WO2013115101A1 - 電子部品及びその製法、並びにそれに用いる封止材料ペースト - Google Patents

電子部品及びその製法、並びにそれに用いる封止材料ペースト Download PDF

Info

Publication number
WO2013115101A1
WO2013115101A1 PCT/JP2013/051625 JP2013051625W WO2013115101A1 WO 2013115101 A1 WO2013115101 A1 WO 2013115101A1 JP 2013051625 W JP2013051625 W JP 2013051625W WO 2013115101 A1 WO2013115101 A1 WO 2013115101A1
Authority
WO
WIPO (PCT)
Prior art keywords
sealing material
glass
oxide
low melting
electronic component
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP2013/051625
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
内藤 孝
拓也 青柳
信一 立薗
圭 吉村
裕司 橋場
沢井 裕一
正 藤枝
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Resonac Corp
Original Assignee
Hitachi Chemical Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Hitachi Chemical Co Ltd filed Critical Hitachi Chemical Co Ltd
Priority to CN201380005016.5A priority Critical patent/CN104081877A/zh
Publication of WO2013115101A1 publication Critical patent/WO2013115101A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Images

Classifications

    • C—CHEMISTRY; METALLURGY
    • C03—GLASS; MINERAL OR SLAG WOOL
    • C03C—CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS
    • C03C8/00—Enamels; Glazes; Fusion seal compositions being frit compositions having non-frit additions
    • C03C8/24—Fusion seal compositions being frit compositions having non-frit additions, i.e. for use as seals between dissimilar materials, e.g. glass and metal; Glass solders
    • C—CHEMISTRY; METALLURGY
    • C03—GLASS; MINERAL OR SLAG WOOL
    • C03C—CHEMICAL COMPOSITION OF GLASSES, GLAZES OR VITREOUS ENAMELS; SURFACE TREATMENT OF GLASS; SURFACE TREATMENT OF FIBRES OR FILAMENTS MADE FROM GLASS, MINERALS OR SLAGS; JOINING GLASS TO GLASS OR OTHER MATERIALS
    • C03C3/00—Glass compositions
    • C03C3/12—Silica-free oxide glass compositions
    • C03C3/16—Silica-free oxide glass compositions containing phosphorus
    • C03C3/21—Silica-free oxide glass compositions containing phosphorus containing titanium, zirconium, vanadium, tungsten or molybdenum
    • H—ELECTRICITY
    • H05—ELECTRIC TECHNIQUES NOT OTHERWISE PROVIDED FOR
    • H05B—ELECTRIC HEATING; ELECTRIC LIGHT SOURCES NOT OTHERWISE PROVIDED FOR; CIRCUIT ARRANGEMENTS FOR ELECTRIC LIGHT SOURCES, IN GENERAL
    • H05B33/00—Electroluminescent light sources
    • H05B33/02—Details
    • H05B33/04—Sealing arrangements, e.g. against humidity
    • H—ELECTRICITY
    • H05—ELECTRIC TECHNIQUES NOT OTHERWISE PROVIDED FOR
    • H05B—ELECTRIC HEATING; ELECTRIC LIGHT SOURCES NOT OTHERWISE PROVIDED FOR; CIRCUIT ARRANGEMENTS FOR ELECTRIC LIGHT SOURCES, IN GENERAL
    • H05B33/00—Electroluminescent light sources
    • H05B33/10—Apparatus or processes specially adapted to the manufacture of electroluminescent light sources
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10K—ORGANIC ELECTRIC SOLID-STATE DEVICES
    • H10K59/00—Integrated devices, or assemblies of multiple devices, comprising at least one organic light-emitting element covered by group H10K50/00
    • H10K59/80—Constructional details
    • H10K59/87—Passivation; Containers; Encapsulations
    • H10K59/871—Self-supporting sealing arrangements
    • H10K59/8722—Peripheral sealing arrangements, e.g. adhesives, sealants
    • Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y02—TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
    • Y02E—REDUCTION OF GREENHOUSE GAS [GHG] EMISSIONS, RELATED TO ENERGY GENERATION, TRANSMISSION OR DISTRIBUTION
    • Y02E10/00—Energy generation through renewable energy sources
    • Y02E10/50—Photovoltaic [PV] energy
    • Y02E10/542—Dye sensitized solar cells
    • Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y02—TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
    • Y02P—CLIMATE CHANGE MITIGATION TECHNOLOGIES IN THE PRODUCTION OR PROCESSING OF GOODS
    • Y02P70/00—Climate change mitigation technologies in the production process for final industrial or consumer products
    • Y02P70/50—Manufacturing or production processes characterised by the final manufactured product

