WO1999048808A1 - VERFAHREN ZUR AUFARBEITUNG VON DÜNNSÄURE AUS DER TiO2-HERSTELLUNG - Google Patents

VERFAHREN ZUR AUFARBEITUNG VON DÜNNSÄURE AUS DER TiO2-HERSTELLUNG Download PDF

Info

Publication number
WO1999048808A1
WO1999048808A1 PCT/EP1999/001735 EP9901735W WO9948808A1 WO 1999048808 A1 WO1999048808 A1 WO 1999048808A1 EP 9901735 W EP9901735 W EP 9901735W WO 9948808 A1 WO9948808 A1 WO 9948808A1
Authority
WO
WIPO (PCT)
Prior art keywords
stage
gypsum
iron
calcium
sulfate
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/EP1999/001735
Other languages
German (de)
English (en)
French (fr)
Inventor
Gerhard Auer
Günter Lailach
Ulrich Meisen
Werner Schuy
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Bayer AG
Original Assignee
Bayer AG
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Bayer AG filed Critical Bayer AG
Priority to US09/646,340 priority Critical patent/US6440377B1/en
Priority to DE59901851T priority patent/DE59901851D1/de
Priority to AU29335/99A priority patent/AU2933599A/en
Priority to BR9908920-3A priority patent/BR9908920A/pt
Priority to JP2000537798A priority patent/JP2002507632A/ja
Priority to EP99910350A priority patent/EP1064223B1/de
Priority to CA002324308A priority patent/CA2324308A1/en
Publication of WO1999048808A1 publication Critical patent/WO1999048808A1/de
Priority to NO20004682A priority patent/NO323628B1/no
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01G—COMPOUNDS CONTAINING METALS NOT COVERED BY SUBCLASSES C01D OR C01F
    • C01G49/00—Compounds of iron
    • C01G49/02—Oxides; Hydroxides
    • C01G49/06—Ferric oxide [Fe2O3]
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01F—COMPOUNDS OF THE METALS BERYLLIUM, MAGNESIUM, ALUMINIUM, CALCIUM, STRONTIUM, BARIUM, RADIUM, THORIUM, OR OF THE RARE-EARTH METALS
    • C01F11/00—Compounds of calcium, strontium, or barium
    • C01F11/46—Sulfates
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2006/00—Physical properties of inorganic compounds
    • C01P2006/12—Surface area
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2006/00—Physical properties of inorganic compounds
    • C01P2006/42—Magnetic properties
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2006/00—Physical properties of inorganic compounds
    • C01P2006/60—Optical properties, e.g. expressed in CIELAB-values
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2006/00—Physical properties of inorganic compounds
    • C01P2006/60—Optical properties, e.g. expressed in CIELAB-values
    • C01P2006/62—L* (lightness axis)
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2006/00—Physical properties of inorganic compounds
    • C01P2006/60—Optical properties, e.g. expressed in CIELAB-values
    • C01P2006/63—Optical properties, e.g. expressed in CIELAB-values a* (red-green axis)
    • C—CHEMISTRY; METALLURGY
    • C01—INORGANIC CHEMISTRY
    • C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
    • C01P2006/00—Physical properties of inorganic compounds
    • C01P2006/60—Optical properties, e.g. expressed in CIELAB-values
    • C01P2006/64—Optical properties, e.g. expressed in CIELAB-values b* (yellow-blue axis)

