CN104526818A - 一种全uv软卷材木皮及其制备工艺 - Google Patents
一种全uv软卷材木皮及其制备工艺 Download PDFInfo
- Publication number
- CN104526818A CN104526818A CN201410760769.3A CN201410760769A CN104526818A CN 104526818 A CN104526818 A CN 104526818A CN 201410760769 A CN201410760769 A CN 201410760769A CN 104526818 A CN104526818 A CN 104526818A
- Authority
- CN
- China
- Prior art keywords
- roller
- curing
- coating
- coiled material
- roller coating
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
本发明涉及一种卷材,还涉及该卷材的制备工艺。一种全UV软卷材木皮,底部是无纺布层粘连而成的实木皮层,实木皮层上滚涂有UV涂层。所述UV涂层可以是透明涂层,也可以是有颜色涂层。本发明的全UV软卷材木皮可以直接包覆在各种造型的基材上,不用另外喷涂PU油漆,更环保及安全,而且生产周期短、效率高、质量好、生产成本底。用于中纤板贴实木皮家具板封边,装饰线条包覆、实木门框包覆等。
Description
技术领域
本发明涉及一种卷材,还涉及该卷材的制备工艺。
背景技术
目前市场上很多装饰线条和实木由封边条都是先包覆后喷涂PU油漆,这样的工艺在喷涂PU过程中产生漆雾严重影响身体健康。
发明内容
本发明所要解决的技术问题是提供一种全UV软卷材木皮,并提供其制备工艺,该UV软卷材木皮可以直接包覆在各种造型的基材上,不用另外喷涂PU油漆,更环保及安全,而且生产周期短、效率高、质量好、生产成本底。可用于中纤板贴实木皮家具板封边,装饰线条包覆、实木门框包覆等。
本发明所要解决的技术问题通过以下技术方案予以实现:
一种全UV软卷材木皮,底部是无纺布层粘连而成的实木皮层,实木皮层上滚涂有UV涂层。
作为本发明的其中一种实现方式,所述UV涂层为透明涂层。
作为本发明的其中一种实现方式,所述UV涂层为有颜色涂层。
其中,UV涂层为透明涂层的全UV软卷材木皮的制备工艺,依次包括如下步骤:
(1)实木皮卷材基材;(2)砂光毛刺;(3)滚涂UV透明腻子;(4)紫外线干燥;(5)正逆辊滚涂专用UV弹性底漆;(6)紫外线干燥;(7)正逆辊滚涂专用UV弹性砂光底;(8)紫外线干燥;(9)砂光。
进一步的,具体工艺步骤为:
(1)实木皮卷材基材:把实木皮通过无纺布粘连成为无限长度实木卷材;
(2)砂光毛刺:用砂纸打磨光滑;
(3)滚涂弹性UV透明腻子;
(4)紫外线干燥:双汞灯照射;
(5)正逆辊滚涂用UV弹性底漆;
(6)紫外线干燥:双汞灯照射;
(7)正逆辊滚涂UV弹性砂光底漆;
(8)紫外线干燥:用双汞灯照射;
(9)砂光。
其中,UV涂层为有颜色涂层的全UV软卷材木皮的制备工艺,依次包括如下步骤:
(1)实木皮卷材基材;(2)砂光毛刺;(3)海绵辊滚涂UV水性有色底漆;(4)毛刷擦色;(5)红外线干燥;(6)滚涂弹性UV透明腻子;(7)紫外线干燥;(8)正逆辊滚涂UV弹性底漆;(9)紫外线干燥;(10)正逆辊滚涂UV弹性砂光底漆;(11)紫外线干燥;(12)砂光;(13)单辊滚涂修色面漆;(14)紫外线干燥;(15)单辊滚涂弹性UV透明面漆;(16)紫外线干燥;(17)正逆辊滚涂弹性UV面漆;(18)紫外线干燥。
进一步的,具体工艺步骤为:
(1)实木皮卷材基材:把实木皮通过无纺布粘连成为无限长度实木卷材;
(2)砂光毛刺:用砂纸打磨光滑;
(3)海绵辊滚涂UV水性有色底漆;
(4)毛刷擦色:用毛刷进一步将上一步滚涂到基材上的有色底漆刷均匀;
(5)红外线干燥;
(6)滚涂弹性UV透明腻子;
(7)紫外线干燥:双汞灯照射;
(8)正逆辊滚涂UV弹性底漆;
(9)紫外线干燥:双汞灯照射;
(10)正逆辊滚涂UV弹性砂光底漆;
(11)紫外线干燥:双汞灯照射;
(12)砂光:用砂纸打磨光滑;
(13)单辊滚涂修色面漆;
(14)紫外线干燥:双汞灯照射;
(15)单辊滚涂弹性UV透明面漆:
(16)紫外线干燥:双汞灯照射;
(17)正逆辊滚涂弹性哑光或中光的UV面漆;
(18)紫外线干燥:双汞灯照射。
本发明具有如下有益效果:
本发明是把实木皮通过无纺布粘连成为无限长度实木卷材,在通过专用设备、专用能折弯软性UV 油漆经过砂光滚涂等把透明UV腻子、UV底漆、UV面漆等经过特殊工艺涂布在实木卷材上。本发明的UV软卷材木皮可以直接包覆在各种造型的基材上,不用另外喷涂PU油漆,更环保及安全,而且生产周期短、效率高、质量好、生产成本底,可用于中纤板贴实木皮家具板封边,装饰线条包覆、实木门框包覆等。