Definitions

  • the present invention relates to an electronic component in which an organic element or an organic material is contained between two transparent substrates, and the outer peripheral portion thereof is joined using a sealing material.
  • an electronic component in which an organic element or an organic material is embedded between two transparent substrates.
  • the outer peripheral portion of the two transparent substrates is joined with a resin sealing material, and a desiccant is further incorporated into the electronic component. It has been installed.
  • bonding with resin has insufficient gas barrier properties (air tightness)
  • water molecules are gradually permeated and sufficient reliability has not been obtained.
  • a sealing material using low melting point glass enables bonding with high gas barrier properties (air tightness), but requires a bonding temperature significantly higher than that of a resin sealing material. At this bonding temperature, the heat resistance of the organic element and organic material incorporated in the electronic component is exceeded.
  • the sealing material uses low melting point glass which enables airtight bonding. It is important that the low melting glass be heated by absorbing the laser light used and softened and flow. Since such a method can heat only the outer peripheral portion of the two transparent substrates, high gas barrier properties (airtightness) can be achieved without causing thermal damage to the organic element or organic material incorporated in the electronic component. Enables glass bonding).
  • Patent Document 1 proposes a sealing material capable of joining the outer peripheral portion with a laser in an OLED display.
  • This sealing material is a V 2 O 5 -P 2 O 5 -Sb 2 O 3 -based low melting glass that can be heated by laser, and a lithium alumino silicate ( ⁇ -eucryptite) for reducing the thermal expansion coefficient. Containing filler particles.
  • the low-melting glass, K 2 comprises O, Fe 2 O 3, ZnO , one of TiO 2, Al 2 O 3, B 2 O 3, WO 3, having a transition point T g of the less than 350 ° C.
  • Patent Document 2 also proposes a glass package to which the same sealing material as in Patent Document 1 is applied.
  • the low melting point glass contained in the sealing material is also similar to that of Patent Document 1.
  • Patent No. 4540669 Japanese Patent Application Publication No. 2008-527656
  • the softening fluidity and the adhesiveness by the laser irradiation are reduced, so that it is necessary to take time for temporary baking at a lower temperature.
  • By increasing the laser output it is possible to improve the softening flowability and adhesion, but there is a possibility that the organic element and the organic material incorporated in the electronic component may be thermally damaged.
  • an object of the present invention is to reduce thermal damage to an organic element or an organic material incorporated in an electronic component, efficiently manufacture the electronic component, and reduce the devitrification of the glass bonding layer.
  • the present invention is an electronic component which has an organic member between two sheets of transparent substrates, and joins the perimeter part of the two sheets of transparent substrates with a sealing material containing low melting glass.
  • the low melting point glass contains vanadium oxide (V 2 O 5 ), tellurium oxide (TeO 2 ), phosphorus oxide (P 2 O 5 ) and iron oxide (Fe 2 O 3 ), and the following oxide conversion V 2 O 5 + TeO 2 + P 2 O 5 + Fe 2 O 3 7575% by mass, and V 2 O 5 > TeO 2 > P 2 O 5 FeFe 2 O 3 (% by mass).
  • the present invention is also a sealing material paste containing low melting point glass, a resin binder and a solvent, wherein the low melting point glass is vanadium oxide (V 2 O 5 ), tellurium oxide (TeO 2 ), phosphorus oxide (P 2 ) 2 O 5 ) and iron oxide (Fe 2 O 3 ), and V 2 O 5 + TeO 2 + P 2 O 5 + Fe 2 O 3 7575 mass% in terms of the following oxide conversion, V 2 O 5 > TeO 2 > P 2 O 5 5Fe 2 O 3 (% by mass).
  • the low melting point glass is vanadium oxide (V 2 O 5 ), tellurium oxide (TeO 2 ), phosphorus oxide (P 2 ) 2 O 5 ) and iron oxide (Fe 2 O 3 ), and V 2 O 5 + TeO 2 + P 2 O 5 + Fe 2 O 3 7575 mass% in terms of the following oxide conversion, V 2 O 5 > TeO 2 > P 2 O 5 5Fe 2 O 3 (% by mass).
  • the thermal damage with respect to the organic element and organic material which are incorporated in an electronic component can be reduced, an electronic component can be manufactured efficiently, and the devitrification of a glass joining layer can be reduced.
  • FIG. 3 is a schematic cross-sectional view of the sealing portion along IIB-IIB shown in FIG. 2A. It is a schematic top view which shows an example of the manufacturing method of the electronic component shown by FIG. 1A, 1B.
  • FIG. 3B is a schematic cross-sectional view along IIIB-IIIB shown in FIG. 3A. It is a schematic top view which shows an example of the manufacturing method of the electronic component shown by FIG. 1A and 1B.
  • FIG. 4B is a schematic cross-sectional view along IVB-IVB shown in FIG.
  • FIG. 4A It is a schematic sectional drawing which shows an example of the manufacturing method of the electronic component shown by FIG. 1A. It is a schematic perspective view which shows an example of the manufacturing method of the electronic component shown by FIG. 2A, 2B. It is a schematic sectional drawing which shows an example of the manufacturing method of the electronic component shown by FIG. 2A, 2B. It is a graph which shows an example of the DTA curve obtained by differential thermal analysis (DTA) of a typical low melting glass. It is a graph which shows an example of the thermal expansion curve of a typical low melting glass. It is the schematic which shows the laser irradiation experiment to a glass compacting body. It is the schematic which shows the state which apply
  • DTA differential thermal analysis
  • FIGS. 1A and 1B and FIGS. 2A and 2B show schematic top views of two types of electronic components according to an embodiment of the present invention and cross-sectional schematic views of the sealing portions thereof.
  • the electronic component shown in FIGS. 1A and 1B has two transparent substrates 1 and 2 and one or more organic members 3 (organic elements or organic materials) between the transparent substrates 1 and 2.
  • the outer peripheral portions of the transparent substrates 1 and 2 were bonded with a sealing material 5 containing low melting glass.
  • the electronic component shown in FIGS. 2A and 2B has two transparent substrates 1 and 2 with a larger gap, and the transparent substrates 1 and 2 are joined by the sealing material 5 and 5A via the spacer 6.
  • the low melting point glass contained in the sealing material 5, 5A contains vanadium oxide, tellurium oxide, phosphorus oxide and iron oxide, and the following oxide conversion V 2 O 5 , TeO 2 , P 2 O 5 And Fe 2 O 3 is at least 75% by mass, and V 2 O 5 > TeO 2 > P 2 O 5 FeFe 2 O 3 (% by mass).
  • the low melting point glass satisfying this condition is efficiently absorbed by the light of the wavelength, heated, and softened and flows easily, particularly by laser irradiation. That is, by using the low melting point glass and the laser, heating can be stopped only at a desired place, and the outer peripheral portions of the two transparent substrates 1 and 2 can be joined without thermally damaging the organic member 3.
  • a wavelength of a laser to be used it is effective in the range of 400 to 1100 nm in which the low melting glass efficiently absorbs light and transmits the transparent substrate. If the wavelength is less than 400 nm, the transparent substrate and the organic element and organic material in the inside may be heated and deteriorated. On the other hand, if the wavelength exceeds 1100 nm, the light absorption of this low melting glass decreases, and it does not show good softening and fluidity, and if there is a place containing moisture, this moisture is heated and has an adverse effect. Sometimes.
  • the low melting point glass it is important to contain the largest amount of V 2 O 5 in terms of oxide. By this, the low melting glass efficiently absorbs light in the wavelength range of 400 to 1100 nm and is heated. At the same time, the softening point T s of the low melting glass can be lowered, and the low melting glass can be easily softened and flowed by irradiating the low melting glass with a laser in the wavelength range of 400 to 1100 nm.
  • TeO 2 and P 2 O 5 are important components for vitrification. If the sealing material is not glass, it can not soften and flow at low temperatures. Also, the sealing material can not be easily softened and flowed by laser irradiation. P 2 O 5 has a greater effect of vitrifying than TeO 2 and is effective for reducing thermal expansion, but when P 2 O 5 has a content of TeO 2 or more, it lowers the moisture resistance and water resistance, and softens. It raises the point T s . However, when the content of TeO 2 is increased, the thermal expansion coefficient tends to increase. If the thermal expansion coefficient becomes too large, heat shock by laser irradiation may be broken before softening and flowing the low melting glass.