Definitions

  • the invention relates to a process for the production of high-quality gypsum and iron oxide pigments from thin acid, which is obtained in the production of titanium dioxide by the sulfate process.
  • EP-A 577 272 describes that a usable gypsum can be obtained from the thin acid by partial neutralization with calcium carbonate.
  • the metal sulfate solution remaining after the separation of this material which is also referred to as “white gypsum”
  • valuable raw materials are removed from recycling and, on the other hand, valuable landfill space is consumed on a large scale, since depending on the titanium raw material, 1 to 2.5 t of this waste is generated per ton of Ti0 2 pigment produced.
  • Solution can then be obtained by crystallization pure ammonium sulfate and used as a fertilizer. Although this increases the proportion of recycled material, the economics of the process are unsatisfactory due to the additional process steps and the lower quality of the magnetite obtained from the solution which contains a large amount of ammonium sulfate.
  • both a high-quality gypsum and high-quality iron oxide pigments can be produced from the thin acid obtained in the production of titanium dioxide by the sulfate process if, in a first step, the thin acid is converted to gypsum with a calcium compound and this, if necessary directly , is separated from the remaining solution.
  • the elements Al, Ti, Cr, V and Fe (III) are at least partially precipitated and separated from the solution thus obtained by increasing the pH.
  • an iron oxide pigment is formed from the remaining iron (II) sulfate-containing solution and then separated from the remaining solution.
  • the invention relates to a process for the production of gypsum and an iron oxide pigment from the thin acid obtained in the production of titanium dioxide by the sulfate process, characterized in that in a first stage a partial neutralization of the thin acid with a calcium compound
  • Precipitation and, if appropriate, direct separation of gypsum takes place, then the remaining solution is further neutralized in a second stage, with precipitation of a Ti, Al, Cr, V and possibly Fe (III) -containing precipitate and that obtained after separating off the solid Iron sulfate-containing solution is converted in a third stage with the addition of alkaline compounds and by adding an oxidizing agent to an iron oxide pigment.
  • the gypsum obtained in the first stage can either be separated off directly after the precipitation, as a result of which a particularly high quality is obtained; however, the gypsum can also be separated off together with the Ti, Al, Cr, V and optionally Fe (III) -containing solid precipitated in the second stage, which simplifies the process.
  • the direct removal of the gypsum obtained in the first stage is preferred.
  • the partial neutralization of the free sulfuric acid in the first stage is preferably carried out by adding calcium carbonate, calcium hydrogen carbonate.
  • Calcium oxide or calcium hydroxide or other alkaline substances which contain one or more of the compounds listed, for example dolomite.
  • the partial neutralization of the free sulfuric acid in the first stage can also be carried out by a combination of the individual substances listed above.
  • Calcium carbonate, calcium oxide or calcium hydroxide is preferably used as the calcium source.
  • Finely ground lime (calcium carbonate) is particularly preferably used, since the C0 2 formed here can also be utilized.
  • iron oxide pigment by neutralizing some of the free sulfuric acid with substances containing metallic iron or iron (II), for example with scrap iron, mill scale, swarf or cast iron shavings.
  • the free sulfuric acid can then be neutralized further with calcium carbonate.
  • Dilution in a ratio of 1: 1 parts by weight of thin acid to parts by weight of water. It is advantageous to mix the Ca compound used for neutralization with part of the dilution water and to neutralize the thin acid with this suspension.
  • the partial neutralization of the thin acid in the first stage by adding the calcium compound is preferably carried out up to a pH of 1.0 to 3.0.
  • the whiteness of the gypsum can be impaired by co-precipitation of colored impurities, for example Fe (III) or other subgroup compounds. It is particularly preferred to neutralize up to a pH of 1.4 to 2.0, since the gypsum precipitated in this way has particularly little colored impurities and contains particularly little Ti0 2 , so that it also meets the requirements for special applications, for example for gypsum screed.
  • the pure calcium sulfate thus obtained is separated from the liquid phase and preferably washed to remove colored solution components.
  • a corresponding barium compound can be selected for the partial neutralization of the free sulfuric acid in the first stage instead of the calcium compound if barium sulfate is desired as the product.
  • the solution is then neutralized further in the second stage, preferably up to a pH of 3.0 to 5.0, particularly preferably up to a pH of 3.5 to 4.8.
  • disruptive titanium compounds and in some cases Al, Cr, V and Fe (III) compounds are precipitated.
  • the precipitate thus obtained is separated from the liquid phase and can either be deposited or used as a raw material for the extraction of Ti, Al, Cr or V.
  • any Fe (III) present is preferably reduced to Fe (II) by adding a reducing agent, in particular metallic iron.
  • a reducing agent in particular metallic iron.
  • Iron is particularly suitable for industrial materials such as swarf, cast iron shavings, stamped sheet metal waste or mill scale. These substances are available inexpensively in large quantities. This reduces the amount of precipitate to be disposed of or reused in the second precipitation stage and the yield of high-quality iron oxide pigment in the subsequent one
  • This Fe (III) reduction can take place either before the gypsum precipitation in the first stage or afterwards, ie immediately before the precipitation of the trivalent and tetravalent metal ions.
  • the reaction must be controlled so that as little Ti 3 * as possible is formed, which would only be incompletely precipitated in the second stage. If necessary, also by adding germs
  • Titanium oxide hydrate the precipitation of titanium can be improved in the second stage. - 6 -
  • either a compound which does not form poorly soluble sulfates can be used as the neutralizing agent, so that the accumulation of solid is minimized.
