JPH0750008A - 磁気記録媒体 - Google Patents

磁気記録媒体

Info

Publication number
JPH0750008A
JPH0750008A JP21214693A JP21214693A JPH0750008A JP H0750008 A JPH0750008 A JP H0750008A JP 21214693 A JP21214693 A JP 21214693A JP 21214693 A JP21214693 A JP 21214693A JP H0750008 A JPH0750008 A JP H0750008A
Authority
JP
Japan
Prior art keywords
magnetic
recording medium
magnetic recording
layer
coercive force
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP21214693A
Other languages
English (en)
Inventor
Daizo Endo
大三 遠藤
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Resonac Holdings Corp
Original Assignee
Showa Denko KK
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Showa Denko KK filed Critical Showa Denko KK
Priority to JP21214693A priority Critical patent/JPH0750008A/ja
Publication of JPH0750008A publication Critical patent/JPH0750008A/ja
Pending legal-status Critical Current

Abstract

(57)【要約】 【目的】 高保磁力及び低ノイズの磁気記録媒体を提案
する。 【構成】 非磁性基体層上に非磁性金属下地層、磁性
層、保護層を設けてなる磁気記録媒体であり、前記磁性
層はCo60〜80at%とCr5〜20at%とPt
1〜20at%とNb,Hf,W,Ti,Taのうちの
1種以上0.5〜6at%とからなる合金組成を有する
薄膜媒体である。

Description

【発明の詳細な説明】
【0001】
【産業上の利用分野】本発明は、磁気ディスク、磁気ド
ラム、磁気テープなどの磁気記録媒体に関する。
【0002】
【従来の技術】近年、磁気記録媒体においては、高記録
密度が要求され、そのために連続薄膜媒体が注目されて
いる。このような連続薄膜媒体の磁性層としては、Co
CrTa系、CoCrPt系などの合金が知られてい
て、スパッタ等の方法により成膜される。
【0003】そして、高記録密度のためには、高保磁力
(以下、保磁力をHcと記載する)及び低ノイズが要求
される。
【0004】
【発明が解決しようとする課題】しかしながら、従来の
CoCrTa系の合金は、低ノイズに関しては優れてい
るが高保磁力(Hc≧1500oe)の点では不十分で
あり、CoCrPt系の合金は、高保磁力に関しては優
れているが低ノイズの点では不十分であった。したがっ
て、高保磁力及び低ノイズの両特性を満足する磁気記録
媒体が嘱望されていた。
【0005】
【課題を解決するための手段】上記高保磁力及び低ノイ
ズの両特性を満足させるため、本発明は、非磁性基体層
上に、Coと、Crと、Ptと、Nb,Hf,W,T
i,Taのうちの1種以上とからなる磁性層を形成し、
その組成割合をCr5〜20at%、Pt1〜20at
%、Nb,Hf,W,Ti,Taのうちの1種以上0.
5〜6at%、残部Coに設定した磁気記録媒体に関す
るものである。
【0006】本発明に先立ち、本発明者はAr圧6mT
orr、投入パワー4W/cm2 、基板温度230℃で
DCマグネトロンスパッタリング法によりTEXを施し
たNiPメッキ基板上に形成したCoCrPtNb合金
磁性膜の記録再生特性を測定した。このとき、CoCr
PtNbの組成割合は、CoCrターゲットにNb及び
Ptチップを埋め込むことによりコントロールした。そ
の結果、CoCrPtNb合金磁性膜は、従来のCoC
rPt磁性膜に比べて媒体ノイズが低減していることが
見出された。このような効果は、Nb0.5at%以
上、Pt20at%以下の条件で認められた。また、N
bをHf,W,Ti,Taに代えても同様の効果が認め
られた。一方、このNb、Hf、W、Ti、Taの添加
により、磁性膜の飽和磁束密度が低下するが、その含有
量が6at%以下であれば実用上十分な値を有すること
がわかった。同様に、Crの含有量が20at%以下で
あれば飽和磁束密度の低下も実用上問題ない。また、C
r、Ptの含有量がそれぞれ5at%以下、1at%以
下の条件ではHcが低下し、面内磁気記録媒体としては
好ましくない。さらに記録再生特性を向上させるために
は、Ptの含有量を3〜20at%とすることが望まし
い。
【0007】また、面内磁気記録としてHcを再現よく
高い値に保つため、非磁性基体層と磁性層との間にCr
またはCr合金からなる非磁性金属下地層を100〜3
000Åの膜厚で設けることが望ましい。
【0008】さらに、上記磁気記録媒体の表面に50〜
500Åの非磁性被覆膜を形成させることにより、耐久
性及び耐蝕性を向上させることができる。
【0009】
【実施例】以下、本発明の実施例を示す。
【0010】[製造方法];日電アネルバ製ILC−3
108を用い、DCマグネトロンスパッタリング法でス
パッタを行った。非磁性基体層としては、NiPメッキ
Al板(95mmφ)を用いた。ターゲットは、Cr/
CoCr合金/Cで、CoCr合金ターゲット上にP
t、M(Nb,Ti,Hf,W,Ta)を埋め込んで実
験を行った。Co合金の組成割合は、ペレットの数によ
りコントロールした。
【0011】次に、上記製造方法により製造された磁気
記録媒体の静磁気特性並びに記録再生特性を調べた。静
磁気特性は振動式磁気特性装置(VSM)を用いて測定
し、記録再生特性は、ギャップ長0.4μm、トラック
幅10μm、フライングハイト0.1μmのMIGヘッ
ドを使用し、測定記録密度36KFCI(半径20m
m)にて測定し、その結果を表1に示した。
【0012】
【表1】
【0013】上記表1より、本発明の実施例1〜7で
は、高保磁力、低ノイズ、低ビットシフトが得られるこ
とが確認された。
【0014】
【発明の効果】以上説明したように、本発明の磁気記録
媒体は、高保磁力及び低ノイズの両特性を満足し、高密
度記録が可能な磁気ディスク、磁気ドラム、磁気テープ
などを得ることができるものである。

Claims (3)

    【特許請求の範囲】
  1. 【請求項1】 非磁性基体層上に非磁性金属下地層、磁
    性層、保護層を設けてなる磁気記録媒体において、前記
    磁性層はCo60〜80at%とCr5〜20at%と
    Pt1〜20at%とNb,Hf,W,Ti,Taのう
    ちの1種以上0.5〜6at%とからなる合金組成を有
    する薄膜媒体であることを特徴とする磁気記録媒体。
  2. 【請求項2】 請求項1に記載の磁気記録媒体におい
    て、磁性層中のPtの含有量が3〜20at%であるこ
    とを特徴とする磁気記録媒体。
  3. 【請求項3】 非磁性金属下地層のCrまたはCr合金
    を用い、その膜厚が100〜3000Åであることを特
    徴とする請求項1乃至2に記載の磁気記録媒体。
JP21214693A 1993-08-05 1993-08-05 磁気記録媒体 Pending JPH0750008A (ja)