CN1818176B - 精毛纺织物经向间隔绒面产品的生产方法 - Google Patents

精毛纺织物经向间隔绒面产品的生产方法 Download PDF

Info

Publication number
CN1818176B
CN1818176B CN 200610038781 CN200610038781A CN1818176B CN 1818176 B CN1818176 B CN 1818176B CN 200610038781 CN200610038781 CN 200610038781 CN 200610038781 A CN200610038781 A CN 200610038781A CN 1818176 B CN1818176 B CN 1818176B
Authority
CN
China
Prior art keywords
silk
yarn
wool
fluffing
temperature
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN 200610038781
Other languages
English (en)
Other versions
CN1818176A (zh
Inventor
孙云丰
张建刚
李敏芳
徐仁忠
庞志红
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shandong Sinoer Co ltd
Original Assignee
JIANGSU HUAXICUN CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by JIANGSU HUAXICUN CO Ltd filed Critical JIANGSU HUAXICUN CO Ltd
Priority to CN 200610038781 priority Critical patent/CN1818176B/zh
Publication of CN1818176A publication Critical patent/CN1818176A/zh
Application granted granted Critical
Publication of CN1818176B publication Critical patent/CN1818176B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明涉及一种精毛纺织物经向间隔绒面产品的生产方法,它是选用全毛或毛涤纱线作经纱,全棉或丝棉混纺纱、或丝毛混纺纱、或丝与再生性纤维素纤维混纺纱作纬纱,通过变化的纬浮长组织制织,采用洗呢、煮呢、烘呢、起绒、剪毛、给湿、蒸呢后整理工艺生产精毛纺织物经向间隔绒面产品。本发明产品绒面丰满致密光泽感好,手感细腻柔软而富有弹性,有良好的挺度和悬垂感,不易起球。