  • a compound as neutralizing agent which forms readily filterable, poorly soluble sulfates, and thus significantly improves the filterability of the entire solid obtained.
  • neutralizing agents one of which forms soluble sulfates, another forms poorly soluble sulfates, can be used to optimize this process step in a targeted manner.
  • neutralizing agents are compounds from the group of gaseous NH 3, NH 3 dissolved in water, oxides, hydroxides, carbonates and bicarbonates of the alkali or alkaline earth metals, and alkaline-reacting mixtures which contain at least one of the compounds listed.
  • alkaline ash for example from coal or waste incineration, as a neutralizing agent is particularly advantageous for economic reasons.
  • the simultaneous use of ammonia and alkaline ash or the simultaneous use of sodium hydroxide solution and ash as neutralizing agent is particularly preferred.
  • Ammonia or sodium hydroxide solution is preferably predominantly used, and only a small proportion of ash, in particular
  • an alkaline calcium compound for example CaO, can also be used, but as a rule the use of the ash is economically more attractive.
  • Iron sulfate-containing solution is preferred for the precipitation of the iron oxide pigment to a concentration of 150 to 250 g, particularly preferably to 180 to 190 g
  • FeS0 4 set per liter. If necessary, this concentration can - 7 -
  • the adjusted iron sulfate-containing solution is converted in a known manner to an iron oxide pigment, preferably a magnetite pigment, by adding alkaline compounds and adding an oxidizing agent, preferably by blowing in oxygen or oxygen-containing gases (Ullmann's Encyclopedia of Industrial Chemistry , 5th ed., Vol. A
  • the alkaline compounds used are preferably those which do not form poorly soluble sulfates, such as NH 3 , NaOH, KOH, Na 2 CO 3 , K 2 CO 3 , MgO, MgCO 3 or Mg (OH) 2 .
  • an amount of an alkaline reacting precipitant is preferably added to the solution containing iron sulfate such that the ratio of iron (II) ions to precipitant is 0.4 to 0.65, in particular 0.5 to 0.58 equivalents. If, for example, NaOH is used as the precipitant, between 40 and 65 mol FeSO 4 can be used per 100 mol NaOH. When using K 2 CO 3 as
  • Precipitants are used on 100 mol K 2 CO 3 between 80 and 130 mol FeSO 4 .
  • the calculated amount of the alkaline component is preferably added to the solution containing iron sulfate at a temperature between 60 and 95 ° C., in particular between 75 and 95 ° C. It is also possible to present the alkaline component.
  • Oxygen or an oxygen-containing gas mixture is preferred, in particular
  • the pigment suspensions are worked up by the known steps of filtration, drying and grinding. By varying the manufacturing conditions appropriately, those skilled in the art will be able to process a wide range of iron oxide - 8th -
  • Pigments can be determined within certain limits by varying the annealing conditions.
  • the gypsum obtained according to the invention contains particularly little coloring impurities, such as those represented by compounds of the elements Fe, Cr, V.
  • the gypsum contains very little Ti compounds, which also makes it suitable for the production of high-quality gypsum screeds or for the production of anhydrite.
  • the iron oxide pigment obtained according to the invention is not contaminated by gypsum and has particularly good pigment-optical properties, since the iron sulfate-containing starting solution used for this contains, on the one hand, particularly little titanium salts and, on the other hand, does not show a very high concentration due to the gypsum precipitation in the first stage Neutral salts, for example Na 2 S0 4 , K 2 SO 4 or (NH_;) 2 S ⁇ 4 , has.
  • the iron oxide pigment produced according to the invention is low in heavy metal compounds, in particular Cr and V, due to the presence of the metal hydroxides in the second stage.
  • the process according to the invention makes it possible to process the thin acid obtained as waste with simple procedural operations and with comparative methods low energy consumption to process high-quality products in the form of pure gypsum, iron oxide with pigment properties and pure CO and to minimize waste.
  • the Falling quantity of 7 to 8 t of thin acid per t of TiO 2 reduced to only 0.2 to 0 J t of filter cake (from the second stage) per t of TiO 2 produced.
  • the iron oxide pigments obtained according to the invention can be used for coloring paints, lacquers, plastics, building materials, paper and other materials.
  • the magnetite obtained according to the invention can also be used as a magnetic pigment for toners.
  • the shade of the iron oxide pigment obtained is determined according to the following rules:
  • the pigment is dispersed in an air-drying lacquer system using a muller (plate-type paint grinder).
  • the paint system (paint) consists of the following
  • ALKYDAL F 48 (binder, Bayer AG, medium-oil, air-drying alkyd resin based on drying vegetable fatty acids in test gasoline / xylene mixture 38: 7 with a non-volatile content of approx. 55%, oil content / triglyceride in the non-volatile content approx. 48%, phthalic anhydride in the non-volatile content approx. 26%)
  • the components are mixed with a high-speed mixer to produce the finished paint.
  • a plate color rubbing machine (Muller) is used, as described in DIN EN ISO 8780-5 (April 1995).
  • An ® ENGELSMANN JEL 25/53 Muller with an effective plate diameter of 24 cm is used.
  • the speed of the lower plate is approx. 75 min -1 .
  • the force between the plates is set to approx. 0.5 kN.
  • 0.8 g of pigment and 2.00 g of lacquer are dispersed in one step at 100 revolutions with a load weight of 2.5 kg according to the process described in DIN EN ISO 8780-5 (April 1995) section 8.1.
  • the muller is opened and the paint is quickly collected on the lower plate outside the center. Then another 2.00 g of lacquer are added and the plates are folded. After two stages of 50 revolutions without load weight, the preparation is finished.
  • the pigmented lacquer is spread on a non-absorbent cardboard with a film puller (gap height at least 150 ⁇ m, at most 250 ⁇ m).
  • Cardboard (spread) is then dried for at least 12 h at room temperature. Before the color measurement, the spread is dried for one hour at approx. 65 ° C ( ⁇ 5 ° C) and cooled.
  • the pigment and the lightening agent are dispersed in an air-drying lacquer system using a muller (plate color grinder).
  • a muller plate color grinder
