WO2023282102A1 - コーティング用組成物 - Google Patents
コーティング用組成物 Download PDFInfo
- Publication number
- WO2023282102A1 WO2023282102A1 PCT/JP2022/025465 JP2022025465W WO2023282102A1 WO 2023282102 A1 WO2023282102 A1 WO 2023282102A1 JP 2022025465 W JP2022025465 W JP 2022025465W WO 2023282102 A1 WO2023282102 A1 WO 2023282102A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- metal oxide
- containing metal
- zirconium element
- zirconium
- coating composition
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D183/00—Coating compositions based on macromolecular compounds obtained by reactions forming in the main chain of the macromolecule a linkage containing silicon, with or without sulfur, nitrogen, oxygen, or carbon only; Coating compositions based on derivatives of such polymers
- C09D183/04—Polysiloxanes
-
- G—PHYSICS
- G02—OPTICS
- G02B—OPTICAL ELEMENTS, SYSTEMS OR APPARATUS
- G02B1/00—Optical elements characterised by the material of which they are made; Optical coatings for optical elements
- G02B1/10—Optical coatings produced by application to, or surface treatment of, optical elements
- G02B1/14—Protective coatings, e.g. hard coatings
-
- C—CHEMISTRY; METALLURGY
- C01—INORGANIC CHEMISTRY
- C01G—COMPOUNDS CONTAINING METALS NOT COVERED BY SUBCLASSES C01D OR C01F
- C01G25/00—Compounds of zirconium
- C01G25/02—Oxides
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D183/00—Coating compositions based on macromolecular compounds obtained by reactions forming in the main chain of the macromolecule a linkage containing silicon, with or without sulfur, nitrogen, oxygen, or carbon only; Coating compositions based on derivatives of such polymers
- C09D183/04—Polysiloxanes
- C09D183/06—Polysiloxanes containing silicon bound to oxygen-containing groups
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D7/00—Features of coating compositions, not provided for in group C09D5/00; Processes for incorporating ingredients in coating compositions
- C09D7/40—Additives
- C09D7/60—Additives non-macromolecular
- C09D7/61—Additives non-macromolecular inorganic
-
- C—CHEMISTRY; METALLURGY
- C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
- C09D—COATING COMPOSITIONS, e.g. PAINTS, VARNISHES OR LACQUERS; FILLING PASTES; CHEMICAL PAINT OR INK REMOVERS; INKS; CORRECTING FLUIDS; WOODSTAINS; PASTES OR SOLIDS FOR COLOURING OR PRINTING; USE OF MATERIALS THEREFOR
- C09D7/00—Features of coating compositions, not provided for in group C09D5/00; Processes for incorporating ingredients in coating compositions
- C09D7/40—Additives
- C09D7/66—Additives characterised by particle size
- C09D7/67—Particle size smaller than 100 nm
-
- C—CHEMISTRY; METALLURGY
- C01—INORGANIC CHEMISTRY
- C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- C01P2004/00—Particle morphology
- C01P2004/60—Particles characterised by their size
- C01P2004/64—Nanometer sized, i.e. from 1-100 nanometer
-
- C—CHEMISTRY; METALLURGY
- C01—INORGANIC CHEMISTRY
- C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- C01P2006/00—Physical properties of inorganic compounds
- C01P2006/22—Rheological behaviour as dispersion, e.g. viscosity, sedimentation stability
-
- C—CHEMISTRY; METALLURGY
- C01—INORGANIC CHEMISTRY
- C01P—INDEXING SCHEME RELATING TO STRUCTURAL AND PHYSICAL ASPECTS OF SOLID INORGANIC COMPOUNDS
- C01P2006/00—Physical properties of inorganic compounds
- C01P2006/60—Optical properties, e.g. expressed in CIELAB-values
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
- C08G77/00—Macromolecular compounds obtained by reactions forming a linkage containing silicon with or without sulfur, nitrogen, oxygen or carbon in the main chain of the macromolecule
- C08G77/04—Polysiloxanes
- C08G77/14—Polysiloxanes containing silicon bound to oxygen-containing groups
- C08G77/18—Polysiloxanes containing silicon bound to oxygen-containing groups to alkoxy or aryloxy groups
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08K—Use of inorganic or non-macromolecular organic substances as compounding ingredients
- C08K3/00—Use of inorganic substances as compounding ingredients
- C08K3/18—Oxygen-containing compounds, e.g. metal carbonyls
- C08K3/20—Oxides; Hydroxides
- C08K3/22—Oxides; Hydroxides of metals
- C08K2003/2244—Oxides; Hydroxides of metals of zirconium
Definitions
- the present invention relates to coating compositions. More particularly, it relates to a coating composition useful for lenses such as spectacles.
- plastic lenses have become mainstream for spectacle lenses, and in particular, high-refractive-index lenses are becoming the mainstream. This is due to the increasing demand for corrective eyeglasses due to the increase in visual acuity deterioration associated with the spread of digital devices such as PCs and smartphones, and the demand for light and thin (high refractive index) lenses in the market.
- the background is what is happening.
- plastic lenses if the refractive index of the hard coat film applied to prevent scratches does not match the refractive index of the substrate lens, light interference causes a rainbow pattern called interference fringes. appears and spoils the aesthetic appearance. Therefore, a technique for matching the refractive index of the hard coat film with the refractive index of the lens has been proposed.
- Patent Document 1 proposes, as a composition for improving the refractive index of a hard coat film, fine particles in which iron oxide and silicon oxide are integrally bonded to titanium oxide in the form of a composite oxide or a solid solution. ing.
