CN108914655B - 提高毛针织品色牢度的整理方法 - Google Patents

提高毛针织品色牢度的整理方法 Download PDF

Info

Publication number
CN108914655B
CN108914655B CN201810426085.8A CN201810426085A CN108914655B CN 108914655 B CN108914655 B CN 108914655B CN 201810426085 A CN201810426085 A CN 201810426085A CN 108914655 B CN108914655 B CN 108914655B
Authority
CN
China
Prior art keywords
wool
knitwear
washing
water
fabric
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201810426085.8A
Other languages
English (en)
Other versions
CN108914655A (zh
Inventor
郝海军
毛继鸿
汪大志
葛超群
任静
李越
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
ZHUHAI JIANXUAN GARMENT CO Ltd
Original Assignee
ZHUHAI JIANXUAN GARMENT CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by ZHUHAI JIANXUAN GARMENT CO Ltd filed Critical ZHUHAI JIANXUAN GARMENT CO Ltd
Priority to CN201810426085.8A priority Critical patent/CN108914655B/zh
Publication of CN108914655A publication Critical patent/CN108914655A/zh
Application granted granted Critical
Publication of CN108914655B publication Critical patent/CN108914655B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明涉及一种提高毛针织品色牢度的整理方法,包括:将毛针织品用含有强力去污精的水溶液进行洗涤;用蒸气对毛针织品进行至少一次透蒸整理;用含有织物膨松剂的水溶液进行洗涤;用含有织物树脂整理剂的水溶液进行洗涤;以及脱水、烘干的步骤。该方法通过特定的洗水处理对毛针织品进行纤维表面和内部处理,提高毛针织品对光的抵抗力、减缓日光的还原作用导致的偶氮类活性染料断健,增强毛针织品中的染料在水中和酸碱溶液中的稳定度,使毛针织品摩擦中脱落的染料浮色和有色纤维微粒子变少,从而综合提高毛针织品的色牢度。

Description

提高毛针织品色牢度的整理方法
技术领域
本发明涉及纺织整理技术领域,特别是涉及一种提高毛针织品色牢度的整理方法。
背景技术
根据纺织行业FZ/T 73018-2012《毛针织品》标准要求,一等品耐汗渍色牢度、耐水色牢度、耐摩擦色牢度、耐光色牢度、耐干洗色牢度达到3级为合格。但是一些毛针织品成衣送检色牢度并不能达到标准,导致衣服在穿着和洗涤时严重脱色,这一品质问题会严重影响产品使用性能,严重影响客户对产品的使用体验,从而影响品牌信誉。因此,急需开发一种提高毛针织品色牢度的方法。
发明内容
基于此,本发明的目的是提供一种提高毛针织品色牢度的整理方法。