  • a commercially available ® Bayertitan R-KB-2 titanium dioxide pigment (Bayer AG) is used as the lightening agent. This pigment corresponds to type R 2 in ISO 591 - 1977.
  • the coating system
  • the components of the paint system are mixed with a high-speed stirrer to produce the finished paint.
  • the pigmented lacquer and the paint spread are prepared as described for the determination of the pureton (see above), weighing 0.1500 g pigment to be tested, 0J500 g Bayertitan R-KB-2 and 2.00 g lacquer .
  • 10 g of the gypsum sample are linearly compacted from 0 to 120 bar in a hydraulic press within 30 seconds and held at 120 bar for 6 seconds.
  • the colorimetric characterization of the powder compact is carried out analogously to the colorimetric characterization of paint spreads.
  • a spectrophotometer with an integrating sphere with the measuring geometry d / 8 is used without a gloss trap. This measurement geometry is in ISO
  • the colorimeter is calibrated against a white, ceramic working standard as described in ISO 7724 / 2-1984 (E) point 8.3.
  • the reflection data of the working standard against an ideal matt white body are stored in the color measuring device, so that after calibration with the white working standard, all color measurements are related to the ideal matt white body.
  • the black point calibration is carried out with a black hollow body from the color measuring device manufacturer.
  • the temperature of the colorimeter and the test object is approx. 25 ° C ⁇ 5 ° C.
  • the paint spread is placed on the color measuring device so that the measuring opening covers a middle point of the paint layer.
  • the spread must be complete and flat.
  • the measuring opening must be completely covered by the lacquer layer. The measurement is then carried out.
  • the CIE coordinates L *, a * and b * from 1976 are calculated from the measured reflection spectrum according to the calculation instructions in ASTM E 308 - 1985, point 7.
  • the weighting functions of the standard illuminant C and the 2 ° standard observer from 1931 in ASTM E 308 - 1985, Table 5.6 are used.
  • the wavelength range is between 400 nm and 700 nm.
  • the wavelength interval is 20 nm. No gloss is deducted from the calculation.
  • the reflectance values obtained are converted into the CIELAB color data system in accordance with DIN 5033, Part 3 (July 1992). - 13 -
  • the relative color strength is calculated in analogy to the relative scattering power according to DIN 53 165 (point 3.4) with Bayertitan R-KB-2 as a lightening agent and a suitable Bayferrox reference pigment (instead of the soot); the standard color value Y / 100 is used as p ⁇ .
  • Fe content of 2.95% is diluted with 50 kg of water and heated to 80 ° C.
  • a suspension consisting of 25.94 kg of ground calcium carbonate (53.9% CaO; 43.1% CO 2 ) and 50 kg of water is pumped into this solution with stirring within 1.5 hours.
  • the mixture is stirred for a further 2 h.
  • the pH of the reaction mixture is then 1.5.
  • the resulting C0 2 can be collected, cleaned and compressed if necessary.
  • Residual moisture 0.03% (24 h at 40 ° C):
  • a suspension consisting of 0.464 kg is added at 75 ° C. to 67.4 kg of the filtrate obtained in the first stage when the gypsum is separated off (35.3 kg of filtrate and 32.1 kg of washing filtrate; pH 1.78) CaO and 4, 176 kg of water pumped in over 2 h.
  • the pH of the reaction mixture is then 4.5.
  • the precipitate is filtered off through suction filters and washed with 1.5 kg of water. 56.3 kg of filtrate, 2.08 kg of washing filtrate and 3.66 kg of filter cake with a solids content of 48.3% (60 ° C. to constant weight) are obtained.
  • After drying the filter cake in a forced-air drying cabinet at 60 ° C, 1.788 kg of solid are obtained with the following properties:
  • Residual moisture 0.21% (24 h at 40 ° C):
  • the precipitated magnetite is filtered off through suction filters and washed with 5.0 kg of water. 50.35 kg of filtrate, 4.1 kg of washing filtrate and 1J6 kg of filter cake with a solids content of 67.4% (60 ° C. to constant weight) are obtained. After drying the filter cake in a convection oven at 60 ° C and
  • the relative color strength against Bayferrox 330 is 131%.
  • the magnetite obtained is also suitable as a magnetic pigment for toners:
  • Fe content of 2.95%) are diluted with 50 kg water and heated to 80 ° C.
  • a suspension consisting of 25.94 kg of ground calcium carbonate (53.9% CaO; 43.1% CO 2 ) and 50 kg of water is pumped into this solution with stirring within 1.5 hours.
  • the mixture is stirred for a further 2 h.
  • the pH of the reaction mixture is then 1.5.
  • the resulting CO 2 can be collected, cleaned and compressed if necessary.
  • Residual fire 0.03% (24 h at 40 ° C):
  • the relative color strength against Bayferrox 330 is 98%.
  • the magnetite obtained is also suitable as a magnetic pigment for toners:
  • the relative color strength against Bayferrox 180 M is 196%.
  • a suspension consisting of 0.464 kg CaO and 4.176 kg water is then pumped in over 2 hours.
  • the pH of the reaction mixture is then 4.5.
  • the precipitate is filtered off through suction filters and washed with about 75 kg of water.
  • the predominantly gypsum-containing solid obtained has a comparable composition and only a slightly lower degree of whiteness than that in the first
  • Precipitation stage obtained from Example 1 is suitable for most applications in the same way.
  • a comparison with gypsum from a flue gas desulfurization plant shows that the whiteness of the gypsum obtained according to the invention is significantly higher than that of REA gypsum.
  • the filtrate is worked up further to give an iron oxide black pigment as in Example 1.
  • the gypsum is precipitated and separated in the first stage analogously to Example 1.
  • the neutralization up to pH 4.5 can only be achieved using NH 3 (without
  • the magnetite obtained from the highly concentrated ammonium sulfate solution has too much lightening or too little color, it is not suitable as a pigment.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Organic Chemistry (AREA)
  • Inorganic Chemistry (AREA)
  • Life Sciences & Earth Sciences (AREA)
  • Geology (AREA)
  • Compounds Of Iron (AREA)
  • Pigments, Carbon Blacks, Or Wood Stains (AREA)
  • Inorganic Compounds Of Heavy Metals (AREA)
  • Compounds Of Alkaline-Earth Elements, Aluminum Or Rare-Earth Metals (AREA)
  • Manufacture And Refinement Of Metals (AREA)
PCT/EP1999/001735 1998-03-20 1999-03-17 VERFAHREN ZUR AUFARBEITUNG VON DÜNNSÄURE AUS DER TiO2-HERSTELLUNG Ceased WO1999048808A1 (de)

