CN102241839B - 高耐磨矿用橡胶筛网的胶料 - Google Patents

高耐磨矿用橡胶筛网的胶料 Download PDF

Info

Publication number
CN102241839B
CN102241839B CN201010169820.5A CN201010169820A CN102241839B CN 102241839 B CN102241839 B CN 102241839B CN 201010169820 A CN201010169820 A CN 201010169820A CN 102241839 B CN102241839 B CN 102241839B
Authority
CN
China
Prior art keywords
rubber
sieve mesh
mineral processing
carbon black
rubber sieve
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN201010169820.5A
Other languages
English (en)
Other versions
CN102241839A (zh
Inventor
卢文燕
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
FUJIAN KEDE HIGH POLYMER MATERIAL CO., LTD.
Original Assignee
Longyan Kelida Rubber and Plastic Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Longyan Kelida Rubber and Plastic Co Ltd filed Critical Longyan Kelida Rubber and Plastic Co Ltd
Priority to CN201010169820.5A priority Critical patent/CN102241839B/zh
Publication of CN102241839A publication Critical patent/CN102241839A/zh
Application granted granted Critical
Publication of CN102241839B publication Critical patent/CN102241839B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明提供了一种高耐磨矿用橡胶筛网的胶料,其原料包括天然橡胶、氧化锌、硬脂酸、橡胶防护蜡、防老剂4010NA、防老剂D、偶联剂KH-580、炭黑N220、白炭黑、芳烃油、促进剂CZ、硫磺。本发明胶料主要用于矿用橡胶筛网,特别适合头选橡胶筛网,可明显提高抗撕裂强度和耐老化性能,延长矿用橡胶筛网的使用寿命。

Description

高耐磨矿用橡胶筛网的胶料
【技术领域】
本发明涉及一种选矿设备,尤其涉及一种高耐磨选矿用的橡胶筛网胶料。
【背景技术】
随着选矿工业的发展和选矿技术的提高,造成高品质的矿产已被大量开采,导致可选矿的品质越来越低。为了提高产量,选矿量必然增加,很多选矿厂选择加大头筛矿石尺寸,甚至不用破碎直接进行筛选的方法来提高产量,这样势必导致对筛网胶料要求越来越高,应更具耐磨性、耐切割性、耐刺轧性、耐老化性,以及能更好地抗崩花掉块,也就是应具有更高的强度和弹性,但目前的橡胶筛网的强度和弹性均达不到要求,容易损坏。
【发明内容】
本发明要解决的技术问题,在于提供一种高耐磨矿用橡胶筛网的胶料,采用白炭黑与偶联剂KH-580添加到综合性能最好的橡胶和化工材料中,具有更高的强度和弹性,其耐磨性、耐切割性、耐刺轧性、耐老化性更佳。
本发明是这样实现的:高耐磨矿用橡胶筛网的胶料,其特征在于:所述胶料由下述原料按重量比配制而成:
天然橡胶           100.0
氧化锌             5.0
硬脂酸             2.0
橡胶防护蜡         1.5
防老剂4010NA       1.5
防老剂D            1.0
偶联剂KH-580       2.5
炭黑N220           40.0
白炭黑      15.0
芳烃油      8.0
促进剂CZ    1.0
硫磺        2.5。
本发明具有如下优点:采用白炭黑与偶联剂KH-580添加到综合性能最好的橡胶和化工材料中,可明显提高矿用橡胶筛网胶料的强度和弹性,其耐磨性、耐切割性、耐老化性、耐刺轧性更佳,且对其它物理性能影响小,特别适合头选橡胶筛网。
【具体实施方式】
一、原料准备:将下述原料按重量比称量:
天然橡胶              100.0
氧化锌                5.0
硬脂酸                2.0
橡胶防护蜡            1.5
防老剂4010NA          1.5
防老剂D               1.0
偶联剂KH-580          1.0
炭黑N220              40.0
白炭黑                15.0
芳烃油                8.0
促进剂CZ              1.0
硫磺                  2.5。
二、将上述称量好的原料采取下述两种工艺进行混炼:
1、小配合试验胶料
将原料放在XK-160开炼机上进行混炼,加料顺序为:
天然橡胶-氧化锌、硬脂酸、橡胶防护蜡、防老剂4010NA、防老剂D和偶联剂KH-580-炭黑N220和白炭黑-芳烃油-促进剂CZ-硫磺。
2、生产胶料工艺
将原料放在XN-55捏炼机上进行混炼,并采用二段混炼法,包括一段混炼和二段混炼。
所述一段混炼加料顺序为:
天然橡胶-氧化锌、硬脂酸、橡胶防护蜡-偶联剂KH-580-白炭黑和三分之二的炭黑N220-芳烃油;
混炼后进行排胶,排胶温度控制在120±10℃,之后再出片。
所述二段混炼加料顺序为:一段母胶-防老剂4010NA、防老剂D、促进剂CZ、剩余三分之一的炭黑N220;
混炼后进行排胶,排胶温度控制在100±10℃,之后再加硫磺出片。
三、性能测试数据表
使用本发明配方(针对生产胶料工艺)与普通配方(针对小配合试验胶料)分别制成的矿用橡胶筛网胶料的性能测试所得的数据如下表所示:
Figure GSA00000117144000031
Figure GSA00000117144000041
由上表可见,使用本发明配方制成的胶料比现有技术中普通配方制成的胶料可明显提高撕裂强度和耐老化性能。
采用本实施例配方与普通配方分别生产了筛孔90×90的筛网在矿山选矿设备(圆盘振动筛选机)上使用,使用结果对比如下。
  项目   本实施例配方   普通配方
  平均选矿量   80万吨以上   45-50万吨

Claims (1)

1.高耐磨矿用橡胶筛网的胶料,其特征在于:所述胶料由下述原料按重量比配制而成:
天然橡胶            100.0
氧化锌              5.0
硬脂酸              2.0
橡胶防护蜡          1.5
防老剂4010NA        1.5
防老剂D             1.0
偶联剂KH-580        2.5
炭黑N220            40.0
白炭黑              15.0
芳烃油              8.0
促进剂CZ            1.0
硫磺                2.5。
CN201010169820.5A 2010-05-12 2010-05-12 高耐磨矿用橡胶筛网的胶料 Expired - Fee Related CN102241839B (zh)