WO2025089285A1 - ポリアミド組成物及び成形品 - Google Patents

ポリアミド組成物及び成形品 Download PDF

Info

Publication number
WO2025089285A1
WO2025089285A1 PCT/JP2024/037627 JP2024037627W WO2025089285A1 WO 2025089285 A1 WO2025089285 A1 WO 2025089285A1 JP 2024037627 W JP2024037627 W JP 2024037627W WO 2025089285 A1 WO2025089285 A1 WO 2025089285A1
Authority
WO
WIPO (PCT)
Prior art keywords
polyamide
acid
mass
polyamide composition
less
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
PCT/JP2024/037627
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
亮佑 横尾
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Asahi Kasei Corp
Asahi Chemical Industry Co Ltd
Original Assignee
Asahi Kasei Corp
Asahi Chemical Industry Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Asahi Kasei Corp, Asahi Chemical Industry Co Ltd filed Critical Asahi Kasei Corp
Priority to CN202480068575.9A priority Critical patent/CN122095025A/zh
Priority to JP2025553375A priority patent/JPWO2025089285A1/ja
Publication of WO2025089285A1 publication Critical patent/WO2025089285A1/ja
Anticipated expiration legal-status Critical
Pending legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G69/00—Macromolecular compounds obtained by reactions forming a carboxylic amide link in the main chain of the macromolecule
    • C08G69/02—Polyamides derived from amino-carboxylic acids or from polyamines and polycarboxylic acids
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K3/00—Use of inorganic substances as compounding ingredients
    • C08K3/01—Use of inorganic substances as compounding ingredients characterized by their specific function
    • C08K3/014—Stabilisers against oxidation, heat, light or ozone
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K5/00—Use of organic ingredients
    • C08K5/49—Phosphorus-containing compounds
    • C08K5/51—Phosphorus bound to oxygen
    • C08K5/53—Phosphorus bound to oxygen bound to oxygen and to carbon only
    • C08K5/5313—Phosphinic compounds, e.g. R2=P(:O)OR'
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
    • C08K5/00—Use of organic ingredients
    • C08K5/49—Phosphorus-containing compounds
    • C08K5/51—Phosphorus bound to oxygen
    • C08K5/53—Phosphorus bound to oxygen bound to oxygen and to carbon only
    • C08K5/5317—Phosphonic compounds, e.g. R—P(:O)(OR')2
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
    • C08L77/00—Compositions of polyamides obtained by reactions forming a carboxylic amide link in the main chain; Compositions of derivatives of such polymers

