polyamide resin composition of this embodiment which is another aspect, preferably contains 0.01 to 10 parts by mass of at least one selected from the group consisting of a crystal nucleating agent, an antioxidant, a sliding property improver, and a lubricant, more preferably 0.1 to 10 parts by mass, and even more preferably 0.1 to 8 parts by mass, relative to 100 parts by mass of the semi-aromatic polyamide resin.
- the polyamide resin composition of this embodiment which is another aspect, preferably contains 0.01 to 10 parts by mass of the crystal nucleating agent, the antioxidant, the sliding property improver, and the lubricant in total, more preferably 0.1 to 10 parts by mass, more preferably 0.1 to 8 parts by mass, and even more preferably 0.2 to 8 parts by mass, relative to 100 parts by mass of the semi-aromatic polyamide resin.
- This makes it possible to improve the sliding properties of a molded body made of the polyamide resin composition.
- Preferred aspects of the crystal nucleating agent, antioxidant, sliding property improver, lubricant, and other additives contained in the polyamide resin composition of this embodiment, which is another embodiment, are the same as those of the polyamide resin composition of the above-mentioned embodiment.
- the polyamide resin composition of this embodiment has excellent fatigue resistance due to the inclusion of the semi-aromatic polyamide resin.
- the fatigue resistance of the polyamide resin composition can be evaluated by the number of repetitions until fatigue failure obtained in a plane bending fatigue test.
- the number of repetitions until fatigue failure of the polyamide resin composition of this embodiment can be measured by the following method. Specifically, the composition is injection molded to prepare a type I test piece I-20 described in JIS K7119 (1972). Using this test piece, a plane bending fatigue test is performed in accordance with JIS K7119 (1972).
- the plane bending fatigue test conditions are a chuck distance of 30 mm, an atmospheric temperature of 23°C, a load of 40 MPa, a load repetition rate of 1800 times per minute, and a stress mode of reverse plane bending. This allows the number of repetitions until fatigue failure to be obtained.
- the number of repetitions until fatigue failure of the polyamide resin composition of this embodiment is preferably 5.0 x 10 5 cycles or more, more preferably 1.0 x 10 6 cycles or more. More specifically, the number of repetitions can be determined by the method described in the Examples.
- the water absorption rate is a method using a test piece obtained by injection molding a polyamide resin composition using an 80-ton injection molding machine manufactured by Nissei Plastic Industrial Co., Ltd. under conditions of a cylinder temperature of 320°C and a mold temperature of 140°C, and more specifically, can be determined by the method described in the examples.
- the polyamide resin composition of this embodiment contains the semi-aromatic polyamide resin, and further contains at least one selected from the group consisting of the crystal nucleating agent and the sliding property improving agent, thereby providing excellent sliding properties.
- the sliding properties of the polyamide resin composition can be evaluated by the wear amount (mg) and dynamic friction coefficient obtained in a sliding wear test.
- the wear amount and dynamic friction coefficient of the polyamide resin composition of this embodiment can be measured by the following method.
- the composition is injection molded to prepare a square plate test piece having a thickness of 3 mm. Using this test piece, a sliding wear test is performed in accordance with JIS K7218 (1986) Method A.
- the conditions of the sliding wear test are 23°C, surface pressure 10 kg/cm 2 , sliding speed 50 cm/sec, and mating material S45C. This allows the wear amount and dynamic friction coefficient to be obtained.
- the wear amount of the polyamide resin composition of this embodiment is preferably as low as possible, and is preferably 250 mg or less, more preferably 200 mg or less, and even more preferably 150 mg or less.
- the dynamic friction coefficient of the polyamide resin composition of this embodiment is preferably 0.5 or less, more preferably 0.45 or less.
- the test piece is obtained by injection molding the polyamide resin composition using an 80-ton injection molding machine manufactured by Nissei Plastic Industrial Co., Ltd. under the conditions of a cylinder temperature of 320° C. and a mold temperature of 140° C. More specifically, the wear amount and dynamic friction coefficient can be determined by the method described in the Examples.
