CN103286477A - 一种无铅焊料用助焊剂及其制备方法 - Google Patents

一种无铅焊料用助焊剂及其制备方法 Download PDF

Info

Publication number
CN103286477A
CN103286477A CN2013101948312A CN201310194831A CN103286477A CN 103286477 A CN103286477 A CN 103286477A CN 2013101948312 A CN2013101948312 A CN 2013101948312A CN 201310194831 A CN201310194831 A CN 201310194831A CN 103286477 A CN103286477 A CN 103286477A
Authority
CN
China
Prior art keywords
scaling powder
lead
cosolvent
free solder
soldering flux
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN2013101948312A
Other languages
English (en)
Other versions
CN103286477B (zh
Inventor
杨鹰
秦春阳
李海普
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Central South University
Original Assignee
Central South University
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Central South University filed Critical Central South University
Priority to CN201310194831.2A priority Critical patent/CN103286477B/zh
Publication of CN103286477A publication Critical patent/CN103286477A/zh
Application granted granted Critical
Publication of CN103286477B publication Critical patent/CN103286477B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明涉及一种无铅焊料用助焊剂及其制备方法,该助焊剂中各组分的质量百分比为:活化剂2.0-4.0%、表面活性剂0.05-0.5%、成膜剂0.4-1.0%、助溶剂18-30%、缓蚀剂0.1-0.4%,余量为去离子水。该助焊剂中不含松香,且固体含量小于3%,从而使焊接时固体残留量少,离子污染度低,焊后免清洗。本发明水溶性免清洗助焊剂使用去离子水做溶剂,无色透明,无刺激性气味,原料获取途径较易,成本较低。助焊剂中的活化成分均不含卤素以增强焊后线路板的绝缘性,且由于成膜剂的作用,线路板经过焊接工序之后,表面形成一层致密保护膜,降低焊后残留物的电迁移,有效提高线路板的绝缘稳定性;可减少有机型助焊剂在焊接时带来的危害,符合环保要求。