Priority Applications (8)

Application Number Priority Date Filing Date Title
US09/646,340 US6440377B1 (en) 1998-03-20 1999-03-17 Method for reprocessing waste acid resulting from TiO2 production
DE59901851T DE59901851D1 (de) 1998-03-20 1999-03-17 VERFAHREN ZUR AUFARBEITUNG VON DÜNNSÄURE AUS DER TiO2-HERSTELLUNG
AU29335/99A AU2933599A (en) 1998-03-20 1999-03-17 Method for reprocessing waste acid resulting from TiO2 production
BR9908920-3A BR9908920A (pt) 1998-03-20 1999-03-17 Processo para o processamento de ácido residual obtido da preparação de tio2
JP2000537798A JP2002507632A (ja) 1998-03-20 1999-03-17 二酸化チタン製造から生じる廃棄酸の再処理方法
EP99910350A EP1064223B1 (de) 1998-03-20 1999-03-17 VERFAHREN ZUR AUFARBEITUNG VON DÜNNSÄURE AUS DER TiO2-HERSTELLUNG
CA002324308A CA2324308A1 (en) 1998-03-20 1999-03-17 Method for reprocessing waste acid resulting from tio2 production
NO20004682A NO323628B1 (no) 1998-03-20 2000-09-19 Fremgangsmate for fremstilling av gips sa vel som et jernoksidpigment fra den ved fremstillingen av TiO2 dannede tynnsyre