具体的技术方案如下:
一种提高毛针织品色牢度的整理方法,包括如下步骤:
(1)将毛针织品用含有强力去污精的水溶液进行洗涤;
(2)将经过步骤(1)洗涤后的毛针织品进行脱水,再平铺放置于洗水机滚筒内胆中,打开洗水机外壳盖,从毛针织品下方放入蒸气对毛针织品进行至少一次透蒸整理;
(3)将经过步骤(2)整理后的毛针织品静置至常温,然后用含有织物膨松剂的水溶液进行洗涤;
(4)将步骤(3)洗涤后的毛针织品用含有织物树脂整理剂的水溶液进行洗涤;
(5)将步骤(4)洗涤后的毛针织品脱水、烘干,即得。
在其中一些实施例中,步骤(1)所述含有强力去污精的水溶液的浓度为0.7-1.5g/L。
在其中一些实施例中,步骤(3)所述含有织物膨松剂的水溶液中织物膨松剂的浓度为4-7g/L。
在其中一些实施例中,步骤(4)所述含有织物树脂整理剂的水溶液中织物树脂整理剂的浓度为6-13g/L。
在其中一些实施例中,步骤(1)所述洗涤的水温为18-26℃。
在其中一些实施例中,步骤(2)所述蒸气的气压为0.35-0.45MPa。
在其中一些实施例中,步骤(4)所述洗涤的水温为36-42℃。
在其中一些实施例中,步骤(5)所述烘干的温度为82-90℃,所述烘干的时间为20-28min。
在其中一些实施例中,所述提高毛针织品色牢度的整理方法包括如下步骤:
(1)洗水机中进水,加入强力去污精和毛针织品,洗涤,浸泡,排水,再加清水洗涤,排水;或者先将毛针织品置于洗水机中,进水,加入强力去污精,洗涤,浸泡,排水,再加清水洗涤,排水;
(2)将经过步骤(1)洗涤后的毛针织品放置于脱水机内进行脱水,再平铺放置于洗水机滚筒内胆中,打开洗水机外壳盖,从毛针织品下方放入蒸气对毛针织品进行透蒸整理,停止进气,静置,再次从毛针织品下方放入蒸气对毛针织品进行二次透蒸整理;
(3)将经过步骤(2)整理后的毛针织品在洗水机中静置至常温,然后洗水机中进水,加入织物膨松剂,洗涤,浸泡,再洗涤,排水;
(4)洗水机中进水,加入织物树脂整理剂,运行,再加入步骤(3)洗涤后的毛针织品,洗涤,浸泡,再洗涤,排水;
(5)将步骤(4)洗涤后的毛针织品脱水后置于烘干机中烘干,即得。
在其中一些实施例中,步骤(1)包括:将毛针织品置于洗水机中,进水,浴比为2.5-6%owf,再按终浓度为0.7-1.5g/L加入强力去污精,在水温为18-26℃的条件下洗涤2-4min,然后浸泡10-15min,排水,再加清水洗涤1-2min,排水;或者
洗水机中进水,按终浓度为0.7-1.5g/L加入强力去污精,在水温为18-26℃的条件下运行1-2min,加入毛针织品,浴比为2.5-6%owf,在水温为18-26℃的条件下洗涤2-4min,然后浸泡10-15min,排水,再加清水洗涤1-2min,排水。
在其中一些实施例中,步骤(2)包括:步骤(2)包括:将经过步骤(1)洗涤后的毛针织品放置于脱水机内进行脱水,再平铺放置于洗水机滚筒内胆中,打开洗水机外壳盖,从毛针织品下方放入气压为0.35-0.45MPa的蒸气对毛针织品进行透蒸整理,时间为2-3min,停止进气,静置10-15min,再次从毛针织品下方放入气压为0.35-0.45MPa的蒸气对毛针织品进行二次透蒸整理,时间为2-3min。
在其中一些实施例中,步骤(3)包括:将经过步骤(2)整理后的毛针织品在洗水机中静置至常温,然后洗水机中进水,浴比为3-5%owf,按终浓度为4-7g/L加入织物膨松剂,洗涤2-3min,然后浸泡10-15min,再洗涤1-2min,排水。
在其中一些实施例中,步骤(4)包括:洗水机中进水,按终浓度为6-13g/L加入织物树脂整理剂,在水温为36-42℃的条件下运行1-2min,再加入步骤(3)洗涤后的毛针织品,浴比为3-6%owf,洗涤2-3min,然后浸泡20-30min,再洗涤3-5min,排水;所述洗涤和浸泡的水温均为36-42℃。
在其中一些实施例中,所述强力去污精为强力去污精360。
在其中一些实施例中,所述织物膨松剂为SC织物膨松剂。
在其中一些实施例中,所述SC织物膨剂为SC-313羊毛膨松剂和/或SC-106羊绒膨松剂。最优选为SC-313羊毛膨松剂。
在其中一些实施例中,所述织物树脂整理剂为208织物整理剂和/或3308织物整理剂。最优选为208织物整理剂。
本发明的提高毛针织品色牢度的整理方法的原理及优点如下:
本发明的整理方法通过特定洗水处理对毛针织品进行纤维表面和内部处理,提高毛针织品对光的抵抗力、减缓日光的还原作用导致的偶氮类活性染料断健;增强毛针织品中的染料在水中和酸碱溶液中的稳定度;使毛针织品摩擦中脱落的染料浮色和有色纤维微粒子变少,从而增强毛针织品的耐光、水、汗渍、摩擦等各项色牢度,综合提高毛针织品的色牢度。
其中,采用强力去污精进行洗涤处理,适度去除一些附着在毛针织品纤维表面的浮色,同时其渗透能力强,能增加织物的光泽度,减缓日光的还原作用,优化毛纤维内部大分子结构排列,提高耐干、湿摩擦强度。对毛针织品进行脱水后平铺,由下方放入蒸气,打开洗水机上盖进行蒸气(优选气压为0.35-0.45MPa)透蒸(优选两次透蒸)处理,毛针织品迅速升温,纤维主干和鳞片包裹蒸气,使染料中活性反应基团分子活跃,增强染料对羊毛纤维的渗透、吸附牢度。打开洗水机上盖使蒸气快速排出,可以避免蒸气冷凝后滴湿、润湿毛针织品致其含热水量过大。采用膨松剂对毛针织品进行浸泡洗涤能够对羊毛鳞片和主干进行膨化舒张,与染料分子反应,提高染料在纤维内部和表面的稳定性。再使用整理剂对毛针织品进行洗涤(优选水温36-42℃),整理剂不仅能与染料分子反应,而且能与羊毛纤维素交联,使染料与纤维更牢固地结合,能够有效提高染料的皂洗牢度。最后烘干时在羊毛纤维表面形成立体网状聚合物薄膜,使染料进一步牢固地附着在织物上。
本发明的整理方法中各步骤的处理和助剂的添加需按特定的顺序进行,比如:如果将步骤2调至步骤1,先进行蒸气透蒸处理,不利于强力去污精增加织物的光泽度,减缓日光的还原作用,而且提高耐干、湿摩擦强度作用不明显,同时不利于步骤3中采用膨松剂对羊毛纤维的处理,影响毛针品各项色牢度性能的提高。本发明的整理方法各步骤按序进行,协同配合,从而达到提高毛针织品的综合色牢度的目的。
通过对各步骤中处理助剂的浓度和种类,处理温度等工艺参数的进一步优选,可以进一步提高整理后毛针织品的综合色牢度。
具体实施方式
以下结合具体实施例对本发明的提高毛针织品色牢度的整理方法做进一步详细的说明。
本发明实施例所使用的原料如下:
强力去污精,pH值:6-8,离子性:非离子,透明油状,纺织化工公司皆有类似产品。
强力去污精360,PH值:7,离子性:非离子,透明液体,购自东莞三川化工公司。
织物膨松剂,pH值:5-7.5,离子性:阳离子/非离子,黄色至乳白色粘稠液体,纺织化工公司皆有类似产品。织物膨松剂包括SC织物膨松剂等品种。
SC织物膨松剂,pH值:6-7.5,离子性:阳离子/非离子,淡黄至乳白色粘稠液体,购自东莞三川化工公司。SC织物膨松剂包括SC-106羊绒膨松剂和SC-313羊毛膨松剂等细分单品。
SC-106羊绒膨松剂,pH值:5.5-7.5,离子性:阳离子/非离子,淡黄色粘稠液体,购自东莞三川化工公司。
SC-313羊毛膨松剂,pH值:6-7,离子性:阳离子,乳白色粘稠液,购自东莞三川化工公司)。
织物树脂整理剂,pH值:5-7.5,离子性:阳离子,淡黄至乳白色粘稠或浆状液,纺织化工公司皆有类似产品。织物树脂整理剂包括208织物整理剂和3308织物整理剂等具体品种。
3308织物整理剂,PH值:5.5-7,离子性:阳离子,乳白色浆状液,购自东莞三川化工公司。
208织物整理剂,pH值:5-6,离子性:弱阳离子,乳白色浆状液,购自东莞三川化工公司。
以下为具体的实施例。
实施例1
本实施例提供的提高毛针织品色牢度的整理方法包括如下步骤:
(1)将毛针织品置于洗水机中,进水,浴比为6%owf,按终浓度为0.7g/L加入强力去污精360,常温(20℃)洗涤3min,浸泡10min,排水,加清水洗涤1min,排水。
(2)将经过步骤(1)洗涤后的毛针织品放置于脱水机内进行脱水,再平铺放置于洗水机滚筒内胆中,打开洗水机外壳盖,从毛针织品下方放入蒸气对毛针织品进行透蒸整理,气压为0.35MPa,时间为3min,停止进气,静置10min,再次放入蒸气对毛针织品进行二次透蒸整理,气压为0.35MPa,时间为3min。
(3)将经过步骤(2)整理后的毛织针品在洗水机中静置至常温,洗水机中进水,浴比为5%owf,按终浓度为4g/L加入SC-106羊绒膨松剂,洗涤2min,浸泡10min,再洗涤1min,排水。
(4)洗水机中进水,按终浓度为6g/L加入3308织物整理剂,水温38℃,运行1min,加入步骤(3)洗涤后的毛针织品,浴比为6%owf,洗涤2min,浸泡20min,再洗涤4min,排水。
(5)将步骤(4)洗涤后的毛针织品脱水后置于烘干机中,82℃烘干21min,即得。
实施例2
本实施例提供的提高毛针织品色牢度的整理方法包括如下步骤:
(1)洗水机中进水,按终浓度为1.5g/L加入强力去污精360,水温20℃,运行1min,加入毛针织品,浴比为6%owf,洗涤2min,浸泡15min,排水,加清水洗涤2min,排水。
(2)将经过步骤(1)洗涤后的毛针织品放置于脱水机内进行脱水,再平铺放置于洗水机滚筒内胆中,打开洗水机外壳盖,从毛针织品下方放入蒸气对毛针织品进行透蒸整理,气压为0.4MPa,时间为3min,停止进气,静置15min,再次放入蒸气对毛针织品进行二次透蒸整理,气压为0.4MPa,时间为2min。
(3)将经过步骤(2)整理后的毛织针品在洗水机中静置至常温,洗水机中进水,浴比为3%owf,按终浓度为5g/L加入SC-106羊绒膨松剂,洗涤3min,浸泡15min,再洗涤2min,排水。
(4)洗水机中进水,按终浓度为9g/L加入208织物整理剂,水温40℃,运行1min,加入步骤(2)洗涤后的毛针织品,浴比为4%owf,洗涤2min,浸泡20min,再洗涤3min,排水。
(5)将步骤(4)洗涤后的毛针织品脱水后置于烘干机中,88℃烘干25min,即得。
实施例3
本实施例提供的提高毛针织品色牢度的整理方法包括如下步骤:
(1)洗水机中进水,按终浓度为1.0g/L加入强力去污精360,水温18℃,运行1min,加入毛针织品,浴比为5%owf,洗涤2min,浸泡15min,排水,加清水洗涤2min,排水。
(2)将经过步骤(1)洗涤后的毛针品放置于脱水机内进行脱水,再平铺放置于洗水机滚筒内胆中,打开洗水机外壳盖,从毛针织品下方放入蒸气对毛针织品进行透蒸整理,气压为0.45MPa,时间为2min,停止进气,静置10min,再次放入蒸气对毛针织品进行二次透蒸整理,气压为0.45MPa,时间为2min。
(3)将经过步骤(2)整理后的毛织针品在洗水机中静置至常温,洗水机中进水,浴比为3%owf,按终浓度为7g/L加入SC-313羊毛膨松剂,洗涤2min,浸泡10min,再洗涤2min,排水。
(4)洗水机中进水,按终浓度为13g/L加入208织物整理剂,水温38℃,运行1min,加入步骤(3)洗涤后的毛针织品,浴比为5%owf,洗涤2min,浸泡30min,再洗涤5min,排水。
(5)将步骤(4)洗涤后的毛针织品脱水后置于烘干机中,90℃烘干20min,即得。
实施例4
本实施例提供的提高毛针织品色牢度的整理方法包括如下步骤:
(1)洗水机中进水,按终浓度为1.2g/L加入强力去污精360,水温26℃,运行1min,加入毛针织品,浴比为4%owf,洗涤3min,浸泡15min,排水,加清水洗涤2min,排水;