Description

一种无铅焊料用助焊剂及其制备方法
技术领域
本发明属于微电子焊接材料技术领域,涉及一种助焊剂,尤其是一种无铅焊料用助焊剂及其制备方法。
背景技术
传统的电子类产品采用铅-锡焊料作为焊接用材料,铅-锡焊料熔点低(183℃),可焊性好。但随着电子信息产品禁铅法令的颁布实施,铅-锡焊料的使用受到限制,无铅焊料逐渐取代铅-锡焊料成为电子工业的重要连接材料。而由于无铅焊料熔点较高,使用时易氧化,润湿性差,传统助焊剂已不能满足无铅焊料的焊接要求。
目前被广泛应用的助焊剂多为有机溶剂型助焊剂,该类型助焊剂的活性成分都必须溶解在有机溶剂中,在使用时存在挥发性大、易燃、对身体有害等缺点。水溶性助焊剂以去离子水做溶剂,环保、安全,能够较好的适应于无铅焊接。
出于对焊接效果的考虑,一些助焊剂选用腐蚀性较强、固含量较高的物质作为活性组分,导致焊后印制组件板残留多且不易清洗,离子污染度大,表面绝缘电阻率下降。
发明内容
本发明针对现有技术的不足,提供一种无铅焊料用助焊剂及其制备方法。以适应焊料的无铅化趋势要求。这种助焊剂使用去离子水做溶剂,降低了生产成本,达到环保、稳定、安全的目的,对无铅焊接有良好的适应性。其较低的固含量使该助焊剂在焊后残留物少,绝缘电阻高,达到免清洗要求。
一种无铅焊料用助焊剂,该助焊剂包括:活化剂、表面活性剂、成膜剂、助溶剂、缓蚀剂以及去离子水;
该助焊剂中,各组分的质量百分含量为:活化剂2.0~4.0%、表面活性剂0.05~0.5%、成膜剂0.4~1.0%、助溶剂18~30%、缓蚀剂0.1~0.4%,余量为去离子水。
所述助焊剂的制备方法包括以下步骤:
第一步:将活化剂与表面活性剂在低温(约20~35℃)下溶解到部分去离子水中,搅拌均匀,作为活化剂部分备用;
第二步:将助溶剂和余量去离子水加入到另一个反应釜内,搅拌下加入成膜剂,并加热至40~60℃,待成膜剂溶解完毕,停止加热,冷却到室温,搅拌下依次加入第一步获得的活化剂部分与缓蚀剂,溶液混合均匀后,静置过滤。
所述的活化剂为有机酸和有机胺的混合物,且有机酸与有机胺的质量比为5:1~9:1。
所述有机酸为有机二元羧酸或有机多元羧酸,其选自苹果酸、柠檬酸、丁二酸、戊二酸、己二酸中的至少一种;所述有机胺为醇胺,选自二乙醇胺、三乙醇胺和三乙胺中的一种。
所述表面活性剂为非离子表面活性剂,或非离子表面活性剂与阴离子表面活性剂的复配;其中,非离子表面活性剂选自OP系列或TX系列表面活性剂中的一种;阴离子表面活性剂为十二烷基磺酸钠,,且阴离子表面活性剂与非离子表面活性剂的质量比为1:1~1:3。
成膜剂选自水溶性丙烯酸树脂、聚乙二醇2000、聚乙二醇4000中的一种。
所述助溶剂包括低沸点助溶剂、高沸点助溶剂,低沸点助溶剂为乙二醇或四氢糠醇中的一种,高沸点助溶剂为丙三醇,且低沸点助溶剂与高沸点助溶剂的质量比为1:1~3:1。
缓蚀剂为含氮杂环化合物。
本发明所选用的活化剂为有机酸与有机胺的复配,可调节助焊剂的pH值,降低有机酸对印制组件板的腐蚀,其中有机酸与有机胺的质量比为4.5:1~8:1。在有机酸活化剂的选取上,选用具有不同热分解温度的羧酸进行复配,从而使活化剂在焊接的整个温度范围内都具有活性,提高助焊效果。
本发明选用水溶性丙烯酸树脂、聚乙二醇2000、聚乙二醇4000等作为成膜剂。这些树脂在较低温度(如40~100℃)下即具有一定的溶解度,且与水的互溶程度较高,在焊接过程中,由于水分挥发与受热作用,即可在焊点周围形成一层致密的保护膜,防止焊料进一步氧化,提高润湿效果。
本发明添加一定量的助溶剂,一方面增加溶剂对活性物质及成膜剂的溶解能力,使助焊剂充分发挥活化作用和成膜效果,另一方面不同热分解温度的助溶剂的复配,在较大的温度范围内为有机酸活化剂电离出游离的H+提供一种电离环境,保证在焊接过程中助焊剂有较宽的活化温度区间,从而提高助焊效果。
本发明在制备方法上,将助焊剂的活性物质作为焊剂体系中的活化部分进行单独配制,以防活性成分与焊剂中的其他组成物质发生反应,且独立配制活化部分的温度较低,可降低加热过程中活性物质性状的变化,保护活化剂的活性。另外,由于表面活性剂本身具有的活性与在溶液中的増溶作用,将其作为活性体系的一部分,也可促进活化剂部分对固体有机酸等的溶解。
本发明水溶性免清洗助焊剂无色透明,无刺激性气味,原料获取途径较易,成本较低。助焊剂中的活化成分均不含卤素以增强焊后线路板的绝缘性,且由于成膜剂的作用,线路板经过焊接工序之后,表面形成一层致密保护膜,降低焊后残留物的电迁移,有效提高线路板的绝缘稳定性。
具体实施方式
下面结合实施例对本发明作进一步详细介绍。
实施例1:
有机酸:丁二酸  1.2g  己二酸1.2g
有机胺:三乙醇胺  0.4g
表面活性剂:OP-10乳化剂  0.1g
成膜剂:聚乙二醇2000  0.5g
助溶剂:乙二醇  20g  丙三醇  10g
缓蚀剂:苯并三氮唑  0.1g
去离子水  66.5g
制备方法:将有机酸、有机胺与表面活性剂在较低温(约20~35℃)下溶解到部分去离子水中,搅拌均匀,得到中间产物,备用。然后将助溶剂和余量去离子水加入到另一个反应釜内,搅拌下加入成膜剂,并加热至40~60℃,待成膜剂溶解完毕,停止加热,冷却到室温,搅拌下依次加入中间产物与缓蚀剂,溶液混合均匀后,静置过滤即得本发明助焊剂。
实施例2:
有机酸:丁二酸  1.2g  己二酸  1.2g
有机胺:三乙胺  0.5g
表面活性剂:OP-10  0.1g
成膜剂:聚乙二醇4000  0.4g
助溶剂:乙二醇  16g  丙三醇  8g
缓蚀剂:苯并三氮唑  0.2g
去离子水  72.4g
制备方法:同实施例1。
实施例3:
有机酸:丁二酸  1.0g  己二酸  1.0g
有机胺:三乙醇胺  0.4g
表面活性剂:TX-10  0.15g  十二烷基磺酸钠  0.15g
成膜剂:聚乙二醇2000  0.8g
助溶剂:四氢糠醇  20g  丙三醇  10g
缓蚀剂:甲基苯并三氮唑  0.1g
去离子水  66.4g
制备方法:同实施例1。
实施例4:
有机酸:丁二酸  1.0g  己二酸  1.0g  柠檬酸  0.25g有机胺:三乙醇胺  0.5g
表面活性剂:OP-10  0.075g  十二烷基磺酸钠  0.025g
成膜剂:聚乙二醇2000  0.5g
助溶剂:乙二醇  22g  丙三醇  8g
缓蚀剂:苯并三氮唑  0.1g
去离子水  66.55g
制备方法:同实施例1。
实施例5:
有机酸:丁二酸  1.6g  己二酸  1.6g
有机胺:三乙胺  0.5g
表面活性剂:OP-10  0.2g
成膜剂:聚乙二醇2000  0.5g
助溶剂:四氢糠醇  9g  丙三醇  9g
缓蚀剂:苯并三氮唑  0.35g
去离子水  77.25g
使用上述实施例配制成的无铅焊料用水溶性免清洗助焊剂时,铜板腐蚀测试无明显腐蚀斑纹,以Sn-0.7Cu系焊料检测焊接效果,施焊中无刺激性气味,焊后固体残留物较少且铺展均匀,可免于清洗,表面绝缘电阻大于2.0×1011Ω,焊点光亮,铺展率均在78%以上。根据对产品的助焊性以及成本等要求,各组份物质含量可做适当调整。