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
DE19812261A DE19812261A1 (de) 1998-03-20 1998-03-20 Verfahren zur Aufarbeitung von Dünnsäure aus der TiO¶2¶-Herstellung
DE19812261.6 1998-03-20

Publications (1)

Publication Number Publication Date
WO1999048808A1 true WO1999048808A1 (de) 1999-09-30

Family

ID=7861668

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/EP1999/001735 Ceased WO1999048808A1 (de) 1998-03-20 1999-03-17 VERFAHREN ZUR AUFARBEITUNG VON DÜNNSÄURE AUS DER TiO2-HERSTELLUNG

Country Status (11)

Country Link
US (1) US6440377B1 (cg-RX-API-DMAC7.html)
EP (1) EP1064223B1 (cg-RX-API-DMAC7.html)
JP (1) JP2002507632A (cg-RX-API-DMAC7.html)
AU (1) AU2933599A (cg-RX-API-DMAC7.html)
BR (1) BR9908920A (cg-RX-API-DMAC7.html)
CA (1) CA2324308A1 (cg-RX-API-DMAC7.html)
DE (2) DE19812261A1 (cg-RX-API-DMAC7.html)
ES (1) ES2179627T3 (cg-RX-API-DMAC7.html)
NO (1) NO323628B1 (cg-RX-API-DMAC7.html)
WO (1) WO1999048808A1 (cg-RX-API-DMAC7.html)
ZA (1) ZA200004672B (cg-RX-API-DMAC7.html)

Cited By (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP1382571A1 (de) * 2002-07-16 2004-01-21 Sachtleben Chemie GmbH Verfahren zur Herstellung von Eisenhydroxid, Eisenoxidhydrat oder Eisenoxid aus Filtersalzen der Dünnsäurerückgewinnung
WO2014084129A1 (ja) * 2012-11-28 2014-06-05 住友金属鉱山株式会社 中和処理方法及び中和剤
CN113493215A (zh) * 2021-07-21 2021-10-12 吉林大学 一种活性氢氧化镁的制备方法