附图说明
图1为实施例1或2的截面结构示意图。
具体实施方式
下面结合实施例对本发明进行详细的说明,实施例仅是本发明的优选实施方式,不是对本发明的限定。
本发明中涂层使用的各种涂料(如UV水性有色底漆、弹性UV透明腻子、UV弹性底漆、UV弹性砂光底漆、修色面漆、弹性UV透明面漆、哑光或中光的UV面漆),都可以使用本领域公知的任何一种厂家和型号的该类产品。
实施例1
如图1所示,一种全UV软卷材木皮,底部是无纺布层1粘连而成的实木皮层2,实木皮层2上滚涂有UV涂层3,所述UV涂层3为透明涂层。
具体工艺步骤为:
(1)实木皮卷材基材:把实木皮通过无纺布粘连成为无限长度实木卷材;
(2)砂光毛刺:用砂纸打磨光滑;
(3)滚涂弹性UV透明腻子;
(4)紫外线干燥:双汞灯照射;
(5)正逆辊滚涂用UV弹性底漆;
(6)紫外线干燥:双汞灯照射;
(7)正逆辊滚涂UV弹性砂光底漆;
(8)紫外线干燥:用双汞灯照射;
(9)砂光:用砂纸打磨光滑。
实施例2
如图1所示,一种全UV软卷材木皮,底部是无纺布层粘连而成的实木皮层,实木皮层2上滚涂有UV涂层3,所述UV涂层3为有色涂层。
具体工艺步骤为:
(1)实木皮卷材基材:把实木皮通过无纺布粘连成为无限长度实木卷材;
(2)砂光毛刺:用砂纸打磨光滑;
(3)海绵辊滚涂UV水性有色底漆;
(4)毛刷擦色:用毛刷进一步将上一步滚涂到基材上的有色底漆刷均匀;
(5)红外线干燥;
(6)滚涂弹性UV透明腻子;
(7)紫外线干燥:双汞灯照射;
(8)正逆辊滚涂UV弹性底漆;
(9)紫外线干燥:双汞灯照射;
(10)正逆辊滚涂UV弹性砂光底漆;
(11)紫外线干燥:双汞灯照射;
(12)砂光:用砂纸打磨光滑;
(13)单辊滚涂修色面漆;
(14)紫外线干燥:双汞灯照射;
(15)单辊滚涂弹性UV透明面漆:
(16)紫外线干燥:双汞灯照射;
(17)正逆辊滚涂弹性哑光或中光的UV面漆;
(18)紫外线干燥:双汞灯照射。
Claims (7)
1.一种全UV软卷材木皮,其特征在于:底部是无纺布层(1)粘连而成的实木皮层(2),实木皮层上滚涂有UV涂层(3)。
2.根据权利要求1所述的全UV软卷材木皮,其特征在于:UV涂层(3)为透明涂层。
3.根据权利要求1所述的全UV软卷材木皮,其特征在于:UV涂层(3)为有颜色涂层。
4.一种权利要求2所述全UV软卷材木皮的制备工艺,其特征在于,依次包括如下步骤:
(1)实木皮卷材基材;(2)砂光毛刺;(3)滚涂UV透明腻子;(4)紫外线干燥;(5)正逆辊滚涂专用UV弹性底漆;(6)紫外线干燥;(7)正逆辊滚涂专用UV弹性砂光底;(8)紫外线干燥;(9)砂光。
5.根据权利要求4所述的全UV软卷材木皮的制备工艺,其特征在于,具体工艺步骤为:
(1)实木皮卷材基材:把实木皮通过无纺布粘连成为无限长度实木卷材;
(2)砂光毛刺:用砂纸打磨光滑;
(3)滚涂弹性UV透明腻子;
(4)紫外线干燥:双汞灯照射;
(5)正逆辊滚涂用UV弹性底漆;
(6)紫外线干燥:双汞灯照射;
(7)正逆辊滚涂UV弹性砂光底漆;
(8)紫外线干燥:用双汞灯照射;
(9)砂光。
6.一种权利要求3所述全UV软卷材木皮的制备工艺,其特征在于,依次包括如下步骤:
(1)实木皮卷材基材;(2)砂光毛刺;(3)海绵辊滚涂UV水性有色底漆;(4)毛刷擦色;(5)红外线干燥;(6)滚涂弹性UV透明腻子;(7)紫外线干燥;(8)正逆辊滚涂UV弹性底漆;(9)紫外线干燥;(10)正逆辊滚涂UV弹性砂光底漆;(11)紫外线干燥;(12)砂光;(13)单辊滚涂修色面漆;(14)紫外线干燥;(15)单辊滚涂弹性UV透明面漆;(16)紫外线干燥;(17)正逆辊滚涂弹性UV面漆;(18)紫外线干燥。
7.根据权利要求6所述的全UV软卷材木皮的制备工艺,其特征在于,具体工艺步骤为:
(1)实木皮卷材基材:把实木皮通过无纺布粘连成为无限长度实木卷材;
(2)砂光毛刺:用砂纸打磨光滑;
(3)海绵辊滚涂UV水性有色底漆;
(4)毛刷擦色:用毛刷进一步将上一步滚涂到基材上的有色底漆刷均匀;
(5)红外线干燥;
(6)滚涂弹性UV透明腻子;
(7)紫外线干燥:双汞灯照射;
(8)正逆辊滚涂UV弹性底漆;
(9)紫外线干燥:双汞灯照射;
(10)正逆辊滚涂UV弹性砂光底漆;
(11)紫外线干燥:双汞灯照射;
(12)砂光:用砂纸打磨光滑;
(13)单辊滚涂修色面漆;
(14) 紫外线干燥:双汞灯照射;
(15)单辊滚涂弹性UV透明面漆:
(16)紫外线干燥:双汞灯照射;
(17)正逆辊滚涂弹性哑光或中光的UV面漆;
(18)紫外线干燥:双汞灯照射。