CN101759161B - 一种高光学质量硒化锌的制备方法 - Google Patents

一种高光学质量硒化锌的制备方法 Download PDF

Info

Publication number
CN101759161B
CN101759161B CN2008102465436A CN200810246543A CN101759161B CN 101759161 B CN101759161 B CN 101759161B CN 2008102465436 A CN2008102465436 A CN 2008102465436A CN 200810246543 A CN200810246543 A CN 200810246543A CN 101759161 B CN101759161 B CN 101759161B
Authority
CN
China
Prior art keywords
zinc
gas
zinc selenide
optical quality
sediment chamber
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN2008102465436A
Other languages
English (en)
Other versions
CN101759161A (zh
Inventor
苏小平
王铁艳
张福昌
霍承松
魏乃光
赵永田
鲁泥藕
付利刚
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Grinm Guojing Advanced Materials Co ltd
Shandong Youyan Guojinghui New Material Co Ltd
Original Assignee
BEIJING GUOJING INFRARED OPTICAL TECHNOLOGY CO LTD
Beijing General Research Institute for Non Ferrous Metals
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by BEIJING GUOJING INFRARED OPTICAL TECHNOLOGY CO LTD, Beijing General Research Institute for Non Ferrous Metals filed Critical BEIJING GUOJING INFRARED OPTICAL TECHNOLOGY CO LTD
Priority to CN2008102465436A priority Critical patent/CN101759161B/zh
Publication of CN101759161A publication Critical patent/CN101759161A/zh
Application granted granted Critical
Publication of CN101759161B publication Critical patent/CN101759161B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了属于无机块体材料制备技术领域的一种高光学质量硒化锌的制备方法。将锌放入沉积炉内,抽真空,将沉积室升温,以氩气作为反应原料气体的携带气体,通过质量流量计将H2Se气体、氩气通入沉积室中,锌与H2Se的摩尔比为0.8~1.2,沉积室内壁发生沉积反应,硒化锌开始生长;使锌与H2Se的摩尔比保持不变,炉内压力恒定,沉积15~25天,然后降至室温,得到高光学质量的硒化锌。本发明有效地解决了化学气相沉积制备硒化锌工艺中的粉末生成问题,消除了产品夹杂,材料具有高红外透过率及低吸收系数,大幅提高了光学质量。