- the method for producing the polyamide resin composition is not particularly limited, and a method that can uniformly mix the semi-aromatic polyamide resin, a crystal nucleating agent and/or an antioxidant, and other additives, etc., as necessary, can be preferably adopted.
- the method for producing the polyamide resin composition is preferably a method that can uniformly mix the semi-aromatic polyamide resin, at least one selected from the group consisting of a crystal nucleating agent and an antioxidant, and other additives, as necessary.
- the mixing is usually preferably performed by melt kneading using a single screw extruder, a twin screw extruder, a kneader, a Banbury mixer, etc.
- the melt kneading conditions are not particularly limited, and an example of the method is a method of melt kneading for about 1 to 30 minutes at a temperature range about 10 to 60°C higher than the melting point of the polyamide resin to obtain a pelletized polyamide resin composition.
- the molded article of this embodiment can be a molded article made of the semi-aromatic polyamide resin.
- the molded article can also be a molded article made of a polyamide resin composition.
- the molded article is produced by a known molding method using a semi-aromatic polyamide resin or a polyamide resin composition. Specifically, it can be obtained by molding using various molding methods such as injection molding, blow molding, extrusion molding, compression molding, stretch molding, vacuum molding, foam molding, rotational molding, impregnation, laser sintering, and fused deposition modeling.
- a molded article can be obtained by composite molding of the semi-aromatic polyamide resin or polyamide resin composition of this embodiment and another polymer, or a composition containing another polymer and a metal.
- a molded article including a layer made of the semi-aromatic polyamide resin composition of this embodiment on the surface of the metal plate can be obtained by extrusion molding a metal plate and the semi-aromatic polyamide resin composition of this embodiment.
- the molded article of this embodiment has excellent fatigue resistance and sliding properties, and can therefore be used as sliding members for automobiles, electric bicycles (especially e-bikes), industrial machinery, household appliances, etc.
- sliding members include various gears, bearings, bushes, chain tensioners, bearings, end face materials for mechanical seals, valve seats, V-rings, rod packings, piston rings, rotating shafts and rotating sleeves for compressors, pistons, impellers, vanes, rotors, etc.
- the molded product of this embodiment is particularly excellent in low water absorption, and therefore can be suitably used for gears that require high dimensional accuracy among the above-mentioned sliding members.
- gears include sprue gears, bevel gears, helical gears, spiral gears, double helical gears, internal gears, worm gears, rack and pinion gears, and Geneva gears.
- the molded product of this embodiment is particularly preferably used for sprue gears and helical gears for e-bike drive units and worm gears for automobile electric power steering.
- the molded product of this embodiment is particularly excellent in low water absorption, and therefore has high dimensional stability of the gears. Therefore, when used for the above-mentioned various gears of e-bikes, noise caused by meshing between gears can be suppressed, and the product has excellent quietness.
- ⁇ inh (dl/g) [ln(t 1 /t 0 )]/c
- t0 represents the flow time (seconds) of the solvent (concentrated sulfuric acid)
- t1 represents the flow time (seconds) of the sample solution
- c represents the concentration (g/dl) of the sample (semi-aromatic polyamide) in the sample solution.
- the terminal blocking rate of the semi-aromatic polyamide resin was calculated by the following formula (1):
- A represents the total amount of terminal groups
- B represents the total amount of terminal carboxyl groups and terminal amino groups.
- Terminal sealing rate (%) [(AB)/A] x 100 Formula (1) The results are shown in Table 2.
- the weight average molecular weight Mw0 of the semi-aromatic polyamide resin was determined as a standard polymethyl methacrylate-equivalent molecular weight using gel permeation chromatography (GPC). Specifically, 1.5 mg of the semi-aromatic polyamide resin was dissolved in 3 mL of eluent, and the solution was filtered through a membrane filter with a pore size of 0.4 ⁇ m to prepare a measurement sample, which was then measured in the same manner as described in "Retention stability" in "2. Evaluation method of polyamide resin composition”. The results are shown in Table 2.