- a hard coat film using such fine particles has a high refractive index, and can be applied to lenses with various refractive indexes by adjusting the blending amount.
- spectacle lenses having an antireflection film on the upper layer of the hard film have the drawback of being blackened by ultraviolet rays and deteriorating in optical performance.
- Patent Document 2 proposes composite fine particles made of oxides of titanium, silicon, zirconium and/or aluminum. However, when these fine particles are used, the blackening described above does not occur. I had a problem.
- Patent document 3 proposes composite fine particles of rutile-type titanium oxide, zirconium oxide, silicon oxide, and tin oxide. When these fine particles are used, the above weather resistance is improved, but there is a problem that spectacle lenses laminated with an antireflection film turn blue when exposed to ultraviolet rays. As described above, when fine particles mainly composed of titanium oxide are used as a component of the hard coat film, there is a problem of light resistance or weather resistance. Therefore, a technique using zirconium oxide fine particles has been proposed (see, for example, Patent Document 4). In systems using zirconium oxide fine particles, the weather resistance as described above is improved, but the transparency of the coating film is not sufficient, and there is also the problem of the stability over time as a coating liquid.
- JP-A-7-76671 JP-A-8-48940 Japanese Patent Application Laid-Open No. 2006-251760 JP 2009-155541 A
- the present invention has been made in view of the above-mentioned current situation, and an object of the present invention is to provide a coating composition that exhibits excellent stability over time and exhibits excellent transparency when a coating film is formed.
- the present inventors found that by combining a zirconium element-containing metal oxide having a zeta potential value of 30 mV or more measured by a predetermined method and a silane compound, excellent stability over time can be obtained.
- the inventors have found that excellent transparency can be exhibited when a coating film is formed, conceived that the above problems can be solved admirably, and have arrived at the present invention.
- the present invention provides a coating composition containing a zirconium element-containing metal oxide (A) and a silane compound (B), wherein the zirconium element-containing metal oxide (A) is measured by the following method.
- the coating composition has a zeta potential value of 30 mV or more.
- ⁇ Method for measuring zeta potential> A 10% by mass zirconium element-containing metal oxide (A) aqueous dispersion is measured at room temperature (25° C.) by an electrophoretic laser Doppler method.
- the zirconium element-containing metal oxide (A) preferably has an average primary particle size of 1 to 20 nm as measured by a dynamic light scattering method.
- the silane compound (B) has the following general formula (1): R 1 R 2 a Si(OR 3 ) 3-a (1)
- R 1 is an alkyl group having 1 to 3 carbon atoms, a phenyl group, a vinyl group, an organic group having an epoxy group, an organic group having a (meth)acryl group, an organic group having an amino group, or mercapto group
- R 2 represents an alkyl group having 1 to 2 carbon atoms
- R 3 is the same or different and represents an alkyl group having 1 to 3 carbon atoms
- a is 0 or 1
- the content of the zirconium element-containing metal oxide (A) is preferably 4 to 25% by mass with respect to 100% by mass of the coating composition.
- the content of the silane compound (B) is preferably 30 to 260 mol % with respect to 100 mol % of the zirconium element-containing metal oxide (A).
- the coating composition is preferably used for lenses.
- the present invention also provides a lens coated with the above coating composition.
- the coating composition of the present invention has the above-described structure, is excellent in stability over time, and can exhibit excellent transparency when a coating film is formed. Therefore, it is suitable for lenses such as spectacles. can be used.
- the coating composition of the present invention is characterized by containing a zirconium element-containing metal oxide (A) having a zeta potential value of 30 mV or more as measured by the above method.
- A zirconium element-containing metal oxide
- the coating composition of the present invention also has excellent adhesion to lenses, and lenses obtained by coating with this composition have excellent scratch resistance and weather resistance.
- the zeta potential of the zirconium element-containing metal oxide (A) may be 30 mV or higher, preferably 35 mV or higher. Thereby, the effects of the present invention can be exhibited more sufficiently. It is more preferably 40 mV or more, and still more preferably 45 mV or more.
- the zeta potential of the zirconium element-containing metal oxide (A) is preferably 100 mV or less.
- the zirconium element-containing metal oxide (A) is not particularly limited as long as it contains zirconium atoms and oxygen atoms, and may contain elements other than zirconium atoms and oxygen atoms. Other elements include, but are not limited to, at least one stabilizing element selected from aluminum, magnesium, titanium, rare earth elements, and the like. When the zirconium element-containing metal oxide (A) contains the other elements, the thermal stability of the metal oxide (A) is further improved.
- a specific example of the rare earth element is yttrium.
- the content of the other elements in the zirconium element-containing metal oxide (A) is not particularly limited, it is preferably 0 to 20 mol % with respect to 100 mol % of the zirconium element. More preferably 0 to 10 mol %, still more preferably 0 to 5 mol %.
- the average primary particle size of the zirconium element-containing metal oxide (A) measured by a dynamic light scattering method is not particularly limited, but is preferably 1 to 20 nm. It is more preferably 1 to 15 nm, still more preferably 1 to 10 nm.
- the zirconium element-containing metal oxide (A) may be surface-treated with an inorganic compound or an organic compound.
- inorganic compounds include silicon oxide and aluminum oxide.
- organic compounds include silane coupling agents, titanate coupling agents, and phosphate esters.
- silane coupling agent a compound represented by the general formula (1) is preferable.
- the content of the zirconium element-containing metal oxide (A) is preferably 4 to 25% by mass with respect to 100% by mass of the coating composition. Thereby, the effects of the present invention can be exhibited more sufficiently.
