JP5208804B2 - 建築板の製造方法 - Google Patents
建築板の製造方法 Download PDFInfo
- Publication number
- JP5208804B2 JP5208804B2 JP2009042635A JP2009042635A JP5208804B2 JP 5208804 B2 JP5208804 B2 JP 5208804B2 JP 2009042635 A JP2009042635 A JP 2009042635A JP 2009042635 A JP2009042635 A JP 2009042635A JP 5208804 B2 JP5208804 B2 JP 5208804B2
- Authority
- JP
- Japan
- Prior art keywords
- ink
- building board
- weight
- diacrylate
- pigment
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Fee Related
Description
(2)(1)の工程の後、UVインクにてインクジェット塗装を施す工程と、
(3)(2)の工程の後、紫外線によりUVインクを硬化させる工程とからなる建築板の製造方法であって、
前記下塗り塗装の塗料が、造膜助剤を含まない状態でのMFT(最低造膜温度)が75℃〜110℃であるアクリル系エマルションであり、
前記UVインクは、2官能の反応性モノマーと、脂肪族の反応性オリゴマーと、光重合開始剤と、顔料とが含まれてなり、
前記(2)の工程における基材の板温が45〜55℃である建築板の製造方法である。
〔下塗り塗装工程〕
樹脂エマルションAD77(樹脂分48.0%、アクリル−スチレンエマルジョン、MFT=75℃、Tg=75℃、ヘンケルテクノロジーズジャパン(株)製)100重量部、造膜助剤キョーワノールM(2,2,4−トリメチルー1,3−ペンタンジオールモノイソブチレート、協和発酵ケミカル(株)製)10重量部、白顔料分散体LIOFAST WHITE H201(顔料分60%、東洋インキ製造(株)製)55重量部、水10量部を加え10分間撹拌後、80メッシュで濾過実施して、下塗り塗料を得た。
青顔料Blue P−BFS(C.I.Pigment Blue 15:4 銅フタロシアニン、クラリアントジャパン(株)製)3重量部、分散剤Disperbyk−168(高分子化合物、BykChemie製)を3重量部、反応性オリゴマーCN985B88(脂肪族ウレタンアクリレート、2官能、サートマー(株)製)を20重量部、反応性モノマーSR238F(1,6−へキサンジオールジアクリレート、2官能、サートマー(株)製)68.3重量部、光重合開始剤ダロキュア1173(2−ヒドロキシ−2−メチル−1−フェニル−プロパン−1−オン、チバ・スペシャリティ・ケミカルズ(株)製)5重量部、濡れ剤DOW CORNING TORAY 32 ADDITIVE(シリコーン系濡れ剤、東レダウコーニングシリコーン(株)製)0.7重量部を加え、ビーズミル分散機を用い分散した後、濾過を行って不純物除去し、均質なブルーUVインクを作製した。作製したインクの粘度は8.5mPas/60℃、表面張力は25.0dyne/cm・25℃であった。
◎インクジェット塗装条件
イ)ノズル径 : 70(μm)
ロ)印加電圧 : 50(V)
ハ)パルス幅 : 15(μs)
ニ)駆動周波数 : 5(KHz)
ホ)解像度 : 180(dpi)
ヘ)ヘッド加熱温度 : 60(℃)
ホ)インク塗布量 : 5(g/m2)
インクジェット塗装後、以下の条件にてUVインクの硬化をおこなって、目的とする建築板を得た。得られた建築板を以下の評価方法にて評価した結果を表1に示す。
◎紫外線照射条件
あ)ランプ種類 : メタルハライドランプ
い)電圧 : 100 (W/cm)
う)照射時間 : 0.5 (秒)
え)照射高さ : 10 (cm)
お)プリント〜照射までのタイミング : 5 (秒)
1)密着性 JIS K 5600−5−6 付着性(クロスカット)
今回の試験においてはカットの間隔は4mm間隔で実施し、セロテープ(登録商標)を貼り、消しゴムで15往復させた後、勢い良く剥がし、その後の状態を確認した。
○:カット縁が完全に滑らかでどの格子も剥れがないか、カット交差点に於ける塗膜
の小さな剥れが5%未満である
△:カット縁および/または交差点に於ける塗膜の小さな剥れで、剥れが5〜35%
である
×:カット縁および/または部分的全面的に大剥れで、剥れが35%以上である
インクジェット塗装した画像の線幅を測定した。
○:200μmより広い
△:200〜150μm
×:150μm未満
実施例1にて得られた建築板のインクジェット塗装した画像を基準値として各実施例および比較例の色差△Eを測定した。なお、色差△Eは分光測色計(型式:CM−2500c コニカミノルタ(株)製)を用いて測定した。
○:0<△E<1.5 熟練者の目視でも識別できない精度
△:1.5≦△E<3.0 目視で識別できない精度
×:3.0≦△E 目視でも識別可能な精度
板温を50℃とした以外は実施例1と同様にして建築板を作製した。得られた建築板を上記の評価方法にて評価した結果を表1に示す。
板温を55℃とした以外は実施例1と同様にして建築板を作製した。得られた建築板を上記の評価方法にて評価した結果を表1に示す。
板温を25℃とした以外は実施例1と同様にして建築板を作製した。得られた建築板を上記の評価方法にて評価した結果を表1に示す。
板温を60℃とした以外は実施例1と同様にして建築板を作製した。得られた建築板を上記の評価方法にて評価した結果を表1に示す。
下塗り塗装の樹脂をAD157(樹脂分49.0%、アクリルエマルジョン、MFT=40℃、Tg=40℃、ヘンケルテクノロジーズジャパン(株)製)に変更する以外は実施例1と同様にして建築板を作製した。得られた建築板を上記の評価方法にて評価した結果を表1に示す。
Claims (3)
- 基材に、(1)下塗り塗装を施す工程と、
(2)(1)の工程の後、UVインクにてインクジェット塗装を施す工程と、
(3)(2)の工程の後、紫外線によりUVインクを硬化させる工程とからなる建築板の製造方法であって、
前記下塗り塗装の塗料が、造膜助剤を含まない状態でのMFT(最低造膜温度)が75℃〜110℃であるアクリル系エマルションであり、
前記UVインクは、2官能の反応性モノマーと、脂肪族の反応性オリゴマーと、光重合開始剤と、顔料とが含まれてなり、
前記(2)の工程における基材の板温が45〜55℃であることを特徴とする建築板の製造方法。 - 前記UVインクの表面張力が20〜30dyne/cm・25℃であることを特徴とする請求項1記載の建築板の製造方法。
- 前記2官能の反応性モノマーが、1,6−ヘキサンジオールジアクリレート、ネオペンチルグリコールジアクリレート、1,3−ブチレングリコールジアクリレート、1,4−ブタンジオールジアクリレートおよび1,9−ノナンジオールジアクリレートから選択される少なくとも1種であることを特徴とする請求項1または2記載の建築板の製造方法。