CN1438276A - 衰减x射线的树脂纳米硫酸钡复合材料 - Google Patents
衰减x射线的树脂纳米硫酸钡复合材料 Download PDFInfo
- Publication number
- CN1438276A CN1438276A CN 03111911 CN03111911A CN1438276A CN 1438276 A CN1438276 A CN 1438276A CN 03111911 CN03111911 CN 03111911 CN 03111911 A CN03111911 A CN 03111911A CN 1438276 A CN1438276 A CN 1438276A
- Authority
- CN
- China
- Prior art keywords
- resin
- barium sulfate
- nano barium
- resin nano
- hours
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
利用一种新的制备方法合成树脂纳米硫酸钡复合材料用于吸收衰减X射线,使其比通常相对应的硫酸钡悬浊液衰减强度高三倍以上。该物质由离子交换树脂、氯化钡、硫酸钠、粘合剂和无机填料合成复配而成。
Description
技术领域
本发明涉及一种衰减X射线的复合材料,更具体的说,涉及一种对生物有机体有较强伤害的X射线的吸收和衰减并对人体起防护作用的树脂纳米硫酸钡复合材料。
技术背景
硫酸钡悬浊液有较强衰减X射线的能力,在医疗上用作检测消化道疾病的X光透视的钡餐。由于该化合物化学结构稳定性极好,而且对X射线的衰减能力强,因此硫酸钡不仅在医学上有着广泛用途,而且,在工业上也可以作为填充原料用于防止电磁辐射和X射线对人的伤害。
中国专利01107744公开了“超细硫酸钡制备方法”它是由溶胶凝胶法,利用氢氧化钡和稀硫酸形成溶胶制得的30%含量的水溶胶体系。主要用于防辐射纤维用添加物。中国专利02112879公开了“从杂质离子悬浮液中分离超细沉淀硫酸钡颗粒的方法”该方法利用悬浮液沿滤膜循环分离回收超细沉淀硫酸钡。以上发明专利制备的超细硫酸钡颗粒在水溶液里形成稳定的胶体分散体系,但是不能作成固体材料使用。
发明内容
本发明的目的在于克服上述现有技术中存在的缺陷,提供了一种既能强烈衰减X射线,也能保持长期稳定性,并且可以根据不司用途,制备工业用、民用、医用各种强衰减X射线的树脂硫酸钡粉,树脂硫酸钡悬浮液,树脂硫酸钡板材。该发明在X光机和X线CT上进行实验,与通常硫酸钡悬浊液(钡餐)相比,树脂硫酸钡的衰减X射线的能力提高3倍以上。而且使用方便,易于推广。本发明提供的这种树脂硫酸钡复合材料,包括如下组份,各组分组成按重量份数计:
组分 配比
树脂纳米硫酸钡 50-80
粘合剂 0-10
无机填料 0-50
上述的树脂纳米硫酸钡复合材料,所述的制备方法是,把粘合剂加到树脂纳米硫酸钡中搅拌均匀,然后加适量无机填料搅拌均匀,在40-80℃下干燥24小时-100小时为止。
上述的树脂纳米硫酸钡复合材料,所述树脂纳米硫酸钡,包括如下组份,各组份组成按重量份数计:
组分 配比
离子交换树脂 100
氯化钡 60-120
硫酸钠 100-120
无离子水 1500-2000
上述的树脂纳米硫酸钡复合材料,所述树脂纳米硫酸钡的制备方法是:
首先把离子交换树脂进行纯化。并称取100份放入容器中,然后把30-60份氯化钡溶在500份无离子水中。混合搅拌至全部溶解后放入盛有离子交换树脂的容器中,在电磁搅拌下浸泡搅拌2小时,用砂芯漏斗过滤后在35℃±5℃下静止存放2个小时,再用等量的氯化钡水溶液浸泡搅拌上述离子交换树脂2小时后再过滤,过滤后用无离子水冲洗,直到无游离的钡离子为止。另外把100-120份硫酸钠配成500份水溶液加到上述体系中,混合搅拌2小时,然后在35℃±5℃下过滤并静止稳定8小时。用无离子水洗涤至无硫酸根为止,然后在80℃±5℃条件下干燥,便得到由树脂包敷的50-150nm的树脂纳米硫酸钡。
上述的树脂纳米硫酸钡,所述离子交换树脂是医用或工业用酸性阳离子交换树脂,粒度在20-1000目之间。
上述的树脂纳米硫酸钡复合材料,所述粘合剂是环氧树脂粘合剂,环氧树脂粘合剂指的是国产双酚A型环氧树脂粘合剂。
上述的树脂纳米硫酸钡复合材料所述的无机填料是蒙脱土、硅粉或金刚粉。