Definitions

  • the present invention relates to a polyamide composition and a molded article.
  • Polyamides such as polyamide 66 have excellent moldability, mechanical properties and chemical resistance, and are therefore widely used as materials for various parts in automobiles, electrical and electronics, industrial materials, industrial materials, daily necessities and household goods, etc.
  • Polyamides are often flame-retarded by the addition of halogen compounds.
  • various regulations have been established to prevent the use of products containing halogen compounds in electrical and electronic components due to hazardous substance restrictions such as RoHS (Restriction of Hazardous Substances) and PoHS (Prohibition on Certain Hazardous Substances in Consumer Products).
  • RoHS Restriction of Hazardous Substances
  • PoHS Prohibition on Certain Hazardous Substances in Consumer Products
  • Non-halogen flame retardants include, for example, phosphorus compounds.
  • phosphorus compounds for example, calcium and aluminum salts of phosphinic or diphosphinic acids as flame retardants for polyamides has been disclosed.
  • Patent Document 1 discloses a glass fiber reinforced polyamide using aluminum metal salts of phosphinic acid and phosphonic acid.
  • Patent Document 2 discloses a technology for adding a dispersant to a granular composite non-halogen flame retardant.
  • Patent Document 3 discloses a polyamide composition using an aliphatic polyamide, an amorphous aromatic polyamide, and a metal salt of phosphinic acid.
  • the object of the present invention is to provide a polyamide composition that has excellent mechanical properties, flame retardancy, metal corrosion resistance, weld strength, and extrusion operation stability.
  • the present invention was made in consideration of the above circumstances, and aims to provide a polyamide composition that has excellent mechanical properties, flame retardancy, metal corrosion resistance, weld strength, and extrusion operation stability.
  • the present invention was made in consideration of the above circumstances, and provides a polyamide composition having high heat resistance, excellent electrical properties, and excellent flame retardancy, and a molded product using the polyamide composition.
  • a polyamide composition comprising, relative to 100% by mass of the total mass of the polyamide composition, (A) 20 to 60% by mass of a polyamide, (B) 10 to 30% by mass of a phosphorus-based flame retardant, and (C) 10 to 60% by mass of an inorganic filler,
  • the (B) phosphorus-based flame retardant contains at least one phosphinic acid-phosphonic acid complex metal salt selected from the group consisting of condensates of phosphinic acid-phosphonic acid complex metal salts represented by the following general formula (1):
  • R 1 , R 2 , and R 3 are each independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms;
  • M m+ is a metal ion;
  • M is an element belonging to Group 2 or Group 15 of the periodic table, a transition element, zinc, aluminum, or a combination thereof;
  • m is 2 to 3; and when there are a pluralitylene
  • the polyamide composition of the above embodiment can provide a polyamide composition that has high low-temperature impact resistance, excellent deflection under load, and excellent flame retardancy when molded into a product.
  • the present embodiment is an example for explaining the present invention, and is not intended to limit the present invention to the following content.
  • the present invention can be carried out with appropriate modifications within the scope of its gist.
  • polyamide refers to a polymer that has amide (-NHCO-) groups in the main chain.
  • the polyamide composition of the present embodiment is a polyamide composition comprising, relative to 100% by mass of the total mass of the polyamide composition, 20 to 60% by mass of (A) a polyamide, 10 to 30% by mass of (B) a phosphorus-based flame retardant, and 10 to 60% by mass of (C) an inorganic filler,
  • the (B) phosphorus-based flame retardant contains at least one phosphinic acid-phosphonic acid complex metal salt selected from the group consisting of condensates of phosphinic acid-phosphonic acid complex metal salts represented by the following general formula (1):
  • R 1 , R 2 , and R 3 are each independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms;
  • M m+ is a metal ion;
  • M is an element belonging to Group 2 or Group 15 of the periodic table, a transition element, zinc, aluminum, or a combination thereof;
  • m is 2 to 3; and when there
  • polyamide (A) examples include polycaprolactam (polyamide 6), polytetramethylene adipamide (polyamide 46), polyhexamethylene adipamide (polyamide 66), polyhexamethylene cyclohexylamide (polyamide 6C), polyhexamethylene sebacamide (polyamide 610), polyhexamethylene dodecamide (polyamide 612), polyundecalactam (polyamide 11), polydodecalactam (polyamide 12), polyhexamethylene isophthalamide (polyamide 6I), polyhexamethylene terephthalamide (polyamide 6T), polynonamethylene terephthalamide (polyamide 9T), polydodecamethylene terephthalamide (polyamide 12T), polymetaxylylene adipamide (polyamide MXD6), and polyamide copolymers obtained by copolymerizing two or more of these polyamides. These polyamides may be used alone or
  • the polyamide (A) may include a crystalline polyamide (A-1).
  • the polyamide (A) may also include an amorphous polyamide (A-2).
  • the polyamide (A) may include a crystalline polyamide (A-1) and an amorphous polyamide (A-2).
  • the melting point (Tm) of the crystalline polyamide (A-1) is preferably 290.0°C or less, more preferably 280.0°C or less, even more preferably 270.0°C or less, and preferably 220.0°C or more, and more preferably 240.0°C or more.
  • the melting point Tm of the (A-1) crystalline polyamide can be measured in accordance with JIS-K7121, and the measuring device can be a differential scanning calorimeter (DSC), more specifically, a Diamond-DSC manufactured by PERKIN-ELMER.
  • DSC differential scanning calorimeter
  • the content of the amorphous polyamide (A-2) is preferably 10.0% by mass or more, more preferably 12.5% by mass or more, even more preferably 15.0% by mass or more, even more preferably 17.5% by mass or more, particularly preferably 20.0% by mass or more, preferably 50.0% by mass or less, more preferably 45.0% by mass or less, even more preferably 42.5% by mass or less, even more preferably 40.0% by mass or less, particularly preferably 35.0% by mass or less, based on the mass of the total polyamide in the polyamide composition.
  • the polyamide composition of the present embodiment has the above-mentioned configuration, and is therefore excellent in melt processing such as extrusion and molding. It is possible to provide a polyamide composition that can further suppress the thermal decomposition of the phosphorus-based flame retardant, has an excellent deflection temperature under load, has good moldability, and is excellent in flame retardancy.
  • the (A) polyamide, the (B) phosphorus-based flame retardant, the (C) inorganic filler, and the (D) other components may be referred to as the (A) component, the (B) component, the (C) component, and the (D) component, respectively.
  • the melting point Tm can be configured as follows.
  • the melting point Tm of the polyamide composition is preferably 330.0°C or lower, more preferably 300.0°C or lower, even more preferably 290.0°C or lower, even more preferably 280.0°C or lower, preferably 220.0°C or higher, more preferably 240.0°C or higher.
  • the polyamide composition By the melting point Tm of the polyamide composition being within the above range, the polyamide composition can be obtained which has excellent mechanical properties, particularly rigidity under atmospheric equilibrium moisture absorption, flame retardancy, and moldability.
  • the polyamide composition containing a component represented by an inorganic filler has excellent heat resistance represented by a load deflection temperature.
  • the melting point Tm of the polyamide composition By the melting point Tm of the polyamide composition being within the above range, the polyamide composition can be obtained which is superior in terms of rigidity under heat, etc.
  • the melting point Tm of the polyamide composition can be measured in accordance with JIS-K7121, and an example of a measuring device is Diamond-DSC manufactured by PERKIN-ELMER.
  • a crystalline polyamide is a polyamide having a heat of fusion of crystals of 15 J/g or more when measured at 20° C./min by a differential scanning calorimeter.
  • Crystalline polyamides include, but are not limited to, (A-1a) polyamides obtained by ring-opening polymerization of lactams, (A-1b) polyamides obtained by self-condensation of ⁇ -aminocarboxylic acids, (A-1c) polyamides obtained by condensing diamines and dicarboxylic acids, and copolymers thereof.
  • the crystalline polyamides may be used alone or as a mixture of two or more kinds. Among them, the crystalline polyamides are preferably aliphatic amides in which the carbon skeleton forming the monomer unit is composed of aliphatic hydrocarbon groups.
  • Lactams used to obtain polyamides by ring-opening polymerization of lactams include, but are not limited to, pyrrolidone, caprolactam, undecalactam, dodecalactam, etc.
  • the ⁇ -amino carboxylic acid used to obtain a polyamide obtained by self-condensation of an ⁇ -amino carboxylic acid is not limited to the following, but examples thereof include ⁇ -amino fatty acids, which are ring-opening compounds of the above-mentioned lactams with water. Two or more monomers of each of the lactams and ⁇ -amino carboxylic acids may be used in combination to be condensed.
  • Diamines (monomers) used to obtain polyamides by condensing diamines and dicarboxylic acids include, but are not limited to, linear saturated aliphatic diamines having 2 to 20 carbon atoms, such as ethylenediamine, propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, dodecamethylenediamine, and tridecamethylenediamine.
  • linear saturated aliphatic diamines having 2 to 20 carbon atoms such as ethylenediamine, propylenediamine, tetramethylenediamine, pentamethylenediamine, hexamethylenediamine, heptamethylenediamine, octamethylenediamine, nonamethylenediamine, decamethylenediamine, undecamethylenediamine, do
  • Diamines constituting diamine units having a substituent branched from the main chain include, but are not limited to, branched saturated aliphatic diamines having 3 to 20 carbon atoms, such as 2-methylpentamethylenediamine (also called 2-methyl-1,5-diaminopentane), 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 2-methyl-1,8-octanediamine (also called 2-methyloctamethylenediamine), and 2,4-dimethyloctamethylenediamine.
  • 2-methylpentamethylenediamine also called 2-methyl-1,5-diaminopentane
  • 2,2,4-trimethylhexamethylenediamine 2,4,4-trimethylhexamethylenediamine
  • 2-methyl-1,8-octanediamine also called 2-methyloctamethylenediamine
  • 2,4-dimethyloctamethylenediamine 2,4-dimethyloctam
  • 2-methylpentamethylenediamine or 2-methyl-1,8-octanediamine is preferred as a diamine constituting a diamine unit having a substituent branched from the main chain, and 2-methylpentamethylenediamine is more preferred.
  • the polyamide composition tends to have better heat resistance, rigidity, etc.
  • the diamines described above as monomers may be used alone or in combination of two or more.
  • the carbon number of the diamine unit is preferably 4 or more and 12 or less, and more preferably 4 or more and 10 or less. If the carbon number is equal to or more than the lower limit, the heat resistance is superior, while if the carbon number is equal to or less than the upper limit, the crystallinity and releasability are superior.
  • the aliphatic diamine may further contain a polyvalent aliphatic amine having three or more valences, such as bishexamethylenetriamine, if necessary. These diamines may be used alone or in combination of two or more kinds.
  • Dicarboxylic acids (monomers) used to obtain polyamides by condensing diamines and dicarboxylic acids include, but are not limited to, aliphatic dicarboxylic acids such as succinic acid, adipic acid, pimelic acid, sebacic acid, dodecanedioic acid, and tetradecanedioic acid; aromatic dicarboxylic acids such as isophthalic acid, terephthalic acid, naphthalenedicarboxylic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, and 5-sodiumsulfoisophthalic acid; and alicyclic dicarboxylic acids such as cyclohexanedicarboxylic acid.
  • the dicarboxylic acids as monomers described above may be used alone or in combination of two or more.
  • the (A-1) crystalline polyamide may further contain units derived from trivalent or higher polyvalent carboxylic acids such as trimellitic acid, trimesic acid, and pyromellitic acid, as necessary.
  • the trivalent or higher polyvalent carboxylic acids may be used alone or in combination of two or more kinds.
  • (A-1) crystalline polyamides include polyamide 4 (poly- ⁇ -pyrrolidone), polyamide 6 (polycaproamide), polyamide 11 (polyundecane amide), polyamide 12 (polydodecane amide), polyamide 46 (polytetramethylene adipamide), polyamide 56 (polypentamethylene adipamide), polyamide 66 (polyhexamethylene adipamide), polyamide 610 (polyhexamethylene sebacamide), polyamide 612 (polyhexamethylene dodecamide), polyamide 4T (polytetramethylene terephthalamide), polyamide 6T (polyhexamethylene terephthalamide), polyamide 9T (polynonamethylene terephthalamide), and copolymer polyamides containing these as constituent components.
  • polyamide 6, polyamide 46, polyamide 66, or polyamide 610 is preferred, polyamide 6, polyamide 66, or polyamide 610 is more preferred, polyamide 6 or polyamide 66 is even more preferred, and polyamide 66 is particularly preferred.
  • Polyamide 66 is considered to be a suitable material for connector parts because of its excellent heat resistance, moldability, and toughness.
