CN103570338B - 一种低温节能一遍烧成红土绘彩上釉陶制品的制造方法 - Google Patents

一种低温节能一遍烧成红土绘彩上釉陶制品的制造方法 Download PDF

Info

Publication number
CN103570338B
CN103570338B CN201310599149.1A CN201310599149A CN103570338B CN 103570338 B CN103570338 B CN 103570338B CN 201310599149 A CN201310599149 A CN 201310599149A CN 103570338 B CN103570338 B CN 103570338B
Authority
CN
China
Prior art keywords
parts
water
laterite
manufacture method
base substrate
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201310599149.1A
Other languages
English (en)
Other versions
CN103570338A (zh
Inventor
陈永定
陈国生
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
FUJIAN CHUNQIU CERAMIC INDUSTRY Co.,Ltd.
Original Assignee
陈永定
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 陈永定 filed Critical 陈永定
Priority to CN201310599149.1A priority Critical patent/CN103570338B/zh
Publication of CN103570338A publication Critical patent/CN103570338A/zh
Application granted granted Critical
Publication of CN103570338B publication Critical patent/CN103570338B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开一种低温节能一遍烧成红土绘彩上釉陶制品的制造方法,包括制造坯体、绘彩、制造釉水、上釉以及烧成等步骤。本发明改变了红土坯体的配方,减少红土在坯体中的比重,增加了坯体的烧结度,烧制时坯体中的气体及时得以释放,不会出现跳釉、起泡、剥壳等现象,只需一遍烧成即可,降低了烧成成本。

Description

一种低温节能一遍烧成红土绘彩上釉陶制品的制造方法
技术领域
    本发明涉及陶瓷工艺技术领域,特别是指一种低温节能一遍烧成红土绘彩上釉陶制品的制造方法。
背景技术
授权公告号CN101993237B是本申请人发明的一种低温红土绘彩上釉生态陶制品制造方法,该制造方法对传统的红土陶制品三次烧成的制造方法进行了改进,采用两次烧成,将红土坯体送入窑炉进行第一次烧制,取出后彩绘、上釉,再送入窑炉内第二次烧制得成品。该方法相对传统三次烧成降低了一定成本,但两次烧成能耗仍然较高。
红土陶制品之所以采用两次烧成,是因为采用传统配方的红土坯体,红土坯体中红土的比重较大,其体积密度也较大,同时,红土的烧结温度高,若红土坯体不是单独烧制,而是与釉一起烧制,在烧制过程中难以释放红土坯体因氧化、分解等反应产生的气体,容易出现跳釉、起泡、剥壳以及开裂等,即红土坯体与釉结合非常不好,破坏釉面的生成,故一次烧成很难做到红土坯体与釉的完美结合。为此,我们提供一种在低温下即能一遍烧成、且可使坯体与釉完美结合的红土绘彩上釉陶制品的制造方法。
发明内容
本发明提供一种低温节能一遍烧成红土绘彩上釉陶制品的制造方法,以解决传统红土陶制品制造方法无法一遍烧成等问题。
本发明采用如下的技术方案:
一种低温节能一遍烧成红土绘彩上釉陶制品的制造方法,包括如下步骤:
(1)制造坯体:将以下重量份数的原料混合:红土60-65份、长石5-10份、黑灰石5-10份、萤石5-10份、高岭土5-10份、石英5-10份、无铅熔块3-5份、滑石2-3份、水20-30份,混匀后研磨成土浆,将土浆注入模具中0.5-1小时后脱模成型,常温下自然风干,再经过修坯擦水处理后自然风干,制得坯体;
(2)绘彩:根据陶制品的器型、图案调配色料,并在步骤(1)中的坯体上进行绘彩;
(3)制造釉水:将以下重量分数的原料混合:低膨胀釉粉80-90份、氧化锌3-5份、着色剂10-15份、石英粉3-5份、碳酸钙2-5份、氧化钛2-5份、水30-40份,混匀后浸泡5-8小时,取出过滤后加入300-400份的水稀释得釉水;
(4)上釉:将步骤(2)中绘彩完成的坯体放入步骤(3)中制得的釉水中浸泡0.5-4秒;
(5)烧成:将上釉完成的产品在1020-1060℃烧制4-6小时,然后经6-10小时冷却后出窑得成品。
优选地,步骤(1)中制造坯体的各原料按以下重量分数混合:红土65份、长石5份、黑灰石5份、萤石5份、高岭土5份、石英5份、无铅熔块3份、滑石2份、水20份。
优选地,步骤(3)中制造釉水的各原料按以下重量分数混合:低膨胀釉粉80份、氧化锌3份、着色剂10份、石英粉3份、碳酸钙2份、氧化钛2份、水30份。
优选地,步骤(5)中的烧制温度为1050℃。
由上述本发明的描述可知,和现有技术相比,本发明具有如下有益效果:
1、本发明突破传统通过改变釉的配方来适应坯体要求的做法,而是改变了红土坯体的配方,减少红土在坯体中的比重,增加其它矿物质原料,改变坯体的物理化学性质,即降低了红土的体积密度,增加了坯体的烧结度,烧制时坯体中的气体及时得以释放,不会出现跳釉、起泡、剥壳等现象,烧制出来的红土绘彩上釉陶制品外表美观。
2、本发明采用独特的红土坯体配方,一遍烧成即可,其烧成温度在1020-1060℃,不但降低了烧成成本,还提高了产品的档次及市场占有率。
具体实施方式
本发明通过以下实施例作进一步阐述。
实施例一
(1)制造坯体:将以下重量份数的原料混合:红土65份、长石5份、黑灰石5份、萤石5份、高岭土5份、石英5份、无铅熔块3份、滑石2份、水20份,混匀后研磨成土浆,将土浆注入模具中0.5小时后脱模成型,常温下自然风干,再经过修坯擦水处理后自然风干,制得坯体;
(2)绘彩:根据陶制品的器型、图案调配色料,并在步骤(1)中的坯体上需要的部位上绘制花草图案;
(3)制造釉水:将以下重量分数的原料混合:低膨胀釉粉80份、氧化锌3份、着色剂10份、石英粉3份、碳酸钙2份、氧化钛2份、水30份,混匀后浸泡5小时,取出过滤后加入300份的水稀释得釉水;
(4)上釉:将步骤(2)中绘彩完成的坯体放入步骤(3)中制得的釉水中浸泡2秒;
(5)烧成:将上釉完成的产品在1050℃烧制5小时,然后经6小时冷却后出窑得成品。
实施例二
(1)制造坯体:将以下重量份数的原料混合:红土60份、长石6份、黑灰石6份、萤石6份、高岭土6份、石英6份、无铅熔块4份、滑石2.5份、水25份,混匀后研磨成土浆,将土浆注入模具中0.75小时后脱模成型,常温下自然风干,再经过修坯擦水处理后自然风干,制得坯体;
(2)绘彩:根据陶制品的器型、图案调配色料,并在步骤(1)中的坯体上需要的部位上绘制动物图案;
(3)制造釉水:将以下重量分数的原料混合:低膨胀釉粉85份、氧化锌4份、着色剂12份、石英粉4份、碳酸钙3份、氧化钛3份、水35份,混匀后浸泡6小时,取出过滤后加入350份的水稀释得釉水;
(4)上釉:将步骤(2)中绘彩完成的坯体放入步骤(3)中制得的釉水中浸泡2.5秒;
(5)烧成:将上釉完成的产品在1020℃烧制6小时,然后经6小时冷却后出窑得成品。
实施例三
(1)制造坯体:将以下重量份数的原料混合:红土63份、长石8份、黑灰石8份、萤石8份、高岭土8份、石英8份、无铅熔块4份、滑石3份、水30份,混匀后研磨成土浆,将土浆注入模具中0.8小时后脱模成型,常温下自然风干,再经过修坯擦水处理后自然风干,制得坯体;
(2)绘彩:根据陶制品的器型、图案调配色料,并在步骤(1)中的坯体上需要的部位上绘制自然景观图案;
(3)制造釉水:将以下重量分数的原料混合:低膨胀釉粉90份、氧化锌5份、着色剂15份、石英粉5份、碳酸钙5份、氧化钛5份、水40份,混匀后浸泡7.5小时,取出过滤后加入400份的水稀释得釉水;
(4)上釉:将步骤(2)中绘彩完成的坯体放入步骤(3)中制得的釉水中浸泡1秒;
(5)烧成:将上釉完成的产品在1060℃烧制4小时,然后经8小时冷却后出窑得成品。
上述仅为本发明的具体实施方式,但本发明的设计构思并不局限于此,凡利用此构思对本发明进行非实质性的改动,均应属于侵犯本发明保护范围的行为。