  • Fe 2 O 3 is a component that acts particularly on P 2 O 5 to improve the moisture resistance and water resistance of the low melting glass. Further, Fe 2 O 3 is also a component that efficiently absorbs light in the wavelength range of 400 to 1100 nm as V 2 O 5 does. However, when the content of Fe 2 O 3 exceeds P 2 O 5 , the low melting point glass is crystallized by heating. This crystallization is a phenomenon that hinders the softening and fluidity of the low melting point glass and is not desirable.
  • V 2 O 5 , TeO 2 , P 2 O 5 and Fe 2 O 3 described above can be obtained by the total content of those being 75 mass% or more, and by laser irradiation A joint portion with high reliability (adhesion, adhesion, moisture resistance, water resistance, etc.) can be obtained.
  • a particularly effective composition range of the low melting point glass is 35 to 55% by mass of V 2 O 5 , 19 to 30% by mass of TeO 2 , 7 to 20% by mass of P 2 O 5 , 5 to 5 in terms of the following oxides. It is 15% by mass of Fe 2 O 3 .
  • the inclusion of WO 3 , MoO 3 , Ta 2 O 5 , ZnO, BaO, SrO is effective for preventing or suppressing crystallization.
  • the inclusion of MnO 2 , Sb 2 O 3 , Bi 2 O 3 , BaO, SrO, Ag 2 O, and K 2 O is effective for improving the moisture resistance and the water resistance. Containing Nb 2 O 5 , Ta 2 O 5 and ZnO is effective for reducing the thermal expansion coefficient.
  • the contents of MoO 3 , Ag 2 O, and K 2 O are effective for lowering the softening point T s .
  • the components promoting crystallization are Nb 2 O 5 , MnO 2 , Sb 2 O 3 , Bi 2 O 3 , Ag 2 O, and K 2 O.
  • Component would raise the softening point T s is Sb 2 O 3, Bi 2 O 3, BaO, is SrO.
  • the components that increase the thermal expansion coefficient are MoO 3 , BaO, SrO, Ag 2 O, and K 2 O.
  • the components that lower the moisture resistance and water resistance are MoO 3 , Nb 2 O 5 , Ta 2 O 5 , and ZnO.
  • the content of WO 3 , MoO 3 , Nb 2 O 5 , Ta 2 O 5 , MnO 2 , Sb 2 O 3 , Bi 2 O 3 , ZnO, BaO, SrO, Ag 2 O, K 2 O is short and long It is. It is necessary to determine the components to be contained and the content thereof with due consideration given to the characteristics of the base composition consisting of V 2 O 5 , TeO 2 , P 2 O 5 and Fe 2 O 3 .
  • WO 3 Of WO 3 , MoO 3 , Nb 2 O 5 , Ta 2 O 5 , MnO 2 , Sb 2 O 3 , Bi 2 O 3 , ZnO, SrO, BaO, Ag 2 O, K 2 O in terms of the following oxides It is preferable that the sum of one or more be 25% by mass or less. When the total content of these components exceeds 25% by mass, the softening point T s may be increased, the thermal expansion coefficient may be increased, or the crystallization tendency may be increased.
  • WO 3 WO 3 , MoO 3 , Nb 2 O 5 , Ta 2 O 5 , MnO 2 , Sb 2 O 3 , Bi 2 O 3 , ZnO, SrO, BaO, Ag 2 O, and K 2 O More preferably, the total is 0 to 20% by mass.
  • V 2 O 5 When V 2 O 5 is less than 35% by mass, the low melting point glass may become difficult to soften and flow easily even when the low melting point glass is irradiated with a laser having a wavelength in the range of 400 to 1100 nm. On the other hand, when V 2 O 5 exceeds 55% by mass, reliability such as moisture resistance and water resistance may be lowered.
  • the TeO 2 is less than 19 mass%, the or crystallization tendency of the low-melting glass becomes large, or the softening point T s is increased, humidity resistance, reliability such as water resistance decreases.
  • the content of P 2 O 5 is less than 7% by mass, the crystallization tendency of the low melting glass may be increased, and furthermore, the low melting glass may be difficult to soften and flow due to the laser irradiation.
  • P 2 O 5 exceeds 20% by mass, the softening point T s of the low melting glass may rise, and the low melting glass may not easily soften and flow even when the laser is irradiated.
  • this P 2 O 5 may lower the reliability of the low melting point glass such as moisture resistance and water resistance.
  • the Fe 2 O 3 is less than 5 wt%, the moisture resistance of the low-melting glass, the reliability of the water resistance is lowered, whereas, Fe 2 O 3 crystallization of the low-melting glass exceeds 15 mass% is promoted May be
  • transition point T g is 320 ° C. or less and a softening point T s of the low melting glass is effective at 380 ° C. or less.
  • the transition point T g and the softening point T s referred to here are characteristic temperatures by differential thermal analysis (DTA), and the transition point T g is the onset temperature of the first endothermic peak, the softening point T s is the second endothermic peak temperature.
  • DTA differential thermal analysis
  • the softening point T s is higher than 380 ° C.
  • the low-melting glass becomes hard to easily soften flow during laser irradiation.
  • the low melting point glass has a thermal expansion coefficient of 100 ⁇ 10 ⁇ 7 / ° C. or less at 30 to 250 ° C. When the thermal expansion coefficient exceeds 100 ⁇ 10 ⁇ 7 / ° C., cracks may occur due to heat shock during laser irradiation.
  • the sealing material 5 may further contain, for example, a filler for reducing the thermal expansion coefficient, in addition to the low melting point glass.
  • the filler is preferably at least one of zirconium phosphate tungstate (Zr 2 (WO 4 ) (PO 4 ) 2 ), niobium oxide (Nb 2 O 5 ), and silicon (Si). These fillers have a thermal expansion coefficient smaller than that of the present low melting glass, and also have good wettability and adhesion to the present low melting glass, so that the thermal expansion coefficient as the sealing material 5 should be reduced. Can.
  • the effect of lowering the thermal expansion coefficient of the sealing material 5 is the largest in Zr 2 (WO 4 ) (PO 4 ) 2 , then in the order of Si and Nb 2 O 5 .
  • Si is particularly effective for laser sealing because it can absorb and generate a laser having a wavelength in the range of 400 to 1100 nm and its thermal conductivity is better than the other two fillers and low melting point glass.
  • the content of the filler in the sealing material is preferably 35 parts by volume or less with respect to 100 parts by volume of the present low melting glass.
  • the content of the filler exceeds 35 parts by volume, the softening and fluidity of the low melting glass in the sealing material may be reduced, and the adhesion may be weakened at the time of laser irradiation.
  • the thickness of the bonding layer made of the sealing material 5 is preferably 20 ⁇ m or less.
  • the thickness of the bonding layer exceeds 20 ⁇ m, the low melting point glass contained in the sealing material 5 far from the transparent substrate side irradiated with the laser is hard to soften and flow, so the entire thickness direction of the sealing material 5 is good. It will not show softening flowability.
  • the thickness of the bonding layer at that time is preferably 20 ⁇ m or less in the same manner as described above for both of the sealing materials 5 and 5A.
  • the transparent substrates 1 and 2 or the spacer 6 are made of glass or resin. Since they are transparent, they have low absorptivity for light of wavelengths of 400 to 1100 nm and high transmittance. For this reason, even when a laser having a wavelength in the range of 400 to 1100 nm is irradiated, the laser can be transmitted without being heated, and only the sealing material 5 or 5A of the desired portion can be irradiated. In the sealing material 5 or 5A irradiated with the laser, since the low melting point glass contained therein softens and flows, the outer peripheral portions of the transparent substrates 1 and 2 can be joined.
  • the present invention is effectively applied to a display incorporating an organic light emitting diode, a dye-sensitized solar cell incorporating an organic dye, a solar cell incorporating a photoelectric conversion element and laminated with a resin, etc. .
  • the present invention is also applicable to the case where a low heat resistant element or material is applied to the inside of an electronic component, and is not limited to the above electronic component.
  • this invention is the sealing material paste containing the powder of the said low melting glass, a resin binder, and a solvent.
  • a resin binder and a solvent By including a resin binder and a solvent, it becomes easy to apply to a substrate like screen printing. Since the sealing material paste is applied to a substrate and then dried to evaporate the resin binder and the solvent, no bubbles are generated at the time of firing, and the airtightness of the formed sealing material can be enhanced.
  • a particle size of this low melting glass it is preferable that an average particle size is 3 micrometers or less.
  • the resin binder ethyl cellulose or nitrocellulose is preferable, and as the solvent, butyl carbitol acetate is preferable.
  • this sealing material paste may contain filler particles.
  • this filler particle As a particle size of this filler particle, it is preferable that an average particle size is larger than the average particle size of the said low melting glass. Moreover, it is preferable that content of this filler particle