  • the weight average molecular weight (Mw) of the crystalline polyamide (A-1) is preferably 10,000 or more, more preferably 15,000 or more, even more preferably 20,000 or more, particularly preferably 25,000 or more, and is preferably 50,000 or less, more preferably 45,000 or less, and even more preferably 40,000 or less.
  • a polyamide composition can be obtained that simultaneously satisfies mechanical properties, particularly drip suppression during combustion tests, fluidity, corrosion resistance, etc. Furthermore, molded articles obtained from polyamide compositions containing components such as inorganic fillers have a more excellent surface appearance.
  • the weight average molecular weight (Mw) of the crystalline polyamide (A-1) can be measured using gel permeation chromatography (GPC).
  • the molecular weight distribution of the (A-1) crystalline polyamide is indicated by the value Mw/Mn obtained by dividing the weight average molecular weight (Mw) of the (A-1) crystalline polyamide by the number average molecular weight (Mn) of the (A-1) crystalline polyamide.
  • the (A-1) crystalline polyamide preferably has an Mw/Mn ratio of 1.0 or more, more preferably 1.8 or more, even more preferably 2.0 or more, and preferably 2.2 or less.
  • Examples of methods for controlling the Mw/Mn of the crystalline polyamide (A-1) within the above range include the following methods 1) and 2). 1) A method in which a known polycondensation catalyst such as phosphoric acid or sodium hypophosphite is added as an additive during the hot melt polymerization of polyamide. 2) In addition to the above method 1), a method of controlling polymerization conditions such as heating conditions and reduced pressure conditions.
  • a known polycondensation catalyst such as phosphoric acid or sodium hypophosphite
  • the Mw/Mn of crystalline polyamide (A-1) can be calculated using the Mw and Mn of crystalline polyamide (A-1) obtained using GPC.
  • the content of the crystalline polyamide (A-1) is preferably 50.0 mass% or more, more preferably 55.0 mass% or more, even more preferably 57.5 mass% or more, even more preferably 60.0 mass% or more, particularly preferably 62.5 mass% or more, and is preferably 90.0 mass% or less, more preferably 87.5 mass% or less, even more preferably 82.5 mass% or less, and particularly preferably 80.0 mass% or less, based on the total polyamide amount in the polyamide composition.
  • the content of crystalline polyamide (A-1) can be, for example, 10.0 mass% or more, 15.0 mass% or more, 20.0 mass% or more, or 25.0 mass% or more, relative to the total mass of the polyamide composition (100 mass%), and can be, for example, 60.0 mass% or less, 55.0 mass% or less, 53.0 mass% or less, or 50.0 mass% or less.
  • Amorphous polyamide refers to a polyamide having a crystallization enthalpy ⁇ H of less than 15 J/g when measured by a differential scanning calorimeter at 20° C./min.
  • the crystallization enthalpy of the amorphous polyamide (A-2) is preferably 10 J/g or less, more preferably 5 J/g or less, and even more preferably 0 J/g.
  • the crystallization enthalpy ⁇ H can be measured, for example, using a measuring device such as Diamond-DSC manufactured by PERKIN-ELMER in accordance with JIS-K7121.
  • the amorphous polyamide is not particularly limited as long as it has a crystallization enthalpy ⁇ H of less than or equal to the upper limit mentioned above, but may be a semi-aromatic polyamide.
  • the (A-2) amorphous polyamide is a semi-aromatic polyamide, it is preferably a polyamide containing (A-2a) dicarboxylic acid units and (A-2b) diamine units. In this case, it is more preferable that the (A-2) amorphous polyamide is a polyamide containing (A-2a) dicarboxylic acid units containing at least 50 mol% isophthalic acid units and (A-2b) diamine units containing at least 50 mol% diamine units having 4 to 10 carbon atoms.
  • the total amount of the isophthalic acid units and diamine units having 4 to 10 carbon atoms is preferably 75 mol% to 100 mol%, more preferably 90 mol% to 100 mol%, and even more preferably 100 mol%, relative to the total amount of all constituent units of the amorphous polyamide (A-2).
  • the proportion of the specified monomer units constituting the amorphous polyamide (A-2) in the present invention can be measured by nuclear magnetic resonance spectroscopy (NMR) or the like.
  • the content of the isophthalic acid unit relative to the total molar amount of the dicarboxylic acid unit is preferably 50 mol% or more, particularly preferably 75 mol% or more and 100 mol% or less, further preferably 90 mol% or more and 100 mol% or less, and particularly preferably 100 mol%.
  • the (A-2a) dicarboxylic acid units may contain aromatic dicarboxylic acid units other than isophthalic acid units, aliphatic dicarboxylic acid units, and alicyclic dicarboxylic acid units.
  • aromatic dicarboxylic acids constituting aromatic dicarboxylic acid units other than isophthalic acid units include, but are not limited to, dicarboxylic acids having a phenyl group or a naphthyl group.
  • the aromatic group of the aromatic dicarboxylic acid may be unsubstituted or substituted.
  • substituents are not particularly limited, but examples include alkyl groups having 1 to 4 carbon atoms, aryl groups having 6 to 10 carbon atoms, arylalkyl groups having 7 to 10 carbon atoms, halogen groups such as chloro and bromo groups, silyl groups having 1 to 6 carbon atoms, sulfonic acid groups and salts thereof (such as sodium salts), etc.
  • aromatic dicarboxylic acids having 8 to 20 carbon atoms which are unsubstituted or substituted with a specific substituent, such as terephthalic acid, naphthalenedicarboxylic acid, 2-chloroterephthalic acid, 2-methylterephthalic acid, 5-methylisophthalic acid, and 5-sodium sulfoisophthalic acid.
  • terephthalic acid is preferred.
  • the aromatic dicarboxylic acids constituting the aromatic dicarboxylic acid unit may be used alone or in combination of two or more.
  • aliphatic dicarboxylic acid unit examples include, but are not limited to, linear or branched saturated aliphatic dicarboxylic acids having 3 to 20 carbon atoms, such as malonic acid, dimethylmalonic acid, succinic acid, 2,2-dimethylsuccinic acid, 2,3-dimethylglutaric acid, 2,2-diethylsuccinic acid, 2,3-diethylglutaric acid, glutaric acid, 2,2-dimethylglutaric acid, adipic acid, 2-methyladipic acid, trimethyladipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, dodecanedioic acid, tetradecanedioic acid, hexadecanedioic acid, octadecanedioic acid, eicosane dioic acid, and dig
  • alicyclic dicarboxylic acid unit examples include, but are not limited to, alicyclic dicarboxylic acids having an alicyclic structure with 3 to 10 carbon atoms, and alicyclic dicarboxylic acids having an alicyclic structure with 5 to 10 carbon atoms are preferred.
  • examples of such alicyclic dicarboxylic acids include, but are not limited to, 1,4-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,3-cyclopentanedicarboxylic acid. Of these, 1,4-cyclohexanedicarboxylic acid is preferred.
  • the alicyclic dicarboxylic acids constituting the alicyclic dicarboxylic acid unit may be used alone or in combination of two or more.
  • the alicyclic group of the alicyclic dicarboxylic acid may be unsubstituted or may have a substituent.
  • substituent include, but are not limited to, alkyl groups having 1 to 4 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, and tert-butyl.
  • the dicarboxylic acid unit other than the isophthalic acid unit preferably contains an aromatic dicarboxylic acid unit, and more preferably contains an aromatic dicarboxylic acid having 6 to 12 carbon atoms.
  • the dicarboxylic acid constituting the (A-2a) dicarboxylic acid unit is not limited to the compounds described above as the dicarboxylic acid, but may be a compound equivalent to the dicarboxylic acid.
  • a compound equivalent to a dicarboxylic acid refers to a compound that can have a dicarboxylic acid structure similar to the dicarboxylic acid structure derived from the dicarboxylic acid. Examples of such compounds include, but are not limited to, anhydrides and halides of dicarboxylic acids.
  • (A-2) amorphous polyamide may further contain units derived from trivalent or higher polyvalent carboxylic acids such as trimellitic acid, trimesic acid, and pyromellitic acid, as necessary. Trivalent or higher polyvalent carboxylic acids may be used alone or in combination of two or more kinds.
  • the diamine units (A-2b) constituting the amorphous polyamide (A-2) preferably contain at least 50 mol % of diamine units having from 4 to 10 carbon atoms.
  • Examples of the diamine units include, but are not limited to, aliphatic diamine units, alicyclic diamine units, and aromatic diamine units.
  • aliphatic diamine constituting the aliphatic diamine unit
  • linear saturated aliphatic diamines having 2 to 20 carbon atoms such as ethylene diamine, propylene diamine, tetramethylene diamine, pentamethylene diamine, hexamethylene diamine, heptamethylene diamine, octamethylene diamine, nonamethylene diamine, decamethylene diamine, undecamethylene diamine, dodecamethylene diamine, and tridecamethylene diamine.
  • alicyclic diamine unit examples of alicyclic diamines (hereinafter also referred to as "alicyclic diamines") constituting the alicyclic diamine unit include, but are not limited to, 1,4-cyclohexanediamine, 1,3-cyclohexanediamine, 1,3-cyclopentanediamine, and the like.
  • aromatic diamine unit The aromatic diamine constituting the aromatic diamine unit is not limited to the following as long as it is a diamine containing an aromatic group, and examples thereof include metaxylylenediamine.
  • an aliphatic diamine unit is preferred, a diamine unit having a linear saturated aliphatic group having 4 to 10 carbon atoms is more preferred, a diamine unit having a linear saturated aliphatic group having 6 to 10 carbon atoms is even more preferred, and a hexamethylenediamine unit is particularly preferred.
  • Use of such a diamine tends to result in a polyamide composition that is more excellent in mechanical properties, particularly rigidity upon absorption of water, rigidity when hot, flowability, surface appearance, corrosion resistance, and the like.
  • the diamines may be used alone or in combination of two or more kinds.
  • polyamide 6I, 6I/6T, 9I, or 10I is preferred, 6I or 6I/6T is more preferred, and 6I is most preferred.
  • the amorphous polyamide (A-2) may further contain a trivalent or higher polyvalent aliphatic amine such as bishexamethylenetriamine, if necessary.
  • the trivalent or higher polyvalent aliphatic amines may be used alone or in combination of two or more kinds.
  • the amorphous polyamide (A-2) may further contain at least one unit selected from the group consisting of lactam units and aminocarboxylic acid units. By containing such units, a polyamide having superior toughness tends to be obtained.
  • the lactam and aminocarboxylic acid constituting the lactam unit and aminocarboxylic acid unit refer to lactam and aminocarboxylic acid capable of being polymerized (condensed).
  • lactam and aminocarboxylic acid constituting the lactam unit and aminocarboxylic acid unit are not limited to the following, but for example, lactams and aminocarboxylic acids having 4 to 14 carbon atoms are preferred, and lactams and aminocarboxylic acids having 6 to 12 carbon atoms are more preferred.
  • the lactams constituting the lactam units include, but are not limited to, butyrolactam, pivalolactam, ⁇ -caprolactam, caprylolactam, enantholactam, undecanolactam, laurolactam (dodecanolactam), etc.
  • ⁇ -caprolactam or laurolactam is preferred as the lactam, and ⁇ -caprolactam is more preferred.
  • the polyamide composition tends to have better toughness.
  • aminocarboxylic acids constituting the aminocarboxylic acid unit include, but are not limited to, ⁇ -aminocarboxylic acids, which are compounds formed by ring-opening of lactams, and ⁇ , ⁇ -amino acids.
  • the aminocarboxylic acid is preferably a linear or branched saturated aliphatic carboxylic acid having from 4 to 14 carbon atoms and substituted with an amino group at the ⁇ position.
  • examples of such aminocarboxylic acids include, but are not limited to, 6-aminocaproic acid, 11-aminoundecanoic acid, 12-aminododecanoic acid, etc.
  • examples of the aminocarboxylic acid include para-aminomethylbenzoic acid, etc.
  • lactam and aminocarboxylic acid constituting the lactam unit and aminocarboxylic acid unit may each be used alone or in combination of two or more kinds.
  • the total proportion (mol %) of lactam units and aminocarboxylic acid units is preferably 0 mol % or more and 20 mol % or less, more preferably 0 mol % or more and 10 mol % or less, and even more preferably 0 mol % or more and 5 mol % or less, based on the entire polyamide.
  • the total ratio of lactam units and aminocarboxylic acid units is within the above range, effects such as improved fluidity tend to be obtained.
  • the weight average molecular weight (Mw) of the amorphous polyamide (A-2) is preferably 10,000 or more, more preferably 13,000 or more, even more preferably 15,000 or more, particularly preferably 18,000 or more, most preferably 19,000 or more, preferably 35,000 or less, more preferably 33,000 or less, even more preferably 30,000 or less, even more preferably 29,000 or less, particularly preferably 27,000 or less, and most preferably 21,000 or less.
  • the weight average molecular weight (Mw) of the amorphous polyamide (A-2) can be measured using GPC.
  • the molecular weight distribution of the amorphous polyamide (A-2) is indicated by Mw/Mn, which is the value obtained by dividing the weight average molecular weight (Mw) of the amorphous polyamide (A-2) by the number average molecular weight (Mn) of the amorphous polyamide (A-2).
  • the Mw/Mn of the (A-2) amorphous polyamide is preferably 1.0 or more, more preferably 1.3 or more, even more preferably 1.5 or more, particularly preferably 1.8 or more, most preferably 2.0 or more, preferably 2.6 or less, more preferably 2.5 or less, and even more preferably 1.8 or more and 2.4 or less.