Claims (4)

1.一种低温节能一遍烧成红土绘彩上釉陶制品的制造方法,其特征在于,包括如下步骤:
(1)制造坯体:将以下重量份数的原料混合:红土60-65份、长石5-10份、黑灰石5-10份、萤石5-10份、高岭土5-10份、石英5-10份、无铅熔块3-5份、滑石2-3份、水20-30份,混匀后研磨成土浆,将土浆注入模具中0.5-1小时后脱模成型,常温下自然风干,再经过修坯擦水处理后自然风干,制得坯体;
(2)绘彩:根据陶制品的器型、图案调配色料,并在步骤(1)中的坯体上进行绘彩;
(3)制造釉水:将以下重量分数的原料混合:低膨胀釉粉80-90份、氧化锌3-5份、着色剂10-15份、石英粉3-5份、碳酸钙2-5份、氧化钛2-5份、水30-40份,混匀后浸泡5-8小时,取出过滤后加入300-400份的水稀释得釉水;
(4)上釉:将步骤(2)中绘彩完成的坯体放入步骤(3)中制得的釉水中浸泡0.5-4秒;
(5)烧成:将上釉完成的产品在1020-1060℃烧制4-6小时,然后经6-10小时冷却后出窑得成品。
2.如权利要求1所述的一种低温节能一遍烧成红土绘彩上釉陶制品的制造方法,其特征在于:步骤(1)中制造坯体的各原料按以下重量分数混合:红土65份、长石5份、黑灰石5份、萤石5份、高岭土5份、石英5份、无铅熔块3份、滑石2份、水20份。
3.如权利要求1所述的一种低温节能一遍烧成红土绘彩上釉陶制品的制造方法,其特征在于:步骤(3)中制造釉水的各原料按以下重量分数混合:低膨胀釉粉80份、氧化锌3份、着色剂10份、石英粉3份、碳酸钙2份、氧化钛2份、水30份。
4.如权利要求1所述的一种低温节能一遍烧成红土绘彩上釉陶制品的制造方法,其特征在于:步骤(5)中的烧制温度为1050℃。
CN201310599149.1A 2013-11-25 2013-11-25 一种低温节能一遍烧成红土绘彩上釉陶制品的制造方法 Active CN103570338B (zh)