- each of the semi-aromatic polyamide resins obtained in the examples and comparative examples were measured using a differential scanning calorimeter "DSC7020" manufactured by Hitachi High-Tech Science Corporation.
- the melting point and heat of fusion ⁇ Hm were measured in accordance with ISO11357-3 (2011, 2nd edition). Specifically, each semi-aromatic polyamide resin sample was heated from 30°C to 340°C at a rate of 10°C/min under a nitrogen atmosphere. The sample was then held at 340°C for 5 minutes to completely melt, and then cooled to 50°C at a rate of 10°C/min and held at 50°C for 5 minutes.
- Terminal Carboxyl Group Amount 0.5 g of each of the polyamide resin compositions obtained in the Examples and Comparative Examples was dissolved in 40 ml of orthocresol to prepare a sample solution. Using a potentiometric titration device, titration was carried out using a 0.01 or 0.1 N potassium hydroxide/ethanol solution to measure the amount of terminal carboxyl groups ([COOH], unit: ⁇ equivalents/g) of the semi-aromatic polyamide resin contained in the polyamide resin composition. (Measurement conditions) Measuring device: AT-710 (Kyoto Electronics Manufacturing Co., Ltd.) ⁇ Main control unit: MCU-710 (Kyoto Electronics Manufacturing Co., Ltd.)
- the retention stability was evaluated based on the rate of decrease in the weight average molecular weight (Mw) of the semi-aromatic polyamide resin contained in the polyamide resin composition before and after melt kneading. Specifically, the retention stability was evaluated based on the rate of decrease in the weight average molecular weight of the semi-aromatic polyamide resin contained in the polyamide resin composition, which is represented by the following formula (4), according to the following criteria. The results are shown in Table 3.
- Reduction rate of weight average molecular weight (%) ( Mw0 - Mw1 ) ⁇ 100/ Mw0 (4)
- Mw 0 indicates the weight average molecular weight of the semi-aromatic polyamide resin before melt-kneading
- Mw 1 indicates the weight average molecular weight of the semi-aromatic polyamide resin contained in the polyamide resin composition after melt-kneading.
- the melt-kneading was carried out using a twin-screw extruder "BTN-32-S2-30-L" manufactured by Plastics Engineering Research Institute Co., Ltd., at a cylinder temperature of 320 to 325°C and a residence time of 1 to 5 minutes.
- the decrease in weight average molecular weight is 20% or less.
- B The decrease in weight average molecular weight is more than 20%.
- the weight average molecular weight Mw0 of the semi-aromatic polyamide resin before melt kneading was measured by gel permeation chromatography (GPC) using the weight average molecular weight calculated as standard polymethyl methacrylate. Specifically, 1.5 mg of the semi-aromatic polyamide resin was dissolved in 3 mL of eluent, and the solution was filtered through a membrane filter with a pore size of 0.4 ⁇ m to prepare a measurement sample, which was then measured under the conditions shown below.
- the weight average molecular weight Mw1 of the semi-aromatic polyamide resin contained in the polyamide resin composition after melt kneading was determined by gel permeation chromatography (GPC) and converted into standard polymethyl methacrylate. Specifically, the weight average molecular weight was determined by the following method.
- the polyamide resin composition was weighed so that the mass of the semi-aromatic polyamide resin contained in the polyamide resin composition was 1.5 mg, and the polyamide resin composition was dissolved in hexafluoroisopropanol (HFIP).Then, the solution was filtered through a membrane filter with a pore size of 0.4 ⁇ m to prepare a measurement sample in which organic components containing the semi-aromatic polyamide resin were separated. The measurement sample was measured under the conditions shown below. Measurement conditions: Apparatus: HLC-8320GPC (manufactured by Tosoh Corporation) Column: Two TSKgel Super HM-N columns (manufactured by Tosoh Corporation) were connected in series.