  • a polyamide composition having superior moldability and appearance can be obtained.
  • molded articles obtained from a polyamide composition containing a component such as an inorganic filler have superior surface appearance.
  • Examples of methods for controlling the Mw/Mn of the amorphous polyamide (A-2) within the above range include the following methods 1) and 2). 1) A method in which a known polycondensation catalyst such as phosphoric acid or sodium hypophosphite is added as an additive during the hot melt polymerization of polyamide. 2) In addition to the above method 1), a method in which polymerization conditions such as heating conditions and reduced pressure conditions are controlled to complete the polycondensation reaction at as low a temperature as possible and in as short a time as possible.
  • a known polycondensation catalyst such as phosphoric acid or sodium hypophosphite
  • the molecular weight distribution (Mw/Mn) of the amorphous polyamide (A-2) tends to increase with increasing molecular weight.
  • a high molecular weight distribution of the amorphous polyamide (A-2) indicates a high proportion of polyamide molecules having a three-dimensional molecular structure.
  • the Mw/Mn of the amorphous polyamide (A-2) within the above range, the progression of three-dimensional structuring of the molecules during high-temperature processing can be suppressed, and a polyamide composition with excellent flowability, welding strength, and better product appearance can be obtained.
  • the surface appearance of molded products obtained from polyamide compositions containing components such as inorganic fillers can be improved.
  • the Mw/Mn of the amorphous polyamide (A-2) can be calculated using the Mw and Mn of the amorphous polyamide (A-2) obtained using GPC.
  • the crystallization enthalpy ⁇ H of the amorphous polyamide (A-2) is preferably 15 J/g or less, more preferably 10 J/g or less, even more preferably 5 J/g or less, and particularly preferably 0 J/g.
  • a method for controlling the crystallization enthalpy ⁇ H of the (A-2) amorphous polyamide within the above range a method for reducing the crystallinity of a known polyamide can be used, and is not particularly limited.
  • the (A-2) amorphous polyamide preferably contains 50 mol% or more of isophthalic acid units, more preferably 75 mol% or more, and even more preferably 100 mol% of isophthalic acid units as the (A-2a) dicarboxylic acid units in the total dicarboxylic acid units constituting the (A-2) amorphous polyamide.
  • the crystallization enthalpy ⁇ H of amorphous polyamide can be measured, for example, in accordance with JIS-K7121 using a measuring device such as Diamond-DSC manufactured by PERKIN-ELMER.
  • the content of the amorphous polyamide (A-2) relative to the total mass (100 mass%) of the polyamide composition can be, for example, 1.0 mass% or more and 60.0 mass% or less, 3.0 mass% or more and 40.0 mass% or less, 5.0 mass% or more and 30.0 mass% or less, or 7.0 mass% or more and 25.0 mass% or less.
  • it can be 1.0 mass% or more and 60.0 mass% or less, 3.0 mass% or more and 40.0 mass% or less, 5.0 mass% or more and 30.0 mass% or less, or 7.0 mass% or more and 25.0 mass% or less.
  • At least one polyamide selected from the group consisting of (A-1) crystalline polyamide and (A-2) amorphous polyamide has terminals blocked with an end-capping agent.
  • Such an end-capping agent can also be added as a molecular weight regulator when producing a polyamide from the above-mentioned dicarboxylic acid, diamine, and, if necessary, at least one compound selected from the group consisting of lactam and aminocarboxylic acid.
  • End-capping agents include, but are not limited to, acid anhydrides, monoisocyanates, monoacid halides, monoesters, monoalcohols, etc.
  • acid anhydrides include monocarboxylic acids, monoamines, phthalic anhydride, etc. Among these, monocarboxylic acids or monoamines are preferred.
  • the end-capping agents may be used alone or in combination of two or more types.
  • Monocarboxylic acids that can be used as end-capping agents may be any monocarboxylic acid that is reactive with amino groups that may be present at the ends of polyamides.
  • Specific examples of monocarboxylic acids include, but are not limited to, aliphatic monocarboxylic acids, alicyclic monocarboxylic acids, and aromatic monocarboxylic acids.
  • Examples of aliphatic monocarboxylic acids include, but are not limited to, formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, caprylic acid, lauric acid, tridecylic acid, myristic acid, palmitic acid, stearic acid, pivalic acid, and isobutyric acid.
  • Examples of alicyclic monocarboxylic acids include, but are not limited to, cyclohexane carboxylic acid.
  • Examples of aromatic monocarboxylic acids include, but are not limited to, benzoic acid, toluic acid, ⁇ -naphthalene carboxylic acid, ⁇ -naphthalene carboxylic acid, methylnaphthalene carboxylic acid, and phenyl acetic acid. These monocarboxylic acids may be used alone or in combination of two or more.
  • Monoamines that can be used as end-capping agents may be any monoamine that is reactive with carboxyl groups that may be present at the ends of polyamides.
  • Specific examples of monoamines include, but are not limited to, aliphatic monoamines, alicyclic monoamines, and aromatic monoamines.
  • Examples of aliphatic amines include, but are not limited to, methylamine, ethylamine, propylamine, butylamine, hexylamine, octylamine, decylamine, stearylamine, dimethylamine, diethylamine, dipropylamine, and dibutylamine.
  • alicyclic amines include, but are not limited to, cyclohexylamine and dicyclohexylamine.
  • aromatic amines include, but are not limited to, aniline, toluidine, diphenylamine, and naphthylamine. These monoamines may be used alone or in combination of two or more.
  • the amount of dicarboxylic acid and the amount of diamine added are preferably approximately the same molar amount.
  • the molar amount of the total diamines relative to the total molar amount of dicarboxylic acids is preferably 0.9 or more, more preferably 0.95 or more, and even more preferably 0.98 or more, preferably 1.2 or less, more preferably 1.1 or less, and even more preferably 1.05 or less.
  • the method for producing polyamide includes, but is not limited to, the following polymerization step (1) or (2).
  • (1) A step of polymerizing a combination of a dicarboxylic acid constituting a dicarboxylic acid unit and a diamine constituting a diamine unit to obtain a polymer.
  • (2) A step of polymerizing one or more members selected from the group consisting of lactams constituting the lactam units and aminocarboxylic acids constituting the aminocarboxylic acid units to obtain a polymer.
  • the method for producing polyamide preferably further includes, after the polymerization step, an increase step for increasing the degree of polymerization of the polyamide. If necessary, the method may include, after the polymerization step and the increase step, a sealing step for sealing the ends of the obtained polymer with a terminal sealing agent.
  • Specific methods for producing polyamide include, for example, the various methods exemplified in 1) to 4) below.
  • 1) A method in which an aqueous solution or suspension of one or more selected from the group consisting of a dicarboxylic acid-diamine salt, a mixture of a dicarboxylic acid and a diamine, a lactam, and an aminocarboxylic acid is heated and polymerized while maintaining the molten state (hereinafter, may be referred to as a "thermal melt polymerization method").
  • hot melt polymerization/solid phase polymerization method A method in which the degree of polymerization of the polyamide obtained by the hot melt polymerization method is increased while maintaining the polyamide in a solid state at a temperature below the melting point.
  • solid-state polymerization method A method of polymerization using a dicarboxylic acid halide component equivalent to a dicarboxylic acid and a diamine component (hereinafter, sometimes referred to as a "solution method”).
  • the polymerization form is not particularly limited, and may be a batch type or a continuous type.
  • the polymerization apparatus used for producing polyamide is not particularly limited, and known apparatuses can be used. Specific examples of the polymerization apparatus include an autoclave type reactor, a tumbler type reactor, and an extruder type reactor (such as a kneader).
  • an aqueous solution containing about 40% to 60% by mass of raw material components for polyamide (a combination of dicarboxylic acid and diamine, and, if necessary, at least one selected from the group consisting of lactam and aminocarboxylic acid) is prepared.
  • the aqueous solution is concentrated to about 65% to 90% by mass in a concentration tank operated at a temperature of 110°C to 180°C and a pressure of about 0.035 MPa to 0.6 MPa (gauge pressure) to obtain a concentrated solution.
  • the concentrated solution obtained is transferred to an autoclave, and heating continues until the pressure in the autoclave is about 1.2 MPa or more and 2.2 MPa or less (gauge pressure).
  • the pressure is maintained at about 1.2 MPa or more and 2.2 MPa or less (gauge pressure) while at least one of the water and gas components is removed.
  • the pressure is reduced to atmospheric pressure (gauge pressure is 0 MPa). After the pressure in the autoclave is reduced to atmospheric pressure, the pressure can be reduced as necessary to effectively remove the by-product water.
  • the autoclave is then pressurized with an inert gas such as nitrogen, and the polyamide melt is extruded from the autoclave as strands.
  • the extruded strands are cooled and cut to obtain polyamide pellets.
  • the polymer terminals of the polyamides ((A-1) crystalline polyamide and (A-2) amorphous polyamide) contained in the polyamide composition of the present embodiment are not particularly limited, but can be classified and defined as follows: 1) to 4). That is, 1) the amino terminus, 2) the carboxy terminus, 3) the terminus provided by a capping agent, and 4) the other terminus.
  • the amino terminus is a polymer end having an amino group (-NH2 group ) and is derived from a diamine unit.
  • the carboxy terminal is a polymer end having a carboxy group (—COOH group) and is derived from a dicarboxylic acid.
  • terminal end by a capping agent refers to an end formed when a capping agent is added during polymerization.
  • examples of the capping agent include the terminal capping agents described below.
  • "Other terminals" are polymer terminals that are not classified into the above-mentioned 1) to 3). Specific examples of other terminals include terminals generated by deammonia reaction of amino terminals, terminals generated by decarboxylation of carboxy terminals, etc.
  • phosphinic acid-phosphonic acid complex metal salts phosphinic acid-phosphonic acid complex metal salts> Specifically, the phosphinic acid flame retardant includes at least one phosphinic acid-phosphonic acid complex metal salt selected from the group consisting of condensates (derivatives) of phosphinic acid-phosphonic acid complex metal salts represented by the following general formula (1):
  • R 1 , R 2 , and R 3 are each independently an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 10 carbon atoms.
  • M m+ is a metal ion.
  • M is an element belonging to Group 2 or Group 15 of the periodic table, a transition element, zinc, aluminum, or a combination thereof.
  • m is 2 to 3.
  • the plurality of R 1s and R 2s may be the same or different.
  • the median diameter (D50) of component (B) observed from the polyamide composition (e.g., in the form of pellets) or a molded article obtained by molding the polyamide composition is 2.5 to 6.0 ⁇ m.
  • the ratio (d75/d25) of the particle diameter (d25) of the smallest 25% (particle number) of particles to the particle diameter (d75) of the smallest 75% (particle number) of particles is less than 2.0.
  • R 1 , R 2 , and R 3 are each independently an alkyl group having 1 to 6 carbon atoms, or an aryl group having 6 to 10 carbon atoms.
  • R 1 , R 2 , and R 3 are each independently an alkyl group having 1 to 6 carbon atoms, or an aryl group having 6 to 10 carbon atoms.
  • the plurality of R 1s and R 2s may be the same or different, but are preferably the same in terms of ease of production.
  • the alkyl group may be either chain-like or cyclic, but is preferably chain-like.
  • the chain-like alkyl group may be either linear or branched. Examples of linear alkyl groups include methyl, ethyl, n-propyl, n-butyl, n-pentyl, and n-hexyl groups.
  • branched alkyl groups include 1-methylethyl, 1-methylpropyl, 2-methylpropyl, 1,1-dimethylethyl, 1-methylbutyl, 2-methylbutyl, 3-methylbutyl, 1,1-dimethylpropyl, 1,2-dimethylpropyl, 2,2-dimethylpropyl, 1-methylpentyl, 2-methylpentyl, 3-methylpentyl, 4-methylpentyl, 1,1-dimethylbutyl, 1,2-dimethylbutyl, 1,3-dimethylbutyl, 2,2-dimethylbutyl, 2,3-dimethylbutyl, 3,3-dimethylbutyl, 1-ethylbutyl, 2-ethylbutyl, and 1,1,2-trimethylpropyl groups.
  • aryl groups include phenyl and naphthyl groups.
  • the alkyl group and the aryl group may have a substituent.
  • substituent in the alkyl group include an aryl group having 6 to 10 carbon atoms.
  • substituent in the aryl group include an alkyl group having 1 to 6 carbon atoms.
  • [M] M is independently an element belonging to Group 2 or Group 15 of the periodic table, a transition element, zinc, or aluminum, or a combination thereof.
  • elements belonging to Group 2 of the periodic table include calcium and magnesium.
  • elements belonging to Group 15 of the periodic table include bismuth. Among them, aluminum is preferred as M.
  • [m+] m+ represents the average cationic valence of M and is 2 to 3.