Description

一种高光学质量硒化锌的制备方法
技术领域
本发明属于无机块体材料制备技术领域,特别涉及一种高光学质量硒化锌的制备方法。 
背景技术
硒化锌是一种高透过率、低吸收系数的红外光学材料,它的透射波段覆盖了可见光、中红外和远红外,并且具备良好的力学和热学性能,被广泛的用作红外探测、成像装置的窗口和透镜。 
化学气相沉积工艺(Chemical Vapor Deposition,简称CVD)制备ZnSe,以Zn和H2Se为原料,在沉积室内部发生反应,反应原理: 
[0004] Zn+H2Se→ZnSe+H2↑ 
[0005] 化学气相沉积工艺制备ZnSe的工艺窗口窄,极易生成粉末,材料内部出现夹杂,显著降低产品光学质量。 
发明内容
本发明的目的是提供一种高光学质量硒化锌的制备方法。 
一种高光学质量硒化锌的制备方法,采用化学气相沉积工艺,其特征在于,该方法步骤为, 
(1)将锌放入沉积炉内; 
(2)通过真空泵对沉积炉抽真空,使真空度为1×104~5×104Pa; 
(3)将沉积室升温至450~600℃,锌融化并蒸发后,继续升温至650~800℃,并保温; 
(4)以氩气作为反应原料气体H2Se的携带气体,通过质量流量计将H2Se气体按照设定值0.5~2L/min、氩气按照5~20L/min的流量通入沉积室中,锌与H2Se的摩尔比为0.8~1.2,沉积室内壁发生沉积反应,硒化锌开始生长; 
(5)每隔一个小时检测一次Zn的蒸发量,通过调节质量流量计使得H2Se与锌的摩尔比保持不变,随时监测沉积室的压力,通过调整真空泵的抽气速率,保持进/出沉积室气体总量不变,沉积室内压力恒定,沉积时间为15~25天,然后以0.1~0.5℃/min的降温速率降至室温,得到高光学质量的硒化锌。 
本发明的有益效果为: 
本发明通过调整进气结构、控制气体流量和空间压力,严格控制反应空间浓度和两种原料进入沉积系统比例,有效地解决了化学气相沉积制备硒化锌工艺中的粉末生成问题,消除了产品夹杂,材料具有高红外透过率及低吸收系数,大幅提高了光学质量。本工艺发明目前可批量制备 
Figure DEST_PATH_GSB00000773831200021
高光学质量的硒化 
锌,并且已经应用于大规模生产中。 
制得的硒化锌材料内部无夹杂,具有高红外透过率及低吸收系数,彻底解决了ZnSe生长过程中出现夹杂等质量难题。 
具体实施方式
本发明优化了反应进气结构:采用进气结构和沉积室保持良好匹配,保证进入沉积室内部的气体分布均匀,并控制气体流量得到合理的沉积气体流型,避免快速生长和粉末的形成;优化了空间压力:化学气相沉积反应空间压力严格控制在一定范围之内。空间压力范围在1×104~5×104Pa内,每次沉积过程中压力保持一致;反应物浓度实时调控:通过质量流量计和原料进气压力调整反应物空间浓度,保持两种原料配比的全程一致性。 
下面结合实施例对本发明作进一步说明: 
实施例1 
一种高光学质量硒化锌的制备方法,在高温沉积炉中,采用化学气相沉积工艺,该方法步骤为, 
(1)将锌放入沉积炉内; 
(2)通过真空泵对设备抽真空,使真空度为2×104Pa; 
(3)将沉积室升温至550℃,锌融化并蒸发后,继续升温至750℃,并保温; 
(4)以氩气作为反应原料气体的携带气体,通过质量流量计将H2Se气体、氩气通入沉积室中,1小时后升至设定值H2Se气体:1L/min,氩气:10L/min,进入正常沉积过程,锌与H2Se的摩尔比为1,沉积室内壁发生沉积反应,硒化锌开始生长; 
(5)每隔一个小时检测一次Zn的蒸发量(通过对反应后尾气的气氛变化反馈检测Zn的蒸发量),通过调节质量流量计使得H2Se与锌的摩尔比保持不变,如果发生变化则需对锌池温度做出相应的调整,随时监测反应室的压力,通过调整真空泵的抽气速率,保持进/出炉体气体总量不变,炉内压力恒定,整个生长过程沉积室温度保持恒定,沉积时间为18天,然后以0.2℃/min的降温速率降至室温,得到高光学质量的硒化锌。 
获得的 
Figure G2008102465436D00031
200mm×10mmZnSe平板材料,内部无夹杂,原生材料长波10.6μm红外透过率达到70.35%,接近了理论透过率为71%,光学质量优秀。 
实施例2 
一种高光学质量硒化锌的制备方法,在高温沉积炉中,采用化学气相沉积工艺,该方法步骤为, 
(1)将锌放入沉积炉内; 
(2)通过真空泵对设备抽真空,使真空度为2.5×104Pa; 
(3)将沉积室升温至600℃,锌融化并蒸发后,继续升温至730℃,并保温; 
(4)以氩气作为反应原料气体的携带气体,通过质量流量计将H2Se气体、氩气通入沉积室中,1.5小时后升至设定值H2Se气体:1.2L/min,氩气:15L/min,进入正常沉积过程,锌与H2Se的摩尔比为0.8,沉积室内壁发生沉积反应,硒化锌开始生长; 
(5)每隔一个小时检测一次Zn的蒸发量(通过对反应后尾气的气氛变化反馈检测Zn的蒸发量),通过调节质量流量计使得锌与H2Se的摩尔比保持不变,如果发生变化则需对锌池温度做出相应的调整,随时监测反应室的压力,通过调整真空泵的抽气速率,保持进/出炉体气体总量不变,炉内压力恒定,整个生长过程沉积室温度保持恒定,沉积时间为25天,然后以0.15℃/min的降温速率降至室温,得到高光学质量的硒化锌。 
得到20mm厚度的高光学质量的硒化锌平板,材料不开裂,厚度均匀性好,表面无粉末,内部无夹杂,原生材料长波10.6μm红外透过率达到70.1%,光学质量优秀。 

Claims (1)

1.一种高光学质量硒化锌的制备方法,采用化学气相沉积工艺,其特征在于,该方法步骤为,
(1)将锌放入沉积炉内;
(2)通过真空泵对沉积炉抽真空,使真空度为1×104~5×104Pa;
(3)将沉积室升温至450~600℃,锌融化并蒸发后,继续升温至650~800℃,并保温;
(4)以氩气作为反应原料气体H2Se的携带气体,通过质量流量计将H2Se气体按照设定值0.5~2L/min、氩气按照5~20L/min的流量通入沉积室中,锌与H2Se的摩尔比为0.8~1.2,沉积室内壁发生沉积反应,硒化锌开始生长;
(5)每隔一个小时检测一次Zn的蒸发量,通过调节质量流量计使得H2Se与锌的摩尔比保持不变,随时监测沉积室的压力,通过调整真空泵的抽气速率,保持进/出沉积室气体总量不变,沉积室内压力恒定,沉积时间为15~25天,然后以0.1~0.5℃/min的降温速率降至室温,得到高光学质量的硒化锌。
CN2008102465436A 2008-12-25 2008-12-25 一种高光学质量硒化锌的制备方法 Active CN101759161B (zh)