- HLC-8320GPC manufactured by Tosoh Corporation
- the obtained dumbbell test piece was used to carry out a plane bending fatigue test in accordance with JIS K7119 (1972).
- the vibration fatigue tester "B-70-TL” manufactured by Toyo Seiki Seisakusho Co., Ltd. was used as the test machine.
- the number of repetitions (number of cycles) until fatigue failure was measured under the conditions of chuck distance: 30 mm, atmospheric temperature: 23°C, load: 40 MPa, load repetition rate: 1800 times per minute, and stress mode: reverse plane bending, and this was taken as fatigue resistance.
- the results are shown in Table 3.
- the mixture was stirred at 100° C. for 30 minutes, and the temperature inside the autoclave was raised to 220° C. over 2 hours. At this time, the pressure inside the autoclave was raised to 2 MPa. Heating was continued for 5 hours while maintaining the pressure at 2 MPa, and the water vapor was gradually removed to allow the reaction. Next, the pressure was reduced to 1.3 MPa over 30 minutes, and the reaction was allowed to proceed for another hour to obtain a prepolymer.
- the obtained prepolymer was dried at 120°C under reduced pressure for 12 hours and pulverized to a particle size of 2 mm or less. This was subjected to solid-phase polymerization at 230°C and 13 Pa (0.1 mmHg) for 10 hours to obtain a white semi-aromatic polyamide resin PA9T-1.
- the semi-aromatic polyamide resins of Examples 1 to 3 have an inherent viscosity ⁇ inh measured in concentrated sulfuric acid at 30°C of 1.6 to 3.0 dl/g, an amount of terminal amino groups of 10 to 70 ⁇ equivalents/g, an amount of terminal carboxyl groups of 10 to 90 ⁇ equivalents/g, and a ratio [NH 2 ]/[COOH] of the amount of terminal amino groups [NH 2 ] ( ⁇ equivalents/g) to the amount of terminal carboxyl groups [COOH] ( ⁇ equivalents/g) of 0.1 or more and less than 1.0.
- Examples 4 to 7 contain the semi-aromatic polyamide resins of Examples 1 to 3 and have high retention stability and fatigue resistance. Therefore, from Tables 2 and 3, it can be seen that the semi-aromatic polyamide resins and polyamide resin compositions of the examples have improved retention stability during melt processing while maintaining excellent fatigue resistance, and are excellent in both fatigue resistance and retention stability.
Landscapes
- Chemical & Material Sciences (AREA)
- Health & Medical Sciences (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Medicinal Chemistry (AREA)
- Polymers & Plastics (AREA)
- Organic Chemistry (AREA)
- Polyamides (AREA)
- Engineering & Computer Science (AREA)
- General Engineering & Computer Science (AREA)
- Crystallography & Structural Chemistry (AREA)
- Mechanical Engineering (AREA)