  • the cationic valence of each M is 2 or 3.
  • m+ can be appropriately selected depending on the type of M and the number of diphosphinic acids.
  • [a and b] a represents the average number of phosphinic acid anions per molecule, and can be appropriately selected depending on the type and number of M.
  • b represents the average number of phosphonate anions per molecule. It can be appropriately selected depending on the type and number of M.
  • a flame retardant represented by chemical formula (1) which is a composite salt of a phosphinate and a phosphonate, is preferred from the viewpoints of heat resistance, flame retardancy, and metal corrosion resistance.
  • Specific examples of the product include "HR8900”, “MADP8900SP”, “MADP8900BS”, and "HR8966” manufactured by Weihai Hirun Co., Ltd.
  • the flame retardant may be in the form of a powder, a columnar, or a scale-like type, but from the viewpoint of extrusion operability and dispersibility, the columnar or scale-like type is preferred.
  • the bulk density is preferably 0.4 to 0.9 g/cm 3 , more preferably 0.5 to 0.8 g/cm 3. More preferably, it is 0.6 to 0.7 g/cm 3. By setting it in this range, less air is brought in during feeding, the torque is stabilized, and it is also easy to disperse in the extruder.
  • the collapse strength is preferably 0.1 N or more, more preferably 1 N or more, more preferably 5 N or more, and preferably 50 N or less, more preferably 30 N or less, and more preferably 20 N or less. By setting it in this range, a polyamide composition with excellent continuous operability and dispersibility can be obtained.
  • the collapse strength can be measured as follows.
  • the collapse stress (unit: N) as the collapse strength of the flame retardant can be measured using a Kiya hardness tester (manufactured by Fujiwara Seisakusho Co., Ltd., product name "043019-A").
  • the measured value may be the average value of 25 granules.
  • the flame retardant granules are allowed to fall naturally into a 1-liter measure, the measure is filled to the brim, and a volume of exactly 1 liter is weighed and the weight is measured, whereby the bulk density (unit: g/ml) of the flame retardant granules can be calculated.
  • the content of the phosphorus-based flame retardant is preferably 10% by mass or more, more preferably 12% by mass or more, particularly preferably 14% by mass or more, and preferably 30% by mass or less, more preferably 25% by mass or less, particularly preferably 20% by mass or less, based on the total mass of the (A-1) crystalline polyamide and the (A-2) amorphous polyamide.
  • a polyamide composition with superior flame retardancy can be obtained.
  • a polyamide composition with superior flame retardancy can be obtained without impairing the properties of the polyamide.
  • the dispersed particle diameter of the phosphorus-based flame retardant is 2.5 ⁇ m or more, preferably 3.0 ⁇ m or more, and 6.0 ⁇ m or less, preferably 5.0 ⁇ m or less, in terms of median diameter (D50).
  • the ratio (d75/d25) of the particle diameter (d25) of the particles that are 25% (number of particles) from the smallest particle diameter to the particle diameter (d75) of the particles that are 75% (number of particles) is preferably less than 2.0, more preferably less than 1.9. By making it equal to or greater than the above lower limit, a polyamide composition having excellent flame retardancy and metal corrosion resistance can be obtained.
  • the dispersed particle diameter of the phosphorus-based flame retardant can be calculated based on an observation image of a digital microscope, SEM, etc.
  • the polyamide composition of the present embodiment further contains (C) an inorganic filler in addition to the above-mentioned components (A) and (B).
  • Inorganic fillers include, but are not limited to, glass fiber, carbon fiber, calcium silicate fiber, potassium titanate fiber, aluminum borate fiber, clay, flaky glass, talc, kaolin, mica, hydrotalcite, calcium carbonate, magnesium carbonate, zinc carbonate, zinc oxide, calcium hydrogen phosphate, wollastonite, silica, zeolite, alumina, boehmite, aluminum hydroxide, titanium oxide, silicon oxide, magnesium oxide, calcium silicate, sodium aluminosilicate, magnesium silicate, ketjen black, acetylene black, furnace black, carbon nanotubes, graphite, brass, copper, silver, aluminum, nickel, iron, calcium fluoride, montmorillonite, swellable fluoromica, apatite, etc. These inorganic fillers may be used alone or in combination of two or more.
  • one or more selected from the group consisting of glass fiber, carbon fiber, wollastonite, kaolin, mica, talc, calcium carbonate, magnesium carbonate, potassium titanate fiber, aluminum borate fiber, and clay are preferred. Furthermore, among these, one or more selected from the group consisting of glass fiber, carbon fiber, wollastonite, kaolin, mica, talc, calcium carbonate, and clay are more preferred. Glass fiber is the most preferred.
  • the number average fiber diameter (d) is preferably 3 ⁇ m or more and 30 ⁇ m or less, more preferably 3 ⁇ m or more and 20 ⁇ m or less, even more preferably 3 ⁇ m or more and 12 ⁇ m or less, particularly preferably 3 ⁇ m or more and 9 ⁇ m or less, and most preferably 4 ⁇ m or more and 6 ⁇ m or less.
  • a polyamide composition with superior toughness and surface appearance of molded products can be obtained.
  • a polyamide composition with a superior balance between cost, powder handling, and physical properties (fluidity, etc.) can be obtained.
  • a polyamide composition with superior vibration fatigue properties and sliding properties can be obtained.
  • the cross section may be circular or flat.
  • flat cross sections include, but are not limited to, rectangular, oval close to rectangular, elliptical, and cocoon-shaped with a narrowed central portion in the longitudinal direction.
  • "flatness" in this specification refers to the value expressed as d2/d1, where d2 is the long diameter of the fiber cross section and d1 is the short diameter of the fiber cross section (a perfect circle has a flatness of approximately 1).
  • the number average fiber diameter (d) is 3 ⁇ m or more and 30 ⁇ m or less
  • the weight average fiber length (l) is 100 ⁇ m or more and 750 ⁇ m or less
  • the ratio of the weight average fiber length (l) to the number average fiber diameter (d), i.e., the aspect ratio (l/d) is 10 to 100.
  • the "number average fiber diameter (d)" referred to here is the average value of the long diameter (d2 above) of the fiber cross section, and is calculated using the calculation method described below.
  • the aspect ratio is preferably 1.5 or more, more preferably 2.5 or more, particularly preferably more than 3.0, most preferably 3.1 or more, preferably 10.0 or less, more preferably 10.0 or less, and most preferably 6.0 or less.
  • the thickness of glass fibers or carbon fibers with an aspect ratio of 1.5 or more is not limited to the following, but it is preferable that the short diameter d1 of the fiber cross section is 0.5 ⁇ m or more and 25 ⁇ m or less, and the long diameter d2 of the fiber cross section is 1.25 ⁇ m or more and 250 ⁇ m or less. It is more preferable that the short diameter d1 of the fiber cross section is 3.0 ⁇ m or more and 25 ⁇ m or less, and the long diameter d2 of the fiber cross section is 1.25 ⁇ m or more and 250 ⁇ m or less.
  • Glass fibers or carbon fibers with an aspect ratio of 1.5 or more are preferably glass fibers manufactured using either an orifice plate having a number of orifices on the bottom surface, with a convex edge surrounding the multiple orifice outlets and extending downward from the bottom surface, or a nozzle tip for spinning irregular cross-section glass fibers, with a nozzle tip having a single or multiple orifice holes and multiple convex edges extending downward from the tip of the outer periphery.
  • These fibrous reinforcing materials may be used as they are as fiber strands, as rovings, or may be further cut and used as chopped glass strands.
  • the "number average fiber diameter (d)" and "weight average fiber length (l)" in this specification can be determined by the following method. First, the polyamide composition is placed in an electric furnace, and the organic matter contained therein is incinerated. From the residue after the treatment, 100 or more glass fibers (or carbon fibers) are arbitrarily selected, observed with a scanning electron microscope (SEM), and the fiber diameter (long diameter) of these glass fibers (or carbon fibers) is measured, whereby the number average fiber diameter can be determined. In addition, the weight average fiber length can be determined by measuring the fiber length using an SEM photograph of the 100 or more glass fibers (or carbon fibers) taken at a magnification of 1000 times.
  • SEM scanning electron microscope
  • the glass fibers or carbon fibers may be surface-treated with a silane coupling agent or the like.
  • silane coupling agents include, but are not limited to, aminosilanes, mercaptosilanes, epoxysilanes, vinylsilanes, etc.
  • aminosilanes include ⁇ -aminopropyltriethoxysilane, ⁇ -aminopropyltrimethoxysilane, N- ⁇ -(aminoethyl)- ⁇ -aminopropylmethyldimethoxysilane, etc.
  • silane coupling agents examples include ⁇ -mercaptopropyltrimethoxysilane and ⁇ -mercaptopropyltriethoxysilane.
  • silane coupling agents may be used alone or in combination of two or more. Among them, aminosilanes are preferred as silane coupling agents.
  • the glass fibers or carbon fibers may further contain a sizing agent.
  • sizing agents include copolymers containing, as constituent units, carboxylic acid anhydride-containing unsaturated vinyl monomers and unsaturated vinyl monomers other than carboxylic acid anhydride-containing unsaturated vinyl monomers, epoxy compounds, polyurethane resins, homopolymers of acrylic acid, copolymers of acrylic acid and other copolymerizable monomers, and salts of these with primary, secondary, and tertiary amines, etc. These sizing agents may be used alone or in combination of two or more.
  • the bundling agent is preferably one or more selected from the group consisting of a copolymer containing a carboxylic anhydride-containing unsaturated vinyl monomer and an unsaturated vinyl monomer other than the carboxylic anhydride-containing unsaturated vinyl monomer as constituent units, an epoxy compound, and a polyurethane resin. Also, one or more selected from the group consisting of a copolymer containing a carboxylic anhydride-containing unsaturated vinyl monomer and an unsaturated vinyl monomer other than the carboxylic anhydride-containing unsaturated vinyl monomer as constituent units, and a polyurethane resin is more preferable.
  • Glass fibers or carbon fibers are obtained by continuously reacting the fibers with the bundling agent in a known process for producing the fibers, using a known method such as a roller-type applicator, to produce fiber strands, which are then dried.
  • the fiber strands may be used as rovings as they are, or may be further cut and used as chopped glass strands.
  • the sizing agent is preferably added in an amount of about 0.2% by mass or more, more preferably about 0.3% by mass or more, more preferably about 3% by mass or less, and more preferably about 2% by mass or less, in terms of solid content, relative to the total mass of the glass fibers or carbon fibers.
  • the amount of the sizing agent added is equal to or more than the above lower limit in terms of solid content, relative to the total mass of the glass fibers or carbon fibers, the bundling of the fibers can be more effectively maintained.
  • the amount of the sizing agent added is equal to or less than the above upper limit in terms of solid content, relative to the total mass of the glass fibers or carbon fibers, the thermal stability of the obtained polyamide composition is further improved. Drying of the strands may occur after the cutting step, or the strands may be dried and then cut.
  • inorganic fillers other than glass fiber and carbon fiber from the viewpoint of improving the strength, rigidity and surface appearance of the molded product, wollastonite, kaolin, mica, talc, calcium carbonate, magnesium carbonate, potassium titanate fiber, aluminum borate fiber or clay is preferred. Wollastonite, kaolin, mica, talc, calcium carbonate or clay is more preferred. Wollastonite, kaolin, mica or talc is even more preferred. Wollastonite, mica or talc is particularly preferred. These inorganic fillers may be used alone or in combination of two or more types.
  • the average particle size of inorganic fillers other than glass fiber and carbon fiber is preferably 0.01 ⁇ m or more, more preferably 0.03 ⁇ m or more, even more preferably 0.05 ⁇ m or more, even more preferably 0.10 ⁇ m or more, particularly preferably 0.15 ⁇ m or more, preferably 38 ⁇ m or less, more preferably 30 ⁇ m or less, even more preferably 25 ⁇ m or less, even more preferably 20 ⁇ m or less, particularly preferably 15 ⁇ m or less, from the viewpoint of improving toughness and the surface appearance of the molded product.
  • a polyamide composition with superior toughness and surface appearance of the molded product can be obtained.
  • a polyamide composition with a superior balance between cost, powder handling, and physical properties (fluidity, etc.) can be obtained.
  • the number average particle diameter (hereinafter sometimes simply referred to as "average particle diameter") is taken as the average particle diameter. Also, if the cross section is not circular, the maximum length is taken as the (number average) fiber diameter.
  • the number average particle length of the acicular inorganic filler (hereinafter sometimes simply referred to as "average particle length") is preferably within the numerical range calculated from the preferred range of the number average particle diameter described above and the preferred range of the aspect ratio (l/d) of the number average particle length (l) to the number average particle diameter (d) described below.