- the content of the zirconium element-containing metal oxide (A) is more preferably 8 to 20% by mass.
- the method for producing the zirconium element-containing metal oxide (A) is not particularly limited.
- a method of deflocculating the zirconium hydroxide neutralization coprecipitation method
- a method of adding an acid and an alkali to zirconium hydroxide and then subjecting it to hydrothermal treatment hydrothermal treatment (hydrothermal synthesis method), and the like.
- the method for producing the zirconium element-containing metal oxide (A) preferably includes a neutralization coprecipitation step of adding an alkali to an aqueous solution containing a zirconium salt to form a hydroxide to peptize it, and a neutralization coprecipitation step.
- a preferred method is to perform a hydrothermal step in which an acid is added to the obtained product and a hydrothermal treatment is performed.
- the zirconium salt used in the neutralization coprecipitation step is not particularly limited as long as it contains a zirconium element, but chlorides, oxychlorides, sulfates, nitrates and the like are preferable. More preferred are chlorides and oxychlorides.
- Zirconium compounds used as raw materials for producing a slurry containing a zirconium element-containing compound include hydroxides, hydroxide oxides, chlorides, sulfides, sulfates, nitrates, carbonates, hydrogen carbonates, acetates, phosphoric acid salts, oxalates, butyrates, selenates, iodates, fluorides, oxychlorides and the like.
- oxychlorides, chlorides, sulfates, nitrates, acetates, and the like which are water-soluble zirconium compounds suitable for production, are preferred.
- the zirconium element-containing metal oxide (A) contains an element other than a zirconium atom and an oxygen atom, it is preferable to add a salt of the other element in the neutralization coprecipitation step.
- Salts of other elements include, for example, chlorides, oxychlorides, sulfates, nitrates, acetates, and the like.
- the alkali used in the above neutralization coprecipitation step is not particularly limited, but examples include hydroxides of alkali metals and alkaline earth metals such as sodium hydroxide, potassium hydroxide and calcium hydroxide; ammonia; mentioned. Among them, alkali metal hydroxides such as sodium hydroxide and potassium hydroxide are preferable.
- the amount of alkali used in the neutralization coprecipitation step is not particularly limited, but it is preferably 10 to 1,000 mol % with respect to 100 mol % of the total of the zirconium element and the other elements.
- the acid used in the hydrothermal step is not particularly limited, but inorganic acids such as nitric acid, hydrochloric acid, sulfuric acid; acetic acid, tartaric acid, glutamic acid, malonic acid, maleic acid, trimellitic anhydride, succinic acid, malic acid, glycolic acid , alanine, fumaric acid, oxalic acid, glutaric acid, and formic acid.
- organic acids are preferred, and acetic acid is more preferred.
- the amount of the acid used in the hydrothermal step is not particularly limited, but it is preferably 50 to 1,000 mol % with respect to the total 100 mol % of the zirconium element and the other elements. Thereby, the zirconium element-containing metal oxide (A) having a zeta potential of 30 mV or more can be sufficiently obtained.
- the amount of acid used is more preferably 100 to 500 mol %.
- the hydrothermal temperature in the hydrothermal step is not particularly limited, it is preferably 170 to 230°C. It is more preferably 175 to 220°C.
- the hydrothermal treatment time in the hydrothermal step is not particularly limited, but is preferably 1 to 10 hours. More preferably 1.5 to 6 hours.
- the method for producing the zirconium element-containing metal oxide (A) preferably includes a washing step after the neutralization coprecipitation step and/or the hydrothermal step.
- the washing method in the washing step is not particularly limited, and a commonly used method can be used.
- a washing method such as filtration and washing with water is preferable.
- the zirconium element-containing metal oxide (A) is produced by the above-mentioned production method, it is obtained as an aqueous dispersion, so that it is preferably substituted with an organic solvent when used in the coating composition of the present invention.
- the organic solvent is not particularly limited as long as it is highly miscible with the silane compound (B).
- examples include alcohols such as methanol, ethanol and isopropanol; ketones such as acetone, methyl ethyl ketone and methyl isobutyl ketone; Esters such as ethyl acetate, butyl acetate, ethyl lactate, propylene glycol monoethyl ether acetate; polyhydric alcohols such as ethylene glycol, ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether and their ethers; dioxane, tetrahydrofuran Those having good compatibility with water, such as cyclic ethers such as These can be used singly or in combination.
- Aromatic hydrocarbons such as benzene and toluene which have good compatibility with these organic solvents, can also be used as appropriate.
- lower alcohols having 1 to 3 carbon atoms are desirable.
- the lower alcohols are highly miscible with water and the silane compound (B), and can easily replace the water-dispersed zirconium element-containing metal oxide (A) with the organic dispersed zirconium element-containing metal oxide (A). is.
- lower alcohols having 1 to 3 carbon atoms are less likely to cause environmental load than alcohols having more carbon atoms, and are preferable in that the solvent can be removed at a low temperature during film formation. .
- the coating composition of the present invention contains a silane compound (B).
- the silane compound (B) is not particularly limited, it is preferably a hydrolyzate of an alkoxysilane compound. More preferably the following general formula (1): R 1 R 2 a Si(OR 3 ) 3-a (1)
- R 1 is an alkyl group having 1 to 3 carbon atoms, a phenyl group, a vinyl group, an organic group having an epoxy group, an organic group having a (meth)acryl group, an organic group having an amino group, or mercapto group
- R 2 represents an alkyl group having 1 to 2 carbon atoms
- R 3 is the same or different and represents an alkyl group having 1 to 3 carbon atoms
- a is 0 or 1
- It is a compound represented by These silane compounds are compounds that can be hydrolyzed and have highly reactive silanol groups and also have organic groups.