Priority Applications (3)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| CN202480069447.6A CN122095007A (zh) | 2023-11-01 | 2024-10-31 | 半芳香族聚酰胺树脂、聚酰胺树脂组合物和半芳香族聚酰胺树脂的制造方法 |
| JP2025555063A JPWO2025095085A1 (cg-RX-API-DMAC7.html) | 2023-11-01 | 2024-10-31 | |
| KR1020267013274A KR20260105717A (ko) | 2023-11-01 | 2024-10-31 | 반방향족 폴리아미드 수지, 폴리아미드 수지 조성물, 및 반방향족 폴리아미드 수지의 제조 방법 |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2023187353 | 2023-11-01 | ||
| JP2023-187353 | 2023-11-01 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2025095085A1 true WO2025095085A1 (ja) | 2025-05-08 |
Family
ID=95580850
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2024/038972 Pending WO2025095085A1 (ja) | 2023-11-01 | 2024-10-31 | 半芳香族ポリアミド樹脂、ポリアミド樹脂組成物、及び半芳香族ポリアミド樹脂の製造方法 |
Country Status (4)
| Country | Link |
|---|---|
| JP (1) | JPWO2025095085A1 (cg-RX-API-DMAC7.html) |
| KR (1) | KR20260105717A (cg-RX-API-DMAC7.html) |
| CN (1) | CN122095007A (cg-RX-API-DMAC7.html) |
| WO (1) | WO2025095085A1 (cg-RX-API-DMAC7.html) |
Citations (14)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2003055549A (ja) * | 2001-06-05 | 2003-02-26 | Kuraray Co Ltd | ポリアミド組成物 |
| WO2006098434A1 (ja) | 2005-03-18 | 2006-09-21 | Kuraray Co., Ltd. | 半芳香族ポリアミド樹脂 |
| JP2007154107A (ja) * | 2005-12-07 | 2007-06-21 | Asahi Kasei Chemicals Corp | 耐熱性樹脂組成物 |
| JP2012020571A (ja) * | 2010-06-14 | 2012-02-02 | Ube Industries Ltd | 積層チューブ |
| JP2014218574A (ja) * | 2013-05-08 | 2014-11-20 | 株式会社クラレ | ポリアミド樹脂組成物 |
| JP2015059164A (ja) * | 2013-09-18 | 2015-03-30 | 株式会社クラレ | ポリアミド樹脂組成物および当該ポリアミド樹脂組成物を含有する成形体 |
| JP2015129271A (ja) * | 2013-12-05 | 2015-07-16 | 東レ株式会社 | 炭素繊維強化ポリアミド樹脂組成物およびそれを成形してなる成形品 |
| JP2015199873A (ja) | 2014-04-09 | 2015-11-12 | 旭化成ケミカルズ株式会社 | 強化高分子量ポリアミド樹脂組成物 |
| WO2015182693A1 (ja) * | 2014-05-30 | 2015-12-03 | 東レ株式会社 | 末端変性ポリアミド樹脂、その製造方法および成形品の製造方法 |
| JP2016094508A (ja) | 2014-11-12 | 2016-05-26 | ユニチカ株式会社 | 半芳香族ポリアミドおよびそれからなる成形体 |
| WO2017115699A1 (ja) * | 2015-12-28 | 2017-07-06 | 株式会社クラレ | ポリアミド樹脂組成物 |
| WO2021065205A1 (ja) | 2019-09-30 | 2021-04-08 | 東洋紡株式会社 | 無機強化半芳香族ポリアミド樹脂組成物 |
| JP2022030403A (ja) * | 2020-08-07 | 2022-02-18 | 株式会社クラレ | ポリアミド樹脂組成物及びその成形体 |
| WO2023282154A1 (ja) * | 2021-07-08 | 2023-01-12 | 株式会社クラレ | ポリアミド組成物 |
-
2024
- 2024-10-31 JP JP2025555063A patent/JPWO2025095085A1/ja active Pending
- 2024-10-31 KR KR1020267013274A patent/KR20260105717A/ko active Pending
- 2024-10-31 WO PCT/JP2024/038972 patent/WO2025095085A1/ja active Pending
- 2024-10-31 CN CN202480069447.6A patent/CN122095007A/zh active Pending
Patent Citations (14)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2003055549A (ja) * | 2001-06-05 | 2003-02-26 | Kuraray Co Ltd | ポリアミド組成物 |
| WO2006098434A1 (ja) | 2005-03-18 | 2006-09-21 | Kuraray Co., Ltd. | 半芳香族ポリアミド樹脂 |