  • the aspect ratio (l/d) of the number average particle length (l) to the number average particle diameter (d) is preferably 1.5 or more, more preferably 2.0 or more, and even more preferably 2.5 or more, from the viewpoint of improving the surface appearance of the molded product and preventing wear of metallic parts of the injection molding machine, etc., and is preferably 10 or less, more preferably 5 or less, and even more preferably 4 or less.
  • inorganic fillers other than glass fiber and carbon fiber may be surface-treated using a silane coupling agent, a titanate-based coupling agent, or the like.
  • silane coupling agents include those exemplified for glass fiber and carbon fiber above. Among them, aminosilanes are preferred as silane coupling agents.
  • Such surface treatment agents may be applied to the surface of the inorganic filler in advance, or may be added when mixing the polyamide and the inorganic filler. Furthermore, the amount of surface treatment agent added is preferably 0.05% by mass or more and 1.5% by mass or less based on the total mass of the inorganic filler.
  • the content of the inorganic filler is preferably 5% by mass or more, more preferably 20% by mass or more, even more preferably 25% by mass or more, particularly preferably 30% by mass or less, most preferably 35% by mass or more, more preferably 70% by mass or less, more preferably 65% by mass or less, even more preferably 60% by mass or less, and most preferably 50% by mass or less, based on the total mass 100% of the polyamide composition.
  • the content of the inorganic filler being equal to or more than the lower limit, the effect of further improving the strength and rigidity of the obtained polyamide composition is exhibited.
  • the content of the inorganic filler being equal to or less than the upper limit, a polyamide composition having better extrudability and moldability can be obtained.
  • the polyamide composition of the present embodiment may contain, in addition to the above-mentioned components (A) to (C), one or more other components (D) selected from the group consisting of flame retardant auxiliaries, lubricants, heat stabilizers, phosphorus-based flame retardants, nucleating agents, other polymers, and other additives.
  • D flame retardant auxiliaries, lubricants, heat stabilizers, phosphorus-based flame retardants, nucleating agents, other polymers, and other additives.
  • Anhydrous zinc borate can be used as a flame retardant auxiliary.
  • the ratio of anhydrous zinc borate to (B) the phosphorus-based flame retardant is preferably 2:98 to 10:90 from the viewpoint of flame retardancy efficiency.
  • the lubricant is not particularly limited, but examples thereof include higher fatty acids, higher fatty acid metal salts, higher fatty acid esters, higher fatty acid amides, etc.
  • the lubricant can also be used as a molding improver.
  • higher fatty acids examples include linear or branched, saturated or unsaturated aliphatic monocarboxylic acids having 8 to 40 carbon atoms.
  • linear or branched, saturated or unsaturated aliphatic monocarboxylic acids having 8 to 40 carbon atoms examples include lauric acid, palmitic acid, stearic acid, behenic acid, and montanic acid.
  • branched saturated aliphatic monocarboxylic acids having 8 to 40 carbon atoms examples include isopalmitic acid and isostearic acid.
  • linear unsaturated aliphatic monocarboxylic acids having 8 to 40 carbon atoms examples include oleic acid and erucic acid.
  • branched unsaturated aliphatic monocarboxylic acids having 8 to 40 carbon atoms examples include isooleic acid. Among these, stearic acid or montanic acid is preferable as the higher fatty acid.
  • the higher fatty acid metal salt is a metal salt of a higher fatty acid.
  • the metal element of the metal salt include elements of Groups 1, 2, and 3 of the Periodic Table of Elements, zinc, aluminum, etc.
  • elements of Group 1 of the Periodic Table of Elements include sodium, potassium, etc.
  • Examples of Group 2 elements in the Periodic Table include calcium, magnesium, etc.
  • Examples of Group 3 elements in the Periodic Table include scandium, yttrium, etc. Among these, Groups 1 and 2 elements in the Periodic Table or aluminum are preferred, and sodium, potassium, calcium, magnesium, or aluminum is more preferred.
  • higher fatty acid metal salts include calcium stearate, aluminum stearate, zinc stearate, magnesium stearate, calcium montanate, sodium montanate, calcium palmitate, etc.
  • metal salts of montanic acid and metal salts of stearic acid are preferred as higher fatty acid metal salts.
  • the higher fatty acid ester is an ester of a higher fatty acid and an alcohol.
  • an ester of an aliphatic carboxylic acid having 8 to 40 carbon atoms and an aliphatic alcohol having 8 to 40 carbon atoms is preferable.
  • the aliphatic alcohol having 8 to 40 carbon atoms for example, stearyl alcohol, behenyl alcohol, lauryl alcohol, etc. are mentioned.
  • Specific examples of the higher fatty acid ester include stearyl stearate, behenyl behenate, etc.
  • the higher fatty acid amide is an amide compound of a higher fatty acid.
  • Examples of the higher fatty acid amide include stearic acid amide, oleic acid amide, erucic acid amide, ethylene bisstearylamide, ethylene bisoleylamide, N-stearyl stearic acid amide, and N-stearyl erucic acid amide.
  • higher fatty acids higher fatty acid metal salts, higher fatty acid esters, and higher fatty acid amides may be used alone or in combination of two or more kinds.
  • the content of the lubricant in the polyamide composition is preferably 0.01% by mass or more and 1% by mass or less, and more preferably 0.1% by mass or more and 1% by mass or less, relative to the total mass of the polyamide composition (100% by mass).
  • the content of the lubricant is equal to or more than the lower limit, the moldability of the polyamide composition can be improved, while when the content is equal to or less than the upper limit, the rigidity of the molded product can be improved.
  • Heat stabilizer examples include, but are not limited to, phenol-based heat stabilizers, phosphorus-based heat stabilizers, amine-based heat stabilizers, metal salts of elements in Groups 3, 4, and 11 to 14 of the Periodic Table, and halides of alkali metals and alkaline earth metals.
  • phenol-based heat stabilizer examples include, but are not limited to, hindered phenol compounds, etc. Hindered phenol compounds have the property of imparting excellent heat resistance and light resistance to resins such as polyamides and fibers.
  • Hindered phenol compounds include, but are not limited to, N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide), pentaerythrityl-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], N,N'-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamamide), triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate], ester], 3,9-bis ⁇ 2-[3-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]-1,1-dimethylethyl ⁇ -2,4,8,10-tetraoxaspiro[5,5]undecane, 3,5-di-tert-butyl-4-hydroxybenzy
  • hindered phenol compounds may be used alone or in combination of two or more.
  • the hindered phenol compound is preferably N,N'-hexane-1,6-diylbis[3-(3,5-di-tert-butyl-4-hydroxyphenylpropionamide)].
  • the content of the phenol-based heat stabilizer in the polyamide composition is preferably 0.01% by mass or more and 1% by mass or less, and more preferably 0.1% by mass or more and 1% by mass or less, relative to 100% by mass of the total mass of the polyamide composition.
  • the content of the phenol-based heat stabilizer is within the above range, the heat aging resistance of the polyamide composition can be further improved and the amount of gas generation can be further reduced.
  • phosphorus-based heat stabilizer examples include, but are not limited to, pentaerythritol-type phosphite compounds, trioctyl phosphite, trilauryl phosphite, tridecyl phosphite, octyl diphenyl phosphite, trisisodecyl phosphite, phenyl diisodecyl phosphite, phenyl di(tridecyl)phosphite, diphenyl isooctyl phosphite, diphenyl isodecyl phosphite, diphenyl (tridecyl) phosphite, triphenyl phosphite, tris(nonylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphi
  • phosphorus-based heat stabilizers may be used alone or in combination of two or more.
  • the phosphorus-based heat stabilizer is preferably at least one selected from the group consisting of pentaerythritol-type phosphite compounds and tris(2,4-di-tert-butylphenyl)phosphite.
  • Pentaerythritol-type phosphite compounds include, but are not limited to, 2,6-di-tert-butyl-4-methylphenyl-phenyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-methyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-2-ethylhexyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-isodecyl-pentaerythritol diphosphite, 2,6-di-tert-butyl-4-methylphenyl-lauryl-pentaerythritol diphosphite, 2,6-di -tert-butyl-4-methylphenyl-isotridecyl-penta
  • pentaerythritol type phosphite compounds may be used alone or in combination of two or more.
  • the pentaerythritol-type phosphite compound is preferably one or more selected from the group consisting of bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-ethylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-amyl-4-methylphenyl)pentaerythritol diphosphite, and bis(2,6-di-tert-octyl-4-methylphenyl)pentaerythritol diphosphite, and more preferably bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, and
  • the content of the phosphorus-based heat stabilizer in the polyamide composition is preferably 0.01% by mass or more and 1% by mass or less, and more preferably 0.1% by mass or more and 1% by mass or less, relative to 100% by mass of the total mass of the polyamide composition.
  • the content of the phosphorus-based heat stabilizer is within the above range, the heat aging resistance of the polyamide composition can be further improved and the amount of gas generation can be further reduced.
  • amine-based heat stabilizer examples include, but are not limited to, 4-acetoxy-2,2,6,6-tetramethylpiperidine, 4-stearoyloxy-2,2,6,6-tetramethylpiperidine, 4-acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-(phenylacetoxy)-2,2,6,6-tetramethylpiperidine, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, 4-methoxy-2,2,6,6-tetramethylpiperidine, 4-stearyloxy-2,2,6,6-tetramethylpiperidine, 4-cyclohexyloxy-2,2,6,6-tetramethylpiperidine, 4-benzyloxy-2,2,6, 6-tetramethylpiperidine, 4-phenoxy-2,2,6,6-tetramethylpiperidine, 4-(ethylcarbamoyloxy)-2,2,6,6-tetramethylpiperidine, 4-(cyclohex
  • the content of the amine-based heat stabilizer in the polyamide composition is preferably 0.01% by mass or more and 1% by mass or less, and more preferably 0.1% by mass or more and 1% by mass or less, relative to 100% by mass of the total mass of the polyamide composition.
  • the content of the amine-based heat stabilizer is within the above range, the heat aging resistance of the polyamide composition can be further improved, and the amount of gas generation can be further reduced.
  • the copper salt is preferably at least one selected from the group consisting of copper iodide, copper (I) bromide, copper (II) bromide, copper (I) chloride, and copper acetate, and more preferably at least one selected from the group consisting of copper iodide and copper acetate.
  • a polyamide composition is obtained which is more excellent in heat aging resistance and can more effectively suppress metal corrosion of the screw and cylinder during extrusion (hereinafter, sometimes simply referred to as "metal corrosion").
  • the content of the copper salt in the polyamide composition is preferably 0.01 mass % or more and 0.60 mass % or less, and more preferably 0.02 mass % or more and 0.40 mass % or less, based on the total mass of the polyamides (the crystalline polyamide (A-1) and the amorphous polyamide (A-2)).
  • the content of the copper salt is within the above range, the heat aging resistance of the polyamide composition can be further improved, and copper precipitation and metal corrosion can be more effectively suppressed.
  • the content concentration of the copper element derived from the copper salt is preferably 10 parts by mass or more and 2000 parts by mass or less, more preferably 30 parts by mass or more and 1500 parts by mass or less, and even more preferably 50 parts by mass or more and 500 parts by mass or less, relative to 106 parts by mass (1 million parts by mass) of the polyamide (crystalline polyamide (A-1) and amorphous polyamide (A-2)).
  • alkali metal and alkaline earth metal halides examples include, but are not limited to, potassium iodide, potassium bromide, potassium chloride, sodium iodide, sodium chloride, and the like.
  • alkali metal and alkaline earth metal halides may be used alone or in combination of two or more kinds.
  • the alkali metal and alkaline earth metal halides are preferably one or more selected from the group consisting of potassium iodide and potassium bromide, and more preferably potassium iodide.
  • the content of alkali metal and alkaline earth metal halides in the polyamide composition is preferably 0.05 parts by mass or more, more preferably 0.2 parts by mass or more, and preferably 20 parts by mass or less, more preferably 10 parts by mass or less, per 100 parts by mass of polyamide ((A-1) crystalline polyamide and (A-2) amorphous polyamide).
  • the content of alkali metal and alkaline earth metal halides is within the above range, the heat aging resistance of the polyamide composition is further improved, and copper precipitation and metal corrosion can be more effectively suppressed.
  • the heat stabilizer components described above may be used alone or in combination of two or more. Among them, hindered phenol compounds are preferred as heat stabilizers from the viewpoint of further improving the heat aging resistance of the polyamide composition.