Description

精毛纺织物经向间隔绒面产品的生产方法
技术领域:
本发明涉及纺织生产领域内的一种产品生产方法;特指精毛纺经向间隔绒面产品的生产方法。属纺织技术领域。
背景技术:
精毛纺绒面产品通过以下两种途径获得:
一、羊毛纤维属蛋白质纤维,羊毛纤维表面具有鳞片层,在湿热条件下,鳞片就会张开,如同时加以反复挤压,则由于逆鳞片方向与顺鳞片方向的摩擦效应不同,使纤维保持根部向前运动的方向性。这样各根纤维带着和它纠缠在一起的纤维按一定方向蠕动,就会使羊毛纤维相互咬合成毡,羊毛织物缩短变厚。这一性质称为羊毛的缩绒性。利用这一性质,人们在一定压力、温度等条件下,对羊毛织物进行缩绒,使羊毛制品获得丰厚、保暖性良好的绒面产品。但经过缩绒工艺处理的产品有以下不足:
(1)影响洗涤后的尺寸稳定性。
(2)影响最终成品的服用性能,易起毛起球。
(3)起绒只能整体起绒,不能间隔起绒,呢面呆板。
二、近几年,在精毛纺织物中,经向间隔绒面的产品有两种。一种是以棉、涤棉、腈纶等纤维为主的雪尼尔纱作经纱,毛纱为纬纱的织物。另一种以羊毛及羊毛与其它纤维混纺生产的精毛纺灯芯绒。前者产品档次较低,间隔条距离受到纱支粗的限制,织物外观疵点较多。后者产品受到原料性能,割绒工艺、后整理的工艺的限制,生产的产品达不到服用要求,实施产业化较为困难。
好的绒面产品应该是:丰满而有光泽,致密而不露底,落毛量少而不损织物,绒毛效果持久,起毛一端外露,另端纠结于织物之中,起“盘根效应”。应该指出,是否容易起毛和是否容易起质量好的绒毛并不完全一回事。比如,容易起毛的织物往往损伤较大,服用性能也较差。影响精毛纺经向间隔绒面织物的风格及服用性能因素有四个方面:起绒部分的原料性能、纱线的结构、织物组织结构、起毛工艺和后整理工艺的控制。四个方面是相互影响,相互依赖,相互结合。
发明内容:
本发明的目的在于克服上述不足,提供一种绒面丰满致密光泽感好,手感细腻柔软而富有弹性,有良好的挺度和悬垂感,不易起球的精毛纺织物经向间隔绒面产品的生产方法。
本发明的目的是这样实现的:一种精毛纺织物经向间隔绒面产品的生产方法,其特征在于:选用全毛或毛涤纱线作经纱,全棉或丝棉混纺纱、丝毛混纺纱、丝与再生性纤维素纤维混纺纱作纬纱,即起绒纱或称绒纬,通过变化的纬浮长组织制织,采用洗呢、煮呢、烘呢、起绒、剪毛、给湿、蒸呢后整理工艺生产精毛纺织物经向间隔绒面产品,其具体方法包括:
a)纬纱原料性能的选择:
纬纱即起绒纱选用长绒棉,该纤维特别细长,手扯长度33mm以上,一般为33-45mm,细度细于143mtex(7000公支以上),该纤维经起绒后绒面丰满,手感细腻,产品柔软而富有弹性;或:
纬纱即起绒纱选用丝棉混纺纱(含色纺纱、染色纱),丝棉混纺纱蚕丝纤维的纤度为2.5-3.5旦,单丝截面呈角圆的三角形,纵面比较平直光滑,该纤维与棉混纺纱经起绒后,织物表面致密,具有较强的光泽感;或
纬纱即起绒纱选用丝毛混纺纱,纱线采用细羊毛与蚕丝混纺,超细羊毛的纤维很细,直径为14.5-20.5μm,有优良的弹性性能,与蚕丝混纺,纺纱性能良好。经起绒后,织物表面细腻,光泽柔和而富有弹性;或
纬纱即起绒纱选用丝与再生性纤维素纤维混纺纱,再生性纤维素纤维含天丝(TENCEL)、蒙旦尔(Modal),天丝(TENCEL)、蒙旦尔(Modal)纤维具有高湿模量,在干或湿的状态下,均极具韧性。它能与丝等多种纤维混纺,蚕丝与天丝或蒙旦尔混纺纱经起绒后,产品具有桃皮绒感,富有弹力,有良好的挺度和悬垂感。
b)纬纱纱线结构:
纬纱捻系数为11.5~12.5(即:捻度/10cm=捻系数*
Figure 061387819_0
Nm),纬纱纱线结构对起绒影响较大,起绒部分纱线捻度的大小,直接影响成品的服用要求。捻度太低,易起球,捻度太高,呢面起毛不匀。
c)织物结构:
选用1/3、3/1联合变化组织为基础,确定规格不同的织物组织,采用粗条、细条、中条、粗细条、粗细间隔条等由纬纱而形成的经向条形组织,使起绒后呈现不同的丰满而不露地的条形间隔绒面效果。
d)起毛工艺及后整理工艺控制:
起毛之前先进行绳状洗呢,使生坯织物消除内应力,织物疏松、易于起毛。洗呢工艺为:(1)初洗:坯布上机,温度38℃±5℃,冲洗5min±2min,(2)皂洗:温度40℃±5℃,浴比:1∶6-10,净洗剂用量1.5-2.0%,油皂酸用量1.5-2.0%,时间40min-45min,呢速120-150m/min,(3)冲洗;用温度36℃±5℃,浴比:1∶13-16,连续冲洗30min±5min,再用温度30℃±5℃冲洗10min±5min,
煮呢作用是去除绳状洗呢形成的折痕,保证织物手感丰厚,滑细、有弹性。煮呢采用双槽煮呢,煮多次,前几次加压,温度为80℃-85℃,PH6.5-7,槽外喷水冷却出机,
烘呢的作用使织物达到要求的回潮率,使织物尺寸稳定,有利于保证成品的规定尺寸。烘呢工艺为:机内温度为100℃-110℃,呢速12-15m/min,经向超喂4%-5%,拉幅3-5cm,烘呢结束,回潮控制在8%-12%之间,
起毛工艺采用干起毛和湿起毛相结合的工艺,在干起毛工艺中,顺辊和逆辊都采用零点起毛,采用植针角80°,工作角40°针布,以柔和的方式形成短毛,然后增大布速和顺辊转速,减低逆辊转速,干起毛起三次以上,使织物具有柔软的手感和风格;湿起毛采用刺果湿起毛,湿起毛在湿润状态下对纤维损伤较小,作用柔和也耐用,易形成光泽自然的厚密绒毛。
剪毛的作用是将起绒后绒面剪齐,使呢面平坦,光泽柔和。剪毛工艺采用织物速度10-12m/min,螺旋刀速度1100r/min,正面剪几次,反面剪一次,隔距为20-30丝,
给湿的作用是改善织物机械性能和手感,同时提高蒸呢加工质量和效果,蒸呢之前给湿,控制其回潮率为12%6-15%,并存放8小时±2小时,
蒸呢的作用主要是稳定尺寸,柔化身骨。蒸呢工艺为蒸汽压力在1.2-2.5kg/cm2,内汽10-12min,抽冷8-10min。
经过上述改进,本发明精毛纺织物经向间隔绒面产品绒面丰满致密光泽感好,手感细腻柔软而富有弹性,有良好的挺度和悬垂感,不易起球。
具体实施方式:
实施例1:
选用全毛纱线作经纱,长绒棉作纬纱,长绒棉手扯长度33(-45)mm细度143mtex,纬纱捻系数为11.5~12.5,选用1/3、3/1联合变化组织为基础,起毛之前先进行绳状洗呢,洗呢工艺为:(1)初洗:坯布上机,温度38℃,冲洗5min。(2)皂洗:温度40℃,浴比:1∶8,净洗剂用量1.5-2.0%,油皂酸用量1.5-2.0%,时间40min-45min,呢速120-150m/min。(3)冲洗:用温度36℃(浴比:1∶15)连续冲洗30min,再用温度30℃冲洗10min;煮呢采用双槽煮呢,煮6次,前2次加压,温度为80℃-85℃,PH 6.5-7,槽外喷水冷却出机;烘呢工艺为:机内温度为100℃-110℃,呢速12-15m/min,经向超喂4%-5%,拉幅3-5cm,烘呢结束,回潮控制在8%-12%之间;起毛工艺采用干起毛和湿起毛相结合的工艺,在干起毛工艺中,顺辊和逆辊都采用零点起毛,采用植针角80℃,工作角40℃针布,以柔和的方式形成短毛,然后增大布速和顺辊转速,减低逆辊转速,干起毛起三次以上;湿起毛采用刺果湿起毛,剪毛工艺采用织物速度10-12m/min,螺旋刀速度1100r/min,正面剪三次,反面剪一次,隔距为20-30丝;蒸呢之前给湿,控制其回潮率为12%-15%,并存放8小时;蒸呢工艺为蒸汽压力在1.2-2.5kg/cm2,内汽10-12min,抽冷8-10min。
实施例2:
选用毛涤纱线作经纱,丝棉混纺纱作纬纱,丝棉混纺纱蚕丝纤维的纤度为2.5-3.5旦,单丝截面呈角圆的三角形,丝棉混纺纱丝与棉的重量比为55:45,纬纱捻系数为11.5~12.5,其余同例1。
实施例3:
选用毛涤纱线作经纱,丝毛混纺纱作纬纱,丝毛混纺纱纱线采用细羊毛与蚕丝混纺,细羊毛直径为14.5-20.5μm,丝毛混纺纱丝与毛的重量比比为15:85,纬纱捻系数为11.5~12.5,其余同例1。
实施例4:
选用毛涤纱线作经纱,丝与再生性纤维素纤维混纺纱作纬纱,丝与再生性纤维素纤维混纺纱丝与再生性纤维素纤维的重量比比为70∶30,纬纱捻系数为11.5~12.5,其余同例1。