- organic group having an epoxy group examples include glycidoxyalkyl groups having 3 to 10 carbon atoms such as 3-glycidoxypropyl group and 4-glycidoxybutyl group, 2-(3,4-epoxy cyclohexyl)ethyl group, 3-(3,4-epoxycyclohexyl)propyl group, 3,4-epoxybutyl group, 7,8-epoxyoctyl group and other epoxyalkyl groups having 3 to 10 carbon atoms.
- glycidoxyalkyl groups having 3 to 10 carbon atoms such as 3-glycidoxypropyl group and 4-glycidoxybutyl group, 2-(3,4-epoxy cyclohexyl)ethyl group, 3-(3,4-epoxycyclohexyl)propyl group, 3,4-epoxybutyl group, 7,8-epoxyoctyl group and other epoxyalkyl groups having 3 to 10 carbon atoms.
- a in the general formula (1) is 0 or 1, preferably 0;
- organic group having a (meth)acryl group examples include (meth)acryloxyalkyl groups having 3 to 10 carbon atoms such as methacryloxypropyl and acryloxypropyl.
- organic group having an amino group examples include aminoalkyl groups having 1 to 10 carbon atoms such as aminomethyl group, aminoethyl group and aminopropyl group; An aminoaryl group and the like can be mentioned.
- organic group having a mercapto group examples include mercaptoalkyl groups having 1 to 10 carbon atoms such as mercaptopropyl.
- R 1 is preferably an organic group having an epoxy group.
- Specific examples of the compound represented by the general formula (1) include methyltrimethoxysilane, ethyltriethoxysilane, methyltriethoxysilane, phenyltriethoxysilane, dimethyldimethoxysilane, phenylmethyldimethoxysilane, and vinyltrimethoxysilane.
- vinyltriethoxysilane vinyltris( ⁇ -methoxyethoxy)silane, ⁇ -glycidoxypropyltrimethoxysilane, ⁇ -glycidoxypropyltriethoxysilane, ⁇ -glycidoxypropylmethyldimethoxysilane, ⁇ -glycidoxy Propylmethyldiethoxysilane, ⁇ -(3,4-epoxycyclohexyl)ethyltrimethoxysilane, ⁇ -methacryloxypropyltrimethoxysilane, N- ⁇ (aminoethyl) ⁇ -aminopropyltrimethoxysilane, N- ⁇ (amino ethyl) ⁇ -aminopropylmethyldimethoxysilane, ⁇ -aminopropyltriethoxysilane, N-phenyl- ⁇ -aminopropyltrimethoxysilane, ⁇ -mercaptopropy
- ⁇ -glycidoxypropyltrimethoxysilane As the compound represented by the general formula (1), ⁇ -glycidoxypropyltrimethoxysilane, ⁇ -glycidoxypropyltriethoxysilane, ⁇ -glycidoxypropylmethyldimethoxysilane, and ⁇ -glycidoxypropyl are preferred. They are methyldiethoxysilane, ⁇ -(3,4-epoxycyclohexyl)ethyltrimethoxysilane, and more preferably ⁇ -glycidoxypropyltrimethoxysilane. Moreover, these silane compounds are preferably hydrolyzed or partially hydrolyzed before use.
- hydrolysis in addition to a method of mixing the silane compound and water in the presence of an acid catalyst, hydrolysis is performed after mixing an organic solvent such as alcohol for uniform hydrolysis. Alternatively, hydrolysis may be performed after mixing with the zirconium oxide fine particles.
- Acid catalysts used for hydrolysis include dilute hydrochloric acid, dilute sulfuric acid, phosphoric acid, acetic acid and formic acid, among which dilute hydrochloric acid, acetic acid and formic acid are preferred.
- the organic solvent in addition to alcohols such as methanol, ethanol, isopropanol and butanol, ethylene glycol monomethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether and the like are used. , propylene glycol monomethyl ether are preferred for use.
- the content of the silane compound represented by the general formula (1) in the coating composition is preferably 25 to 75% by weight, and is in the range of 30 to 70% by weight, as a solid content in the resulting hard coat film. is more preferable.
- the content of the silane compound in the hard coat film is 25% by weight or more, it is possible to sufficiently suppress the deterioration of adhesion to the plastic substrate and the primer film, and the zirconium oxide fine particles and other components are hardened. It can be firmly fixed in the coating film, and can sufficiently suppress scratching due to application of strong rubbing stress to the lens for spectacles. If the content of the silane compound in the hard coat film is 75% by weight or less, the refractive index of the hard coat film can be further improved.
- addition of the (di)silane compounds represented by the general formulas (2) and (3) is effective as described above.
- Specific examples of the silane compound represented by formula (2) include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, tetrabutoxysilane and the like.
- the disilane compound represented by the general formula (3) can be synthesized by a conventionally known method, and can be obtained, for example, by addition reaction of diallyl carbonate and trichlorosilane, followed by alkoxylation.
- the total amount of the (di)silane compounds represented by the general formulas (2) and (3) is in the range of 0.05 to 0.3 parts per part of the silane compound represented by the general formula (1). and more preferably 0.1 to 0.25 parts. If the amount of the (di)silane compound represented by the general formulas (2) and (3) is 0.05 parts or more, the scratch resistance of the hard coat film is further improved, and if it is 0.3 parts or less, the hard It is possible to more sufficiently suppress the deterioration of the water resistance of the coat film and the occurrence of cracks during hardening of the hard coat film.