| JP2007154107A (ja) * | 2005-12-07 | 2007-06-21 | Asahi Kasei Chemicals Corp | 耐熱性樹脂組成物 |
| JP2012020571A (ja) * | 2010-06-14 | 2012-02-02 | Ube Industries Ltd | 積層チューブ |
| JP2014218574A (ja) * | 2013-05-08 | 2014-11-20 | 株式会社クラレ | ポリアミド樹脂組成物 |
| JP2015059164A (ja) * | 2013-09-18 | 2015-03-30 | 株式会社クラレ | ポリアミド樹脂組成物および当該ポリアミド樹脂組成物を含有する成形体 |
| JP2015129271A (ja) * | 2013-12-05 | 2015-07-16 | 東レ株式会社 | 炭素繊維強化ポリアミド樹脂組成物およびそれを成形してなる成形品 |
| JP2015199873A (ja) | 2014-04-09 | 2015-11-12 | 旭化成ケミカルズ株式会社 | 強化高分子量ポリアミド樹脂組成物 |
| WO2015182693A1 (ja) * | 2014-05-30 | 2015-12-03 | 東レ株式会社 | 末端変性ポリアミド樹脂、その製造方法および成形品の製造方法 |
| JP2016094508A (ja) | 2014-11-12 | 2016-05-26 | ユニチカ株式会社 | 半芳香族ポリアミドおよびそれからなる成形体 |
| WO2017115699A1 (ja) * | 2015-12-28 | 2017-07-06 | 株式会社クラレ | ポリアミド樹脂組成物 |
| WO2021065205A1 (ja) | 2019-09-30 | 2021-04-08 | 東洋紡株式会社 | 無機強化半芳香族ポリアミド樹脂組成物 |
| JP2022030403A (ja) * | 2020-08-07 | 2022-02-18 | 株式会社クラレ | ポリアミド樹脂組成物及びその成形体 |
| WO2023282154A1 (ja) * | 2021-07-08 | 2023-01-12 | 株式会社クラレ | ポリアミド組成物 |
Also Published As
| Publication number | Publication date |
|---|---|
| KR20260105717A (ko) | 2026-07-07 |
| CN122095007A (zh) | 2026-05-26 |
| JPWO2025095085A1 (cg-RX-API-DMAC7.html) | 2025-05-08 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| EP2792714B2 (en) | Molded products | |
| RU2544013C2 (ru) | Полиамидная смола | |
| JP3466330B2 (ja) | ポリアミドおよびポリアミド組成物 | |
| CA2764882A1 (en) | Polyamide resin composition and molded product | |
| JP7252827B2 (ja) | ポリアミド組成物 | |
| EP0659799A2 (en) | Polyamide and polyamide composition | |
| JPH07228776A (ja) | 成形材料用ポリアミド組成物 | |
| JP2000191771A (ja) | ポリアミドおよびその組成物 | |
| JPWO2020040283A1 (ja) | ポリアミド組成物 | |
| JP2022030403A (ja) | ポリアミド樹脂組成物及びその成形体 | |
| CN109161015B (zh) | 一种高耐热交替共聚酰胺树脂及其制备方法 | |
| JP2006176597A (ja) | ポリアミド樹脂組成物 | |
| JP2000086759A (ja) | ポリアミドおよびその組成物 | |
| EP2468796B1 (en) | Polyamide | |
| JPH07228774A (ja) | 摺動特性に優れたポリアミド組成物 | |
| JP2023113400A (ja) | ポリアミド系樹脂、ポリアミド系樹脂組成物、及び成形品 | |
| JP2004107526A (ja) | ポリアミド組成物 | |
| JP4150136B2 (ja) | ポリアミド樹脂組成物 | |
| JP2004244579A (ja) | ポリアミド成形品 | |
| JP2004107525A (ja) | ポリアミド組成物 | |
| JP2011057932A (ja) | 輸送機器部品 | |
| JP2003171550A (ja) | ポリアミド組成物 | |
| JPH07228768A (ja) | 耐熱老化性ポリアミド組成物 | |
| WO2023089941A1 (ja) | ポリアミド樹脂の製造方法、および、樹脂組成物 | |
| JP2013253197A (ja) | ポリアミド組成物及びポリアミド組成物を成形した成形体 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 24885851 Country of ref document: EP Kind code of ref document: A1 |
|
| ENP | Entry into the national phase |
Ref document number: 2025555063 Country of ref document: JP Kind code of ref document: A |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 2025555063 Country of ref document: JP |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 2601002914 Country of ref document: TH |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |