WO2017094806A1 - Procédé de production de propylène ou d'un hydrocarbure aromatique - Google Patents

Procédé de production de propylène ou d'un hydrocarbure aromatique Download PDF

Info

Publication number
WO2017094806A1
WO2017094806A1 PCT/JP2016/085645 JP2016085645W WO2017094806A1 WO 2017094806 A1 WO2017094806 A1 WO 2017094806A1 JP 2016085645 W JP2016085645 W JP 2016085645W WO 2017094806 A1 WO2017094806 A1 WO 2017094806A1
Authority
WO
WIPO (PCT)
Prior art keywords
catalyst
zeolite
regeneration
reactor
raw material
Prior art date
Application number
PCT/JP2016/085645
Other languages
English (en)
Japanese (ja)
Inventor
光弘 関口
正嗣 川瀬
Original Assignee
旭化成株式会社
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 旭化成株式会社 filed Critical 旭化成株式会社
Priority to JP2017554161A priority Critical patent/JP6505866B2/ja
Publication of WO2017094806A1 publication Critical patent/WO2017094806A1/fr

Abstract

L'invention concerne un procédé de production de propylène ou d'un hydrocarbure aromatique comprenant une étape consistant en une réaction de conversion dans laquelle une matière première hydrocarbonée comprenant un composé de soufre comme impureté et contenant au moins une oléfine en C4-12 est mise en contact avec un catalyseur contenant une zéolite dans un réacteur de production, et une étape de régénération du catalyseur consistant en la combustion de la substance carbonée adhérant au catalyseur contenant la zéolite. Lors de l'étape de régénération du catalyseur, la température de l'équipement et du circuit à travers lesquels circule le gaz de régénération est maintenue égale ou supérieure à la température du point de rosée de l'acide sulfurique contenu dans le gaz de régénération circulant à travers l'équipement et le circuit.
PCT/JP2016/085645 2015-12-03 2016-11-30 Procédé de production de propylène ou d'un hydrocarbure aromatique WO2017094806A1 (fr)

Priority Applications (1)

Application Number Priority Date Filing Date Title
JP2017554161A JP6505866B2 (ja) 2015-12-03 2016-11-30 プロピレンまたは芳香族炭化水素の製造方法

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2015236785 2015-12-03
JP2015-236785 2015-12-03

Publications (1)

Publication Number Publication Date
WO2017094806A1 true WO2017094806A1 (fr) 2017-06-08

Family

ID=58797522

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2016/085645 WO2017094806A1 (fr) 2015-12-03 2016-11-30 Procédé de production de propylène ou d'un hydrocarbure aromatique

Country Status (3)

Country Link
JP (1) JP6505866B2 (fr)
TW (1) TWI629101B (fr)
WO (1) WO2017094806A1 (fr)

Cited By (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2020081991A (ja) * 2018-11-28 2020-06-04 東ソー株式会社 金属イオン担持ゼオライト触媒の再生方法
JP2020082004A (ja) * 2018-11-29 2020-06-04 東ソー株式会社 銀イオン担持ゼオライト触媒の再生方法
TWI711695B (zh) * 2019-04-03 2020-12-01 芬蘭商耐斯特公司 製造碳氫化合物的方法及原料
CN113646081A (zh) * 2019-03-18 2021-11-12 埃克森美孚研究工程公司 中孔催化剂化合物及其用途
EP3793727B1 (fr) 2018-05-14 2022-06-22 UMICORE AG & Co. KG Zéolites à petits pores stables

Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH08157399A (ja) * 1994-10-03 1996-06-18 Sanyo Sekiyu Kagaku Kk 芳香族炭化水素の製造方法
WO2000010948A1 (fr) * 1998-08-25 2000-03-02 Asahi Kasei Kogyo Kabushiki Kaisha Procede de production d'ethylene et de propylene
JP2009136839A (ja) * 2007-12-10 2009-06-25 Sumitomo Heavy Ind Ltd 燃焼・排ガス処理装置及び燃焼・排ガス処理方法
WO2011013780A1 (fr) * 2009-07-30 2011-02-03 三菱化学株式会社 Procédé de production du propylène et catalyseur de production du propylène

Family Cites Families (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN1234460C (zh) * 2003-01-30 2006-01-04 中国石油化工股份有限公司 一种固体酸催化剂的再生方法
EP1770080B1 (fr) * 2004-07-16 2015-05-27 Asahi Kasei Chemicals Corporation Procédé de production d'éthylène et de propylène

Patent Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH08157399A (ja) * 1994-10-03 1996-06-18 Sanyo Sekiyu Kagaku Kk 芳香族炭化水素の製造方法
WO2000010948A1 (fr) * 1998-08-25 2000-03-02 Asahi Kasei Kogyo Kabushiki Kaisha Procede de production d'ethylene et de propylene
JP2009136839A (ja) * 2007-12-10 2009-06-25 Sumitomo Heavy Ind Ltd 燃焼・排ガス処理装置及び燃焼・排ガス処理方法
WO2011013780A1 (fr) * 2009-07-30 2011-02-03 三菱化学株式会社 Procédé de production du propylène et catalyseur de production du propylène

Non-Patent Citations (2)

* Cited by examiner, † Cited by third party
Title
MASAMICHI KOWAKA ET AL.: "Corrosion of Iron and Steels in Flue Gas", JOURNAL OF THE IRON & STEEL INSTITUTE OF JAPAN, 1976, pages 1052 - 1065, XP055388780 *
MASAMICHI KOWAKA ET AL.: "Recent Progress on the Prevention of Dew Point Corrosion", BOSHOKU GIJUTSU, vol. 30, no. 11, 1981, pages 650, XP055388782 *

Cited By (8)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP3793727B1 (fr) 2018-05-14 2022-06-22 UMICORE AG & Co. KG Zéolites à petits pores stables
JP2020081991A (ja) * 2018-11-28 2020-06-04 東ソー株式会社 金属イオン担持ゼオライト触媒の再生方法
JP7293622B2 (ja) 2018-11-28 2023-06-20 東ソー株式会社 金属イオン担持ゼオライト触媒の再生方法
JP2020082004A (ja) * 2018-11-29 2020-06-04 東ソー株式会社 銀イオン担持ゼオライト触媒の再生方法
JP7218553B2 (ja) 2018-11-29 2023-02-07 東ソー株式会社 銀イオン担持ゼオライト触媒の再生方法
CN113646081A (zh) * 2019-03-18 2021-11-12 埃克森美孚研究工程公司 中孔催化剂化合物及其用途
CN113646081B (zh) * 2019-03-18 2024-01-09 埃克森美孚科技工程公司 中孔催化剂化合物及其用途
TWI711695B (zh) * 2019-04-03 2020-12-01 芬蘭商耐斯特公司 製造碳氫化合物的方法及原料

Also Published As

Publication number Publication date
TW201720522A (zh) 2017-06-16
JPWO2017094806A1 (ja) 2018-08-02
TWI629101B (zh) 2018-07-11
JP6505866B2 (ja) 2019-04-24

Similar Documents

Publication Publication Date Title
WO2017094806A1 (fr) Procédé de production de propylène ou d'un hydrocarbure aromatique
JP4953817B2 (ja) エチレン及びプロピレンの製造法
EP2184269B1 (fr) Procédé de production d'hydrocarbures aromatiques
EP1642641B1 (fr) Catalyseur et procédé de préparation des composés aromatiques monocycyliques
RU2118634C1 (ru) Способ получения ароматических углеводородов
RU2398630C2 (ru) Катализатор для производства ароматических углеводородных соединений
US10351787B2 (en) Process for the aromatization of dilute ethylene
US7815793B2 (en) Process for reducing bromine index of hydrocarbon feedstock
WO2007058703A1 (fr) Procede pour reduire l'indice de brome de charges d'alimentation d'hydrocarbure
US10240094B2 (en) Conversion of oxygenates to hydrocarbons with variable catalyst composition
RU2425091C1 (ru) Способ получения высокооктанового бензина и/или ароматических углеводородов с низким содержанием бензола
JP4240339B2 (ja) 芳香族炭化水素の製造方法
US8853480B2 (en) Method for producing aromatic hydrocarbon
JP3966429B2 (ja) 芳香族炭化水素製造用触媒
WO2018111955A1 (fr) Procédé catalytique pour la coproduction de benzène, d'éthylène et d'hydrogène
WO2012169651A1 (fr) Procédé de fabrication d'un hydrocarbure aromatique et/ou d'une oléfine ayant au plus 4 atomes de carbone et appareil de fabrication d'un hydrocarbure aromatique et/ou d'une oléfine ayant au plus 4 atomes de carbone
US11084983B2 (en) Fluidized bed conversion of oxygenates with increased aromatic selectivity
TWI609852B (zh) 低級烯烴之製造方法

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 16870743

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2017554161

Country of ref document: JP

Kind code of ref document: A

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 16870743

Country of ref document: EP

Kind code of ref document: A1