- the content of the silane compound (B) is preferably 30 to 260 mol % with respect to 100 mol % of the zirconium element-containing metal oxide (A). Thereby, the effects of the present invention can be exhibited more sufficiently.
- the content of the silane compound (B) is more preferably 50-215 mol %, still more preferably 70-150 mol %, and particularly preferably 80-110 mol %. Even when the silane compound represented by the general formula (1) and the (di)silane compounds represented by the general formulas (2) and (3) are used in combination, the preferred range of the total amount of these silane compounds is as described above. By using such a formulation, a hard coat film having a refractive index in the range of 1.56 to 1.67 can be produced.
- the coating composition may contain components other than the zirconium element-containing metal oxide (A) and the silane compound (B).
- other components include solvents, curing agents or curing catalysts, surfactants, ultraviolet absorbers, and antioxidants.
- other thermosetting resins such as melamine resin, urea resin, epoxy resin, and phenol resin can be used together for the purpose of improving adhesion and dyeability. It is preferably 0 to 30% by mass with respect to 100% by mass of the coating composition. It is more preferably 0 to 20% by mass, still more preferably 0 to 10% by mass, and particularly preferably 0 to 5% by mass.
- the above other components are not particularly limited, and examples thereof include solvents, curing catalysts, surfactants, dispersants, ultraviolet absorbers, antioxidants, disperse dyes, and the like.
- Examples of the solvent include water and the above-described organic solvents.
- the curing catalyst is not particularly limited, examples include amines, amino acids, metal acetylacetonates, organic acid metal salts, perchloric acids, salts of perchloric acids, acids, inorganic acids, organic acids and metal chlorides. are mentioned. Aluminum chelate, tin chelate and iron chelate are preferred.
- anionic, cationic, nonionic, or amphoteric surfactants can be used as the surfactant, and nonionic surfactants are preferred.
- a benzophenone-based UV absorber a benzotriazole-based UV absorber, a hindered amine-based light stabilizer, and the like can be added for the purpose of improving the light resistance of the hard coat film.
- a benzophenone-based UV absorber a benzotriazole-based UV absorber, a hindered amine-based light stabilizer, and the like can be added for the purpose of improving the light resistance of the hard coat film.
- polyfunctional epoxy resins polyvinyl butyral resins, and the like.
- a coating method for forming the hard coat film is not particularly limited, and known methods such as dipping, spin coating, flow coating, and spraying can be used.
- the hard coat layer applied to the ophthalmic lens surface using such methods is then cured by thermal energy (heat transfer, convection, radiation).
- thermal energy heat transfer, convection, radiation
- the curing conditions for example, in the case of curing in a thermal environment of hot air convection, treatment at an ambient temperature of 80° C. to 130° C. for 1 to 5 hours is preferable.
- aliphatic allyl carbonate-based, polyamide-based, polyurea-based, methacrylate-based, aromatic allyl carbonate-based, polycarbonate-based, polyurethane-based, polythiourethane-based, and episulfide-based resins are commercially available. and these can be preferably used.
- the coating composition of the present invention can be suitably used for coating optical plastics such as lenses.
- the present invention is also a method of coating an optical plastic such as a lens with the above coating composition.
- the present invention is also a method of coating an optical plastic such as a lens with the above coating composition.
- the present invention is also a lens coated with the above coating composition.
- the lens is not particularly limited as long as it is coated with the coating composition, but a primer film is provided on the substrate of the lens, and a hard coat film containing the coating composition is applied to the outer layer. It is preferable to be It is preferable that the lens is further laminated with an antireflection film.
- the lens preferably has a refractive index of 1.55 to 1.70. More preferably 1.56 to 1.67.
- the lens preferably has a haze of 0.5% or less as measured by a haze meter. More preferably, it is 0.3% or less.
- the lens is not particularly limited, it is preferably used for spectacles.
- a form in which the lens is a spectacle lens is one of preferred embodiments of the present invention.
- the physical properties and the like of the obtained zirconium element-containing metal oxide (A) and the coating composition were evaluated by the following procedures.
- Zeta Potential of Zirconium Element-Containing Metal Oxide Particles was measured by an electrophoretic laser Doppler method using SZ-100 (manufactured by Horiba, Ltd.). A portion of the aqueous dispersions obtained in Examples and Comparative Examples was collected, diluted with ion-exchanged water, and adjusted to 20 g of a 10% by mass zirconium element-containing metal oxide (A) aqueous dispersion, which was used as a measurement sample. .
- Example 1 Preparation of aqueous dispersion of zirconium element-containing metal oxide particles having a zeta potential of 30 mV or more /L concentration of sodium hydroxide aqueous solution was prepared.
- a mixed aqueous solution of zirconium oxychloride and yttrium chloride and an aqueous sodium hydroxide solution are simultaneously poured into a precipitation reactor filled with 82 L of pure water in advance, and zirconium oxychloride and yttrium chloride are co-precipitated by simultaneous neutralization, and oxidized.
- a first aqueous slurry of zirconium and yttrium coprecipitate particles was obtained.
- This first aqueous slurry was filtered, washed, and repulped with pure water so that the solid content was 11% by weight in terms of zirconium oxide and yttrium oxide to obtain 60 L of a second aqueous slurry.
- the electrical conductivity of this second aqueous slurry was 70 ⁇ S/cm.