(2)将经过步骤(1)洗涤后的毛针织品放置于脱水机内进行脱水,再平铺放置于洗水机滚筒内胆中,打开洗水机外壳盖,从毛针织品下方放入蒸气对毛针织品进行透蒸整理,气压为0.42MPa,时间为3min,停止进气,静置15min,再次放入蒸气对毛针织品进行二次透蒸整理,气压为0.42MPa,时间为2min。
(3)将经过步骤(2)整理后的毛织针品在洗水机中静置至常温,洗水机中进水,浴比为4%owf,按终浓度为6g/L加入SC-313羊毛膨松剂,洗涤2min,浸泡15min,再洗涤2min,排水。
(4)洗水机中进水,按终浓度为12g/L加入208织物整理剂,水温40℃,运行1min,加入步骤(3)洗涤后的毛针织品,浴比为3%owf,洗涤2min,浸泡30min,再洗涤5min,排水。
(5)将步骤(4)洗涤后的毛针织品脱水后置于烘干机中,88℃烘干25min,即得。
对比例1
本对比例提供的提高毛针织品色牢度的整理方法中,蒸气透蒸整理与强力去污精360洗涤的整理步骤与实施例4相比进行了对换。具体包括如下步骤:
(1)将毛针织品平铺放置于洗水机滚筒内胆中,打开洗水机外壳盖,从毛针织品下方放入蒸气对毛针织品进行透蒸整理,气压为0.42MPa,时间为3min,停止进气,静置15min,再次放入蒸气对毛针织品进行二次透蒸整理,气压为0.42MPa,时间为2min。
(2)将经过步骤(1)整理后的毛织针品静置至常温,洗水机中进水,按终浓度为1.2g/L加入强力去污精360,水温26℃,运行1min,加入静置至常温的毛针织品,浴比为4%owf,洗涤3min,浸泡15min,排水,加清水洗涤2min,排水。
(3)洗水机中进水,浴比为4%owf,按终浓度为6g/L加入SC-313羊毛膨松剂,洗涤2min,浸泡15min,再洗涤2min,排水。
(4)洗水机中进水,按终浓度为12g/L加入208织物整理剂,水温40℃,运行1min,加入步骤(3)洗涤后的毛针织品,浴比为3%owf,洗涤2min,浸泡30min,再洗涤5min,排水;
(5)将步骤(4)洗涤后的毛针织品脱水后置于烘干机中,88℃烘干25min,即得。
实验例
对用实施例和对比例的整理方法整理后的毛针织品进行织物色牢度性能测试,采用12件纱线成份为2\48NM 100%羊毛,颜色为沐绿(#65)的成衣(单边组织)进行色牢度性能测试。此12件成衣分为6组检测,每组成衣2件,第1组不进行整理,直接进行测试,第2-5组用实施例1-4的整理方法进行整理后再进行测试,第6组用对比例1的整理方法进行整理后再进行测试。结果如下:
Figure BDA0001652123370000071
通过未经织物色牢度性能整理的2件成衣的色牢度值与实施例1、实施例2、实施例3、实施例4的色牢度值对比,我们可以明显发现,经过本发明所述的提高毛针织品色牢度的整理方法整理后的成衣,能有效提高其色牢度性能,且对于不同颜色的成衣皆能整体提升色牢度性能。
对比例结果显示,改变本发明的整理方法中的蒸气透蒸整理与强力去污精360洗涤整理的顺序,会显著影响毛针织品色牢度性能的提高。
以上所述实施例的各技术特征可以进行任意的组合,为使描述简洁,未对上述实施例中的各个技术特征所有可能的组合都进行描述,然而,只要这些技术特征的组合不存在矛盾,都应当认为是本说明书记载的范围。
以上所述实施例仅表达了本发明的几种实施方式,其描述较为具体和详细,但并不能因此而理解为对发明专利范围的限制。应当指出的是,对于本领域的普通技术人员来说,在不脱离本发明构思的前提下,还可以做出若干变形和改进,这些都属于本发明的保护范围。因此,本发明专利的保护范围应以所附权利要求为准。

Claims (10)

1.一种提高毛针织品色牢度的整理方法,其特征在于,包括如下步骤:
(1)将毛针织品用含有强力去污精的水溶液进行洗涤;所述强力去污精为强力去污精360;
(2)将经过步骤(1)洗涤后的毛针织品进行脱水,再平铺放置于洗水机滚筒内胆中,打开洗水机外壳盖,从毛针织品下方放入蒸气对毛针织品进行至少一次透蒸整理;
(3)将经过步骤(2)整理后的毛针织品静置至常温,然后用含有织物膨松剂的水溶液进行洗涤;所述织物膨松剂为SC织物膨松剂;
(4)将步骤(3)洗涤后的毛针织品用含有织物树脂整理剂的水溶液进行洗涤;所述织物树脂整理剂为208织物整理剂和/或3308织物整理剂;
(5)将步骤(4)洗涤后的毛针织品脱水、烘干,即得。
2.根据权利要求1所述的提高毛针织品色牢度的整理方法,其特征在于,步骤(1)所述含有强力去污精的水溶液的浓度为0.7-1.5g/L;及/或,
步骤(3)所述含有织物膨松剂的水溶液中织物膨松剂的浓度为4-7g/L;及/或,
步骤(4)所述含有织物树脂整理剂的水溶液中织物树脂整理剂的浓度为6-13g/L。
3.根据权利要求1所述的提高毛针织品色牢度的整理方法,其特征在于,步骤(1)所述洗涤的水温为18-26℃;及/或,
步骤(2)所述蒸气的气压为0.35-0.45MPa;及/或,
步骤(4)所述洗涤的水温为36-42℃;及/或,
步骤(5)所述烘干的温度为82-90℃,所述烘干的时间为20-28min。
4.根据权利要求1所述的提高毛针织品色牢度的整理方法,其特征在于,步骤(1)包括:将毛针织品置于洗水机中,进水,浴比为2.5-6%owf,再按终浓度为0.7-1.5g/L加入强力去污精,在水温为18-26℃的条件下洗涤2-4min,然后浸泡10-15min,排水,再加清水洗涤1-2min,排水;或者
洗水机中进水,按终浓度为0.7-1.5g/L加入强力去污精,在水温为18-26℃的条件下运行1-2min,加入毛针织品,浴比为2.5-6%owf,在水温为18-26℃的条件下洗涤2-4min,然后浸泡10-15min,排水,再加清水洗涤1-2min,排水。
5.根据权利要求1所述的提高毛针织品色牢度的整理方法,其特征在于,步骤(2)包括两次透蒸整理。
6.根据权利要求1所述的提高毛针织品色牢度的整理方法,其特征在于,步骤(2)包括:将经过步骤(1)洗涤后的毛针织品放置于脱水机内进行脱水,再平铺放置于洗水机滚筒内胆中,打开洗水机外壳盖,从毛针织品下方放入气压为0.35-0.45MPa的蒸气对毛针织品进行透蒸整理,时间为2-3min,停止进气,静置10-15min,再次从毛针织品下方放入气压为0.35-0.45MPa的蒸气对毛针织品进行二次透蒸整理,时间为2-3min。
7.根据权利要求1所述的提高毛针织品色牢度的整理方法,其特征在于,步骤(3)包括:将经过步骤(2)整理后的毛针织品在洗水机中静置至常温,然后洗水机中进水,浴比为3-5%owf,按终浓度为4-7g/L加入织物膨松剂,洗涤2-3min,然后浸泡10-15min,再洗涤1-2min,排水。
8.根据权利要求1所述的提高毛针织品色牢度的整理方法,其特征在于,步骤(4)包括:洗水机中进水,按终浓度为6-13g/L加入织物树脂整理剂,在水温为36-42℃的条件下运行1-2min,再加入步骤(3)洗涤后的毛针织品,浴比为3-6%owf,洗涤2-3min,然后浸泡20-30min,再洗涤3-5min,排水;所述洗涤和浸泡的水温均为36-42℃。
9.根据权利要求1-8任一项所述的提高毛针织品色牢度的整理方法,其特征在于,所述SC织物膨松剂为SC-313羊毛膨松剂和/或SC-106羊绒膨松剂。
10.根据权利要求1-8任一项所述的提高毛针织品色牢度的整理方法,其特征在于,所述织物树脂整理剂为208织物整理剂。
CN201810426085.8A 2018-05-07 2018-05-07 提高毛针织品色牢度的整理方法 Active CN108914655B (zh)