CN103722044B - 高性能无缝钢管的生产方法 - Google Patents

高性能无缝钢管的生产方法 Download PDF

Info

Publication number
CN103722044B
CN103722044B CN201310621587.3A CN201310621587A CN103722044B CN 103722044 B CN103722044 B CN 103722044B CN 201310621587 A CN201310621587 A CN 201310621587A CN 103722044 B CN103722044 B CN 103722044B
Authority
CN
China
Prior art keywords
steel pipe
carried out
pipe
carry out
production method
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN201310621587.3A
Other languages
English (en)
Other versions
CN103722044A (zh
Inventor
须晓东
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Foshan Nanhai Hongxing Steel Tube Co., Ltd.
Original Assignee
CHANGSHU DONGXIN STEEL PIPE Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by CHANGSHU DONGXIN STEEL PIPE Co Ltd filed Critical CHANGSHU DONGXIN STEEL PIPE Co Ltd
Priority to CN201310621587.3A priority Critical patent/CN103722044B/zh
Publication of CN103722044A publication Critical patent/CN103722044A/zh
Application granted granted Critical
Publication of CN103722044B publication Critical patent/CN103722044B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种高性能无缝钢管的生产方法,包括如下步骤:1)选择总延伸率为4.8-7.7的钢管管坯;2)对管坯进行前处理;3)再对钢管进行4-5道冷拔;每道次延伸率1.2-1.3,总延伸率5.5-6.5;4)再对钢管进行无氧化光亮退火处理;5)再对钢管进行中间处理;6)再将钢管在三辊轧管机上进行冷轧,延伸率为1.2-1.25;7)再对钢管进行无氧化光亮正火处理;8)再对钢管进行后处理,包括矫直、无损探伤、精整;9)再对钢管表面进行无铬达克罗涂层处理,烘烤固化温度为300-330℃。本发明提供的高性能无缝钢管的生产方法,其生产效率高,无缝钢管产品尺寸精度高,加工性能好。