  • the nucleating agent refers to a substance that, when added, provides at least one of the following effects (1) to (3): (1) The effect of increasing the crystallization peak temperature of the polyamide composition. (2) The effect of reducing the difference between the extrapolated onset temperature and the extrapolated end temperature of the crystallization peak. (3) The effect of making the spherulites in the resulting molded product finer and more uniform in size.
  • Nucleating agents include, but are not limited to, talc, boron nitride, mica, kaolin, silicon nitride, potassium titanate, molybdenum disulfide, etc.
  • the nucleating agents may be used alone or in combination of two or more. Among them, talc or boron nitride is preferred as the nucleating agent from the viewpoint of nucleating agent effect.
  • the number average particle size of the nucleating agent is preferably 0.01 ⁇ m or more and 10 ⁇ m or less.
  • the number average particle size of the nucleating agent can be measured using the following method. First, the molded product is dissolved in a solvent in which polyamide is soluble, such as formic acid. Next, from the resulting insoluble components, for example, 100 or more nucleating agents are arbitrarily selected. Next, the particle size can be determined by observing with an optical microscope, scanning electron microscope, etc., and measuring the particle size.
  • the other polymers are not particularly limited as long as they are not polyamides, and examples thereof include polyesters, liquid crystal polyesters, polyphenylene sulfides, polyphenylene ethers, polycarbonates, polyarylates, phenolic resins, epoxy resins, etc.
  • the polyesters are not limited to the following, and examples thereof include polybutylene terephthalate, polytrimethylene terephthalate, polyethylene terephthalate, polyethylene naphthalate, etc.
  • the content of the other polymers is preferably from 1% by mass to 30% by mass, more preferably from 5% by mass to 20% by mass, and even more preferably from 5% by mass to 15% by mass, based on the total amount of polyamide in the polyamide composition.
  • the polyamide composition can have superior heat resistance and releasability.
  • the polyamide composition obtained by the production method of this embodiment may contain other additives commonly used in polyamide compositions, within the range that does not impair the effects of the polyamide composition obtained by the production method of this embodiment.
  • other additives include colorants such as pigments and dyes (including colored masterbatches), flame retardants, fibrillating agents, fluorescent bleaching agents, plasticizers, antioxidants, ultraviolet absorbers, antistatic agents, flow improvers, spreading agents, etc.
  • the content of the other additives varies depending on the type and use of the polyamide composition, and is not particularly limited as long as it is within a range that does not impair the effects of the polyamide composition obtained by the manufacturing method of this embodiment.
  • the method for producing the polyamide composition of the present embodiment is not particularly limited as long as it is a method including a step of melt-kneading the raw material components including the above-mentioned (A) polyamide, (B) phosphorus-based flame retardant, and (C) inorganic filler.
  • a method including a step of melt-kneading the raw material components including the above-mentioned (A) polyamide, (B) phosphorus-based flame retardant, and (C) inorganic filler in an extruder, and setting the extruder temperature to the melting peak temperature Tm of the above-mentioned polyamide composition + 30°C or less is preferred.
  • Methods for melt-kneading raw material components including polyamide include, for example, a method in which (A) polyamide and (D) other raw materials are mixed using a tumbler, Henschel mixer, or the like, and then fed to a melt kneader for kneading, and a method in which (B) phosphorus-based flame retardant and (C) other raw materials including inorganic filler are blended from a side feeder to the above-mentioned (A) polyamide in a molten state using a single-screw or twin-screw extruder.
  • the components constituting the polyamide composition may be fed to the melt kneader by feeding all of the components to the same feed port at once, or by feeding each component through a different feed port.
  • the melt-kneading temperature is preferably about 250°C or more and 350°C or less in terms of the resin temperature.
  • the melt-kneading time is preferably about 0.25 minutes or more and 5 minutes or less.
  • the melt-kneading device is not particularly limited, and for example, a known melt-kneading device such as a single-screw or twin-screw extruder, a Banbury mixer, or a mixing roll can be used.
  • the melt-kneading device is preferably a twin-screw extruder having a screw diameter of 30 mm or more in the same direction, and the ratio (L/D) of the barrel length (L) and the screw diameter length (D) of the twin-screw extruder is preferably 35 or more.
  • the screw rotation speed (N) is preferably 350 rpm or more, and the ratio Q/N of the screw rotation speed (N) and the discharge amount (Q) is preferably 1.14 or less.
  • the phosphorus-based flame retardant (B) and the inorganic filler (C) improve the kneading efficiency, it is preferable to dry-blend the polyamide (A) and then supply it from the upstream supply port of the twin-screw extruder, and supply the phosphorus-based flame retardant (B) and the inorganic filler (C) from the first downstream supply port of the twin-screw extruder.
  • the molded article of the present embodiment is produced by molding the above-mentioned polyamide composition.
  • the molded product of this embodiment uses the polyamide composition described above, and as such has excellent low-temperature impact properties, deflection temperature under load, electrical properties, and flame retardancy.
  • the molded product of this embodiment can be obtained by molding the above-mentioned polyamide composition using a well-known molding method, such as press molding, injection molding, gas-assisted injection molding, welding molding, extrusion molding, blow molding, film molding, blow molding, multi-layer molding, melt spinning, etc.
  • a well-known molding method such as press molding, injection molding, gas-assisted injection molding, welding molding, extrusion molding, blow molding, film molding, blow molding, multi-layer molding, melt spinning, etc.
  • the polyamide composition of the present embodiment can be used in applications where heat resistance, flame retardancy, and electrical properties are important, and can be suitably used for electrical and electronic parts and automotive electrical and electronic parts.
  • the electrical parts can be used as industrial equipment such as office machines, measuring instruments, chassis, internal parts of electrical equipment, power adapters for home appliances, recording media and their drives, sensor equipment, terminal blocks, secondary batteries in the energy and environmental fields, fuel cells, solar cells, solar thermal power generation, geothermal power generation, wind power generation, smart meters, and other electrical and electronic parts used in power transmission equipment, cable terminals, automotive parts, particularly solar power generation module connectors, solar cell junction boxes, and other solar power generation module connection structures, and hybrid and electric automotive parts.
  • B-1 Phosphinic acid flame retardant Aluminum complex salt of diethylphosphinic acid and ethylphosphonic acid (manufactured by Weihaijun Co., Ltd., trade name "MADP8900SP", bulk density 0.59 g/mL, flake-like, collapse strength 35 N)
  • B-2 Phosphinic acid flame retardant Aluminum complex salt of diethylphosphinic acid and ethylphosphonic acid (manufactured by Weihaijun Co., Ltd., trade name "MADP8900BP", bulk density 0.65 g/mL, cylindrical, collapse strength 9N)
  • B-3 Phosphinic acid flame retardant Aluminum complex salt of diethylphosphinic acid and ethylphosphonic acid (manufactured by Weihaijun Co., Ltd., trade name "HR8900", bulk density 0.34 g/mL, powder)
  • B-4 Phosphinic acid flame retardant Aluminum complex salt of diethylphos
  • C-1 Glass fiber (GF) (manufactured by Nippon Electric Glass, product name “ECS03T275H”, average fiber diameter 10 ⁇ m ⁇ , cut length 3 mm)
  • Crystalline polyamide A-1 and amorphous polyamide A-2 obtained by the production methods described below were dried in a nitrogen stream to adjust the moisture content to about 0.2% by mass, and then used as raw materials for polyamide compositions in the examples and comparative examples described below.
  • the internal temperature was raised to 220°C.
  • the autoclave was pressurized to 1.8 MPa.
  • the reaction was continued for 1 hour while gradually removing steam and maintaining the pressure at 1.8 MPa until the internal temperature reached 245°C.
  • the pressure was lowered over 1 hour.
  • the inside of the autoclave was maintained at a reduced pressure of 650 torr (86.66 kPa) for 10 minutes using a vacuum device.
  • the final internal temperature of the polymerization was 265°C.
  • the mixture was then pressurized with nitrogen to form a strand from the lower spinneret (nozzle), cooled with water, cut, and discharged in the form of pellets.
  • the pellets were then dried at 100° C.
  • polyamide A-1 (polyamide 66).
  • amorphous polyamide A-2 (polyamide 6I).
  • Glass transition temperature Tg The glass transition temperature Tg (°C) was measured using a Diamond-DSC manufactured by PERKIN-ELMER in accordance with JIS-K7121. The measurement conditions were as follows: a molten sample obtained by melting the polyamide on a hot stage (EP80 manufactured by Mettler) was quenched with liquid nitrogen and solidified to obtain a measurement sample. The glass transition temperature Tg (°C) was measured using 10 mg of the sample, which was heated in the range from 30°C to 350°C at a heating rate of 20°C/min.
  • B-1 Phosphinic acid flame retardant Aluminum complex salt of diethylphosphinic acid and ethylphosphonic acid (manufactured by Weihaijun Co., Ltd., trade name "MADP8900SP", bulk density 0.59 g/mL, flake-like, collapse strength 35 N)
  • B-2 Phosphinic acid flame retardant Aluminum complex salt of diethylphosphinic acid and ethylphosphonic acid (manufactured by Weihaijun Co., Ltd., product name "MADP8900BS”, bulk density 0.65 g/mL, cylindrical, collapse strength 9 N)
  • B-3 Phosphinic acid flame retardant Aluminum complex salt of diethylphosphinic acid and ethylphosphonic acid (manufactured by Weihaijun Co., Ltd., trade name "HR8900", bulk density 0.34 g/mL, powder)
  • B-4 Phosphinic acid flame retardant Aluminum diethylphosphinic acid flame retardant Aluminum
  • Inorganic filler Inorganic filler: Inorganic filler C-1 (glass fiber (GF) (manufactured by Nippon Electric Glass Co., Ltd., product name "ECS03T275H", average fiber diameter 10 ⁇ m ⁇ , cut length 3 mm))
  • the carbon steel test pieces were taken out from the molten and solidified pellets, and the resin adhering to the carbon steel test pieces was dissolved and removed with toluene.
  • the carbon steel test piece was air-dried, weighed to the nearest 0.1 mg, and divided by the weight of the carbon steel test piece before the corrosion test, which had been measured in advance, to determine the rate of weight loss before and after the test in ppm by mass.
  • test piece was obtained by molding using an injection molding machine (PS40E manufactured by Nissei Plastic Industrial Co., Ltd.) equipped with a mold in which molten resin flows from both ends of the length direction of a shape of 127 mm in length, 12.7 mm in width, and 1.6 mm in thickness, and a weld is formed in the center in the length direction.
  • a tensile test was performed on this molded test piece according to the method conforming to ISO527, except that the chuck distance was 50 mm and the tensile speed was 5 mm/min, and the tensile strength was obtained.
  • the flame retardant grade was evaluated according to the UL94 standard (vertical flame test) to see whether it was V-0, V-1, or V-2. The smaller the grade number, the higher the flame retardancy.
  • NEX50IV manufactured by Nissei Plastics Co., Ltd.
  • the raw material polyamide (A) was dried in a nitrogen stream to adjust the moisture content to approximately 0.2% by mass before being used as a raw material for the polyamide composition.
  • the polyamide composition was manufactured using a twin-screw extruder (Toshiba Machine Co., Ltd., product name "TEM-58SS").
  • the screw of the extruder was provided with three kneading blocks. The first kneading block was provided in the third barrel of the extruder, the second kneading block was provided in the sixth barrel of the extruder, and the third kneading block was provided in the eighth barrel of the extruder.
  • the "kneading block” here refers to a block in which a plurality of screw elements called kneading disks, which have a high kneading effect, are connected in succession.
  • the polymer was discharged in the form of strands from the nozzle at the tip of the extruder, and after the resin temperature was measured, the polymer was cooled with water and cut to obtain pellets of the polyamide composition.
  • the strand-shaped molten mixture extruded from the die head was cooled and pelletized to obtain pellets of the polyamide composition.
  • the pellets of the polyamide composition thus obtained were dried in a nitrogen stream to reduce the moisture content in the polyamide composition to 500 ppm or less.
  • the polyamide composition of this embodiment can provide a polyamide composition with excellent flame retardancy.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Organic Chemistry (AREA)
  • Compositions Of Macromolecular Compounds (AREA)
PCT/JP2024/037627 2023-10-27 2024-10-22 ポリアミド組成物及び成形品 Pending WO2025089285A1 (ja)