Claims (1)

1.一种精毛纺织物经向间隔绒面产品的生产方法,其特征在于:它是选用全毛或毛涤纱线作经纱,全棉或丝棉混纺纱、或丝与再生性纤维素纤维混纺纱作纬纱,通过变化的纬浮长组织制织,采用洗呢、煮呢、烘呢、起绒、剪毛、给湿、蒸呢后整理工艺生产精毛纺织物经向间隔绒面产品,其具体方法包括:
a)纬纱选择:
纬纱选用长绒棉,长绒棉手扯长度33-45mm,细度细于143mtex;或:
纬纱选用丝棉混纺纱,丝棉混纺纱蚕丝纤维的纤度为2.5-3.5旦,单丝截面呈角圆的三角形;或:
纬纱即起绒纱选用丝与再生性纤维素纤维混纺纱,
b)纬纱纱线结构:
纬纱捻系数为11.5~12.5,
c)织物结构:
选用1/3、3/1联合变化组织为基础,
d)起毛工艺及后整理工艺控制:
起毛之前先进行绳状洗呢,(1)初洗:坯布上机,温度38℃±5℃,冲洗5min±2min,(2)皂洗:温度40℃±5℃,浴比:1∶6-10,净洗剂用量1.5-2.0%,油皂酸用量1.5-2.0%,时间40min-45min,呢速120-150m/min,(3)冲洗;用温度36℃±5℃,浴比:1∶13-16,连续冲洗30min±5min,再用温度30℃±5℃冲洗10min±5min,
煮呢采用双槽煮呢,煮多次,前几次加压,温度为80℃-85℃,PH6.5-7,槽外喷水冷却出机,
烘呢工艺为:机内温度为100℃-110℃,呢速12-15m/min,经向超喂4%-5%,拉幅3-5cm,烘呢结束,回潮控制在8%-12%之间,
起毛工艺采用干起毛和湿起毛相结合的工艺,在干起毛工艺中,顺辊和逆辊都采用零点起毛,采用植针角80°,工作角40°针布,以柔和的方式形成短毛,然后增大布速和顺辊转速,减低逆辊转速,干起毛起三次以上;湿起毛采用刺果湿起毛,
剪毛工艺采用织物速度10-12m/min,螺旋刀速度1100r/min,正面剪几次,反面剪一次,隔距为20-30丝,
蒸呢之前给湿,控制其回潮率为12%-15%,并存放8小时±2小时,
蒸呢工艺为蒸汽压力在1.2-2.5kg/cm2,内汽10-12min,抽冷8-10min。
CN 200610038781 2006-03-07 2006-03-07 精毛纺织物经向间隔绒面产品的生产方法 Active CN1818176B (zh)