- Add 4.2 kg of acetic acid (1.3 mol parts per 1 mol part of the total amount of zirconium and yttrium in the slurry) to the second aqueous slurry, and hydrothermally treat at 190° C. for 3 hours to obtain clear water. A dispersion was obtained.
- This transparent dispersion is washed with an ultrafiltration membrane, concentrated, and water of zirconium element-containing metal oxide particles having a content of 30% by weight of zirconium element-containing metal oxide particles, which is a solid solution containing 4.8 mol % of yttrium.
- a dispersion was obtained.
- the aqueous dispersion of zirconium element-containing metal oxide particles thus obtained had a total light transmittance of 90% and a viscosity of 6 mPa ⁇ s at a temperature of 25°C. Further, water was removed from the obtained aqueous dispersion of the zirconium element-containing metal oxide particles, and the obtained zirconium element-containing metal oxide particles were dried.
- the average primary particle size of the zirconium element-containing metal oxide particles was 3 nm.
- the dispersed particle diameter D50 of the zirconium element-containing metal oxide particles in the aqueous dispersion of the zirconium element-containing metal oxide particles was 3 nm. Therefore, it was found that almost no aggregation of the zirconium element-containing metal oxide particles occurred in the obtained aqueous dispersion of the zirconium element-containing metal oxide particles. Further, when the zeta potential of the aqueous dispersion of the obtained zirconium element-containing metal oxide particles was measured, it was confirmed to be 60 mV.
- the dispersion medium of the dispersion is replaced from water with methanol, so that the content of the zirconium element-containing metal oxide particles is 30% by weight.
- % of zirconium element-containing metal oxide particles methanol dispersion was obtained.
- the amount of methanol used for dilution was 90 L.
- the methanol dispersion of the zirconium element-containing metal oxide particles thus obtained had a total light transmittance of 90% and a viscosity of 2 mPa ⁇ s at a temperature of 25°C.
- a hard coating composition paint (hard coating liquid) having a refractive index of 1.60.
- the ratio of the zirconium element-containing metal oxide in the hard coating liquid was 11.5% by mass, and the ratio of the hydrolyzate of ⁇ -glycidoxypropyltrimethoxysilane to the zirconium element-containing metal oxide was 106 mol%. .
- (IV) Lens Coating The hard coating liquid prepared in (III) was dropped onto the lens base material, and the coating liquid was made uniform on the lens surface while tilting the lens in all directions. After that, the lens coated with the hard coating liquid was cured in a drier at 120° C. for 3 hours to obtain a lens having a hard coating film.
- Example 2 Preparation of an aqueous dispersion of zirconium element-containing metal oxide particles having a zeta potential of 30 mV or more 53L was prepared.
- the zirconium oxychloride aqueous solution and the sodium hydroxide aqueous solution were simultaneously poured into a precipitation reactor previously filled with 0.74 L of pure water to neutralize the zirconium oxychloride to obtain a slurry of zirconium element-containing metal oxide particles. .
- the resulting slurry was filtered, washed, and repulped in pure water so that the content of zirconium oxide in the slurry was 5.6% by weight to obtain 1 L of slurry.
- the electrical conductivity of this slurry was 258 ⁇ S/cm. 82.2 g of acetic acid (3 mol parts per 1 mol part of zirconium in the slurry) was added to the slurry and hydrothermally treated at 200° C. for 3 hours to obtain a translucent dispersion. This translucent dispersion was washed with an ultrafiltration membrane to obtain a zirconium element-containing metal oxide dispersion C having a zirconium oxide content of 30% by weight. The aqueous dispersion of zirconium element-containing metal oxide particles thus obtained had a total light transmittance of 75% and a viscosity of 4 mPa ⁇ s at a temperature of 25°C.
- the obtained zirconium element-containing metal oxide particles were dried.
- the average primary particle size of the zirconium element-containing metal oxide particles was 8 nm.
- the dispersed particle diameter D50 of the zirconium element-containing metal oxide particles in the aqueous dispersion of the zirconium element-containing metal oxide particles was 8 nm.
- the resulting slurry was filtered, washed, and repulped with pure water so that the solid content of the slurry was 5.6% by weight in terms of zirconium oxide and yttrium oxide to obtain 1 L of slurry.
- the electrical conductivity of this slurry was 235 ⁇ S/cm. 140.8 g of sodium citrate dihydrate (1 mol part per 1 mol part of the total amount of zirconium and yttrium in the slurry) was added to the slurry and hydrothermally treated at 200° C. for 3 hours to form a translucent dispersion. I got the liquid.
- This translucent dispersion is washed with an ultrafiltration membrane and concentrated to obtain an aqueous dispersion of zirconium element-containing metal oxide particles having a zirconium element-containing metal oxide content of 30% by weight, which is a solid solution containing yttrium. rice field.
- the aqueous dispersion of zirconium element-containing metal oxide particles thus obtained had a total light transmittance of 80% and a viscosity of 4 mPa ⁇ s at a temperature of 25°C. Further, water was removed from the obtained aqueous dispersion of the zirconium element-containing metal oxide particles, and the obtained zirconium element-containing metal oxide particles were dried.
- the average primary particle size of the zirconium element-containing metal oxide particles was 6 nm.
- the dispersed particle diameter D50 of the zirconium element-containing metal oxide particles in the aqueous dispersion of the zirconium element-containing metal oxide particles was 6 nm. Therefore, it was found that almost no aggregation of the zirconium element-containing metal oxide particles occurred in the obtained aqueous dispersion of the zirconium element-containing metal oxide particles. Further, when the zeta potential of the aqueous dispersion of the obtained zirconium element-containing metal oxide particles was measured, it was confirmed to be ⁇ 41 mV.