  • FIGS. 3A and 3B-5 A method of manufacturing the electronic component shown in FIGS. 1A and 1B is briefly shown in FIGS. 3A and 3B-5.
  • the sealing material 5 containing low melting glass is formed in the outer peripheral part of the transparent substrate 1.
  • FIG. 3A and 3B the sealing material 5 containing low melting glass is formed in the outer peripheral part of the transparent substrate 1.
  • FIG. 3A and 3B the sealing material 5 containing low melting glass is formed in the outer peripheral part of the transparent substrate 1.
  • FIG. In the formation method first, the above-mentioned sealing material paste to be the sealing material 5 is applied to the outer peripheral portion of the transparent substrate 1 and dried.
  • the low melting point glass contained in the sealing material 5 is softened and flowed by the firing furnace or the irradiation of the laser 7 in the wavelength range of 400 to 1100 nm to bake the transparent substrate 1.
  • a resin substrate is used for the transparent substrate 1, the heat resistance of the resin is low, and a firing furnace can not be used. Therefore, the sealing material
  • the other transparent substrate 2 on which one or more organic members 3 are formed is manufactured.
  • the transparent substrate 2 may be either a glass substrate or a resin substrate, but is preferably combined with the material of the transparent substrate 1.
  • the surface of the transparent substrate 1 on which the sealing material 5 is formed and the surface of the transparent substrate 2 on which the organic member 3 is formed are opposed as shown in FIG. 5 to align the two transparent substrates 1 and 2
  • the organic member 3 is disposed in the internal space formed by the transparent substrates 1 and 2 and the sealing material 5.
  • the organic member 3 may be formed on the transparent substrate 1 because it is difficult to heat other than the outer peripheral portion of the transparent substrate 1.
  • the sealing material 5 is irradiated with a laser 7 in the wavelength range of 400 to 1100 nm through the transparent substrate.
  • the laser 7 may be applied to the sealing material 5 from the outside of any transparent substrate, but since the sealing material 5 is previously formed on the transparent substrate 1, the laser from the outside of the transparent substrate 2 to the sealing material 5 When 7 is irradiated, sealing can be performed more efficiently. At that time, care must be taken not to irradiate the laser 7 to the organic member 3 incorporated in the electronic component. This is because there is a high possibility that the organic member 3 may be damaged or degraded by the irradiation of the laser 7.
  • the sealing material 5 softens and flows the low melting point glass contained in the sealing material 5 by the irradiation of the laser 7 and bonds the outer peripheral portions of the two transparent substrates 1 and 2.
  • the manufacturing method of the electronic component shown to FIG. 2A, 2B is simply shown to FIG. 6 and FIG.
  • the sealing materials 5 and 5A are formed on at least the bonding surface of the spacer 6.
  • the above-mentioned sealing material paste to be the sealing materials 5 and 5A is applied to the bonding surface where the spacer 6 is to be bonded to at least the transparent substrate, and dried.
  • the glass spacer 6 is contained in the sealing materials 5 and 5A by irradiating from both sides of the transparent substrates 1 and 2 with a baking furnace or lasers 7 and 7A in the wavelength range of 400 to 1100 nm.
  • the low melting point glass is softened to flow and fired to form the spacer 6.
  • the spacer 6 made of resin since the heat resistance of the resin is low and the firing furnace can not be used, the sealing material 5 is fired and formed on the spacer 6 by the irradiation of the laser 7 and 7A.
  • the spacer 6 on which the sealing materials 5 and 5A are formed is installed and fixed on the outer peripheral portion of the transparent substrate 1 and the other transparent substrate 2 on which one or more organic members 3 are formed. Then, the lasers 7 and 7A in the wavelength range of 400 to 1100 nm are irradiated to the sealing materials 5 and 5A through the transparent substrate. At this time, care must be taken not to irradiate the lasers 7 and 7A to the organic member 3 incorporated in the electronic component as described above.
  • the sealing materials 5 and 5A soften and flow the low melting point glass contained in the sealing materials 5 and 5A by the irradiation of the lasers 7 and 7A, and bond the outer peripheral portions of the two transparent substrates 1 and 2.
  • the transparent substrates 1 and 2 may be either a glass substrate or a resin substrate as long as the reflectance of light in the wavelength range of 400 to 1100 nm is low and the transmittance is high.
  • the electronic component of the present invention the method for producing the same, and the sealing material paste used therefor efficiently produce the electronic component without causing thermal damage to the organic element and the organic material incorporated in the electronic component.
  • the composition and characteristics of the low melting point glass contained in the sealing material were examined. Examples are shown in Tables 1 to 4 and Comparative Examples are shown in Table 5.
  • reagents V 2 O 5 , TeO 2 , P 2 O 5 , Fe 2 O 3 , WO 3 , MoO 3 , Nb made by High-Purity Chemical Laboratory make as raw materials 2 O 5 , Ta 2 O 5 , MnO 2 , Sb 2 O 3 , Bi 2 O 3 , ZnO, SrCO 3 , BaCO 3 , Ag 2 O and K 2 CO 3 were used.
  • a predetermined amount was blended and mixed so as to be 200 g in total, placed in a platinum crucible, and heated to 900 to 1000 ° C. at a heating rate of 5 to 10 ° C./min in an electric furnace to melt.
  • the raw material was held for 2 hours while stirring to obtain a uniform glass at this temperature. Thereafter, the crucible was taken out, and the raw material was poured on a stainless steel plate preheated to 150 to 200 ° C. to produce a low melting point glass.
  • the produced low melting glass was crushed by a jet mill until the average particle size became 3 ⁇ m or less.
  • the powder is subjected to differential thermal analysis (DTA) up to 500 ° C. at a heating rate of 5 ° C./min to obtain a transition point (T g ), a deformation point (M g ), a softening point (T s ) and crystals.
  • DTA differential thermal analysis
  • T g transition point
  • M g deformation point
  • T s softening point
  • Tcry crystallization temperature
  • An alumina (Al 2 O 3 ) powder was used as a standard sample.
  • FIG. 8 shows a DTA curve of a typical low melting point glass. As shown in FIG.
  • T g is the start temperature of the first endothermic peak
  • M g is the peak temperature
  • T s is the second endothermic peak temperature
  • T cry is the start temperature of the exothermic peak due to crystallization.
  • the characteristic temperature of the glass is defined by the viscosity, and T g , M g and T s are said to be temperatures at which the viscosity corresponds to 10 13.3 poise, 10 11.0 poise and 10 7.65 poise, respectively.
  • Tcry is the temperature at which the glass starts to crystallize. Crystallization, for inhibiting the softening fluidity of the glass, as much as possible, it is preferable that the T cry to the high temperature side than T s.
  • the produced low melting point glass was subjected to thermal strain removal in a temperature range of T g to M g and processed into a 4 ⁇ 4 ⁇ 20 mm prism. Using this, the thermal expansion coefficient of 30 to 250 ° C., transition temperature TG and deformation temperature AT were measured with a thermal expansion meter. The heating rate was 5 ° C./min. Further, as a standard sample, a cylindrical quartz glass of ⁇ 5 ⁇ 20 mm was used.
  • FIG. 9 shows a thermal expansion curve of a typical low melting point glass. In FIG. 9, the amount of elongation of quartz glass as a standard sample is subtracted. The thermal expansion coefficient was calculated from the gradient of the amount of elongation in the temperature range of 30 to 250.degree.
  • T G is a temperature at which elongation starts significantly
  • a T is a temperature at which deformation occurs due to load.
  • T G was measured slightly higher than T g of the above DTA.
  • a T was between M g and T s of the above DTA.
  • the softness and fluidity of the produced low melting point glass is obtained by compacting the glass powder crushed by the jet mill with a hand press (1 ton / cm 2 ) with a hand press (1 ton / cm 2 ) and irradiating the glass compact with a variety of lasers over the transparent substrate. Evaluated by. The outline of the laser irradiation experiment to the glass compacting body is shown in FIG. The size of the glass green compact 8 was ⁇ 10 ⁇ 2 mm. The glass compacting body 8 was placed on the transparent substrate 1, and the laser 7 was irradiated toward the central portion of the glass compacting body 8 from the back side. A slide glass was used for the transparent substrate 1.
  • a semiconductor laser with a wavelength of 405 nm, a double wave of a YAG laser with a wavelength of 532 nm, a semiconductor laser with a wavelength of 630 nm, a semiconductor laser with a wavelength of 805 nm, and a YAG laser with a wavelength of 1064 nm are used.