Priority Applications (2)

Application Number Priority Date Filing Date Title
CN202480068575.9A CN122095025A (zh) 2023-10-27 2024-10-22 聚酰胺组合物和成型品
JP2025553375A JPWO2025089285A1 (cg-RX-API-DMAC7.html) 2023-10-27 2024-10-22

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2023-185090 2023-10-27
JP2023185090 2023-10-27

Publications (1)

Publication Number Publication Date
WO2025089285A1 true WO2025089285A1 (ja) 2025-05-01

Family

ID=95515601

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2024/037627 Pending WO2025089285A1 (ja) 2023-10-27 2024-10-22 ポリアミド組成物及び成形品

Country Status (3)

Country Link
JP (1) JPWO2025089285A1 (cg-RX-API-DMAC7.html)
CN (1) CN122095025A (cg-RX-API-DMAC7.html)
WO (1) WO2025089285A1 (cg-RX-API-DMAC7.html)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN120484336A (zh) * 2025-06-18 2025-08-15 辽宁金发生物材料有限公司 一种聚合物添加剂及其制备方法和应用

Citations (7)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2010260995A (ja) * 2009-05-11 2010-11-18 Asahi Kasei Chemicals Corp 樹脂組成物及びその製造方法
CN111320781A (zh) * 2020-03-13 2020-06-23 威海海润新材料科技有限公司 一种有机磷化物阻燃剂及其制备和应用
CN115418026A (zh) * 2022-09-16 2022-12-02 威海海润新材料科技有限公司 一种磷系阻燃剂组合物的合成及应用
JP2023504352A (ja) * 2020-11-06 2023-02-03 ジィァンスー リースーデェァ ニュー マテリアル カンパニー リミテッド 二峰性の加熱減量分解特徴を有する亜リン酸アルミニウムベースの複合体並びにその調製及び適用
JP2023504908A (ja) * 2020-01-07 2023-02-07 ウェイハイ ヘレン ニュー-マテアリアル テック カンパニー リミテッド 有機リン化合物難燃剤及びその製造方法と利用
CN116285328A (zh) * 2022-12-30 2023-06-23 上海普利特复合材料股份有限公司 一种高强度、低析出无卤阻燃聚酰胺组合物及其制备方法
WO2023168790A1 (zh) * 2022-03-10 2023-09-14 江苏利思德新材料有限公司 低细粉含量的二乙基次膦酸铝结晶物及其制备方法和应用

Patent Citations (7)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2010260995A (ja) * 2009-05-11 2010-11-18 Asahi Kasei Chemicals Corp 樹脂組成物及びその製造方法
JP2023504908A (ja) * 2020-01-07 2023-02-07 ウェイハイ ヘレン ニュー-マテアリアル テック カンパニー リミテッド 有機リン化合物難燃剤及びその製造方法と利用
CN111320781A (zh) * 2020-03-13 2020-06-23 威海海润新材料科技有限公司 一种有机磷化物阻燃剂及其制备和应用
JP2023504352A (ja) * 2020-11-06 2023-02-03 ジィァンスー リースーデェァ ニュー マテリアル カンパニー リミテッド 二峰性の加熱減量分解特徴を有する亜リン酸アルミニウムベースの複合体並びにその調製及び適用
WO2023168790A1 (zh) * 2022-03-10 2023-09-14 江苏利思德新材料有限公司 低细粉含量的二乙基次膦酸铝结晶物及其制备方法和应用
CN115418026A (zh) * 2022-09-16 2022-12-02 威海海润新材料科技有限公司 一种磷系阻燃剂组合物的合成及应用
CN116285328A (zh) * 2022-12-30 2023-06-23 上海普利特复合材料股份有限公司 一种高强度、低析出无卤阻燃聚酰胺组合物及其制备方法

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN120484336A (zh) * 2025-06-18 2025-08-15 辽宁金发生物材料有限公司 一种聚合物添加剂及其制备方法和应用

Also Published As

Publication number Publication date
CN122095025A (zh) 2026-05-26
JPWO2025089285A1 (cg-RX-API-DMAC7.html) 2025-05-01

Similar Documents

Publication Publication Date Title
KR101530464B1 (ko) 공중합 폴리아미드
TWI472552B (zh) 聚醯胺及聚醯胺組成物
KR20100115796A (ko) 폴리아미드, 폴리아미드 조성물 및 폴리아미드의 제조 방법
JP7280146B2 (ja) ポリアミド組成物及びその製造方法、並びに、成形品
CN110964316B (zh) 聚酰胺组合物、成型品和半芳香族聚酰胺
KR20150013748A (ko) 폴리아미드, 폴리아미드 조성물 및 성형품
JP7812411B2 (ja) ポリアミド組成物及びその製造方法、並びに、成形品
JP7440996B2 (ja) ポリアミド組成物及び成形品
JP6843698B2 (ja) ポリアミド組成物及び成形品
JP7548752B2 (ja) ポリアミド組成物及びその製造方法、並びに、成形品
JP2023028935A (ja) ポリアミド組成物及び成形品
JP7524361B2 (ja) ポリアミド組成物、成形体、及び装置の振動又は音の伝搬を抑制する方法
JP2023072690A (ja) ポリアミド組成物、成形品、及び積層体
JP2024010978A (ja) ポリアミド組成物、及び成形体
JP2023050575A (ja) ポリアミド組成物、成形品、及びポリアミド組成物の製造方法
JP2023157584A (ja) ポリアミド組成物及び成形品
JP2025073909A (ja) ポリアミド組成物、成形品
JP2022051850A (ja) ポリアミド組成物及び成形品
JP5461052B2 (ja) ポリアミド組成物
JP2022044221A (ja) ポリアミド及びポリアミド組成物
CN110527289B (zh) 聚酰胺树脂颗粒及其制造方法以及聚酰胺组合物的制造方法
JP2024167063A (ja) ポリアミド樹脂組成物、成形品、及びポリアミド樹脂組成物の製造方法
WO2025159207A1 (ja) ポリアミド樹脂組成物及び成形体
JP2023105490A (ja) ポリアミド、ポリアミド組成物及び成形品
JP2023086896A (ja) ポリアミド組成物及び成形品

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 24882396

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2025553375

Country of ref document: JP

Kind code of ref document: A

WWE Wipo information: entry into national phase

Ref document number: 2025553375

Country of ref document: JP

NENP Non-entry into the national phase

Ref country code: DE