- a hard coating liquid having a refractive index of 1.60 was prepared using an aqueous dispersion of zirconia particles having a particle size of 10 nm (zirconium oxide concentration of 20 wt% manufactured by Daiichi Kigenso Co., Ltd.). Using the obtained hard coating liquid, a lens having a hard coating film was obtained in the same manner as in Example 1 (IV). The zeta potential of the zirconia aqueous dispersion was measured and found to be -61 mV.
- Table 1 shows the measurement results of the physical properties of the zirconia sols, the hard coating liquids, and the lenses having hard coating films obtained in Examples 1 and 2 and Comparative Examples 1 to 3.
- a lens having a low haze hard coating film can be obtained by using a zirconium element-containing metal oxide having a zeta potential (surface charge) of 30 mV or more.
- a zirconium element-containing metal oxide having a zeta potential surface charge of 30 mV or more.
- the physical properties of the hard coating liquid immediately after preparation are comparable to those in Examples 1 and 2, but the stability over time is inferior.
- the use of a zirconium element-containing metal oxide having a potential of 30 mV or higher improves the stability of transparency and viscosity over time.
- the coating compositions of Examples 1 and 2 are excellent in adhesion to lenses, and the lenses obtained by coating these are excellent in scratch resistance and weather resistance.
Landscapes
- Chemical & Material Sciences (AREA)
- Engineering & Computer Science (AREA)
- Organic Chemistry (AREA)
- Physics & Mathematics (AREA)
- Materials Engineering (AREA)
- Life Sciences & Earth Sciences (AREA)
- Wood Science & Technology (AREA)
- General Physics & Mathematics (AREA)
- Optics & Photonics (AREA)
- Inorganic Chemistry (AREA)
- Nanotechnology (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Paints Or Removers (AREA)
Priority Applications (5)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| US18/577,096 US20240345292A1 (en) | 2021-07-06 | 2022-06-27 | Coating composition |
| KR1020247000265A KR20240032015A (ko) | 2021-07-06 | 2022-06-27 | 코팅용 조성물 |
| CN202280047709.XA CN117651745A (zh) | 2021-07-06 | 2022-06-27 | 涂覆用组合物 |
| EP22837519.2A EP4368679A4 (en) | 2021-07-06 | 2022-06-27 | COATING COMPOSITION |
| JP2023533539A JPWO2023282102A1 (cg-RX-API-DMAC7.html) | 2021-07-06 | 2022-06-27 |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2021112226 | 2021-07-06 | ||
| JP2021-112226 | 2021-07-06 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2023282102A1 true WO2023282102A1 (ja) | 2023-01-12 |
Family
ID=84801055
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2022/025465 Ceased WO2023282102A1 (ja) | 2021-07-06 | 2022-06-27 | コーティング用組成物 |
Country Status (7)
| Country | Link |
|---|---|
| US (1) | US20240345292A1 (cg-RX-API-DMAC7.html) |
| EP (1) | EP4368679A4 (cg-RX-API-DMAC7.html) |
| JP (1) | JPWO2023282102A1 (cg-RX-API-DMAC7.html) |
| KR (1) | KR20240032015A (cg-RX-API-DMAC7.html) |
| CN (1) | CN117651745A (cg-RX-API-DMAC7.html) |
| TW (1) | TW202311444A (cg-RX-API-DMAC7.html) |
| WO (1) | WO2023282102A1 (cg-RX-API-DMAC7.html) |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO2025115735A1 (ja) * | 2023-11-28 | 2025-06-05 | 堺化学工業株式会社 | プライマー層形成用組成物 |
Citations (6)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH0776671A (ja) | 1991-06-25 | 1995-03-20 | Ito Kogaku Kogyo Kk | 光学プラスチック成形品用塗料組成物 |
| JPH0848940A (ja) | 1994-04-21 | 1996-02-20 | Seiko Epson Corp | 被膜形成用塗布液および合成樹脂製レンズ |
| JP2006251760A (ja) | 2005-02-08 | 2006-09-21 | Seiko Epson Corp | 光学部品およびその製造方法 |
| JP2009155541A (ja) | 2007-12-27 | 2009-07-16 | Ito Kogaku Kogyo Kk | ハードコート組成物 |
| JP2015507043A (ja) * | 2011-12-30 | 2015-03-05 | エシロール アンテルナシオナル (コンパニー ジェネラル ドプティック) | ジルコニア粒子のコロイド懸濁液を含んでなる、光学物品用コーティング |
| JP2016501825A (ja) * | 2012-12-26 | 2016-01-21 | エシロール アンテルナシオナル (コンパニー ジェネラル ドプティック) | ジルコニアコロイドの作製方法 |
Family Cites Families (3)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| EP2142478B1 (fr) * | 2007-04-04 | 2011-05-25 | Essilor International (Compagnie Générale D'Optique) | Procede de preparation d'une solution colloïdale de zircone |