  • the evaluation of the softness and fluidity was “o” when the laser-irradiated part of the glass green compact 8 flowed, but it flowed, “ ⁇ ” when cracks frequently occurred, and “ ⁇ ” when softened. Although it softened, when the crack occurred frequently, it was set as "x” when neither flow nor softening was possible.
  • production state of a crack were determined by observing with the optical microscope through the transparent substrate 1.
  • the low melting point glasses of Examples G1 to G 64 are Comparative Examples G67, 69, 73 to 76 and 78.
  • the softening point T s is lower than the low melting point glass of ⁇ 80, and the thermal expansion coefficient is smaller than that of the low melting point glasses of Comparative Examples G68, 70 to 73, 77 and 78.
  • Comparative Examples G65 to 68, 70 to 74, 76, Moisture resistance was better than the low melting point glasses of 78 and 80.
  • the low melting point glass of Example G1 to 64 has better softening flowability by laser irradiation than the low melting point glass of Comparative Examples G67, 69, 73 to 76, and 78 to 80, and Comparative Examples 68, 70 to 72. Even when the softening and fluidity was good as in the low melting point glass of No. 77 and No. 77, cracks did not occur frequently.
  • the low melting glass of Example G1 to V64 contains vanadium oxide, tellurium oxide, phosphorus oxide and iron oxide, and the total of V 2 O 5 , TeO 2 , P 2 O 5 and Fe 2 O 3 in terms of the following oxides.
  • the glass component contains at least one of tungsten oxide, molybdenum oxide, niobium oxide, tantalum oxide, manganese oxide, antimony oxide, bismuth oxide, zinc oxide, barium oxide, strontium oxide, silver oxide and potassium oxide.
  • a particularly effective composition range is that 35 to 55% by mass of V 2 O 5, 19 to 30% by mass of TeO 2 and P 2 O 5 in terms of the following oxides are satisfied while satisfying the above conditions.
  • the low melting glass of Example G1 to 64 efficiently absorbs a laser having a wavelength in the range of 400 to 1100 nm and is heated, and further, since the softening point T s is as low as 380 ° C. or less Indicated. Furthermore, the transition point T g is 320 ° C. or less and low thermal expansion coefficient is relatively small as 100 ⁇ 10 -7 / °C less, cracks in the heat shock by laser irradiation was small.
  • a laser sealing experiment was performed using the low melting glass of Example G19 shown in Table 2 and a slide glass as a transparent substrate.
  • a sealing material paste was produced using a G19 low melting point glass powder ground to an average particle size of 3 ⁇ m or less by a jet mill, a resin binder, and a solvent.
  • the resin binder was nitrocellulose
  • the solvent was butyl carbitol acetate.
  • the sealing material paste was applied to the outer peripheral portion of the transparent substrate by screen printing as shown in FIG. 11, and after drying, the sealing material paste was fired at 380 ° C. for 30 minutes in the air. .
  • the line width of the sealing material 5 formed on the transparent substrate 1 was 1.5 mm, and the thickness of the fired film was adjusted to about 5, 10, 20, and 30 ⁇ m by changing the application amount.
  • the transparent substrate 2 is installed opposite to each other, and the laser 7 is irradiated while moving at a speed of 8 mm / sec from the direction of the transparent substrate 1 to the sealing material 5.
  • the parts were joined.
  • the laser 7 used was the four types of lasers used in Example 1. All samples were able to be joined and the airtightness (gas barrier property) and adhesiveness were evaluated. The evaluation results are shown in Table 6.
  • the gas tightness was evaluated by carrying out a helium leak test, “o” when not leaking, and “x” when leaked. Also, the adhesiveness was evaluated as a peeling test, and when the transparent substrate and the sealing material were broken, it was evaluated as “ ⁇ ”, and when it was easily peeled from the interface between the transparent substrate and the sealing material, it was evaluated as “ ⁇ ”. .
  • the fired film thickness 20 ⁇ m or less, the airtightness and adhesiveness were good regardless of which laser was used. However, with the fired film thickness of 30 ⁇ m, depending on the laser used, there were cases where good air tightness and adhesiveness could not be obtained.
  • the wavelengths of 532 nm and 1064 nm use YAG lasers, and YAG lasers are considered to have obtained good airtightness and adhesiveness because they have higher power than other semiconductor lasers. Since the semiconductor laser is very inexpensive compared to the YAG laser, it is better than the semiconductor laser can be used for laser sealing, and the thickness of the bonding layer is preferably 20 ⁇ m or less.
  • the transmittance curve of the coating film which baked the low melting glass of Example G19 in FIG. 13 is shown.
  • Example G43 shown in Table 3 was used for the low melting glass contained in the sealing material. Further, as a filler, zirconium phosphate tungstate (Zr 2 (WO 4 ) (PO 4 ) 2 ), niobium oxide (Nb 2 O 5 ) and silicon (Si) were used as a filler. And the same laser sealing experiment as Example 2 was implemented.
  • a low melting point glass powder of G43 ground to an average particle size of 3 ⁇ m or less by a jet mill, and a filler of Zr 2 (WO 4 ) (PO 4 ) 2 , Nb 2 O 5 or Si having an average particle size of about 5 ⁇ m.
  • the sealing material paste was produced using particles, a resin binder, and a solvent.
  • the content of the filler particles was 15, 25, 35, and 45 parts by volume with respect to 100 parts by volume of the G43 low melting glass, respectively.
  • the density of the low-melting glass G43 used was 3.53g / cm 3, Zr 2 ( WO 4) (PO 4) 2 of the density 3.80g / cm 3, Nb 2 density of O 5 is 4.57 g / cm 3
  • the density of Si was 2.33 g / cm 3 .
  • ethyl cellulose was used as a resin binder, and butyl carbitol acetate was used as a solvent.
  • the sealing material paste was applied to the outer peripheral portion of the transparent substrate by screen printing as shown in FIG. 11, dried, and fired at 400 ° C. for 30 minutes in the air.
  • the sealing material 5 formed on the transparent substrate 1 had a line width of 1.5 mm and a film thickness of about 10 ⁇ m.
  • the transparent substrate 2 is installed opposite to each other, and the semiconductor laser 7 having a wavelength of 805 nm is moved from the direction of the transparent substrate 1 to the sealing material 5 while moving at a speed of 8 mm / sec.
  • the outer peripheral parts of 1 and 2 were joined.
  • the air tightness (gas barrier property) and adhesion were evaluated in the same manner as in Example 2. The evaluation results are shown in Table 7.
  • the filler is contained in the sealing material 5 so that the thermal expansion coefficient of the sealing material 5 is obtained.
  • a filler of Zr 2 (WO 4 ) (PO 4 ) 2 , Nb 2 O 5 or Si is contained. The inclusion of the filler resulted in good air tightness and adhesion.
  • the content of the filler is 45 parts by volume, the content of the low melting point glass G43 for bonding the transparent substrates 1 and 2 is decreased, and although the adhesion is inferior as compared with the other examples, it is good. Airtightness was maintained.
  • filler particle contained in the sealing material 5 35 volume parts or less are preferable with respect to 100 volume parts of low melting glass. It is conceivable that.
  • Zr 2 (WO 4 ) (PO 4 ) 2 , Nb 2 O 5 and Si having good wettability with the present low melting point glass as filler particles were selected and examined.
  • the filler particles are not limited to these, and ⁇ -eucryptite having a small thermal expansion coefficient, cordierite, zirconium phosphate, zirconium silicate and the like can also be used.
  • the transparent substrates 1 and 2 are bonded via the spacer 6.
  • the transparent substrates 1 and 2 were joined to the transparent substrates 1 and 2 and the spacer 6 by the manufacturing method shown to FIG. 6 and FIG. 7 using the white plate glass with high transmittance
  • sealing material paste 100 parts by volume of the low melting point glass powder of G43 and 10 parts by volume of Zr 2 (WO 4 ) (PO 4 ) 2 filler particles shown in Table 3 as in Example 3 for the sealing materials 5 and 5A, and ethylcellulose and butylcarbi
  • the sealing material paste was applied to the spacer 6 as shown in FIG. 6 using a sealing material paste consisting of tol acetate, and after drying, the sealing material paste was fired at 400 ° C. in the air for 20 minutes.
  • the fired film thickness was 15 ⁇ m each.
  • the width of the spacer 6 was fixed at 3 mm, and the thickness was 70, 320, 500, and 1000 ⁇ m, respectively.
  • the thicknesses of the sealing materials 5 and 5A are respectively 100, 350, 530, and 1030 ⁇ m. As shown in FIG. 7, they were placed on the outer circumferences of the four sides, and both sides of the transparent substrates 1 and 2 were irradiated with semiconductor lasers 7 and 7A having a wavelength of 630 nm for bonding. The feed rate of the laser was 8 mm / sec. The adhesion was evaluated in the same manner as in Example 2. It was found that good adhesion was obtained regardless of the thickness of the spacer 6, and it was effective to use the spacer 6 when the distance between the transparent substrates 1 and 2 was large.
