WO2022272224A1 - Conductive paste comprising copper particles and use thereof to produce electronic components - Google Patents
Conductive paste comprising copper particles and use thereof to produce electronic components Download PDFInfo
- Publication number
- WO2022272224A1 WO2022272224A1 PCT/US2022/072979 US2022072979W WO2022272224A1 WO 2022272224 A1 WO2022272224 A1 WO 2022272224A1 US 2022072979 W US2022072979 W US 2022072979W WO 2022272224 A1 WO2022272224 A1 WO 2022272224A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- paste
- glass frit
- copper powder
- conductive paste
- organic vehicle
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01B—CABLES; CONDUCTORS; INSULATORS; SELECTION OF MATERIALS FOR THEIR CONDUCTIVE, INSULATING OR DIELECTRIC PROPERTIES
- H01B1/00—Conductors or conductive bodies characterised by the conductive materials; Selection of materials as conductors
- H01B1/20—Conductive material dispersed in non-conductive organic material
- H01B1/22—Conductive material dispersed in non-conductive organic material the conductive material comprising metals or alloys
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01B—CABLES; CONDUCTORS; INSULATORS; SELECTION OF MATERIALS FOR THEIR CONDUCTIVE, INSULATING OR DIELECTRIC PROPERTIES
- H01B1/00—Conductors or conductive bodies characterised by the conductive materials; Selection of materials as conductors
- H01B1/02—Conductors or conductive bodies characterised by the conductive materials; Selection of materials as conductors mainly consisting of metals or alloys
- H01B1/026—Alloys based on copper
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01B—CABLES; CONDUCTORS; INSULATORS; SELECTION OF MATERIALS FOR THEIR CONDUCTIVE, INSULATING OR DIELECTRIC PROPERTIES
- H01B13/00—Apparatus or processes specially adapted for manufacturing conductors or cables
- H01B13/0016—Apparatus or processes specially adapted for manufacturing conductors or cables for heat treatment
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01B—CABLES; CONDUCTORS; INSULATORS; SELECTION OF MATERIALS FOR THEIR CONDUCTIVE, INSULATING OR DIELECTRIC PROPERTIES
- H01B13/00—Apparatus or processes specially adapted for manufacturing conductors or cables
- H01B13/30—Drying; Impregnating
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01B—CABLES; CONDUCTORS; INSULATORS; SELECTION OF MATERIALS FOR THEIR CONDUCTIVE, INSULATING OR DIELECTRIC PROPERTIES
- H01B3/00—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties
- H01B3/02—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties mainly consisting of inorganic substances
- H01B3/08—Insulators or insulating bodies characterised by the insulating materials; Selection of materials for their insulating or dielectric properties mainly consisting of inorganic substances quartz; glass; glass wool; slag wool; vitreous enamels
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01B—CABLES; CONDUCTORS; INSULATORS; SELECTION OF MATERIALS FOR THEIR CONDUCTIVE, INSULATING OR DIELECTRIC PROPERTIES
- H01B5/00—Non-insulated conductors or conductive bodies characterised by their form
- H01B5/14—Non-insulated conductors or conductive bodies characterised by their form comprising conductive layers or films on insulating-supports
-
- H—ELECTRICITY
- H01—ELECTRIC ELEMENTS
- H01P—WAVEGUIDES; RESONATORS, LINES, OR OTHER DEVICES OF THE WAVEGUIDE TYPE
- H01P1/00—Auxiliary devices
- H01P1/20—Frequency-selective devices, e.g. filters
- H01P1/2002—Dielectric waveguide filters
-
- H—ELECTRICITY
- H05—ELECTRIC TECHNIQUES NOT OTHERWISE PROVIDED FOR
- H05K—PRINTED CIRCUITS; CASINGS OR CONSTRUCTIONAL DETAILS OF ELECTRIC APPARATUS; MANUFACTURE OF ASSEMBLAGES OF ELECTRICAL COMPONENTS
- H05K1/00—Printed circuits
- H05K1/02—Details
- H05K1/09—Use of materials for the conductive, e.g. metallic pattern
- H05K1/092—Dispersed materials, e.g. conductive pastes or inks
-
- H—ELECTRICITY
- H05—ELECTRIC TECHNIQUES NOT OTHERWISE PROVIDED FOR
- H05K—PRINTED CIRCUITS; CASINGS OR CONSTRUCTIONAL DETAILS OF ELECTRIC APPARATUS; MANUFACTURE OF ASSEMBLAGES OF ELECTRICAL COMPONENTS
- H05K2203/00—Indexing scheme relating to apparatus or processes for manufacturing printed circuits covered by H05K3/00
- H05K2203/11—Treatments characterised by their effect, e.g. heating, cooling, roughening
- H05K2203/1126—Firing, i.e. heating a powder or paste above the melting temperature of at least one of its constituents
Definitions
- the present invention relates to the field of electronic components, particularly to electrodes deposited on a substrate and components manufactured with such electrodes, such as dielectric filters.
- Radio waves with a variety of frequencies are used in communication systems. Depending on the application, a specific range of frequencies is allocated.
- Band filters select a range of frequencies for which they are designed, and reject non-selected frequencies.
- Several types of filter are known, including metal cavity filters and dielectric filters. Dielectric filters have the advantage of permitting downsizing and weight saving, high reliability and relatively low cost of manufacture.
- the invention provides a conductive paste, wherein the conductive paste comprises: (i) Cu powder having a Dso from 0.8 to 2.6 pm, (ii) glass frit, and (iii) an organic vehicle.
- the invention provides a method of manufacturing an electronic component, comprising the steps of: (a) preparing a ceramic substrate; (b) applying a conductive paste on the ceramic substrate, wherein the conductive paste comprises, (i) Cu powder having a Dso from 0.8 to 2.6 pm, (ii) glass frit, and (iii) an organic vehicle; and (c) firing the ceramic substrate and the applied conductive paste.
- conductive pastes made with copper particles having a Dso from 0.8 to 2.6 pm give good results when sintered onto a ceramic substrate, particularly as measured by quality factor.
- the invention provides a conductive paste, wherein the conductive paste comprises: (i) Cu powder having a Dso from 0.8 to 2.6 pm,
- the copper powder is preferably a pure copper powder. Also suitable are copper powders that are wholly or partially coated by organic materials, and copper powders that are wholly or partially coated by oxidized copper.
- the pure copper powder, whether coated, uncoated, or partially coated, preferably comprises at least 99.0 wt%, at least 99.5 wt%, at least 99.9 wt%, or at least 99.99 wt% of elemental copper.
- Any copper powder is suitable for use in the invention, provided it has a Dso from 0.8 to 2.6 pm as measured by laser diffraction according to the method ASTM B822-20, using water as the suspending medium and calculations based on MIE theory.
- the copper powder has a Dso from 0.8 to 2.5 pm, more preferably from 0.9 to 2.5 pm, more particularly preferably from 1 .0 to 2.4 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder has an average particle size of from 1 to 2.6 pm, as measured by laser diffraction, using water as the suspending medium.
- the method of measuring the particle size is the same as described above to determine the Dso of the copper powder.
- the copper powder has from 2.9 to 39.8% of particles having a size of less than 1 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder has from 36 to 98% of particles having a size of less than 2 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder has less than 50% of particles having a size of less than 1 pm.
- the copper powder has greater than 32% of particles having a size of less than 2 pm.
- the copper powder has a Ds from 0.5 to 1.0 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder has a Dio from 0.6 to 1.2 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder has a D90 from 1.2 to
- the copper powder has a D95 from 1.5 to 5.5 pm, preferably 1.7 to 5.1 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder has an average particle size of from 1 .0 to 2.6 pm.
- the copper powder has a D50 from 0.8 to 2.6 pm as measured by laser diffraction, using water as the suspending medium and less than 50 % of particles having a size of less than 1 pm.
- the copper powder has a D50 from 0.8 to 2.6 pm as measured by laser diffraction, using water as the suspending medium and greater than 32 % of particles having a size of less than 2 pm.
- the copper powder has a D50 from 0.8 to 2.6 pm as measured by laser diffraction, using water as the suspending medium, less than 50 % of particles having a size of less than 1 pm, and greater than 32 % of particles having a size of less than 2 pm.
- the copper powder has a D50 from 0.8 to 2.6 pm and a D90 from 1.2 to 4.5 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder has a Ds of 0.5 to 1.0 pm and a D50 of from 1.0 to 2.4 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder has a D10 of 0.6 to 1.2 pm and a D50 of from 1.0 to 2.4 pm, as measured by laser diffraction, using water as the suspending medium. In another preferred embodiment, the copper powder has a D90 of 1.5 to 4.3 pm and a D50 of from 1.0 to 2.4 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder has a D95 of 1.7 to 5.1 pm and a D50 of from 1.0 to 2.4 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder has a D5 of 0.5 to 1.0 pm, a D10 of 0.6 to 1.2 pm and a D50 of from 1.0 to 2.4 pm, a D90 of 1 .5 to 4.3 pm, a D95 of 1.7 to 5.1 pm and a D50 of from 1.0 to 2.4 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder particles are not particularly limited in shape, although spherical particles are preferred.
- spherical is meant particles that appear generally isometric (i.e. having approximately the same dimensions in any axis) under a scanning electron microscope at 400- to 5500X magnification, preferably at 5000X magnification.
- the particles also have an aspect ratio of 1 to 1.2, more preferably 1 to 1.1.
- the specific surface area (SA) of the copper powder is preferably 0.1 to 8.0 m 2 /g, more preferably 0.3 to 4.0 m 2 /g, particularly preferably 0.5 to 2.0 m 2 /g.
- the specific surface area can be measured by a BET method such as ASTM B922-22 with a device such as MonosorbTM from Quantachrome Instruments Corporation.
- the copper powder is preferably used at 40 to 95 weight percent (wt%), more preferably 52 to 93 wt%, particularly preferably 65 to 92 wt%, based on the weight of the conductive paste.
- Suitable copper powders are commercially available from a number of well-known suppliers.
- the glass frit functions to increase adhesion of the sintered conductive paste to the ceramic substrate. Any glass that fulfills this function is suitable for use in the conductive paste described herein. Its chemical composition is not otherwise limited.
- the glass frit is produced from a metal oxide selected from the group consisting of bismuth oxide (B12O3), boron oxide (B2O3), zinc oxide (ZnO), aluminum oxide (AI2O3), silicon oxide (S1O2) and mixtures of two or more thereof.
- a metal oxide selected from the group consisting of bismuth oxide (B12O3), boron oxide (B2O3), zinc oxide (ZnO), aluminum oxide (AI2O3), silicon oxide (S1O2) and mixtures of two or more thereof.
- the glass frit is a Si -B -Zn glass, a Bi -B -Zn glass, or a mixture thereof.
- the glass frit comprises less than 100 ppm, less than 50 ppm, less than 5 ppm, or less than 1 ppm of lead.
- the softening point of the glass frit is preferably at least about 350°C, 400°C, 450°C, 500°C, or 550°C. In addition, the softening point of the glass frit is preferably no greater than about 900°C, 875°C, 850°C, 750°C, or 700°C. In some preferred embodiments, the softening point of the glass frit is about 524°C.
- the glass frit is prepared from a mixture comprising S1O2, B2O3, AI2O3, B12O3, CaO and ZnO.
- the glass frit is prepared from a mixture comprising 5 to 9 wt% S1O2, 5 to 12 wt% B2O3, 1 to 3 wt% AI2O3, 65 to 75 wt% B12O3, 0.1 to 1 wt% CaO and 8 to 16 wt% ZnO, based on the total weight of the glass frit.
- the glass frit is prepared from a mixture comprising 7.1 wt% S1O2, 8.4 wt% B2O3, 2.1 wt% AI2O3, 69.8 wt% B12O3, 0.5 wt% CaO and 12.0 wt% ZnO, based on the total weight of the glass frit.
- the sum of the weight percentages of the components from which the glass frit is produced is 100 wt%.
- the particle diameter (D50) of the glass frit is preferably 0.1 to 15 pm, more preferably 0.5 to 11 pm, more particularly preferably 1.0 to 6.8 pm, and 1.5 to 4.5 pm in another embodiment.
- the particle diameter (D50) can be measured by laser scattering method, for example with Microtrac model S-3500, with water as suspending medium. The method of measuring the particle size is the same as described above to determine the D50 of the copper powder.
- the glass frit is preferably used in the conductive paste at a level of 0.5 to 2 wt%, more preferably at 0.7 to 1.8 wt%, particularly preferably at 0.8 to 1 .5 wt%, based on the total weight of the conductive paste.
- Suitable glass frits may be prepared by methods that are well-known in the art, for example the methods described in U.S. Patent No. 5,439,852, issued to Jacob Hormadaly. Some, but not all, of the glass frits described herein may be commercially available from well-known suppliers.
- the conductive powder and the glass frit are dispersed in an organic vehicle to form a conductive paste.
- the conductive paste has a suitable viscosity for application to a substrate by conventional means such as, for example, screen-printing, spraying or dipping.
- the organic vehicle preferably comprises an organic polymer and a solvent, or at least one organic polymer and at least one organic solvent.
- the organic polymer(s) can be selected from the group consisting of ethyl cellulose, ethylhydroxyethyl cellulose, wood rosin, phenolic resin, polymethacrylate of a lower (CI-Q) alcohol, and mixtures of two or more thereof.
- the organic polymer(s) are preferably used at a level of 0.1 to 50 wt%, 0.5 to 42 wt%, 1 to 35 wt%, 2 to 27 wt%, and particularly preferably 3 to 15 wt%, based on the weight of the organic vehicle.
- the solvent(s) are preferably selected from the group consisting of texanol (2,2,4-trimethyl-1 ,3-pentanediol monoisobutyrate), ester alcohol, terpineol, kerosene, dibutylphthalate, butyl carbitol, butyl carbitol acetate, dibutyl carbitol, hexylene glycol, dibasic ester, and mixtures of two or more thereof.
- the solvent(s) are chosen so that the organic polymer(s) are readily soluble therein.
- the solvent(s) are used at a level of 50 to 99.9 wt%, 48 to 99.5 wt%, 65 to 99 wt%, 73 to 98 wt%, preferably 75 to 95 wt%, more preferably 80 to 93 wt%, more particularly preferably at 85 to 93 or 97 wt%, based on the weight of the organic vehicle.
- the organic vehicle comprises a mixture of ethyl cellulose and texanol. Particularly preferably the organic vehicle comprises 3 to 15 wt% ethyl cellulose and 85 to 93 or 97 wt% texanol, based on the weight of the organic vehicle.
- the organic vehicle may optionally comprise an organic additive.
- the organic additive can be one or more of a thickener, stabilizer, viscosity modifier, surfactant and thixotropic agent in an embodiment.
- the amount of the organic additive(s) depends on the desired characteristics of the resulting electrically conductive paste.
- the optional organic additives(s) are preferably used at a level of up to 25 wt%, up to 10 wt%, up to 5 wt%, up to 2 wt%, or up to 1 wt%, based on the total weight of the organic vehicle.
- the sum of the weight percentages of the organic polymer, the solvent, and the optional organic additive(s), if present, is 100 wt%, based on the total weight of the organic vehicle.
- the organic vehicle preferably is used at a level of 5 to 30 wt%, more preferably 6 to 15 wt%, particularly preferably 7 to 10 wt%, based on the weight of the conductive paste.
- the conductive pastes may further comprise one or more other components.
- Materials suitable for use as other components and suitable amounts of the other components are described in U.S. Patent No. 11 ,228,080, issued to Yusuke Tachibana.
- the other components include organic materials and inorganic additives.
- Preferred organic materials include, without limitation, thickeners, stabilizers, viscosity modifiers, surfactants, and thixotropic agents.
- Preferred inorganic additives include, without limitation, metal oxides selected from the group consisting of copper oxide (CuO,
- the metal oxide(s) are powders having a D50 of 0.1 to 10 urn.
- the conductive pastes of the invention are manufactured by dispersing the copper powder, the glass frit, and the other component(s), if present, in the organic vehicle in a mixer, such as a dispersator, and homogenizing the mixture, for example using a three-roll mill.
- the invention also provides a method of manufacturing an electronic component, comprising the steps of: (a) preparing a ceramic substrate; (b) applying a conductive paste on the ceramic substrate, wherein the conductive paste comprises (i) copper powder having a Dso from 0.8 to 2.6 pm, (ii) glass frit, and (iii) an organic vehicle; and (c) firing the ceramic with the applied conductive paste.
- the ceramic substrate preferably has a dielectric constant, e g , of 9 to 50, more preferably 15 to 45, particularly preferably 20 to 40.
- the dielectric constant of the ceramic substrate can be measured by a known method, for example by the method of ASTM Standard D2520(2013) at 5 GHz.
- Such ceramic substrates are suitable, for example, for ceramic filters used in the radio frequency range. More specifically, such ceramic substrates are suitable for use in the range of 1 GHz to 10 GHz.
- Preferred ceramic substrates include those made with certain metal oxide components.
- Metal components of the ceramic substrate are, for example, selected from the group consisting of Al, Ba, Ca, La, Mg, Mn, Nb, Nd, Ni, Pb, Sm, Sn, Sr,
- the ceramic substrate comprises at least 60 mol %, at least 70 mol %, at least 80 mol %, at least 90 mol %, at least 95 mol%, or 100 mol % of one or more metal components selected from this group. In an embodiment, other metal(s) are included in the metal component of the ceramic substrate.
- the ceramic substrate is not particularly limited, and may be selected from, for example, AI2O3, BaT 09, Ba2Ti902o, BaSnCte, BaMgCb, BaTaCte, BaZrCb, Ba(ZrTi)C>3, Ba(NiTa)03, Ba(ZrZnTa)03, Ba(Mgi/3Ta2/3)03, Ba(Mgi/3Nb2/3)03, Ba(Zm/3Ta2/3)C>3, Ba(Zm/3Nb2/3)03, Ba(Mm/3Ta2/3)03, CaTiC>3, (CaSrBa)ZrC>3, MgTiC>3, (Mgo.95Cao.o5)Ti03, SrZrCb, Sr(Zm/3Nb2/3)C>3, Sr(Zm/3Ta2/3)C>3, ZrTiC>2, (Zro.8Sno.2)Ti04, and mixtures of two or more thereof.
- the ceramic substrate is selected from the group consisting of AI2O3, MgTiCb, (Mgo.95Cao.o5)TiC>3, Ba(Mgi/3Ta2/3)C>3, BaTUC>9, Ba2Ti902o, Ba(Zm/3Ta2/3)C>3 and Ba(Zm/3Nb2/3)C>3, (Zro.8Sno.2)TiC>4.
- the ceramic substrate may be surface treated. For example, it may be smoothed or roughened.
- a primer layer may also be used.
- a primer layer may be formed, for example, by chemical vapor deposition or by plating.
- the conductive paste of the invention is applied on the ceramic substrate.
- the conductive paste may be applied, for example, by screen-printing, spraying or dipping.
- the conductive paste is applied by screen-printing in another embodiment.
- the conductive paste may be applied on the entire surface of the ceramic substrate, or on a portion of the surface.
- the conductive paste viscosity can be adjusted to be suitable for the applying method chosen. Suitable methods for adjusting the viscosity include adjusting the amount of organic vehicle in the conductive paste, adjusting the ratio of solvent and organic polymer in the organic vehicle, adjusting the molecular weight of the organic polymer, selecting a different organic polymer, or selecting a different solvent. Two or more of these methods may be used in combination.
- the preferred viscosity range is from 200 to 450 Pa s.