| CN100560779C (zh) * | 2008-03-31 | 2009-11-18 | 中国地质大学(武汉) | 一种热喷涂用纳米结构钇稳定球形氧化锆粉末的制备方法 |
| CN103702940B (zh) * | 2011-07-12 | 2015-06-24 | 埃西勒国际通用光学公司 | 用于制备氧化锆胶体的方法 |
-
2022
- 2022-06-27 US US18/577,096 patent/US20240345292A1/en active Pending
- 2022-06-27 JP JP2023533539A patent/JPWO2023282102A1/ja active Pending
- 2022-06-27 CN CN202280047709.XA patent/CN117651745A/zh active Pending
- 2022-06-27 KR KR1020247000265A patent/KR20240032015A/ko active Pending
- 2022-06-27 WO PCT/JP2022/025465 patent/WO2023282102A1/ja not_active Ceased
- 2022-06-27 EP EP22837519.2A patent/EP4368679A4/en active Pending
- 2022-06-28 TW TW111124048A patent/TW202311444A/zh unknown
Patent Citations (7)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JPH0776671A (ja) | 1991-06-25 | 1995-03-20 | Ito Kogaku Kogyo Kk | 光学プラスチック成形品用塗料組成物 |
| JPH0848940A (ja) | 1994-04-21 | 1996-02-20 | Seiko Epson Corp | 被膜形成用塗布液および合成樹脂製レンズ |
| JP2006251760A (ja) | 2005-02-08 | 2006-09-21 | Seiko Epson Corp | 光学部品およびその製造方法 |
| JP2009155541A (ja) | 2007-12-27 | 2009-07-16 | Ito Kogaku Kogyo Kk | ハードコート組成物 |
| JP5196993B2 (ja) | 2007-12-27 | 2013-05-15 | 伊藤光学工業株式会社 | ハードコート組成物 |
| JP2015507043A (ja) * | 2011-12-30 | 2015-03-05 | エシロール アンテルナシオナル (コンパニー ジェネラル ドプティック) | ジルコニア粒子のコロイド懸濁液を含んでなる、光学物品用コーティング |
| JP2016501825A (ja) * | 2012-12-26 | 2016-01-21 | エシロール アンテルナシオナル (コンパニー ジェネラル ドプティック) | ジルコニアコロイドの作製方法 |
Non-Patent Citations (1)
| Title |
|---|
| See also references of EP4368679A4 |
Cited By (1)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO2025115735A1 (ja) * | 2023-11-28 | 2025-06-05 | 堺化学工業株式会社 | プライマー層形成用組成物 |
Also Published As
| Publication number | Publication date |
|---|---|
| EP4368679A4 (en) | 2025-12-24 |
| TW202311444A (zh) | 2023-03-16 |
| EP4368679A1 (en) | 2024-05-15 |
| JPWO2023282102A1 (cg-RX-API-DMAC7.html) | 2023-01-12 |
| KR20240032015A (ko) | 2024-03-08 |
| CN117651745A (zh) | 2024-03-05 |
| US20240345292A1 (en) | 2024-10-17 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP5127458B2 (ja) | ハードコート層形成用組成物および光学レンズ | |
| CN103717535B (zh) | 含有二氧化硅-二氧化锡复合氧化物被覆二氧化钛的金属氧化物粒子 | |
| KR20100076000A (ko) | 금속산화물 복합졸, 코팅 조성물 및 광학 부재 | |
| KR20100075999A (ko) | 변성 금속산화물 복합 졸, 코팅조성물 및 광학부재 | |
| EP1568659B1 (en) | Modified stannic oxide sol, stannic oxide-zirconium oxide composite sol, coating composition and optical member | |
| WO2019117088A1 (ja) | 窒素含有環を含むシラン化合物を含むコーティング組成物 | |
| WO2019117086A1 (ja) | 窒素含有環を含むシラン化合物で被覆された無機酸化物粒子、及びコーティング組成物 | |
| JP2011136490A (ja) | ハードコート膜付基材およびハードコート膜形成用塗布液 | |
| JP2009162848A (ja) | 合成樹脂製レンズ用透明被膜形成用塗布液および合成樹脂製レンズ | |
| EP3101075B1 (en) | Coating composition and optical member | |
| CA2178892A1 (en) | Hydrated zinc stannate sols, coating compositions and optical elements | |
| JP4288432B2 (ja) | コーティング組成物及び光学部材 | |
| JP5713668B2 (ja) | ハードコート層膜形成用塗料組成物 | |
| WO2005093465A1 (ja) | 反射防止膜を有する光学部材 | |
| EP2796513A1 (en) | Oligomer-modified fine particles, method for producing same, and coating material | |
| JP2009227500A (ja) | 透明酸化チタンオルガノゾルおよびそれを配合したコーティング組成物,光学基材 | |
| JP6253484B2 (ja) | 塗料組成物、ハードコート層およびハードコート層付き光学基材ならびにこれらの製造方法 | |
| EP4368679A1 (en) | Coating composition | |
| JP4510489B2 (ja) | コーティング組成物の製造方法 | |
| JP4287534B2 (ja) | コーティング組成物 | |
| KR102191949B1 (ko) | 안경렌즈용 하드코팅 조성물 | |
| JP5432430B2 (ja) | 透明被膜形成用塗布液および透明被膜付基材 | |
| JPWO2005088352A1 (ja) | プラスチックレンズの製造方法 | |
| JP7805185B2 (ja) | 塗料組成物 | |
| JP5000528B2 (ja) | コーティング組成物及び眼鏡用プラスチックレンズ |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 22837519 Country of ref document: EP Kind code of ref document: A1 |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 2023533539 Country of ref document: JP |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 202280047709.X Country of ref document: CN |
|
| WWE | Wipo information: entry into national phase |
Ref document number: 2022837519 Country of ref document: EP |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| ENP | Entry into the national phase |
Ref document number: 2022837519 Country of ref document: EP Effective date: 20240206 |