Families Citing this family (13)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
DE20321107U1 (de) † 2003-07-17 2005-12-15 Kerr-Mcgee Pigments Gmbh Zubereitung zur Reduktion des löslichen Chromatgehaltes in Zement
WO2005068358A1 (en) * 2003-12-18 2005-07-28 Millennium Chemicals Production of 'useful material(s)' from waste acid issued from the production of titanium dioxyde
US7704470B2 (en) * 2007-04-24 2010-04-27 Haydock Consulting Services, Lc Removal of contaminants from by-product acids
RU2400505C2 (ru) * 2008-03-26 2010-09-27 Александр Васильевич Вальков Способ получения железосодержащего пигмента
CN102115210B (zh) * 2010-12-31 2012-10-17 谢善情 用硫酸法生产钛白粉所得废酸生产硝酸亚铁和硫酸钙的方法
CN103572058B (zh) * 2012-07-31 2016-01-20 有研稀土新材料股份有限公司 一种从硫酸法钛白废液中富集稀土稀有元素和制备白石膏的方法
US9840896B2 (en) * 2012-09-21 2017-12-12 Thru Tubing Solutions, Inc. Acid soluble abrasive material and method of use
CN104086027B (zh) * 2014-07-15 2015-06-10 铜陵化学工业集团有限公司 一种硫酸法钛白废水处理方法
JP5704280B2 (ja) * 2014-11-17 2015-04-22 住友金属鉱山株式会社 中和処理方法及び中和剤
JP6638345B2 (ja) * 2015-03-17 2020-01-29 住友大阪セメント株式会社 石膏の製造方法およびセメント組成物の製造方法
CN111485102A (zh) * 2020-04-26 2020-08-04 张响 一种全资源化利用钛白废酸的工艺
CN116411165B (zh) * 2021-12-31 2026-06-05 比亚迪股份有限公司 一种分离卤水中铁元素的方法及其应用
CN116589127A (zh) * 2023-05-22 2023-08-15 龙佰四川钛业有限公司 一种钛白废水无废化处理方法

Citations (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0638515A2 (de) * 1993-08-12 1995-02-15 Bayer Antwerpen N.V. Verfahren zur Aufarbeitung von Dünnsäure

Family Cites Families (8)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US3375066A (en) * 1963-08-24 1968-03-26 Yawata Chem Ind Co Ltd Process for the continuous production of gypsum and iron oxide from waste sulfuric acid pickle liquor and a calcium compound
GB1421773A (en) 1972-10-20 1976-01-21 Laporte Industries Ltd Production of iron oxide
CA1053876A (en) 1973-12-14 1979-05-08 Arthur A. Bellinger Method and means of growing coarse gypsum and magnetite
JPS5110198A (cg-RX-API-DMAC7.html) * 1974-07-15 1976-01-27 Toda Kogyo Corp
US4137293A (en) * 1977-12-16 1979-01-30 Ishihara Sangyo Kaisha, Ltd. Producing gypsum and magnetite from ferrous sulfate and separating
US4137292A (en) 1978-03-02 1979-01-30 Uop Inc. Purification of titanium trichloride
DE3327769A1 (de) 1983-08-02 1985-02-14 Bayer Ag, 5090 Leverkusen Verfahren zur aufarbeitung von duennsaeuren
GB9213998D0 (en) 1992-07-01 1992-08-12 Tioxide Group Services Ltd Process for preparing calcium sulphate

Patent Citations (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0638515A2 (de) * 1993-08-12 1995-02-15 Bayer Antwerpen N.V. Verfahren zur Aufarbeitung von Dünnsäure

Non-Patent Citations (1)

* Cited by examiner, † Cited by third party
Title
DATABASE WPI Section Ch Derwent World Patents Index; Class E31, AN 71-25991S, XP002107325 *

Cited By (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP1382571A1 (de) * 2002-07-16 2004-01-21 Sachtleben Chemie GmbH Verfahren zur Herstellung von Eisenhydroxid, Eisenoxidhydrat oder Eisenoxid aus Filtersalzen der Dünnsäurerückgewinnung
WO2014084129A1 (ja) * 2012-11-28 2014-06-05 住友金属鉱山株式会社 中和処理方法及び中和剤
CN113493215A (zh) * 2021-07-21 2021-10-12 吉林大学 一种活性氢氧化镁的制备方法
CN113493215B (zh) * 2021-07-21 2022-11-15 吉林大学 一种活性氢氧化镁的制备方法

Also Published As

Publication number Publication date
CA2324308A1 (en) 1999-09-30
DE59901851D1 (de) 2002-08-01
AU2933599A (en) 1999-10-18
NO20004682L (no) 2000-10-04
EP1064223B1 (de) 2002-06-26
ZA200004672B (en) 2002-02-27
NO323628B1 (no) 2007-06-18
ES2179627T3 (es) 2003-01-16
BR9908920A (pt) 2000-11-21
EP1064223A1 (de) 2001-01-03
DE19812261A1 (de) 1999-09-23
US6440377B1 (en) 2002-08-27
NO20004682D0 (no) 2000-09-19
JP2002507632A (ja) 2002-03-12