- the viscosity is preferably in the range of 4 to 10 Pa s.
- the preferred viscosity range is 0.5 to 4 Pa s.
- the viscosity of the conductive paste is from 0.5 to 450 Pa s, 1 to 400 Pa s in another embodiment, 5 to 350 Pa s in another embodiment, 10 to 300 Pa s in another embodiment, as measured by Brookfield HBT with a spindle SC4-14 at 10 rpm, RVT with a spindle SC4-14 at 10 rpm or LVT with a spindle SC4-14 at 10 rpm.
- the conductive paste is typically applied at 5 to 40 pm thick in an embodiment, 7 to 30 pm thick in another embodiment, 10 to 20 pm thick in another embodiment, or 7 to 16 pm in another embodiment. If the thickness is significantly less than 5 pm the quality factor drops. If the thickness is significantly more than 40 pm peeling may be a problem.
- the conductive paste may optionally be dried after application to the ceramic substrate and before the firing step. Typical drying conditions are 50 to 250°C, or 100 to 150°C for 3 to 30 minutes. Drying serves to remove volatile elements and improves the conductive layer. Firing without drying can lead to blistering or the formation of voids.
- the ceramic substrate with the applied conductive paste is fired to sinter the paste on the substrate.
- This process produces the electronic component.
- the glass frit softens gradually with increasing the temperature and eventually flows.
- the glass frit helps to sinter copper powder during the process, so that an electrically conductive layer is formed.
- the melted glass reacts with the ceramic substrate.
- a glass layer is formed between the ceramic substrate and the copper metal rich upper layer of the sintered conductive paste.
- the firing peak temperature is preferably 600 to 1100°C, 650 to 1050°C in another embodiment, 800 to 1000°C in another embodiment.
- Firing time at the peak temperature is preferably 3 to 30 minutes, 5 to 20 minutes, or 7 to 15 minutes. Firing is preferably carried out under oxygen-poor conditions, for example, under a blanket of nitrogen or argon, or under vacuum.
- the electronic component is used, for example, in the radio frequency range. More specifically, the electronic component is suitable for filters used in 1 GHz to 10 GHz. In a preferred embodiment, the electronic component is a dielectric filter.
- the quality factor is preferably greater than 2,550, more preferably greater than 2,600, more particularly preferably greater than 2,750, or greater than 2,800.
- the quality factor is preferably greater than 2,200, more preferably greater than
- a conductive paste wherein the conductive paste comprises: (i) Cu powder having a Dso from 0.8 to 2.6 pm, (ii) glass frit, and (iii) an organic vehicle.
- a method of manufacturing an electronic component comprising the steps of: (a) preparing a ceramic substrate; (b) applying a conductive paste on the ceramic substrate, wherein the conductive paste comprises, (i) Cu powder having a Dso from 0.8 to 2.6 pm, (ii) glass frit, and (iii) an organic vehicle; and (c) firing the applied conductive paste.
- Embodiment 1 or 2 wherein the copper powder has less than 50 % of particles having a size of less than 1 pm.
- the copper powder has a Dso from 0.8 to 2.6 pm as measured by laser diffraction, using water as the suspending medium and less than 50 % of particles having a size of less than 1 pm.
- the copper powder has a D10 from 0.6 to 1.2 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder has a D90 from 1 .2 to 4.5 pm, preferably 1.5 to 4.3 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder has a D95 from 1.5 to 5.5 pm, preferably 1.7 to 5.1 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder has a Ds of 0.5 to 1 .0 pm and a D50 of from 1.0 to 2.4 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder has a D10 of 0.6 to 1 .2 pm and a D50 of from 1 .0 to 2.4 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder has a D90 of 1 .5 to 4.3 pm and a D50 of from 1 .0 to 2.4 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder has a D95 of 1 .7 to 5.1 pm and a D50 of from 1 .0 to 2.4 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper powder has a Ds of 0.5 to 1 .0 pm, a D10 of 0.6 to 1.2 pm and a Dso of from 1.0 to 2.4 pm, a D90 of 1.5 to 4.3 pm, a D95 of 1.7 to 5.1 pm and a Dso of from 1.0 to 2.4 pm, as measured by laser diffraction, using water as the suspending medium.
- the copper particles have an aspect ratio of 1 to 1.2, preferably 1 to 1 .1 .
- the specific surface area of the copper powder is 0.1 to 8.0 m 2 /g, more preferably 0.3 to 4.0 m 2 /g, particularly preferably 0.5 to 2.0 m 2 /g.
- the copper powder is used at 40 to 95 weight percent (wt%), more preferably 52 to 93 wt%, particularly preferably 65 to 92 wt%, based on the weight of the conductive paste.
- the glass frit comprises a metal oxide selected from the group consisting of bismuth oxide (B12O3), boron oxide (B2O3), zinc oxide (ZnO), aluminum oxide (AI2O3), silicon oxide (S1O2) and mixtures thereof.
- the glass frit is a Si -B -Zn glass, a Bi -B -Zn glass or a mixture thereof.