  • OLEDs organic light emitting diodes
  • This OLED display has the structure shown in FIGS. 1A and 1B. Since the OLED which is the built-in organic element 3 is easily deteriorated by moisture and oxygen, it is very difficult to airtightly and firmly bond the outer peripheral portions of the transparent substrates 1 and 2 with the sealing material 5 containing the low melting point glass. It is valid.
  • non-alkali glass used for a liquid crystal display was used for the transparent substrates 1 and 2.
  • the sealing material paste is applied to the outer peripheral portion of the transparent substrate 1 as shown in FIGS. 3A and 3B using a sealing material paste made of butyl carbitol acetate, and after drying, the sealing material for 30 minutes at 400 ° C. in the air.
  • the paste was fired to form a sealing material 5.
  • the formed sealing material had a width of 2.5 mm and a fired film thickness of 10 ⁇ m.
  • a large number of OLEDs corresponding to the number of pixels were formed on the transparent substrate 2 as shown in FIGS. 4A and 4B.
  • the transparent substrate 2 and the transparent substrate 1 were made to face each other as shown in FIG. 5, and the laser 7 was irradiated toward the sealing material 5 from the direction of the transparent substrate 1.
  • the laser 7 used the semiconductor laser with a wavelength of 805 nm, moved the outer peripheral portion at a speed of 8 mm / sec, and bonded the outer peripheral portions of the transparent substrates 1 and 2.
  • the display was subjected to a high temperature and high humidity test under the conditions of 85 ° C. and 85% Rh for 10 days, 25 days and 50 days, and a lighting test was performed.
  • a resin bonded OLED display was also included as a comparison.
  • the resin bonding layer had a width of 3 mm and a thickness of 10 ⁇ m. In the 10-day high-temperature and high-humidity test, although both OLED displays turned on without any problem, the display joined with the resin was greatly deteriorated by lighting after 25 days.
  • the present invention can be effectively applied to an OLED display. Further, it goes without saying that the invention can also be applied to electronic parts such as lighting fixtures on which the OLED is mounted.
  • a dye-sensitized solar cell incorporating an organic dye was produced and evaluated.
  • organic dye molecules are formed on the surface of a large number of titania (TiO 2 ) nanoparticles, and when the dye is irradiated with light, excited electrons are injected into TiO 2 to form nano-sized particles. It reaches the electrode while diffusing in the particle.
  • the counter electrode electrons are injected into the electrolyte to reduce iodine (I). Power can be generated by this.
  • Dye-sensitized solar cells are effective for cost reduction because they do not use non-vacuum, low-temperature processes and silicon, but there are major problems in reliability.
  • Sealing technology is the key to improving its reliability. Since an organic dye or an electrolyte having low heat resistance is used, sealing needs to be performed at a low temperature equal to or lower than the heat resistance temperature, and resin sealing is generally used. However, resin sealing has a big problem that long-term reliability can not be secured.
  • the present invention was applied to sealing of a dye-sensitized solar cell in the same manner as in Example 5.
  • white sheet glass with high transmittance was used for the transparent substrates 1 and 2.
  • the formation of the sealing material 5 on the transparent substrate 1 was performed using the same sealing material paste and the same baking conditions as in Example 4.
  • a cell containing a large number of organic dyes and the like was formed or placed in the transparent substrate 2 side, and the peripheral portions of the transparent substrates 1 and 2 were joined by laser irradiation in the same manner as in Example 5.
  • the transparent substrates 1 and 2 were able to be joined firmly by the sealing material 5, and adhesiveness was favorable. Moreover, there was no problem even in the same high temperature and high humidity test as in Example 5, and good airtightness was maintained.
  • the low melting glass according to the present invention can be expanded to the coating of an electrode.
  • the present invention can be effectively applied to dye-sensitized solar cells. Further, it goes without saying that the invention can be applied not only to dye-sensitized solar cells but also to electronic components such as organic solar cells.
  • a large number of photoelectric conversion elements were incorporated, and a solar cell bonded with a resin was manufactured and evaluated.
  • a photoelectric conversion element a double-sided light receiving cell using a single crystal silicon substrate was used. Also, these cells are connected in series by tab lines.
  • an EVA sheet is pasted between two transparent substrates, and the end is fixed by an aluminum frame and a resin sealing material. In general, white sheet glass with high transmittance is applied to the transparent substrate. Most of the solar cell's subsequent accidents are caused by the water that penetrates inside.
  • EVA sheets do not have high gas barrier properties (airtightness), and moisture permeates over many years gradually, and the tab wires connecting between cells with the moisture and the connections, and the cells The formed electrode may be corroded and broken. For this reason, it is very important to ensure that the water does not penetrate, in order to ensure the long-term reliability of the solar cell.
  • the white sheet glass was used for the transparent substrate, and an EVA sheet was used for the resin to be bonded. Since the thickness of the double-sided light receiving cell used was about 250 ⁇ m including the electrode part on both sides and the bonding layer made of EVA sheet was about 250 ⁇ m on both sides of the cell, it was decided to join through the spacer as shown in FIGS. . Since the distance between the transparent substrates 1 and 2 is about 500 ⁇ m, a white sheet glass having a width of 3.5 mm and a thickness of 470 ⁇ m was used as the spacer 6.
  • the sealing material paste was prepared using the low melting point glass powder of G55 shown in Table 4, Si filler particles, ethyl cellulose and butyl carbitol acetate.
  • the content of the Si filler particles was 15 parts by volume with respect to 100 parts by volume of the low melting point glass of G55.
  • a sealing material paste was applied to the outer peripheral portion of the transparent substrate 1 and one side of the spacer 6 with a width of 3 mm by screen printing, and dried. After drying, the sealing material paste was fired at 400 ° C. in the atmosphere for 30 minutes to form the sealing material 5 on the transparent substrate 1 and the sealing material 5A on the spacer. The fired film thickness at that time was 15 ⁇ m respectively.
  • the spacer 6 on which the sealing material 5A was formed was placed on the transparent substrate 2 and was weighted and heated at 400 ° C. in the atmosphere for 30 minutes to bond the spacer 6 and the transparent substrate 2 with the sealing material 5A.
  • the low melting point glass paste of G55 was applied to the joint of the spacers 6 and simultaneously fired.
  • the transparent substrates 1 and 2 produced as described above several double-sided light receiving cells connected by tab wires were set so that the sealing material 5 and the spacer 6 face each other, and they were bonded by an EVA sheet.
  • the semiconductor laser with a wavelength of 805 nm was moved from the transparent substrate 1 side at a speed of 8 mm / sec, and the transparent substrates 1 and 2 were bonded with the sealing material 5 and 5A via the spacer 6.
  • the airtightness and adhesion of the sealing materials 5 and 5A were both good. It goes without saying that long-term reliability can be ensured as compared with a resin sealing material.
  • the present invention can be applied to general solar cells in which a cell and a transparent substrate are adhered and fixed using a resin.
  • it can be applied to thin film solar cells.
  • the OLED display, the dye-sensitized solar cell, and the Si solar cell to which the present invention is applied have been described above.
  • the present invention is not limited to the above, and can be applied to low heat resistant organic elements and electronic components in general containing an organic material, and the reliability of the electronic components can be remarkably improved.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Life Sciences & Earth Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • General Chemical & Material Sciences (AREA)
  • Geochemistry & Mineralogy (AREA)
  • Materials Engineering (AREA)
  • Organic Chemistry (AREA)
  • Manufacturing & Machinery (AREA)
  • Glass Compositions (AREA)
  • Electroluminescent Light Sources (AREA)
  • Hybrid Cells (AREA)
PCT/JP2013/051625 2012-01-30 2013-01-25 電子部品及びその製法、並びにそれに用いる封止材料ペースト Ceased WO2013115101A1 (ja)