该树脂纳米硫酸钡复合材料具有以下特点:1、用医用离子交换树脂交换制备的包敷树脂硫酸钡,色泽浅黄透明、无味、无臭、无毒害、稳定性好,可以研磨成粉状。2、加入粘合剂的或加入粘合剂和无机填料的制成的树脂纳米硫酸钡复合材料可以根据需要做成各种型材。3、由于本发明使用的离子交换树脂稳定性好,耐热、耐电磁波、耐辐射,可以进一步拓宽该树脂纳米硫酸钡复合材料的应用领域。
具体实施方案实例1
树脂纳米硫酸钡合成配方以重量份数计:
组分 配比
离子交换树脂 100
氯化钡 120
硫酸钠 120
无离子水 1500-2000
上述树脂纳米硫酸钡的合成配方,所述的制备方法举例:
首先把离子交换树脂进行纯化。并称取100克放入烧杯中。然后把60克氯化钡溶在500毫升无离子水中,混合搅拌至全部溶解后放入盛有离子交换树脂的烧杯中,在电磁搅拌下浸泡搅拌2个小时,用砂芯漏斗过滤后在35℃±5℃下静止存放2小时,再用等量的氯化钡水溶液浸泡搅拌上述离子交换树脂2小时后再过滤,过滤后用无离子水冲洗直到无游离的钡离子为止。另外把120克硫酸钠配成500ml水溶液加到上述体系中,混合搅拌2小时,然后在35℃±5℃下过滤并静止稳定8小时。用无离子水洗涤至无硫酸根为止,然后在80℃条件下干燥,便得到在树脂包敷的50-150nm的树脂纳米硫酸钡。±5℃实例2
树脂纳米硫酸钡复合材料配方(一)以重量份数计
组分 配比
树脂纳米硫酸钡 95
环氧树脂(E51) 5
(其中“650聚酰胺”占50%)
(固化剂用二乙烯三胺)
上述的树脂纳米硫酸钡复合材料,所述制备方法是:
粘合剂和树脂纳米硫酸钡搅拌均匀为止,然后在45℃±5℃下干燥24小时。
实例3
树脂纳米硫酸钡复合材料(二)以重量份数计
组分 配比
树脂纳米硫酸钡 90
环氧树脂(E51) 5
(其中“650聚酰胺”占50%)
硅粉 5上述的树脂纳米硫酸钡复合材料的制备方法是:
把环氧树脂加到树脂纳米硫酸钡中,搅拌均匀,然后加入硅粉搅拌均匀,在50℃下干燥24小时。使用效果一览表仪器:菲力浦X线螺旋扫描CT型号:DHF-155HII
材料名称 | 规格 | CT值1 | CT值2 | 平均CT值 |
硫酸钡 | 普通型20%水悬浮液 | 920 | 926 | 923 |
树脂纳米硫酸钡 | 15%水悬浮液 | 2895 | 2895 | 2895 |
树脂纳米硫酸钡材料(一) | 板材 | 3624 | 3246 | 3435 |
树脂纳米硫酸钡材料(二) | 板材 | 3759 | 3331 | 3545 |
水 | 无离子水 | 0 | 0 | 0 |
Claims (7)
1、一种强衰减X射线的树脂纳米硫酸钡复合材料,其特征在于,它是按以下重量配比的组份为原料配制而成
组份 配比
树脂纳米硫酸钡 50-80
粘合剂 0-10
无机填料 0-50、
2、根据权利要求1所述的树脂纳米硫酸钡复合材料,其特征在于,所述的制备方法是:把粘合剂加到树脂纳米硫酸钡中,搅拌均匀,然后加适量无机填料搅拌均匀,在40-80℃下干燥24小时-100小时为止。
3、根据权利要求1所述的树脂纳米硫酸钡复合材料,其特征在于,所述树脂纳米硫酸钡,它是按以下重量配比的组份为原料配制而成
组份 配比
离子交换树脂 100
氯化钡 60-120
硫酸钠 100-120
无离子水 1500-2000
4、根据权利要求1所述的树脂纳米硫酸钡复合材料,其特征在于,所述树脂纳米硫酸钡制备方法是:
首先把离子交换树脂进行纯化。并称取100份放入容器中,然后把30-60份氯化钡溶在500份无离子水中。混合搅拌至全部溶解后放入盛有离子交换树脂的容器中,在电磁搅拌下浸泡搅拌2小时,用砂芯漏斗过滤后在35℃±5℃下静止存放2小时,再用等量的氯化钡水溶液浸泡搅拌上述离子交换树脂2小时后再过滤,过滤后用无离子水冲洗直到无游离的钡离子为止。另外把100-120份硫酸钠配成500份水溶液加到上述体系中,混合搅拌2小时,然后在35℃±5℃下过滤并静止稳定8小时。用无离子水洗涤至无硫酸根为止,然后在80℃±5℃条件下干燥,便得到由树脂包敷的50-150nm的树脂纳米硫酸钡。
5、根据权利要求3所述的树脂纳米硫酸钡,其特征在于,所述离子交换树脂是医用或工业用酸性阳离子交换树脂。粒度在20-1000目。
6、根据权利要求1所述的树脂纳米硫酸钡复合材料,其特征在于,所述粘合剂是环氧树脂粘合剂,环氧树脂粘合剂指的是国产双酚A型环氧树脂粘合剂。
7、根据权利要求1所述的树脂纳米硫酸钡复合材料,其特征在于,所述的无机填料是蒙脱土、硅粉或金刚粉。