Description

高性能无缝钢管的生产方法
技术领域
本发明涉及高性能无缝钢管的生产方法。
背景技术
目前碳钢无缝钢管常用的冷加工方法主要有二种:
一种采用冷拔工艺管,其制造的钢管抗压能力较低、加工性能较差、内外表面的质量较低、强度较低、韧性不足,容易出现裂纹;
另一种采用冷轧工艺,其生产效率低。
发明内容
本发明的目的在于提供一种高性能无缝钢管的生产方法,其生产效率高,无缝钢管产品尺寸精度高,加工性能好。
为实现上述目的,本发明的技术方案是设计一种高性能无缝钢管的生产方法,包括如下步骤:
1)选择总延伸率为4.8-7.7的钢管管坯;
2)对管坯进行前处理,浸涂时间为20-25分钟,润滑液采用浓度为20-25%、pH值为11-12的高分子润滑剂配制,配液温度为60-65℃;
3)再对钢管进行4-5道冷拔;每道次延伸率1.2-1.3,总延伸率5.5-6.5;
4)再对钢管进行无氧化光亮退火处理;
5)再对钢管进行中间处理,浸涂时间为10-15分钟,润滑液采用浓度为15-20%、pH值为11-12的高分子润滑剂配制,配液温度为60-65℃;
6)再将钢管在三辊轧管机上进行冷轧,延伸率为1.2-1.25;
7)再对钢管进行无氧化光亮正火处理;
8)再对钢管进行后处理,包括矫直、无损探伤、精整;
9)再对钢管表面进行无铬达克罗涂层处理,烘烤固化温度为300-330℃。
本发明的优点和有益效果在于:提供一种高性能无缝钢管的生产方法,其生产效率高,无缝钢管产品尺寸精度高,加工性能好。
具体实施方式
下面结合实施例,对本发明的具体实施方式作进一步描述。以下实施例仅用于更加清楚地说明本发明的技术方案,而不能以此来限制本发明的保护范围。
本发明具体实施的技术方案是:
实施例1
一种高性能无缝钢管的生产方法,包括如下步骤:
1)选择总延伸率为7.7的钢管管坯;
2)对管坯进行前处理,浸涂时间为25分钟,润滑液采用浓度为25%、pH值为12的高分子润滑剂配制,配液温度为65℃;
3)再对钢管进行5道冷拔;每道次延伸率1.3,总延伸率6.5;
4)再对钢管进行无氧化光亮退火处理;
5)再对钢管进行中间处理,浸涂时间为15分钟,润滑液采用浓度为20%、pH值为12的高分子润滑剂配制,配液温度为65℃;
6)再将钢管在三辊轧管机上进行冷轧,延伸率为1.25;
7)再对钢管进行无氧化光亮正火处理;
8)再对钢管进行后处理,包括矫直、无损探伤、精整;
9)再对钢管表面进行无铬达克罗涂层处理,烘烤固化温度为330℃。
实施例2
一种高性能无缝钢管的生产方法,包括如下步骤:
1)选择总延伸率为4.8的钢管管坯;
2)对管坯进行前处理,浸涂时间为20分钟,润滑液采用浓度为20%、pH值为11的高分子润滑剂配制,配液温度为60℃;
3)再对钢管进行4道冷拔;每道次延伸率1.2,总延伸率5.5;
4)再对钢管进行无氧化光亮退火处理;
5)再对钢管进行中间处理,浸涂时间为10分钟,润滑液采用浓度为15%、pH值为11的高分子润滑剂配制,配液温度为60℃;
6)再将钢管在三辊轧管机上进行冷轧,延伸率为1.2;
7)再对钢管进行无氧化光亮正火处理;
8)再对钢管进行后处理,包括矫直、无损探伤、精整;
9)再对钢管表面进行无铬达克罗涂层处理,烘烤固化温度为300℃。
实施例3
一种高性能无缝钢管的生产方法,包括如下步骤:
1)选择总延伸率为5.7的钢管管坯;
2)对管坯进行前处理,浸涂时间为22分钟,润滑液采用浓度为24%、pH值为11.5的高分子润滑剂配制,配液温度为62℃;
3)再对钢管进行4道冷拔;每道次延伸率1.23,总延伸率6;
4)再对钢管进行无氧化光亮退火处理;
5)再对钢管进行中间处理,浸涂时间为12分钟,润滑液采用浓度为17%、pH值为11.5的高分子润滑剂配制,配液温度为62℃;
6)再将钢管在三辊轧管机上进行冷轧,延伸率为1.23;
7)再对钢管进行无氧化光亮正火处理;
8)再对钢管进行后处理,包括矫直、无损探伤、精整;
9)再对钢管表面进行无铬达克罗涂层处理,烘烤固化温度为320℃。
以上所述仅是本发明的优选实施方式,应当指出,对于本技术领域的普通技术人员来说,在不脱离本发明技术原理的前提下,还可以做出若干改进和润饰,这些改进和润饰也应视为本发明的保护范围。

Claims (1)

1.高性能无缝钢管的生产方法,其特征在于,包括如下步骤:
1)选择总延伸率为4.8-7.7的钢管管坯;
2)对管坯进行前处理,浸涂时间为20-25分钟,润滑液采用浓度为20-25%、pH值为11-12的高分子润滑剂配制,配液温度为60-65℃;
3)再对钢管进行4-5道冷拔;每道次延伸率1.2-1.3,总延伸率5.5-6.5;
4)再对钢管进行无氧化光亮退火处理;
5)再对钢管进行中间处理,浸涂时间为10-15分钟,润滑液采用浓度为15-20%、pH值为11-12的高分子润滑剂配制,配液温度为60-65℃;
6)再将钢管在三辊轧管机上进行冷轧,延伸率为1.2-1.25;
7)再对钢管进行无氧化光亮正火处理;
8)再对钢管进行后处理,包括矫直、无损探伤、精整;
9)再对钢管表面进行无铬达克罗涂层处理,烘烤固化温度为300-330℃。
CN201310621587.3A 2013-11-30 2013-11-30 高性能无缝钢管的生产方法 Expired - Fee Related CN103722044B (zh)