Similar Documents

Publication Publication Date Title
EP1064226B1 (de) VERFAHREN ZUR HERSTELLUNG VON EISENOXID-PIGMENTEN AUS DÜNNSÄURE AUS DER TiO2-HERSTELLUNG
EP0911369B1 (de) Eisenoxidrotpigmente, Verfahren zur Herstellung von Eisenoxidrotpigmenten und deren Verwendung
EP1064223B1 (de) VERFAHREN ZUR AUFARBEITUNG VON DÜNNSÄURE AUS DER TiO2-HERSTELLUNG
EP0911370B1 (de) Eisenoxidgelbpigmente, Verfahren zur Herstellung von Eisenoxidgelbpigmenten und deren Verwendung
EP1064227B1 (de) Verfahren zur aufarbeitung von dünnsäure aus der tio2-herstellung
EP1339803B1 (de) Verfahren zur herstellung von eisenoxidgelbpigmenten
DE4003255A1 (de) Schwarzes mangan-eisenoxid-pigment, verfahren zu seiner herstellung sowie dessen verwendung
EP0202567B1 (de) Verfahren zur Herstellung von Schwarzpigmenten auf Eisenbasis
DE2518283A1 (de) Verfahren zur herstellung von eisenoxidschwarzpigmenten
EP1317514A1 (de) Verfahren zur herstellung eines aluminiumhaltigen eisenoxidkeims
EP1132343A2 (de) Verfahren zur Herstellung von Eisenoxid und seine Verwendung
EP0233975B1 (de) Verfahren zur Verbesserung von Titandioxid-Pigmenten durch eine Nachbehandlung
EP0849226B1 (de) Verfahren zur Herstellung von Eisenoxidgelbpigmenten und deren Verwendung
EP1512726A2 (de) Verfahren zur Herstellung von Eisenoxidgelbpigmenten mit CACO3 als Fällungsmittel
EP1606355A1 (de) Eisenoxidpigmente
DE3509268A1 (de) Verfahren zur herstellung von roten eisenoxid-pigmenten aus eisen(ii)-sulfatrueckstaenden
DE19725021B4 (de) Sulfatarmer, neutraler, inerter, feinteiliger Füllstoff, Verfahren zu dessen Herstellung sowie dessen Verwendung
EP1317513A1 (de) Verfahren zur herstellung eines aluminiumhaltigen eisenoxidkeims
DE10044095A1 (de) Verfahren zur Herstellung eines aluminiumhaltigen Eisenoxidkeims
DE10050683A1 (de) Verfahren zur Herstellung eines aluminiumhaltigen Eisenoxidkeims
DE10340501A1 (de) Verfahren zur Herstellung von Eisenoxidgelbpigmenten mit CaCO3 als Fällungsmittel

Legal Events

Date Code Title Description
AK Designated states

Kind code of ref document: A1

Designated state(s): AE AL AM AT AU AZ BA BB BG BR BY CA CH CN CU CZ DE DK EE ES FI GB GD GE GH GM HR HU ID IL IN IS JP KE KG KP KR KZ LC LK LR LS LT LU LV MD MG MK MN MW MX NO NZ PL PT RO RU SD SE SG SI SK SL TJ TM TR TT UA UG US UZ VN YU ZA ZW

AL Designated countries for regional patents

Kind code of ref document: A1

Designated state(s): GH GM KE LS MW SD SL SZ UG ZW AM AZ BY KG KZ MD RU TJ TM AT BE CH CY DE DK ES FI FR GB GR IE IT LU MC NL PT SE BF BJ CF CG CI CM GA GN GW ML MR NE SN TD TG

121 Ep: the epo has been informed by wipo that ep was designated in this application
DFPE Request for preliminary examination filed prior to expiration of 19th month from priority date (pct application filed before 20040101)
WWE Wipo information: entry into national phase

Ref document number: 1999910350

Country of ref document: EP

WWE Wipo information: entry into national phase

Ref document number: 09646340

Country of ref document: US

ENP Entry into the national phase

Ref document number: 2324308

Country of ref document: CA

Ref country code: CA

Ref document number: 2324308

Kind code of ref document: A

Format of ref document f/p: F

NENP Non-entry into the national phase

Ref country code: KR

WWP Wipo information: published in national office

Ref document number: 1999910350

Country of ref document: EP

REG Reference to national code

Ref country code: DE

Ref legal event code: 8642

NENP Non-entry into the national phase

Ref country code: CA

WWG Wipo information: grant in national office

Ref document number: 1999910350

Country of ref document: EP