Priority Applications (1)

Application Number Priority Date Filing Date Title
CN201380005016.5A CN104081877A (zh) 2012-01-30 2013-01-25 电子零件及其制法、以及用于其的密封材料糊剂

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2012-016047 2012-01-30
JP2012016047A JP2013157161A (ja) 2012-01-30 2012-01-30 電子部品及びその製法、並びにそれに用いる封止材料ペースト

Publications (1)

Publication Number Publication Date
WO2013115101A1 true WO2013115101A1 (ja) 2013-08-08

Family

ID=48905141

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2013/051625 Ceased WO2013115101A1 (ja) 2012-01-30 2013-01-25 電子部品及びその製法、並びにそれに用いる封止材料ペースト

Country Status (4)

Country Link
JP (1) JP2013157161A (enExample)
CN (1) CN104081877A (enExample)
TW (1) TWI501934B (enExample)
WO (1) WO2013115101A1 (enExample)

Cited By (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP5882507B1 (ja) * 2015-01-19 2016-03-09 株式会社フジクラ 光電変換素子
CN105492403A (zh) * 2013-08-29 2016-04-13 中央硝子株式会社 无铅玻璃和密封材料
WO2016123273A1 (en) * 2015-01-28 2016-08-04 Corning Incorporated A glass frit and a glass assembly sealed with the glass frit
WO2021074560A1 (en) * 2019-10-17 2021-04-22 Johnson Matthey Public Limited Company Composition, paste and methods
CN116553829A (zh) * 2017-11-28 2023-08-08 日立化成株式会社 密封材料和使用其的多层玻璃面板

Families Citing this family (10)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US9573840B2 (en) * 2013-08-27 2017-02-21 Corning Incorporated Antimony-free glass, antimony-free frit and a glass package that is hermetically sealed with the frit
JP6256480B2 (ja) * 2013-12-11 2018-01-10 日立化成株式会社 断熱部材及び低融点ガラス組成物、並びに封止材料ペースト
CN104150778B (zh) * 2014-08-11 2016-07-06 海南中航特玻材料有限公司 一种无铅低熔点封接玻璃
DE102014014322B4 (de) * 2014-10-01 2017-11-23 Ferro Gmbh Tellurat-Fügeglas mit Verarbeitungstemperaturen ≦ 400 °C
DE102017216422B3 (de) * 2017-09-15 2019-01-03 Schott Ag Hochdehnendes Fügeglas mit verbesserter Wasserbeständigkeit und seine Anwendungen
JP2019123637A (ja) * 2018-01-16 2019-07-25 日立化成株式会社 接合材
CN108298822B (zh) * 2018-04-08 2020-08-04 武汉理工大学 一种真空玻璃封接用低熔点玻璃粉及其阳极键合增强封装方法
JP6927154B2 (ja) * 2018-05-30 2021-08-25 昭和電工マテリアルズ株式会社 無鉛ガラス組成物ならびにそれを含むガラス複合材料、ガラスペーストおよび封止構造体
JP2021048247A (ja) * 2019-09-18 2021-03-25 日本電気硝子株式会社 パッケージ基材、パッケージ、及びパッケージ基材の製造方法
CN115305035B (zh) * 2021-05-08 2024-08-20 深圳市首骋新材料科技有限公司 用于oled密封的玻璃胶、oled元件的封装方法、oled器件

Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2005251629A (ja) * 2004-03-05 2005-09-15 Tohoku Pioneer Corp 有機elパネル及びその製造方法
JP2008171811A (ja) * 2007-01-05 2008-07-24 Samsung Sdi Co Ltd ガラスフリット、シーリング材形成用の組成物及び発光装置
JP2010052990A (ja) * 2008-08-28 2010-03-11 Yamato Denshi Kk 封着用無鉛ガラス材とこれを用いた有機elディスプレイパネル
WO2010067848A1 (ja) * 2008-12-12 2010-06-17 旭硝子株式会社 封着ガラス、封着材料層付きガラス部材、および電子デバイスとその製造方法
JP2012014971A (ja) * 2010-07-01 2012-01-19 Asahi Glass Co Ltd 電子デバイス及びその製造方法
WO2012011268A1 (ja) * 2010-07-23 2012-01-26 パナソニック株式会社 表示パネル及びその製造方法

Family Cites Families (7)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US5066621A (en) * 1990-06-21 1991-11-19 Johnson Matthey Inc. Sealing glass composition and electrically conductive formulation containing same
KR100732816B1 (ko) * 2006-01-24 2007-06-27 삼성에스디아이 주식회사 유기전계발광 표시장치 및 그 제조방법
JP2008249839A (ja) * 2007-03-29 2008-10-16 Fujifilm Corp 有機elパネルおよびその製造方法
CN101265024A (zh) * 2008-04-08 2008-09-17 中国计量学院 一种低熔点无铅硼磷酸盐封接玻璃粉及其制备方法
CN101633560B (zh) * 2008-07-23 2011-07-27 中国科学院过程工程研究所 一种无铅低熔玻璃及其制备方法
JP5414409B2 (ja) * 2009-01-16 2014-02-12 日立粉末冶金株式会社 低融点ガラス組成物、それを用いた低温封着材料及び電子部品
CN101857371A (zh) * 2010-05-25 2010-10-13 中国科学院过程工程研究所 一种无铅低熔电子显示器封接玻璃及其制备方法

Patent Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2005251629A (ja) * 2004-03-05 2005-09-15 Tohoku Pioneer Corp 有機elパネル及びその製造方法
JP2008171811A (ja) * 2007-01-05 2008-07-24 Samsung Sdi Co Ltd ガラスフリット、シーリング材形成用の組成物及び発光装置
JP2010052990A (ja) * 2008-08-28 2010-03-11 Yamato Denshi Kk 封着用無鉛ガラス材とこれを用いた有機elディスプレイパネル
WO2010067848A1 (ja) * 2008-12-12 2010-06-17 旭硝子株式会社 封着ガラス、封着材料層付きガラス部材、および電子デバイスとその製造方法
JP2012014971A (ja) * 2010-07-01 2012-01-19 Asahi Glass Co Ltd 電子デバイス及びその製造方法
WO2012011268A1 (ja) * 2010-07-23 2012-01-26 パナソニック株式会社 表示パネル及びその製造方法

Cited By (15)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN105492403A (zh) * 2013-08-29 2016-04-13 中央硝子株式会社 无铅玻璃和密封材料
CN105492403B (zh) * 2013-08-29 2019-01-22 中央硝子株式会社 无铅玻璃和密封材料
WO2016117546A1 (ja) * 2015-01-19 2016-07-28 株式会社フジクラ 光電変換素子
JP5882507B1 (ja) * 2015-01-19 2016-03-09 株式会社フジクラ 光電変換素子
WO2016123273A1 (en) * 2015-01-28 2016-08-04 Corning Incorporated A glass frit and a glass assembly sealed with the glass frit
CN107406305A (zh) * 2015-01-28 2017-11-28 康宁股份有限公司 玻璃料以及用该玻璃料进行密封的玻璃组件
CN116553829A (zh) * 2017-11-28 2023-08-08 日立化成株式会社 密封材料和使用其的多层玻璃面板
CN116553829B (zh) * 2017-11-28 2026-04-10 株式会社力森诺科 密封材料和使用其的多层玻璃面板
WO2021074560A1 (en) * 2019-10-17 2021-04-22 Johnson Matthey Public Limited Company Composition, paste and methods
CN114585593A (zh) * 2019-10-17 2022-06-03 芬齐Agt荷兰有限责任公司 组合物、糊剂和方法
KR20220161251A (ko) * 2019-10-17 2022-12-06 펜지 에이지티 네덜란드 비.브이. 조성물, 페이스트 및 방법
GB2589703B (en) * 2019-10-17 2022-01-12 Johnson Matthey Advanced Glass Tech B V Composition for sealing inorganic substrates
KR102801868B1 (ko) 2019-10-17 2025-05-02 펜지 에이지티 네덜란드 비.브이. 조성물, 페이스트 및 방법
US12497325B2 (en) 2019-10-17 2025-12-16 Fenzi Agt Netherlands B.V. Composition, paste and methods
GB2589703A (en) * 2019-10-17 2021-06-09 Johnson Matthey Plc Composition, paste and methods

Also Published As

Publication number Publication date
CN104081877A (zh) 2014-10-01
TWI501934B (zh) 2015-10-01
JP2013157161A (ja) 2013-08-15
TW201343592A (zh) 2013-11-01

Similar Documents

Publication Publication Date Title
JP5733279B2 (ja) 電子部品及びその製法、並びにそれに用いる封止材料ペースト
TWI501934B (zh) Electronic parts and their manufacturing methods, as well as the use of its sealing material paste
US9614178B2 (en) Electronic component, process for producing same, sealing material paste, and filler particles
CN102245525B (zh) 密封玻璃、带密封材料层的玻璃构件以及电子器件及其制造方法
CN103328402B (zh) 带封接材料层的玻璃构件和使用其的电子装置及其制造方法
TWI497466B (zh) Electronic device and manufacturing method thereof
JP2011126722A (ja) レーザ封着用封着材料、封着材料層付きガラス部材、およびそれを用いた太陽電池とその製造方法
JP2012113968A (ja) 電気素子パッケージ
WO2020050031A1 (ja) 気密パッケージ
JPWO2012090695A1 (ja) 電子デバイスとその製造方法
JP2012014971A (ja) 電子デバイス及びその製造方法
JP6090703B2 (ja) 複合封着材料
JP6079011B2 (ja) 封着材料層付きガラス基板の製造方法
JP5935120B2 (ja) 密封容器、電子装置及び太陽電池モジュール
US20140342136A1 (en) Member with sealing material layer, electronic device, and method of manufacturing electronic device
CN116253515A (zh) 玻璃浆料
TW201222847A (en) Electronic device and method of manufacturing thereof
JP6156675B2 (ja) ガラスパッケージの製造方法

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 13744107

Country of ref document: EP

Kind code of ref document: A1

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 13744107

Country of ref document: EP

Kind code of ref document: A1