Claims (10)

1.一种无铅焊料用助焊剂,其特征在于,该助焊剂包括:活化剂、表面活性剂、成膜剂、助溶剂、缓蚀剂以及去离子水;
该助焊剂中,各组分的质量百分比为:活化剂2.0~4.0%、表面活性剂0.05~0.5%、成膜剂0.4~1.0%、助溶剂18~30%、缓蚀剂0.1~0.4%,余量为去离子水。
2.根据权利要求1所述的无铅焊料用助焊剂,其特征在于,所述助焊剂的制备方法包括以下步骤:
第一步:将活化剂与表面活性剂在20~35℃下溶解到部分去离子水中,搅拌均匀,作为活化剂部分备用;
第二步:将助溶剂和余量去离子水加入到另一个反应釜内,搅拌下加入成膜剂,并加热至40~60℃,待成膜剂溶解完毕,停止加热,冷却到室温,搅拌下依次加入第一步获得的活化剂部分与缓蚀剂,溶液混合均匀后,静置过滤。
3.根据权利要求1或2所述的无铅焊料用助焊剂,其特征在于:所述的活化剂为有机酸和有机胺的混合物,且有机酸与有机胺的质量比为4.5:1~8:1。
4.根据权利要求1或2所述的无铅焊料用助焊剂,其特征在于:所述有机酸为有机二元羧酸或有机多元羧酸,其选自苹果酸、柠檬酸、丁二酸、戊二酸、己二酸中的至少一种;所述有机胺为醇胺,选自二乙醇胺、三乙醇胺和三乙胺中的一种。
5.根据权利要求1或2所述的无铅焊料用助焊剂,其特征在于:所述表面活性剂为非离子表面活性剂,或非离子表面活性剂与阴离子表面活性剂的复配;其中,非离子表面活性剂选自OP系列或TX系列表面活性剂中的一种;阴离子表面活性剂为十二烷基磺酸钠,且阴离子表面活性剂与非离子表面活性剂的质量比为1:1~1:3。
6.根据权利要求1或2所述的无铅焊料用助焊剂,其特征在于:成膜剂选自水溶性丙烯酸树脂、聚乙二醇2000、聚乙二醇4000中的一种。
7.根据权利要求1或2所述的无铅焊料用助焊剂,其特征在于:助溶剂为醇和/或醇醚的复配混合物,所述醇和/或醇醚的复配混合物沸点大于等于150℃。
8.根据权利要求1或2所述的无铅焊料用助焊剂,其特征在于:所述助溶剂包括低沸点助溶剂、高沸点助溶剂,低沸点助溶剂为乙二醇或四氢糠醇中的一种,高沸点助溶剂为丙三醇,且低沸点助溶剂与高沸点助溶剂的质量比为1:1~3:1。
9.根据权利要求1或2所述的无铅焊料用助焊剂,其特征在于:缓蚀剂为含氮杂环化合物。
10.根据权利要求9所述的无铅焊料用助焊剂,其特征在于:缓蚀剂选自苯并三氮唑、甲基苯并三氮唑中的一种。
CN201310194831.2A 2013-05-22 2013-05-22 一种无铅焊料用助焊剂及其制备方法 Active CN103286477B (zh)