- the glass frit has a softening point of at least about 350°C, 400°C, 450°C, 500°C, or 550°C.
- the softening point of the glass frit is preferably no greater than about 900°C, 875°C, 850°C, 750°C, or 700°C. In some preferred embodiments, the softening point of the glass frit is about 524°C.
- any one preceding embodiment wherein the glass frit comprises 5 to9 wt% S1O2, 5 to 12 wt% B2O3, 1 to 3 wt% AI2O3, 65 to 75 wt% B12O3, 0.1 to 1 wt% CaO and 8 to 16 wt% ZnO.
- the glass frit has a softening point of 524°C.
- the particle diameter (D50) of the glass frit is 0.1 to 15 pm, more preferably 0.5 to 11 pm, more particularly preferably 1 .0 to 6.8 pm, and 1 .5 to 4.5 pm.
- the organic vehicle comprises an organic polymer selected from the group consisting of ethyl cellulose, ethylhydroxyethyl cellulose, wood rosin, phenolic resin, polymethacrylate of a lower (C1-6) alcohol, and mixtures thereof.
- the organic polymer is preferably used at 0.1 to 50 wt%, 0.5 to 42 wt%, 1 to 35 wt%, 2 to 27 wt%, and particularly preferably 3 to 15 wt% based on the weight of the organic vehicle.
- the organic vehicle comprises a solvent selected from the group consisting of texanol (2, 2, 4-Trim ethyl- 1 , 3-pentanediol monoisobutyrate), ester alcohol, terpineol, kerosene, dibutylphthalate, butyl carbitol, butyl carbitol acetate, dibutyl carbitol, hexylene glycol, dibasic ester, and mixtures thereof.
- texanol 2, 2, 4-Trim ethyl- 1 , 3-pentanediol monoisobutyrate
- ester alcohol terpineol
- kerosene dibutylphthalate
- butyl carbitol butyl carbitol acetate
- dibutyl carbitol hexylene glycol, dibasic ester, and mixtures thereof.
- Embodiment 32 wherein the solvent is used at 75 to 95 wt%, more preferably 80 to 93 wt%, more particularly preferably at 85 to 93 wt%, based on the weight of the organic vehicle.
- organic vehicle comprises a mixture of ethyl cellulose and texanol.
- the organic vehicle comprises 3 to 15 wt% ethyl cellulose and 85 to 93 wt% texanol, based on the weight of the organic vehicle.
- the conductive paste is applied by screen printing, spraying or dipping.
- Embodiment 2 and any one preceding embodiment as it relates to Embodiment 2, wherein the firing step is carried out at 600 to 1100°C, 650 to 1050°C in another embodiment, 800 to 1000°C.
- an oxygen- poor atmosphere such as nitrogen, argon or under a vacuum.
- the glass frit was prepared by methods described in U.S. Patent
- the composition of the mixture from which the glass frit was prepared was 7.1 wt% S1O2, 8.4 wt% B2O3, 2.1 wt% AI2O3, 69.8 wt% B12O3, 0.5 wt% CaO and 12.0 wt% ZnO.
- the glass frit had a softening point of 524°C.
- the organic vehicle was a mixture of 6 wt% of an organic polymer, 91 wt% of a solvent and 34 wt% of organic additives based on the weight of the organic vehicle.
- the paste viscosity was about 250 to 400 Pa s measured by Brookfield HBT with a spindle SC4-14 at 10 rpm.
- the conductive paste was screen printed on AI2O3 and Mgo.95Cao.o5Ti03 substrates (25 mm long, 25 mm wide, 0.6 mm thick) in a ring pattern (2.5 mm wide, 10 pm thick, 80 mm round length).
- Dielectric constants of the substrates were 9.6 for AI2O3 and 21 for Mgo.95Cao.o5TiC>3.
- the electrodes were formed by firing the ring pattern at peak temperature of 900°C for 10 minutes under N2 after drying at 150°C for 10 minutes.
- the results are shown in Table 2.
- the conductive paste comprising Cu powder with D50 between 0.8 and 2.6 pm show higher quality factor Q.
- the quality factor Q was determined according to methods that are set forth in U.S. Patent No. 11 ,228,080, cited above. Briefly, the ring pattern that was formed on the fired substrates was connected to a network analyzer (Keysight, E5063A). The Q value and the associated frequency were measured and recorded.
Landscapes
- Chemical & Material Sciences (AREA)
- Engineering & Computer Science (AREA)
- Physics & Mathematics (AREA)
- Dispersion Chemistry (AREA)
- Manufacturing & Machinery (AREA)
- Spectroscopy & Molecular Physics (AREA)
- Thermal Sciences (AREA)
- Inorganic Chemistry (AREA)
- Microelectronics & Electronic Packaging (AREA)
- Conductive Materials (AREA)
- Parts Printed On Printed Circuit Boards (AREA)
Priority Applications (3)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| KR1020247002850A KR20240023179A (ko) | 2021-06-24 | 2022-06-16 | 구리 입자를 포함하는 전도성 페이스트, 및 전자 부품 제조를 위한 이의 용도 |
| JP2023579055A JP2024526577A (ja) | 2021-06-24 | 2022-06-16 | 銅粒子を含む導電性ペーストおよび電子部品の製造のためのその使用 |
| CN202280043917.2A CN117529786A (zh) | 2021-06-24 | 2022-06-16 | 包含铜颗粒的导电浆料及其生产电子元件的用途 |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| US202163214627P | 2021-06-24 | 2021-06-24 | |
| US63/214,627 | 2021-06-24 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2022272224A1 true WO2022272224A1 (en) | 2022-12-29 |
Family
ID=82608555
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/US2022/072979 Ceased WO2022272224A1 (en) | 2021-06-24 | 2022-06-16 | Conductive paste comprising copper particles and use thereof to produce electronic components |
Country Status (4)
| Country | Link |
|---|---|
| JP (1) | JP2024526577A (enExample) |
| KR (1) | KR20240023179A (enExample) |
| CN (1) | CN117529786A (enExample) |
| WO (1) | WO2022272224A1 (enExample) |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN117198593A (zh) * | 2023-10-09 | 2023-12-08 | 中国电力科学研究院有限公司 | 可调控铜基电子浆料体系及其制备方法 |
Families Citing this family (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN122455430A (zh) * | 2025-01-22 | 2026-07-24 | 隆基绿能科技股份有限公司西咸新区分公司 | 片状铜粉体、包含该片状铜粉体的铜浆料、铜电极和太阳能电池 |
Citations (7)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US5439852A (en) | 1994-08-01 | 1995-08-08 | E. I. Du Pont De Nemours And Company | Cadmium-free and lead-free thick film conductor composition |
| US20130026424A1 (en) * | 2011-01-28 | 2013-01-31 | E. I. Du Pont De Nemours And Company | Electrode and method for manufacturing the same |
| EP2822000A1 (en) * | 2013-07-03 | 2015-01-07 | Heraeus Precious Metals North America Conshohocken LLC | Thick print copper pastes for aluminium nitride substrates |
| US20180240576A1 (en) * | 2017-02-23 | 2018-08-23 | E I Du Pont De Nemours And Company | Chip resistor |
| WO2019005452A1 (en) * | 2017-06-29 | 2019-01-03 | Heraeus Precious Metals North America Conshohocken Llc | THICK PRINTING ELECTROCONDUCTIVE PASTES CONTAINING COPPER |
| US20200144691A1 (en) * | 2018-11-07 | 2020-05-07 | Dupont Electronics, Inc. | Dielectric filter and method for manufacturing the same |
| CN112289482A (zh) * | 2020-09-18 | 2021-01-29 | 西安宏星电子浆料科技股份有限公司 | 一种5g陶瓷介质滤波器用高q值银浆 |
Family Cites Families (11)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP3507084B2 (ja) * | 1991-12-13 | 2004-03-15 | イー・アイ・デュポン・ドウ・ヌムール・アンド・カンパニー | 銅導体組成物 |
| US5378408A (en) * | 1993-07-29 | 1995-01-03 | E. I. Du Pont De Nemours And Company | Lead-free thick film paste composition |
| US7438829B2 (en) * | 2003-11-13 | 2008-10-21 | E.I. Du Pont De Nemours And Company | Thick film getter paste compositions for use in moisture control |
| JP4427785B2 (ja) * | 2004-02-06 | 2010-03-10 | 昭栄化学工業株式会社 | 積層セラミック電子部品の端子電極用導体ペースト |
| US6982864B1 (en) * | 2004-06-09 | 2006-01-03 | Ferro Corporation | Copper termination inks containing lead free and cadmium free glasses for capacitors |
| JP4613362B2 (ja) * | 2005-01-31 | 2011-01-19 | Dowaエレクトロニクス株式会社 | 導電ペースト用金属粉および導電ペースト |
| US7531416B2 (en) * | 2005-12-21 | 2009-05-12 | E. I. Du Pont De Nemours And Company | Thick film capacitors on ceramic interconnect substrates |
| JP2011006739A (ja) * | 2009-06-25 | 2011-01-13 | Mitsui Mining & Smelting Co Ltd | 導電性ペースト用銅粉及び導電性ペースト |
| CN104505137A (zh) * | 2014-12-10 | 2015-04-08 | 南京工业大学 | 一种导电铜浆及其制备方法和用途 |
| JP6623919B2 (ja) * | 2016-04-27 | 2019-12-25 | 住友金属鉱山株式会社 | 導電性組成物、導体の製造方法及び電子部品の配線の形成方法 |
| CN111584155B (zh) * | 2020-05-29 | 2021-12-03 | 宁波鑫智达新材料有限公司 | 一种应用于陶瓷滤波器的导电银浆及其制备方法 |
-
2022
- 2022-06-16 JP JP2023579055A patent/JP2024526577A/ja active Pending
- 2022-06-16 WO PCT/US2022/072979 patent/WO2022272224A1/en not_active Ceased
- 2022-06-16 CN CN202280043917.2A patent/CN117529786A/zh active Pending
- 2022-06-16 KR KR1020247002850A patent/KR20240023179A/ko active Pending
Patent Citations (8)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| US5439852A (en) | 1994-08-01 | 1995-08-08 | E. I. Du Pont De Nemours And Company | Cadmium-free and lead-free thick film conductor composition |
| US20130026424A1 (en) * | 2011-01-28 | 2013-01-31 | E. I. Du Pont De Nemours And Company | Electrode and method for manufacturing the same |
| EP2822000A1 (en) * | 2013-07-03 | 2015-01-07 | Heraeus Precious Metals North America Conshohocken LLC | Thick print copper pastes for aluminium nitride substrates |
| US20180240576A1 (en) * | 2017-02-23 | 2018-08-23 | E I Du Pont De Nemours And Company | Chip resistor |
| WO2019005452A1 (en) * | 2017-06-29 | 2019-01-03 | Heraeus Precious Metals North America Conshohocken Llc | THICK PRINTING ELECTROCONDUCTIVE PASTES CONTAINING COPPER |
| US20200144691A1 (en) * | 2018-11-07 | 2020-05-07 | Dupont Electronics, Inc. | Dielectric filter and method for manufacturing the same |
| US11228080B2 (en) | 2018-11-07 | 2022-01-18 | Dupont Electronics, Inc. | Dielectric filter and method for manufacturing the same |
| CN112289482A (zh) * | 2020-09-18 | 2021-01-29 | 西安宏星电子浆料科技股份有限公司 | 一种5g陶瓷介质滤波器用高q值银浆 |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| CN117198593A (zh) * | 2023-10-09 | 2023-12-08 | 中国电力科学研究院有限公司 | 可调控铜基电子浆料体系及其制备方法 |
Also Published As
| Publication number | Publication date |
|---|---|
| JP2024526577A (ja) | 2024-07-19 |
| CN117529786A (zh) | 2024-02-06 |
| KR20240023179A (ko) | 2024-02-20 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP4647224B2 (ja) | 積層セラミック電子部品端子電極用導体ペースト | |
| TWI772671B (zh) | 多層陶瓷電子元件的外部電極形成用之導電性糊 | |
| KR100668549B1 (ko) | 다층 세라믹 축전기용 말단 전극 조성물 | |
| WO2005048667A1 (ja) | 導電性ペーストおよび多層セラミック基板 | |
| CN1162869C (zh) | 导电胶体 | |
| JP2002245874A (ja) | 導体ペースト及びその製造方法 | |
| KR20240023179A (ko) | 구리 입자를 포함하는 전도성 페이스트, 및 전자 부품 제조를 위한 이의 용도 | |
| EP1443531B1 (en) | Terminal electrode compositions for multilayer ceramic capacitors | |
| JP3827060B2 (ja) | 積層セラミック部品端子電極用導体ペースト | |
| JP2005085495A (ja) | 導電性ペースト及びセラミック電子部品 | |
| JP2002110444A (ja) | 導電性ペーストおよび積層セラミック電子部品 | |
| US11228080B2 (en) | Dielectric filter and method for manufacturing the same | |
| JP4427785B2 (ja) | 積層セラミック電子部品の端子電極用導体ペースト | |
| JP2006196421A (ja) | 被覆導体粉末および導体ペースト | |
| JP3414502B2 (ja) | 高温焼成対応貴金属粉末および導体ペースト | |
| KR102851511B1 (ko) | 후막 저항 페이스트, 후막 저항체, 및 전자 부품 | |
| JP2024526577A5 (enExample) | ||
| JP5630363B2 (ja) | 導電性ペーストおよびその製造方法 | |
| KR101848694B1 (ko) | 무연 후막 저항체 및 이를 포함하는 전자부품 | |
| JP2018152218A (ja) | 導電性ペースト、チップ電子部品及びその製造方法 | |
| JP2020015635A (ja) | セラミックス組成物及び当該セラミックス組成物を用いた電子部品 | |
| KR20230110244A (ko) | 도전성 페이스트 및 적층 세라믹 콘덴서 | |
| JP3862042B2 (ja) | 導電性ペースト、それを用いたセラミックス構造物及びその製造方法 | |
| JP4562282B2 (ja) | セラミック回路基板の製法 | |
| JP2009187695A (ja) | ディスプレイ用導体ペースト組成物 |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 22744087 Country of ref document: EP Kind code of ref document: A1 |
|
| ENP | Entry into the national phase |
Ref document number: 2023579055 Country of ref document: JP Kind code of ref document: A |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 202280043917.2 Country of ref document: CN |
|
| ENP | Entry into the national phase |
Ref document number: 20247002850 Country of ref document: KR Kind code of ref document: A |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 1020247002850 Country of ref document: KR |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| 122 | Ep: pct application non-entry in european phase |
Ref document number: 22744087 Country of ref document: EP Kind code of ref document: A1 |